Flux composition, and solder composition, and method for producing electronic board

The flux composition with specific activators and antioxidants improves ionic cleanliness and solder meltability, addressing flux residue issues in atmospheric reflow, enabling efficient aqueous cleaning and reliable soldering for electronic boards.

JP2024139686AActive Publication Date: 2024-10-09TAMURA KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024004141
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-01-15
Publication Date
2024-10-09
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

Existing solder compositions leave behind flux residue that can cause ion migration and cleaning performance issues, especially in atmospheric reflow, leading to potential failures in electronic board manufacturing.

Method used

A flux composition containing specific ratios of rosin resin, activators, solvents, and imidazole compounds, along with hindered phenolic and amine antioxidants, enhances ionic cleanliness and solder meltability, allowing effective cleaning with aqueous agents and improved soldering performance in atmospheric conditions.

Benefits of technology

The composition achieves good ionic cleanliness, effective flux residue removal, and excellent solder meltability, ensuring reliable electronic board manufacturing without the need for solvent-based cleaning and maintaining solder joint integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139686000001
    Figure 2024139686000001
  • Figure 2024139686000002
    Figure 2024139686000002
  • Figure 2024139686000003
    Figure 2024139686000003
Patent Text Reader

Abstract

To provide a flux composition that exhibits superior ionic cleanliness, excels in the removal of flux residue with aqueous cleaners, and demonstrates superior solder melting capability in atmospheric reflow.SOLUTION: A flux composition comprises (A) a rosin-based resin, (B) an activator, (C) a solvent, and (D) an imidazole compound. The component (B) comprises (B1) at least one selected from the group consisting of tricarboxylic acids and tetracarboxylic acids with a molecular weight of 500 or less. The content of the (B1) component is 1 mass% or more relative to 100 mass% of the flux composition. The mass ratio of the component (D) to the (B1) component ((D) / (B1)) is 0.25 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux composition, a solder composition, and a method for producing an electronic board. [Background technology]

[0002] The solder composition is a mixture prepared by kneading a solder powder with a flux composition (rosin-based resin, an activator, a solvent, and the like) to form a paste (see Patent Document 1). When soldering is performed using a solder composition, flux residue remains around the joint after soldering. This residue contains activator components, etc., and there is a concern that moisture may enter the residue distributed across the electrodes due to condensation or the like, causing ion migration. Therefore, it is desirable to have a small amount of ion residue that may cause ion migration. This can be evaluated by ionic cleanliness. Furthermore, the presence of flux residue on the surface may cause defects in the molding process or coating process, or poor bonding in wire bonding. Therefore, it is desirable to remove this residue by cleaning after bonding.

[0003] Conventionally, cleaning has been carried out using cleaning agents whose main component is organic solvents with high cleaning power. However, because these agents contain a large amount of solvent, regulations have been strengthened from the viewpoints of preventing water pollution, fire and air pollution, and from the viewpoint of occupational health. In recent years, the amount of solvent used has been reduced and water-based cleaning chemicals, which are mainly composed of water, have come to be used. However, due to the change in the cleaning chemicals' ingredients, the cleaning performance of flux residues has tended to deteriorate, which has become a problem. Also, from the viewpoint of equipment costs, there is an increasing need to perform soldering by reflow under atmospheric conditions. In the case of air reflow, oxidation of the solder powder progresses, and solder melting property decreases. This tendency is more pronounced in the joints of small components where the amount of solder composition printed is small. Furthermore, in air reflow, the metal salts contained in the flux residue after soldering increase due to the effect of metal oxidation, and the cleanability of the flux residue also tends to deteriorate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5887330 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a flux composition and a solder composition which have a good ionic cleanliness, excellent cleaning properties for flux residues in an aqueous cleaner, and excellent solder melting properties in air reflow, and a method for producing an electronic board. [Means for solving the problem]

[0006] According to the present invention, there are provided a flux composition, a solder composition, and a method for producing an electronic substrate, as described below. [1] A flux composition comprising: (A) a rosin-based resin; (B) an activator; (C) a solvent; and (D) an imidazole compound, the component (B) contains (B1) at least one selected from the group consisting of tricarboxylic acids and tetracarboxylic acids, each having a molecular weight of 500 or less; The blending amount of the (B1) component is 1 mass % or more with respect to 100 mass % of the flux composition, the mass ratio ((D) / (B1)) of the component (D) to the component (B1) is 0.25 or more; Flux composition. [2] The flux composition according to [1], Further, (E) a hindered phenol-based antioxidant is contained, Flux composition. [3] The flux composition according to [1] or [2], Further, (F) a hindered amine-based antioxidant is contained, Flux composition. [4] A flux composition according to any one of [1] to [3] and (G) a solder powder. Solder composition