Coated cutting tool

The coated cutting tool with a controlled layered structure addresses the challenges of fracture and wear resistance, offering improved durability and extended tool life through optimized layer orientations and thicknesses.

JP2024139281AActive Publication Date: 2024-10-09TUNGALOY CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023050153
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Conventional coated cutting tools face challenges in improving fracture resistance, wear resistance, and tool life due to insufficient thermal shock resistance and crack propagation during high-speed cutting processes, particularly with increased loads and stronger workpiece materials.

Method used

A coated cutting tool configuration featuring a base material with a specific layered structure, including a lower α-Al2O3 layer, a middle Ti compound layer, and an upper α-Al2O3 layer, where the orientations and thicknesses of these layers are controlled to enhance adhesion and resistance to chipping, wear, and thermal shock.

Benefits of technology

The improved coated cutting tool exhibits enhanced fracture resistance, wear resistance, and extended tool life by suppressing peeling, crater wear, and crack propagation, thereby increasing durability in demanding cutting conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139281000001_ABST
    Figure 2024139281000001_ABST
Patent Text Reader

Abstract

To provide a coated cutting tool which has improved defect resistance and wear resistance, and a long tool life.SOLUTION: A coated cutting tool contains a base material and a coating layer formed on a surface of the base material. The coating layer contains a lower layer, a lower α type Al2O3 layer, an intermediate layer and an upper α type Al2O3 layer in this order toward the surface of the coating layer from the base material side. The lower layer contains Ti compound layer comprising Ti compound of Ti, and at least one element selected from a group comprising C, N, O and B, and an average thickness of the lower layer falls within a specific range. The lower α type Al2O3 layer has an average thickness T1 which falls within a specific range, and satisfies conditions represented by specific formulae 1 and 2. The intermediate layer contains one or more layers of Ti compound layer comprising Ti compound of Ti and at least one element selected from a group comprising C, N, O and B, and has an average thickness which falls within a specific range. The upper α type Al2O3 layer has an average thickness T2 which falls within a specific range, and satisfies conditions represented by specific formula 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated cutting tool. [Background technology]

[0002] It is well known that coated cutting tools, which are formed by depositing a coating layer with a total thickness of 3 to 20 μm by chemical vapor deposition on the surface of a substrate made of cemented carbide or the like, are used for cutting steel, cast iron, etc. As the coating layer, for example, a coating layer consisting of a single layer or a multilayer of two or more types selected from the group consisting of Ti carbides, nitrides, carbonitrides, carbonates, and carbonitrides, and aluminum oxide (Al2O3) is known.

[0003] For example, Patent Document 1 discloses a surface-coated cutting tool having a substrate and a coating formed on the substrate, the coating including an α-Al2O3 layer including a plurality of α-Al2O3 crystal grains, the α-Al2O3 layer including a lower layer portion disposed on the substrate side, an intermediate portion disposed on the lower layer portion, and an upper layer portion disposed on the intermediate portion, and the lower layer portion is characterized in that, in crystal orientation mapping of a cross-sectional polished surface of the α-Al2O3 layer using an electron backscatter diffraction device, the area ratio of (001)-oriented α-Al2O3 crystal grains is 1 / 1000. has been proposed a surface-coated cutting tool in which the area ratio of (001) oriented α-Al2O3 crystal grains in crystal orientation mapping is less than 35%, in the middle portion the area ratio of (001) oriented α-Al2O3 crystal grains is 35% or more, and in the upper layer portion the area ratio of (001) oriented α-Al2O3 crystal grains is less than 35% in crystal orientation mapping, the thickness of the α-Al2O3 layer is 4 to 18 μm, the thickness of the middle portion is 50% or more of the thickness of the α-Al2O3 layer, and the thicknesses of the lower layer and upper layer are both 1 μm or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 061058 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent cutting processes, the trend toward higher speeds, higher feed rates, and deeper cuts has become more prominent. In addition, the strength of work materials has increased, and it is therefore necessary to improve the chipping resistance and wear resistance of tools. In particular, in recent years, cutting processes in which a load acts on coated cutting tools, such as high-speed cutting of steel, have become more common. The coated cutting tool described in Patent Document 1 has a low ratio of (110) orientation in the upper α-Al2O3 layer, and is insufficient in thermal shock resistance, leaving room for improvement in chipping resistance. In addition, the coated cutting tool described in Patent Document 1 does not control the direction of (110) orientation of the upper α-Al2O3 layer relative to the (001)-oriented middle α-Al2O3 layer, and is therefore insufficient in suppressing the occurrence and growth of cracks during cutting, leaving room for improvement in chipping resistance.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a coated cutting tool having improved chipping resistance and wear resistance and a long tool life. [Means for solving the problem]

[0007] As a result of extensive research, the inventors discovered that by giving a coated cutting tool a specific configuration, it is possible to improve its chipping resistance and wear resistance, and as a result, to extend the tool life of the coated cutting tool, which led to the completion of the present invention.

[0008] That is, the gist of the present invention is as follows. [1] A coated cutting tool comprising a substrate and a coating layer formed on a surface of the substrate, the coating layer includes, in this order from the substrate side toward the surface of the coating layer, a lower layer, a lower α-Al2O3 layer, an intermediate layer, and an upper α-Al2O3 layer; the lower layer includes one or more Ti compound layers each comprising a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; The average thickness of the lower layer is 3.00 μm or more and 15.00 μm or less, the average thickness T1 of the lower α-Al2O3 layer is 2.00 μm or more and 15.00 μm or less, The lower α-AlO layer satisfies the condition represented by the following formula (1), 60≦RSA<100 (1) (In formula (1), RSA is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the misorientation A, which is the angle between the normal to the surface of the substrate and the normal to the (001) plane of the particles in the lower α-AlO layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the lower α-AlO layer in a direction perpendicular to the surface of the substrate is taken as 100 area %).) In the lower α-AlO layer, the condition represented by the following formula (2) is satisfied, 15≦average angle β≦45 (2) (In formula (2), the average angle β (degrees) is expressed by the following formula (2-1).)

[0009]

number

[0010] (In formula (2-1), L n represents the length (μm) of the nth line segment from the left in an observation field including a cross section of the lower α-Al2O3 layer in a direction perpendicular to the surface of the substrate, among the line segments created by identifying the lowest point of each identified concave portion and the highest point of each convex portion on the surface of the lower α-Al2O3 layer opposite to the substrate, and connecting the identified lowest point of each concave portion with the highest point of the convex portion adjacent to the lowest point of the concave portion with a straight line, and β n represents the n-th angle (degrees) from the left of the observation field of view among the angles formed by each of the created line segments and a straight line parallel to the substrate surface. However, the region of the observation field of view is each (L n ×cosβ n ) is an area in which the total length of the the intermediate layer includes one or more Ti compound layers each comprising a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; The average thickness of the intermediate layer is 0.05 μm or more and 1.00 μm or less, the average thickness T2 of the upper α-Al2O3 layer is 0.50 μm or more and 5.00 μm or less, In the upper α-type Al2O3 layer, the condition represented by the following formula (3) is satisfied: 50 <RSB<100 (3) (In formula (3), RSB is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the orientation misorientation B, which is the angle between the normal to the line segment created when determining the average angle β (degrees) and the normal to the (110) plane of the particles in the upper α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the upper α-Al2O3 layer in a direction perpendicular to the surface of the base material is taken as 100 area %. However, the orientation misorientation B is determined for each region divided by dividing the upper α-Al2O3 layer by each normal to the surface of the base material that passes through each of the specified lowest points of the concave portions and each of the specified highest points of the convex portions in the observation field for determining the average angle β (degrees).) Coated cutting tools. [2] in the lower α-Al2O3 layer, an average particle size of particles in a direction parallel to a surface of the substrate at a position 0.2 μm toward the substrate from the lowest point located closest to the substrate among the lowest points of the individual recesses on a surface of the lower α-Al2O3 layer opposite to the substrate in an observation field for determining the average angle β (degrees) is 0.3 μm or more and 2.0 μm or less. [1] A coated cutting tool according to the present invention. [3] a ratio (T1 / T2) of an average thickness T1 of the lower α-Al2O3 layer to an average thickness T2 of the upper α-Al2O3 layer is 1.0 or more and 12.0 or less; A coated cutting tool according to [1] or [2]. [4] The average thickness of the coating layer is 8.00 μm or more and 25.00 μm or less. The coated cutting tool according to any one of [1] to [3]. [5] The substrate is a cemented carbide, a cermet, a ceramic, or a cubic boron nitride sintered body; The coated cutting tool according to any one of [1] to [4]. Effect of the Invention

[0011] According to the present invention, it is possible to provide a coated cutting tool having improved chipping resistance and wear resistance and a long tool life. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram showing an example of a coated cutting tool of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] A detailed description will be given below of an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment"); however, the present invention is not limited to the present embodiment. Various modifications of the present invention are possible without departing from the gist of the present invention. In the drawings, the same elements are given the same reference numerals, and duplicated explanations will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.

[0014] [Coated cutting tools] The coated cutting tool of the present embodiment is a coated cutting tool including a substrate and a coating layer formed on the surface of the substrate, the coating layer including, from the substrate side toward the surface of the coating layer, a lower layer, a lower α-Al2O3 layer, an intermediate layer, and an upper α-Al2O3 layer, in this order, the lower layer including one or more Ti compound layers including a Ti compound with Ti and at least one element selected from the group consisting of C, N, O, and B, the lower layer having an average thickness of 3.00 μm or more and 15.00 μm or less, the lower α-Al2O3 layer having an average thickness T1 of 2.00 μm or more and 15.00 μm or less, In the lower α-type Al2O3 layer, the condition represented by the following formula (1) is satisfied, 60≦RSA<100 (1) (In formula (1), RSA is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the misorientation A, which is the angle between the normal to the surface of the substrate and the normal to the (001) plane of the particles in the lower α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the lower α-Al2O3 layer perpendicular to the surface of the substrate is taken as 100 area %).) In the lower α-type Al2O3 layer, the condition represented by the following formula (2) is satisfied, 15≦average angle β≦45 (2) (In formula (2), the average angle β (degrees) is expressed by the following formula (2-1).)

[0015]

number

[0016] (In formula (2-1), L n represents the length (μm) of the nth line segment from the left in the observation field of view, which is created by identifying the lowest point of each concave portion and the highest point of each convex portion on the surface of the lower α-AlO layer opposite the substrate in an observation field of view including a cross section of the lower α-AlO layer in a direction perpendicular to the surface of the substrate, and connecting the lowest point of each identified concave portion with the highest point of the convex portion adjacent to the lowest point of the concave portion with a straight line; β n represents the n-th angle (degrees) from the left of the observation field of view among the angles formed by each line segment and a straight line parallel to the substrate surface. However, the observation field of view is the area of ​​each (L n ×cosβ n ) is an area in which the total length of the the intermediate layer includes one or more Ti compound layers each composed of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B, the intermediate layer has an average thickness of 0.05 μm or more and 1.00 μm or less, and the upper α-type Al2O3 layer has an average thickness T2 of 0.50 μm or more and 5.00 μm or less, In the upper α-type Al2O3 layer, the condition expressed by the following formula (3) is satisfied. 50 <RSB<100 (3) (In formula (3), RSB is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the misorientation B, which is the angle between the normal to the line segment created when determining the average angle β (degrees) and the normal to the (110) plane of the particles in the upper α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the upper α-Al2O3 layer in the direction perpendicular to the surface of the substrate is taken as 100 area %. However, the misorientation B is determined for each region separated by dividing the upper α-Al2O3 layer by the normals to the substrate surface that pass through the identified lowest points of the concave portions and the highest points of the convex portions in the observation field for determining the average angle β (degrees).)

[0017] By configuring the coated cutting tool of this embodiment as described above, it is possible to improve the fracture resistance and wear resistance, and as a result, the tool life can be extended. The reasons why such a coated cutting tool has excellent fracture resistance and wear resistance are not clear in detail, but are presumed to be as follows, although the reasons are not limited to the following. The coated cutting tool of this embodiment has excellent wear resistance and plastic deformation resistance because the average thickness of the lower layer is 3.00 μm or more, and has excellent chipping resistance and defect resistance because the average thickness of the lower layer is 15.00 μm or less, which suppresses peeling of the coating layer. The coated cutting tool of this embodiment has excellent wear resistance and plastic deformation resistance because the average thickness T1 of the lower α-Al2O3 layer is 2.00 μm or more, and has excellent chipping resistance and defect resistance because the average thickness T1 of the lower α-Al2O3 layer is 15.00 μm or less, which suppresses peeling of the coating layer. The coated cutting tool of this embodiment has excellent wear resistance and plastic deformation resistance because the RSA is 60 area % or more in the lower α-Al2O3 layer, which suppresses the progress of crater wear, and has excellent wear resistance and plastic deformation resistance because the RSA is less than 100 area %, which makes it easy to form the lower α-Al2O3 layer. In addition, in the coated cutting tool of this embodiment, the lower α-type Al2O3 layer has an average angle β of 15 degrees or more, which improves the adhesion between the lower α-type Al2O3 layer and the upper α-type Al2O3 layer via the intermediate layer, and therefore has excellent chipping resistance and fracture resistance, and the average angle β is 45 degrees or less, which reduces the surface unevenness of the coating layer and reduces the cutting resistance, thereby providing excellent wear resistance and fracture resistance. In addition, in the coated cutting tool of this embodiment, the lower α-type Al2O3 layer has an average angle β in the range of 15 degrees or more and 45 degrees or less, which suppresses the growth of cracks during cutting, thereby improving fracture resistance. In addition, in the coated cutting tool of this embodiment, the average thickness of the intermediate layer is 0.05 μm or more and 1.00 μm or less, which makes it easy to set the RSB value within a predetermined range. In addition, in the coated cutting tool of this embodiment, since the average thickness T2 of the upper α-Al2O3 layer is 0.50 μm or more, the thermal shock resistance is improved and thus the fracture resistance is improved, and since the average thickness T2 of the upper α-Al2O3 layer is 5.00 μm or less, peeling of the coating layer is suppressed, and the coated cutting tool of this embodiment has excellent chipping resistance and fracture resistance. In addition, since the upper α-Al2O3 layer has RSB of more than 50 area %, the thermal shock resistance is improved and thus the fracture resistance is improved, and since RSB is less than 100 area %, the upper α-Al2O3 layer can be easily formed. The combined effects described above result in the coated cutting tool of this embodiment having improved chipping resistance and wear resistance and a long tool life.

[0018] In general, in the prior art, for example, in a single α-type Al2O3 layer, the lower side is oriented to the (001) plane and the upper side is oriented to the (110) plane (this structure is also referred to as "structure A" below), as in Patent Document 1. In this case, it tends to be difficult to increase the ratio of orientation on either or both of the lower and upper sides. In view of the above circumstances, this embodiment has a configuration in which an intermediate layer including a Ti compound layer is formed between the lower α-Al2O3 layer and the upper α-Al2O3 layer (hereinafter, this configuration is also referred to as "configuration B") in order to simultaneously provide a lower α-Al2O3 layer oriented in the (001) plane so that RSA falls within a specific range, and an upper α-Al2O3 layer oriented in the (110) plane so that RSB falls within a specific range, as described above. It is estimated that by forming the intermediate layer in this manner, the coated cutting tool of this embodiment can provide the effects of both an α-Al2O3 layer oriented in the (001) plane, which has excellent wear resistance, and an α-Al2O3 layer oriented in the (110) plane, which has excellent fracture resistance. Furthermore, the present inventors found that the adhesion between the lower and upper sides of the α-Al2O3 layer is improved by controlling the surface unevenness of the lower α-Al2O3 layer in structure B. That is, the inventors found that the fracture resistance is further improved by controlling the "average angle β (degrees)" of the lower α-Al2O3 layer in structure B to a range of 15 degrees or more and 45 degrees or less (this structure is hereinafter also referred to as "structure C"), and thus completed the present invention.

[0019] 1 is a schematic cross-sectional view partially illustrating an example of a coated cutting tool according to this embodiment. The coated cutting tool 7 has a substrate 1 and a coating layer 6 formed on the surface of the substrate 1. In the coating layer 6, a lower layer 2, a lower α-Al2O3 layer 3, an intermediate layer 4, and an upper α-Al2O3 layer 5 are laminated in this order from the substrate 1 side upwards.

[0020] The substrate in this embodiment is not particularly limited as long as it can be used as a substrate for a coated cutting tool. Examples of such substrates include cemented carbide, cermet, ceramics, and cubic boron nitride sintered body. Among these, it is preferable that the substrate is a cemented carbide. By using such a substrate, the coated cutting tool tends to have excellent chipping resistance and wear resistance.

[0021] In this embodiment, the coating layer includes, from the substrate side toward the surface of the coating layer, a lower layer, a lower α-Al2O3 layer, an intermediate layer, and an upper α-Al2O3 layer, in this order, and may also include an outer layer as necessary. The average thickness of the coating layer is not particularly limited, but is preferably 8.00 μm or more and 25.00 μm or less. When the average thickness of the coating layer is 8.00 μm or more, the wear resistance and plastic deformation resistance tend to be excellent, and when the average thickness is 25.00 μm or less, the adhesion of the coating layer is improved, and the chipping resistance and defect resistance tend to be excellent. From the same viewpoint, the average thickness of the coating layer is more preferably 8.50 μm or more and 24.60 μm or less, and even more preferably 15.40 μm or more and 21.30 μm or less.

[0022] Bottom Layer In this embodiment, the lower layer includes one or more Ti compound layers made of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B. The coated cutting tool has the above-mentioned lower layer between the substrate and the lower α-Al2O3 layer, thereby improving adhesion and wear resistance.

[0023] The Ti compound layer in the lower layer is not particularly limited, but may be, for example, a TiC layer made of TiC (hereinafter, simply referred to as "TiC layer"), a TiN layer made of TiN (hereinafter, simply referred to as "TiN layer"), a TiCN layer made of TiCN (hereinafter, simply referred to as "TiCN layer"), a TiCO layer made of TiCO (hereinafter, simply referred to as "TiCO layer"), a TiCNO layer made of TiCNO (hereinafter, simply referred to as "TiCNO layer"), a TiON layer made of TiON (hereinafter, simply referred to as "TiON layer"), and a TiB2 layer made of TiB2 (hereinafter, simply referred to as "TiB2 layer"). From the viewpoint of more effectively and reliably achieving the effects of the present invention, it is preferable that the Ti compound layer in the lower layer includes a TiN layer, a TiCN layer, a TiCO layer, and / or a TiCNO layer.

[0024] The lower layer may be composed of one layer or may be composed of multiple layers (for example, two or three layers). From the viewpoint of more effectively and reliably achieving the effects of the present invention, it is preferable that it is composed of multiple layers, more preferably composed of two or more layers, even more preferably composed of three or more layers, and even more preferably composed of three layers. When the lower layer is composed of three layers, it may have a TiC layer or TiN layer as a first layer on the surface of the base material, a TiCN layer as a second layer on the surface of the first layer, and a TiCNO layer or TiCO layer as a third layer on the surface of the second layer. Among these, it is preferable that the lower layer has a TiN layer as a first layer on the surface of the base material, a TiCN layer as a second layer on the surface of the first layer, and a TiCNO layer or TiCO layer as a third layer on the surface of the second layer.

[0025] In this embodiment, the average thickness of the lower layer is 3.00 μm or more and 15.00 μm or less. When the average thickness of the lower layer is 3.00 μm or more, the wear resistance and plastic deformation resistance are excellent, and when the average thickness of the lower layer is 15.00 μm or less, peeling of the coating layer is suppressed, and chipping resistance and defect resistance are excellent. From the same viewpoint, the average thickness of the lower layer is preferably 3.20 μm or more and 14.80 μm or less, and more preferably 4.50 μm or more and 14.30 μm or less.

[0026] The average thickness of the lower layer is measured by the following method. Among the lowest points of the recesses and the highest points of the protrusions on the surface of the lower α-type Al2O3 layer opposite to the substrate, which are specified in the method for measuring the average angle β, three lowest points of the recesses having a smallest shortest distance to the substrate surface are specified in order from the side with the smallest shortest distance, and three highest points of the protrusions having a largeest shortest distance to the substrate surface are specified in order from the side with the largest shortest distance. A normal line to the substrate surface passing through the specified six points is drawn, and the arithmetic mean of the lengths of these normal lines crossing the lower layer is taken as the average thickness of the lower layer. In the present embodiment, the average thickness of each layer is determined by specifying three lowest points of the recesses having a smallest shortest distance to the substrate surface in order from the side with the smallest shortest distance, and three highest points of the protrusions having a largeest shortest distance to the substrate surface in order from the side with the largest shortest distance, as in the above method, and using the specified total of six points. In other words, a normal line to the substrate surface passing through the specified total of six points is drawn, and the arithmetic mean of the lengths of these normal lines crossing each layer is taken as the average thickness of each layer. More precisely, the above-mentioned "normal line to the substrate surface" refers to a normal line to a straight line that is approximately parallel to the substrate surface in the method for measuring the average angle β.

[0027] When the lower layer is formed of the first to third layers as described above, the average thickness of the first layer formed on the surface of the substrate is preferably 0.10 μm or more and 1.00 μm or less from the viewpoint of further improving the chipping resistance and / or the wear resistance, and more preferably 0.20 μm or more and 0.50 μm or less from the same viewpoint.

[0028] When the lower layer is formed of the first to third layers as described above, the average thickness of the second layer formed on the surface of the first layer is preferably 3.00 μm to 14.00 μm in order to further improve the chipping resistance and / or wear resistance. From the same viewpoint, the average thickness of the second layer is more preferably 3.80 μm to 13.50 μm, and even more preferably 4.30 μm to 12.50 μm.

[0029] When the lower layer is formed of the first to third layers as described above, the average thickness of the third layer formed on the surface of the second layer is preferably 0.10 μm to 1.00 μm in order to further improve the chipping resistance and / or wear resistance. From the same viewpoint, the average thickness of the third layer is more preferably 0.10 μm to 0.80 μm, and even more preferably 0.10 μm to 0.50 μm.

[0030] The Ti compound layer is a layer consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B, but may contain trace amounts of components other than the above elements as long as the effect of the lower layer is achieved.

[0031] [Lower α-type Al2O3 layer] In this embodiment, the lower α-Al2O3 layer includes an α-Al2O3 layer made of α-Al2O3. The lower α-type Al2O3 layer has an average thickness T1 of 2.00 μm or more and 15.00 μm or less, satisfies the condition represented by the above formula (1), and satisfies the condition represented by the above formula (2).

[0032] The average thickness T1 of the lower α-Al2O3 layer is 2.00 μm or more and 15.00 μm or less. When the average thickness T1 of the lower α-Al2O3 layer is 2.00 μm or more, the wear resistance and plastic deformation resistance are excellent, and when the average thickness T1 of the lower α-Al2O3 layer is 15.00 μm or less, peeling of the coating layer is suppressed, and the chipping resistance and defect resistance are excellent. From the same viewpoint, the average thickness T1 of the lower α-Al2O3 layer is preferably 2.80 μm or more and 14.80 μm or less, and more preferably 4.00 μm or more and 14.00 μm or less.

[0033] The average thickness T1 of the lower α-type Al2O3 layer is measured by the following method. Among the lowest points of the concave portions and the highest points of the convex portions on the surface of the lower α-Al2O3 layer opposite the substrate, which were identified in the method for measuring the average angle β, three lowest points of the concave portions having the shortest distance from the substrate surface are identified in order from the side with the shortest distance, and three highest points of the convex portions having the longest distance from the substrate surface are identified in order from the side with the longest shortest distance. A normal line to the substrate surface is drawn passing through the six identified points, and the arithmetic mean of the lengths that these normal lines cross through the lower α-Al2O3 layer is taken as the average thickness of the lower α-Al2O3 layer.

[0034] The lower α-type Al2O3 layer satisfies the condition represented by the following formula (1). 60≦RSA<100 (1) (In formula (1), RSA is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the misorientation A, which is the angle between the normal to the surface of the substrate and the normal to the (001) plane of the particles in the lower α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the lower α-Al2O3 layer perpendicular to the surface of the substrate is taken as 100 area %).)

[0035] When the RSA is 60% or more by area in the lower α-Al2O3 layer, the progression of crater wear is suppressed, and therefore the wear resistance and plastic deformation resistance are excellent. Also, when the RSA is less than 100% by area, the lower α-Al2O3 layer is easily formed. From the same viewpoint, the RSA is preferably 63% or more and 96% or less by area, and more preferably 70% or more and 90% or less by area.

[0036] The lower α-type Al2O3 layer satisfies the condition represented by the following formula (2). 15≦average angle β≦45 (2) (In formula (2), the average angle β (degrees) is expressed by the following formula (2-1).)

[0037]

number

[0038] (In formula (2-1), L nrepresents the length (μm) of the nth line segment from the left of the observation field of view, among the line segments created by identifying the lowest point of each identified concave portion and the highest point of each convex portion on the surface of the lower α-AlO3 layer opposite the substrate in an observation field of view including a cross section of the lower α-AlO3 layer in a direction perpendicular to the surface of the substrate, and connecting the lowest point of each identified concave portion with the highest point of the convex portion adjacent to the lowest point of the concave portion with a straight line; β n represents the n-th angle (degrees) from the left of the observation field of view among the angles formed by each line segment and a straight line parallel to the substrate surface. However, the observation field of view is the area of ​​each (L n ×cosβ n ) is an area in which the total length of the

[0039] In the lower α-Al2O3 layer, when the average angle β is 15 degrees or more, the adhesion between the lower α-Al2O3 layer and the upper α-Al2O3 layer via the intermediate layer is improved, resulting in excellent chipping resistance and fracture resistance. In addition, when the average angle β is 45 degrees or less in the lower α-Al2O3 layer, the unevenness of the surface of the coating layer is reduced, reducing the cutting resistance, resulting in excellent wear resistance and fracture resistance. In addition, by setting the average angle β in the range of 15 degrees to 45 degrees in the lower α-Al2O3 layer, the growth of cracks during cutting is suppressed, resulting in improved fracture resistance.

[0040] Furthermore, the coated cutting tool of this embodiment has a configuration in which the average angle β in the lower α-Al2O3 layer is controlled to a range of 15 degrees or more and 45 degrees or less (this configuration is hereinafter also referred to as "configuration C"), and in which the average angle β is further controlled to a range of 22 degrees or more and 38 degrees or less (this configuration is hereinafter also referred to as "configuration D"), and is particularly excellent in fracture resistance. In structure C, the larger the average angle β in the lower α-Al2O3 layer, the lower the ratio of orientation of the (110) plane of the upper α-Al2O3 layer with respect to the normal line of the substrate surface. Therefore, it can be predicted that, in general, the larger the average angle β in the upper α-Al2O3 layer, the better the adhesion, but the lower the chipping resistance, making it difficult to improve the fracture resistance. However, it has been found that, in fact, structure D of structure C is particularly excellent in fracture resistance. In this regard, it is presumed that by using structure D of structure C in particular, the effect of improving the fracture resistance other than adhesion is obtained. The reason for this is unclear, but is presumed to be as follows. In general, the (012) plane is known as the cleavage plane of Al2O3 with an α-type crystal structure, and is prone to fracture due to cracks. In the lower α-type Al2O3 layer oriented to the (001) plane so that the RSA is in a specific range, the (012) plane is inclined at about 58 degrees to the substrate surface (32 degrees to the normal to the substrate surface). In addition, the (110) plane of Al2O3, which has an α-type crystal structure, generally has a smaller thermal expansion coefficient than other planes, and so orientation to the (110) plane is thought to have the effect of suppressing the generation and propagation of cracks perpendicular to the (110) plane due to thermal shock. From the above two points, in the configuration D, cracks are less likely to occur in the upper α-Al2O3 layer in a direction in the range of 22 degrees to 38 degrees with respect to the substrate surface due to thermal shock during cutting, and the probability of cracks propagating in a direction along the cleavage plane of the lower α-Al2O3 layer is reduced. Therefore, it is considered that chipping resistance during cutting with thermal shock is improved and fracture resistance is excellent.

[0041] The average angle β is measured by the following method. The cross section of the lower α-Al2O3 layer in the direction perpendicular to the surface of the substrate is observed using an FE-SEM to obtain an observation image of the cross section of the lower α-Al2O3 layer. At this time, the observation image is obtained so that the direction approximately parallel to the substrate surface is parallel to the left-right direction of the observation image. More specifically, "obtaining an observation image such that the direction approximately parallel to the substrate surface is parallel to the left-right direction of the observation image" means that the interface between the coating layer and the substrate crosses from the left end to the right end of the observation image, and the straight line connecting the interface between the coating layer and the substrate at the left end and the interface between the coating layer and the substrate at the right end is parallel to the left-right direction of the observation image. The straight line refers to a straight line approximately parallel to the substrate surface. In the observation image, a straight line approximately parallel to the substrate surface is drawn at a position closer to the substrate than the surface of the lower α-Al2O3 layer opposite the substrate. In the observation image, the surface of the lower α-Al2O3 layer opposite the substrate is observed as a continuous form in which the shortest distance between the surface and the straight line approximately parallel to the substrate surface is small and large from the left end to the right end. From the left end to the right end of the observation image, all points where the shortest distance between the surface of the lower α-Al2O3 layer opposite the substrate and the straight line changes from a large part to a small part are identified, and are taken as the lowest points of each recess. From the left end to the right end of the observation image, all points where the shortest distance between the surface of the lower α-Al2O3 layer opposite the substrate and the straight line changes from a small part to a large part are identified, and are taken as the lowest points of each recess. A line segment is drawn connecting the lowest point of each identified recess and the highest point of the adjacent protrusion to the lowest point of the recess. The lengths of all the line segments and the angles between the line segments and a straight line approximately parallel to the substrate surface are determined individually. At this time, the length of the nth line segment from the left of the observation field is defined as L n The angle between the nth line segment and a line approximately parallel to the substrate surface is expressed as β n This is expressed as: The obtained value is substituted into equation (2-1) and the calculated value is set as the average angle β.

[0042] In this embodiment, the lower α-Al2O3 layer includes an α-Al2O3 layer made of α-Al2O3, but may include components other than α-Al2O3 as long as the effects of the present invention are achieved.

[0043] In the lower α-Al2O3 layer, the average particle size of particles in a direction parallel to the surface of the substrate at a position 0.2 μm toward the substrate from the lowest point located closest to the substrate among the lowest points of each recess on the surface of the lower α-Al2O3 layer opposite the substrate in the observation field for determining the average angle β (degrees) is preferably 0.3 μm or more and 2.0 μm or less. In the lower α-Al2O3 layer, when the average grain size is 0.3 μm or more, the RSB value tends to be easily controlled within a predetermined range. In addition, in the coated cutting tool of this embodiment, when the average grain size is 2.0 μm or less in the lower α-Al2O3 layer, the adhesion between the lower α-Al2O3 layer and the upper α-Al2O3 layer via the intermediate layer is improved, so that the chipping resistance and fracture resistance tend to be excellent. From the same viewpoint, in the lower α-Al2O3 layer, the average grain size is more preferably 0.4 μm to 1.9 μm, and even more preferably 0.7 μm to 1.6 μm.

[0044] [Middle layer] In this embodiment, the intermediate layer includes one or more Ti compound layers consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B, and has an average thickness of 0.05 μm or more and 1.00 μm or less. As described above, in general, in an α-type Al2O3 layer consisting of one layer, the lower side may be oriented to the (001) plane and the upper side may be oriented to the (110) plane (hereinafter, this structure may be referred to as "structure A"). In this case, it tends to be difficult to increase the ratio of orientation on either or both of the lower side and the upper side. In the present embodiment, by forming an intermediate layer including a Ti compound layer between the lower α-Al2O3 layer and the upper α-Al2O3 layer in the coating layer (this configuration is hereinafter also referred to as “configuration B”), it is possible to simultaneously arrange a lower α-Al2O3 layer oriented in the (001) plane so that RSA falls within a specific range, and an upper α-Al2O3 layer oriented in the (110) plane so that RSB falls within a specific range, as described above, and it is presumed that this provides the effects of both.

[0045] The intermediate layer includes one or more Ti compound layers consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B, and preferably includes one or more Ti compound layers consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, and O.

[0046] The Ti compound layer in the intermediate layer is not particularly limited, but may be, for example, a TiC layer made of TiC (hereinafter, simply referred to as "TiC layer"), a TiN layer made of TiN (hereinafter, simply referred to as "TiN layer"), a TiCN layer made of TiCN (hereinafter, simply referred to as "TiCN layer"), a TiCO layer made of TiCO (hereinafter, simply referred to as "TiCO layer"), a TiCNO layer made of TiCNO (hereinafter, simply referred to as "TiCNO layer"), a TiON layer made of TiON (hereinafter, simply referred to as "TiON layer"), and a TiB2 layer made of TiB2 (hereinafter, simply referred to as "TiB2 layer"). From the viewpoint of more effectively and reliably achieving the effects of the present invention, it is preferable that the Ti compound layer in the intermediate layer includes a TiCO layer and / or a TiCNO layer.

[0047] The intermediate layer may be composed of one layer, or may be composed of multiple layers (for example, two or three layers). From the viewpoint of more effectively and reliably achieving the effects of the present invention, it is preferable that the intermediate layer is composed of one layer.

[0048] The average thickness of the intermediate layer is 0.05 μm or more and 1.00 μm or less. This provides excellent chipping resistance. From the same viewpoint, the average thickness of the intermediate layer is preferably 0.05 μm or more and 0.90 μm or less, and more preferably 0.20 μm or more and 0.80 μm or less. Moreover, by setting the average thickness of the intermediate layer within the above range, the RSB (area %) in the upper α-type Al2O3 layer can be easily adjusted to fall within a predetermined range.

[0049] The average thickness of the intermediate layer is measured by the following method. Among the lowest points of the concave portions and the highest points of the convex portions on the surface of the lower α-Al2O3 layer opposite the substrate, which were identified in the method for measuring the average angle β, three lowest points of the concave portions that have the shortest distance from the substrate surface are identified in order from the side with the shortest distance, and three highest points of the convex portions that have the longest distance from the substrate surface are identified in order from the side with the longest shortest distance. A normal line to the substrate surface is drawn through the six identified points, and the arithmetic mean of the lengths that these normal lines cross through the intermediate layer is taken as the average thickness of the intermediate layer.

[0050] [Top α-type Al2O3 layer] In this embodiment, the upper α-type Al2O3 layer has an average thickness T2 of 0.50 μm or more and 5.00 μm or less, and the upper α-type Al2O3 layer satisfies the condition represented by the above formula (3).

[0051] In this embodiment, the average thickness T2 of the upper α-type Al2O3 layer is not less than 0.50 μm and not more than 5.00 μm. In the coated cutting tool of this embodiment, the average thickness T2 of the upper α-Al2O3 layer is 0.50 μm or more, thereby improving thermal shock resistance and fracture resistance, and the average thickness T2 of the upper α-Al2O3 layer is 5.00 μm or less, thereby suppressing peeling of the coating layer and providing excellent chipping resistance and fracture resistance. From the same viewpoint, the average thickness T2 of the upper α-Al2O3 layer is preferably 0.60 μm to 4.50 μm, and more preferably 0.80 μm to 2.20 μm.

[0052] The average thickness T2 of the upper α-type Al2O3 layer is measured by the following method. Among the lowest points of the concave portions and the highest points of the convex portions on the surface of the lower α-Al2O3 layer opposite the substrate, which were identified in the method for measuring the average angle β, three lowest points of the concave portions having the shortest distance from the substrate surface are identified in order from the side with the shortest distance, and three highest points of the convex portions having the longest distance from the substrate surface are identified in order from the side with the longest shortest distance. A normal line to the substrate surface is drawn passing through the six identified points, and the arithmetic mean of the lengths that these normal lines cross through the upper α-Al2O3 layer is taken as the average thickness of the upper α-Al2O3 layer.

[0053] In this embodiment, the upper α-type Al2O3 layer satisfies the condition represented by the following formula (3). 50 <RSB<100 (3) (In formula (3), RSB is the ratio (unit: area %) of the cross-sectional area of ​​particles in which the misorientation B, which is the angle between the normal to the line segment created when determining the average angle β (degrees) and the normal to the (110) plane of the particles in the upper α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the upper α-Al2O3 layer in the direction perpendicular to the surface of the substrate is taken as 100 area %. However, the misorientation B is determined for each region separated by dividing the upper α-Al2O3 layer by the normals to the substrate surface that pass through the identified lowest points of the concave portions and the highest points of the convex portions in the observation field for determining the average angle β (degrees).)

[0054] In the coated cutting tool of this embodiment, when the RSB is more than 50 area % in the upper α-Al2O3 layer, the thermal shock resistance is improved, and therefore the chipping resistance is improved. Also, when the RSB is less than 100 area %, the upper α-Al2O3 layer is easily formed. From the same viewpoint, the RSB is preferably 52 area % or more and 91 area % or less, and more preferably 54 area % or more and 82 area % or less.

[0055] In this embodiment, the upper α-Al2O3 layer includes an α-Al2O3 layer made of α-Al2O3, but may include components other than α-Al2O3 as long as the effects of the present invention are achieved.

[0056] In this embodiment, the ratio (T1 / T2) of the average thickness T1 of the lower α-type Al2O3 layer to the average thickness T2 of the upper α-type Al2O3 layer is preferably 1.0 or more and 12.0 or less. In the coated cutting tool of this embodiment, when T1 / T2 is 1.0 or more, the progression of crater wear is suppressed, so that the wear resistance and plastic deformation resistance tend to be excellent, and when T1 / T2 is 12.0 or less, the thermal shock resistance tends to be improved, so that the chipping resistance tends to be improved. From the same viewpoint, T1 / T2 is more preferably 1.3 to 10.7, and even more preferably 3.5 to 9.3.

[0057] [External layer] In this embodiment, the coating layer may include an outer layer on the interface of the upper α-Al2O3 layer on the side opposite to the substrate (i.e., the surface of the upper α-Al2O3 layer). The outer layer of the coating layer can improve the wear resistance. Also, the used corner can be easily identified. The outer layer is preferably a layer of a compound consisting of at least one element selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, and Y, and at least one element selected from the group consisting of C, N, O, and B (preferably C element and / or N element), as it tends to have excellent wear resistance. From the same viewpoint, the outer layer is more preferably a layer of a compound consisting of at least one element selected from the group consisting of Ti, Nb, Cr, Al, and Si, and at least one element selected from the group consisting of C, N, O, and B, and is further preferably a layer of a compound consisting of at least one element selected from the group consisting of Ti, Cr, Al, and Si, and at least one element selected from the group consisting of C, N, and O. Among them, specific examples of the outer layer are preferably a TiN layer consisting of TiN, a TiCNO layer consisting of TiCNO, and a TiCN layer consisting of TiCN.

[0058] The average thickness of the outer layer is not particularly limited and may be, for example, 0.1 μm or more and 5.0 μm or less. From the viewpoint of more effectively and reliably achieving the effects of the present invention, the average thickness of the outer layer is preferably 0.15 μm or more and 3.0 μm or less, and more preferably 0.2 μm or more and 3.0 μm or less.

[0059] The average thickness of the outer layer is measured by the following method. Among the lowest points of the concaves and the highest points of the convexities on the surface of the lower α-Al2O3 layer opposite the substrate, which were identified in the method for measuring the average angle β, three lowest points of the concaves that have the shortest distance from the substrate surface are identified in order from the side with the shortest distance, and three highest points of the convexities that have the longest distance from the substrate surface are identified in order from the side with the longest distance. A normal line to the substrate surface is drawn through the six identified points, and the arithmetic mean of the lengths that these normal lines cross through the outer layer is taken as the average thickness of the outer layer.

[0060] [Measurement method for RSA and RSB] In this embodiment, the method of measuring RSA and RSB can be, for example, to observe the cross section to be measured with a field emission scanning electron microscope (FE-SEM) and measure the cross-sectional area of ​​a particle having a specific orientation difference using an electron backscattering diffraction (EBSD) device attached to the FE-SEM. The RSA and RSB may be similarly measured to measure the orientation difference and calculate the cross-sectional area of ​​the particle, except that the crystal planes measured are different. More specifically, they can be determined, for example, by the method described in the Examples below.

[0061] [Method of forming coating layer] The method for forming the coating layer in the coated cutting tool of this embodiment is not particularly limited, but may be, for example, the following method. However, the method for forming each layer is not limited to this.

[0062] For example, the Ti compound layer of the lower layer is formed by the following method. The Ti compound layer consisting of a Ti nitride layer can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 5.0 to 10.0 mol%, N2: 20 to 60 mol%, H2: balance, at a temperature of 850 to 950°C and a pressure of 300 to 400 hPa.

[0063] The Ti compound layer consisting of a Ti carbide layer can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 1.5 to 3.5 mol%, CH4: 3.5 to 5.5 mol%, H2: balance, at a temperature of 950 to 1050°C and a pressure of 70 to 80 hPa.

[0064] The Ti compound layer consisting of a Ti carbonitride layer can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 5.0 to 7.0 mol%, CH3CN: 0.5 to 1.5 mol%, H2: balance, at a temperature of 800 to 900°C and a pressure of 60 to 80 hPa.

[0065] The Ti compound layer consisting of a Ti oxycarbonitride layer can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 3.0-4.0 mol%, CO: 0.5-1.0 mol%, N2: 30-40 mol%, H2: balance, at a temperature of 950-1050°C and a pressure of 50-150 hPa.

[0066] The Ti compound layer consisting of a Ti carbonate layer can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 1.0-2.0 mol%, CO: 2.0-3.0 mol%, H2: balance, at a temperature of 950-1050°C and a pressure of 50-150 hPa.

[0067] After the lower layer is formed, the α-Al2O3 layer of the lower α-Al2O3 layer is formed on the surface of the lower layer by, for example, the following method. First, a lower layer consisting of one or more Ti compound layers is formed on the surface of the substrate. Next, the surface of the layer farthest from the substrate (the layer that is not the substrate) is oxidized. After that, a lower α-type Al2O3 layer is formed on the surface of the layer farthest from the substrate through a nucleation process.

[0068] More specifically, the oxidation of the surface of the layer furthest from the substrate may be carried out under conditions of a raw material composition of CO2: 0.3 to 1.0 mol%, H2: balance, temperature of 950 to 1050°C, and pressure of 50 to 60 hPa (oxidation step 1). The oxidation treatment time is preferably 1 to 5 minutes.

[0069] Then, a nucleation step is performed to form nuclei on the surface of the layer farthest from the substrate. The nucleation step may be performed by chemical vapor deposition under conditions of a raw material composition of AlCl3: 1.0-5.0 mol%, CO2: 0.5-2.5 mol%, CO: 0.5-2.5 mol%, HCl: 1.0-3.0 mol%, H2: balance, a temperature of 950-1050°C, and a pressure of 60-80 hPa (nucleation step 1). In this case, the treatment time of the nucleation step 1 is preferably 1-10 minutes.

[0070] After that, the lower α-type Al2O3 layer is formed on the surface of the lower layer. Below, a case where the lower α-type Al2O3 layer is formed in three stages will be explained. The first stage of formation of the α-Al2O3 layer of the lower α-Al2O3 layer may be performed by chemical vapor deposition under conditions of a raw material composition of AlCl3: 1.5-2.5 mol%, CO2: 1.0-2.5 mol%, HCl: 3.0-6.0 mol%, H2S: 0.05-0.10 mol%, H2: balance, a temperature of 970-1030°C, and a pressure of 60-80 hPa (film formation process 1). In this case, the processing time of film formation process 1 is preferably a time for the thickness of the film formed by film formation process 1 to be 5%-15% of the average thickness of the desired lower α-Al2O3 layer, and more preferably a time for the thickness to be 10%.

[0071] After the film-forming step 1, the second-stage formation of the α-Al2O3 layer of the lower α-Al2O3 layer may be performed by chemical vapor deposition under conditions of a raw material composition of AlCl3: 2.0-4.0 mol%, CO2: 1.0-2.5 mol%, HCl: 2.0-4.0 mol%, H2S: 0.6-1.0 mol%, H2: balance, a temperature of 970-1030°C, and a pressure of 60-80 hPa (film-forming step 2). In this case, the processing time of the film-forming step 2 is preferably a time for the thickness of the film formed by the film-forming step 2 to be 50%-70% of the average thickness of the desired lower α-Al2O3 layer, and more preferably a time for the thickness to be 60%.

[0072] After the film-forming step 2, the third stage of the formation of the α-Al2O3 layer of the lower α-Al2O3 layer may be performed by chemical vapor deposition under the conditions of a raw material composition of AlCl3: 4.0-7.0 mol%, CO2: 1.5-3.0 mol%, HCl: 0.3-0.8 mol%, H2S: 0.6-1.0 mol%, H2: balance, a temperature of 930-970°C, and a pressure of 100-140 hPa (film-forming step 3). In this case, the processing time of the film-forming step 3 is preferably a time for the thickness of the film formed by the film-forming step 3 to be 25%-35% of the average thickness of the desired lower α-Al2O3 layer, and more preferably a time for the thickness to be 30%.

[0073] In order to set the RSA (area %) within a predetermined range, the proportion of H2S in the raw material composition may be controlled in the film formation process 1 and / or the film formation process 2. Specifically, for example, by increasing the proportion of H2S in the raw material composition in the film formation process 1 and / or the film formation process 2, the RSA tends to become higher.

[0074] In order to set the average particle size of the particles in the direction parallel to the surface of the substrate at a position 0.2 μm toward the substrate from the lowest point located closest to the substrate among the lowest points of the individual recesses on the surface of the lower α-Al2O3 layer opposite to the substrate in the observation field for determining the average angle β (degrees) in the lower α-Al2O3 layer within a predetermined range, the ratio of CO2 and / or HCl in the raw material composition may be controlled in the film formation process 1. Specifically, for example, the average particle size tends to increase by decreasing the ratio of CO2 or increasing the ratio of HCl in the raw material composition in the film formation process 1.

[0075] In order to set the average angle β within a predetermined range, the ratio of AlCl3 and / or HCl in the raw material composition may be controlled in the film formation process 3. Specifically, for example, by increasing the ratio of AlCl3 and decreasing the ratio of HCl in the raw material composition in the film formation process 3, the average angle β tends to increase.

[0076] Next, an intermediate layer is formed on the surface of the lower α-Al2O3 layer, the intermediate layer including one or more Ti compound layers made of a Ti compound with Ti and at least one element selected from the group consisting of C, N, O, and B. The intermediate layer can be formed, for example, by the following method.

[0077] For example, a Ti compound layer consisting of a Ti oxycarbonitride layer as an intermediate layer can be formed by a chemical vapor deposition method with a raw material composition of TiCl4: 4.0-7.0 mol%, CO: 2.0-4.0 mol%, N2: 30-40 mol%, H2: balance, at a temperature of 930-970°C and a pressure of 80-120 hPa.

[0078] The Ti compound layer consisting of a Ti carbonate layer as an intermediate layer can be formed by a chemical vapor deposition method using a raw material composition of TiCl4: 4.0-7.0 mol%, CO: 2.0-4.0 mol%, H2: balance, at a temperature of 930-970°C and a pressure of 80-120 hPa.

[0079] After the intermediate layer is formed, the α-Al2O3 layer of the upper α-Al2O3 layer is formed on the surface of the intermediate layer by, for example, the following method. First, the surface of the intermediate layer is oxidized, and then a nucleation process is performed to form an upper α-type Al2O3 layer on the surface of the intermediate layer.

[0080] More specifically, the oxidation of the surface of the intermediate layer may be carried out under conditions of a raw material composition of CO2: 0.3 to 1.0 mol%, H2: balance, a temperature of 950 to 1050°C, and a pressure of 50 to 60 hPa (oxidation step 2). The oxidation treatment time is preferably 1 to 5 minutes.

[0081] Then, a nucleation step is performed to form nuclei on the surface of the intermediate layer. The nucleation step may be performed by chemical vapor deposition under conditions of a raw material composition of AlCl3: 3.0-7.0 mol%, CO2: 2.0-5.0 mol%, HCl: 3.0-5.0 mol%, H2: balance, a temperature of 950-1050°C, and a pressure of 70-90 hPa (nucleation step 2). In this case, the treatment time of the nucleation step 2 is preferably 1-10 minutes.

[0082] Thereafter, the α-type Al2O3 layer of the upper α-type Al2O3 layer may be formed by a chemical vapor deposition method under conditions of a raw material composition of AlCl3: 2.0-4.0 mol%, CO2: 4.0-7.0 mol%, HCl: 1.0-2.5 mol%, H2S: 0.05-0.10 mol%, H2: balance, a temperature of 930-970°C, and a pressure of 100-140 hPa (film formation process 4).

[0083] In order to set RSB (area %) within a predetermined range, it is sufficient to control the ratio of CO in the raw material composition in the intermediate layer formation step and the ratio of CO2 in the raw material composition in the film formation step 4. Specifically, when the ratio of CO in the raw material composition in the intermediate layer formation step is increased, or when the ratio of CO2 in the raw material composition in the film formation step 4 is increased, RSB tends to become higher. Furthermore, when the average thickness of the intermediate layer is within a certain range, the RSB tends to be high.

[0084] On the surface of the upper α-type Al2O3 layer, an outer layer such as a TiCNO layer, a TiN layer, a TiCN layer, etc. may be formed as necessary. The outer layer can be formed, for example, by the following method.

[0085] The TiN layer as the outer layer can be formed by chemical vapor deposition using a raw material composition of TiCl4: 5.0-10.0 mol %, N2: 20-60 mol %, H2: balance, at a temperature of 950-1050°C and a pressure of 300-400 hPa.

[0086] The TiCN layer as the outer layer can be formed by chemical vapor deposition using a raw material composition of TiCl4: 4.0-8.0 mol %, CH3CN: 0.5-2.0 mol %, H2: balance, at a temperature of 950-1050°C and a pressure of 60-80 hPa.

[0087] The TiCNO layer as the outer layer can be formed by chemical vapor deposition using a raw material composition of TiCl4: 3.0-4.0 mol%, CO: 0.5-1.0 mol%, N2: 30-40 mol%, H2: balance, at a temperature of 950-1050°C and a pressure of 80-120 hPa.

[0088] The coated cutting tool of this embodiment is considered to have an effect of extending the tool life compared to conventional tools due to its excellent resistance to at least chipping and wear (however, the factors that enable the tool life to be extended are not limited to those mentioned above). Specific examples of the types of the coated cutting tool of this embodiment include indexable cutting inserts for milling or turning, drills, and end mills. EXAMPLES

[0089] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0090] [Invention products 1-27 and comparison products 1-17] A cemented carbide alloy with a composition of 88.5% WC-6.7% Co-1.4% TiC-0.6% TiN-0.5% TaC-2.0% NbC-0.2% ZrC-0.1% Cr3C2 (all mass%) was prepared as the substrate, which was machined into the insert shape of CNMG120408. After circular honing was performed on the cutting edge of this substrate with a SiC brush, the surface of the substrate was cleaned.

[0091] After cleaning the surface of the substrate, the coating layer was formed by chemical vapor deposition. First, the substrate was loaded into the thermal chemical vapor deposition apparatus, and the first layer showing the composition shown in Tables 14 and 15 was formed on the surface of the substrate under the conditions of the raw material composition, temperature, and pressure shown in Table 1 to have the average thickness shown in Tables 14 and 15. Next, under the conditions of the raw material composition, temperature, and pressure shown in Table 1, the second layer shown in Tables 14 and 15 was formed on the surface of the first layer to have the average thickness shown in Tables 14 and 15. Next, under the conditions of the raw material composition, temperature, and pressure shown in Table 1, the third layer shown in Tables 14 and 15 was formed on the surface of the second layer to have the average thickness shown in Tables 14 and 15. This formed a lower layer composed of three layers. Then, under the conditions of the raw material composition, temperature, and pressure shown in Table 2, the surface of the third layer was subjected to an oxidation treatment for the time shown in Table 2.

[0092] Next, a nucleation step of the lower α-type Al2O3 layer was carried out on the surface of the oxidized third layer under the conditions of the raw material composition, temperature, and pressure shown in Table 2 for the time shown in Table 2. Then, on the surface of the third layer, a film-forming process 1 was performed under the conditions of the raw material composition, temperature, and pressure shown in Tables 4 and 5, a film-forming process 2 was performed under the conditions of the raw material composition, temperature, and pressure shown in Tables 6 and 7, and a film-forming process 3 was performed under the conditions of the raw material composition, temperature, and pressure shown in Tables 8 and 9, so that the average thickness T1 of the lower α-Al2O3 layer was the average thickness shown in Tables 14 and 15. The layer formed in the film-forming process 1 was formed to have a thickness of 10% of the desired average thickness T1 of the lower α-Al2O3 layer, the layer formed in the film-forming process 2 was formed to have a thickness of 60% of the desired average thickness T1 of the lower α-Al2O3 layer, and the layer formed in the film-forming process 3 was formed to have a thickness of 30% of the desired average thickness T1 of the lower α-Al2O3 layer. However, as an exception, in comparative sample 12, the layer formed in coating process 1 was formed to have a thickness of 10% of the desired average thickness T1 of the lower α-Al2O3 layer, and the layer formed in coating process 2 was formed to have a thickness of 90% of the desired average thickness T1 of the lower α-Al2O3 layer.

[0093] Next, an intermediate layer was formed on the surface of the lower α-Al2O3 layer under the conditions of the raw material composition, temperature, and pressure shown in Tables 10 and 11 so as to have an overall average thickness as shown in Tables 16 and 17. Thereafter, the surface of the intermediate layer was subjected to an oxidation treatment under the conditions of the raw material composition, temperature, and pressure shown in Table 3 for the time shown in Table 3.

[0094] Next, a nucleation step of the upper α-type Al2O3 layer was carried out on the surface of the intermediate layer that had been subjected to the oxidation treatment under the conditions of the raw material composition, temperature, and pressure shown in Table 3 for the time shown in Table 3. Thereafter, an upper α-Al2O3 layer was formed on the surface of the intermediate layer under the conditions of the raw material composition, temperature, and pressure shown in Tables 12 and 13, by adjusting the deposition time so that the average thickness T2 of the upper α-Al2O3 layer became the average thickness shown in Tables 16 and 17. However, in Comparative Samples 11 and 12, the intermediate layer and the upper α-type Al2O3 layer were not formed.

[0095] Furthermore, for Invention Products 24 to 26 and Comparative Products 11 and 12, an outer layer having the composition shown in Tables 16 and 17 was formed on the surface of the upper α-AlO layer under the conditions of raw material composition, temperature, and pressure shown in Table 1, to have the average thickness shown in Tables 16 and 17. In this manner, coated cutting tools, invention products 1 to 27 and comparison products 1 to 17, were obtained.

[0096] The thickness of each layer of the sample was determined by the method described above. The measurement results are shown in Tables 14 to 17.

[0097] [Table 1]

[0098] [Table 2]

[0099] [Table 3]

[0100]

Table 4

[0101]

Table 5

[0102]

Table 6

[0103]

Table 7

[0104]

Table 8

[0105]

Table 9

[0106]

Table 10

[0107]

Table 11

[0108]

Table 12

[0109]

Table 13

[0110] [Table 14]

[0111] [Table 15]

[0112] [Table 16]

[0113] [Table 17]

[0114] [Measurement of the average angle β] The average angle β was measured by the method described above.

[0115] [Measurement and calculation of RSA and RSB] For RSA and RSB, the following measurement cross sections were observed using a field emission scanning electron microscope (hereinafter also referred to as "FE-SEM") under the following conditions, and the sum of the cross-sectional areas of particles with orientation mismatch A of 0 degrees or more and 15 degrees or less, and the sum of the cross-sectional areas of particles with orientation mismatch B of 0 degrees or more and 15 degrees or less were measured using an electron backscattering diffraction image analyzer (hereinafter also referred to as "EBSD") attached to the FE-SEM according to the "Method for measuring the cross-sectional area of ​​particles having a specific orientation mismatch" described below. From the obtained values, the RSA was calculated as the percentage of the cross-sectional area of ​​particles in which the misorientation A, which is the angle between the normal to the surface of the substrate and the normal to the (001) plane of the particle in the lower α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, when the total area of ​​the entire cross-section of the lower α-Al2O3 layer perpendicular to the surface of the substrate is taken as 100 area %. In the cross section of the upper α-Al2O3 layer perpendicular to the surface of the substrate, when the total area of ​​the entire cross section is taken as 100 area%, the ratio of the cross-sectional area of ​​particles in which the misorientation B, which is the angle between the normal to the line segment created when determining the above-mentioned average angle β (degrees) and the normal to the (110) plane of the particles in the upper α-Al2O3 layer, is 0 degrees or more and 15 degrees or less, was calculated as RSB. Note that the misorientation B was determined for each region divided by the normals to the substrate surface that pass through the specified lowest points of the concave portions and the specified highest points of the convex portions in the observation field for determining the average angle β (degrees). The results of the above measurements are shown in Tables 18 and 19. (conditions) How to cut out the cross section to be measured RSA and RSB: The coated cutting tools were polished with diamond paste to obtain a cross-sectional structure perpendicular to the substrate surface. Then, the cutter was polished with colloidal silica to obtain a mirror-polished surface of the cross-sectional structure. Measurement cross section RSA: Cross section of the lower α-type Al2O3 layer in the direction perpendicular to the substrate surface RSB: Cross section of the upper α-type Al2O3 layer in the direction perpendicular to the substrate surface ·Direction difference RSA: Misorientation A (the angle between the normal to the substrate surface and the normal to the (001) plane of the grains in the lower α-type Al2O3 layer (unit: degrees)) RSB: Misorientation B (the angle between the normal of the line segment created when calculating the average angle β (degrees) and the normal of the (110) plane of the grains in the upper α-type Al2O3 layer (unit: degrees))

[0116] (Method for measuring the cross-sectional area of ​​particles with specific misorientation) The sample was set in the FE-SEM. The sample was irradiated with an electron beam at an incidence angle of 70 degrees, an acceleration voltage of 15 kV, and a probe current of 1.0 nA. The orientation mismatch and cross-sectional area of ​​each grain were measured with EBSD settings of a measurement range of 30 μm × 50 μm and a step size of 0.05 μm. The cross-sectional area of ​​a grain within the measurement range was the sum of the pixels corresponding to that cross-sectional area. In other words, the total cross-sectional area of ​​grains in the range of 0 degrees to 15 degrees based on orientation mismatch A or mismatch B in each layer was calculated by counting the pixels occupied by the grain cross-sections corresponding to each range and converting them into areas.

[0117] [Average particle size of α-Al2O3 particles in the lower α-Al2O3 layer] The average particle size of the α-Al2O3 particles constituting the lower α-Al2O3 layer of the obtained invention products 1 to 27 and comparison products 1 to 17 was measured using EBSD attached to an FE-SEM. Specifically, the coated cutting tool was polished using diamond paste to obtain a cross-sectional structure parallel to the surface of the substrate. Then, finish polishing was performed using colloidal silica to obtain a mirror-polished surface of the cross-sectional structure. The sample having the cross-sectional structure was set in the FE-SEM, and the sample was irradiated with an electron beam at an incidence angle of 70 degrees, an acceleration voltage of 15 kV, and an irradiation current of 1.0 nA. The measurement was performed with EBSD settings of a measurement range of 30 μm × 50 μm and a step size of 0.05 μm. In the lower α-Al2O3 layer of a coated cutting tool, the average grain size was measured in the direction parallel to the surface of the substrate by EBSD at a position 0.2 μm toward the substrate from the lowest point located closest to the substrate among the lowest points of each recess on the surface of the lower α-Al2O3 layer opposite the substrate in the observation field to determine the average angle β (degrees). More specifically, if there was an orientation difference of 5 degrees or more between adjacent measurement points, the point was defined as a grain boundary. The area surrounded by the grain boundary was defined as one crystal grain, and the average grain size was calculated. A straight line was drawn in a direction parallel to the surface of the substrate at a position 0.2 μm toward the substrate side from the lowest point located closest to the substrate side. Next, the number of crystal grains included in the range of the straight line was calculated. The value obtained by dividing the length of the straight line by the number of each crystal grain was determined as the average grain size of α-Al2O3 in the lower α-Al2O3 layer. In this case, the length of the straight line was set to 40 μm. The results of the average grain size obtained are shown in Tables 18 and 19.

[0118] [Table 18]

[0119] [Table 19]

[0120] The obtained samples were subjected to the following cutting test and evaluated.

[0121] [Cutting test 1] Insert: CNMG120408 (ISO standard), Base material composition: 88.5%WC-6.7%Co-1.4%TiC-0.6%TiN-0.5%TaC-2.0%NbC-0.2%ZrC-0.1%Cr3C2 (mass%), ·Work material: S45C, · Shape of workpiece: round bar, ·Cutting speed: 350m / min, -Cutting depth: 2.0mm, Feed: 0.3mm / rev, Coolant: Water-soluble coolant, Evaluation item: The machining time (minutes) until the maximum flank wear width of the sample reached 0.3 mm was defined as the tool life. The better the wear resistance and plastic deformation resistance, the longer the tool life (machining time) in this cutting test.

[0122] [Cutting test 2] Insert: CNMG120408 (ISO standard), Base material composition: 88.5%WC-6.7%Co-1.4%TiC-0.6%TiN-0.5%TaC-2.0%NbC-0.2%ZrC-0.1%Cr3C2 (mass%), ·Work material: S45C, - Workpiece shape: Round bar with four equally spaced grooves on the outer periphery. ·Cutting speed: 240m / min, Cutting depth: 1.5mm, Feed: 0.15mm / rev, Coolant: Water-soluble coolant, Evaluation item: The tool life was determined when the sample was chipped, and the number of impacts until the tool life was reached was measured. The better the chipping resistance, the longer the tool life (the more impacts) in this cutting test.

[0123] The obtained evaluation results are shown in Tables 20 and 21. Regarding the processing time in cutting test 1, 28 minutes or more was evaluated as "A", 20 minutes or more but less than 28 minutes was evaluated as "B", and less than 20 minutes was evaluated as "C". Regarding the number of impacts in cutting test 2, 10,000 times or more was evaluated as "A", 7,000 times or more but less than 10,000 times was evaluated as "B", and less than 7,000 times was evaluated as "C".

[0124] [Table 20]

[0125] [Table 21]

[0126] As shown in Tables 20 and 21, the inventive product was evaluated as B or higher in both cutting test 1 and cutting test 2. From these results, it was found that the coated cutting tool is a coated cutting tool having a substrate and a coating layer formed on the substrate surface, the coating layer includes, from the substrate side toward the surface of the coating layer, a lower layer, a lower α-type Al2O3 layer, an intermediate layer, and an upper α-type Al2O3 layer, in this order, the lower layer includes one or more Ti compound layers consisting of a Ti compound with Ti and at least one element selected from the group consisting of C, N, O, and B, the average thickness of the lower layer is 3.00 μm to 15.00 μm, the average thickness T1 of the lower α-type Al2O3 layer is 2.00 μm to 15.00 μm, and the lower α-type Al2O3 layer has a thickness of B or higher. It has been found that a product of the invention in which the upper α-Al2O3 layer satisfies the condition represented by formula (1), the lower α-Al2O3 layer satisfies the condition represented by formula (2), the intermediate layer includes one or more Ti compound layers consisting of a Ti compound of Ti and at least one element selected from the group consisting of C, N, O and B, the average thickness of the intermediate layer is 0.05 μm or more and 1.00 μm or less, the average thickness T2 of the upper α-Al2O3 layer is 0.50 μm or more and 5.00 μm or less, and the upper α-Al2O3 layer satisfies the condition represented by formula (3) has excellent fracture resistance and wear resistance and has a long tool life. [Industrial Applicability]

[0127] INDUSTRIAL APPLICABILITY The coated cutting tool of the present invention has excellent fracture resistance and wear resistance, and therefore can extend the tool life as compared with conventional tools, and in that respect has high industrial applicability. [Explanation of symbols]

[0128] 1...Base material, 2...Lower layer, 3...Lower α-type Al2O3 layer, 4...Middle layer, 5...Upper α-type Al2O3 layer, 6...Coating layer, 7...Coated cutting tool

Claims

1. A coated cutting tool comprising a substrate and a coating layer formed on a surface of the substrate, The coating layer is formed by stacking a lower layer and a lower α-type Al layer from the substrate side toward the surface of the coating layer. 2 O 3 layer, an intermediate layer, and an upper α-type Al 2 O 3 layers, in that order, the lower layer includes one or more Ti compound layers each comprising a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; The average thickness of the lower layer is 3.00 μm or more and 15.00 μm or less, The lower α-type Al 2 O 3 The average thickness T1 of the layer is 2.00 μm or more and 15.00 μm or less, The lower α-type Al 2 O 3 In the layer, the condition represented by the following formula (1) is satisfied, 60≦RSA<100 (1) (In formula (1), RSA represents the lower α-type Al in a direction perpendicular to the surface of the substrate.) 2 O 3 In the cross section of the layer, when the total area of ​​the entire cross section is taken as 100%, the normal line to the surface of the base material and the lower α-type Al 2 O 3 The ratio (unit: area %) of the cross-sectional area of ​​grains in which the misorientation A, which is the angle between the (001) plane of the grain of the layer and the normal line, is 0 degrees or more and 15 degrees or less. The lower α-type Al 2 O 3 In the layer, the condition represented by the following formula (2) is satisfied, 15≦average angle β≦45 (2) (In formula (2), the average angle β (degrees) is expressed by the following formula (2-1).) [0010] (In formula (2-1), L n is the lower α-type Al in a direction perpendicular to the surface of the substrate 2 O 3 In an observation field including a cross section of the layer, 2 O 3 the lowest point of each concave portion and the highest point of each convex portion on the surface of the layer opposite to the substrate are identified, and among the line segments created by connecting the identified lowest point of each concave portion and the highest point of the convex portion adjacent to the lowest point of the concave portion with a straight line, the length (μm) of the nth line segment from the left in the observation field of view is represented, and β n represents the n-th angle (degrees) from the left of the observation field of view among the angles formed by each of the created line segments and a straight line parallel to the substrate surface. However, the region of the observation field of view is each (L n ×cosβ n ) is a region in which the total length of the the intermediate layer includes one or more Ti compound layers each including a Ti compound of Ti and at least one element selected from the group consisting of C, N, O, and B; The average thickness of the intermediate layer is 0.05 μm or more and 1.00 μm or less, The upper α-type Al 2 O 3 The average thickness T2 of the layer is 0.50 μm or more and 5.00 μm or less, The upper α-type Al 2 O 3 In the layer, the condition represented by the following formula (3) is satisfied: 50<RSB<100 (3) (In formula (3), RS is the upper α-type Al in a direction perpendicular to the surface of the substrate. 2 O 3 In the cross section of the layer, when the total area of ​​the entire cross section is taken as 100 area %, the normal line of the line segment created when calculating the average angle β (degrees) and the upper α-type Al 2 O 3 The average angle β (degrees) is the ratio (unit: area %) of the cross-sectional area of ​​grains in which the misorientation B, which is the angle between the normal line of the (110) plane of the grain of the upper α-type Al layer and the grain in the upper α-type Al layer, is 0 degrees or more and 15 degrees or less. 2 O 3 The layer is divided by each normal line of the substrate surface that passes through each of the lowest points of the identified concave portions and each of the highest points of the identified convex portions, and the thickness is determined for each of the divided regions. Coated cutting tools.

2. The lower α-type Al 2 O 3 In the layer, the lower α-type Al in the observation field for determining the average angle β (degrees) 2 O 3 the average particle size of particles in a direction parallel to the surface of the substrate at a position 0.2 μm toward the substrate from the lowest point located closest to the substrate among the lowest points of each of the recesses on the surface of the layer opposite to the substrate is 0.3 μm or more and 2.0 μm or less; The coated cutting tool of claim 1 .

3. The upper α-type Al 2 O 3 The lower α-type Al layer average thickness T2 2 O 3 The ratio (T1 / T2) of the average thickness T1 of the layer is 1.0 or more and 12.0 or less; The coated cutting tool according to claim 1 or 2.

4. The average thickness of the coating layer is 8.00 μm or more and 25.00 μm or less. The coated cutting tool according to claim 1 or 2.

5. The substrate is a cemented carbide, a cermet, a ceramic, or a cubic boron nitride sintered body; The coated cutting tool according to claim 1 or 2.

Citation Information

Patent Citations

  • Improved alpha alumina layer deposited with controlled textures

    EP3848485A1

  • Surface-coated cutting tool having hard coating layer exhibiting excellent chipping resistance in high-speed intermittent cutting

    JP2013248675A

  • Coated cutting tool and its manufacturing method

    JP2016502936A

  • Coated cutting tool

    JP2019098430A

  • Surface-coated cutting tool

    WO2017061058A1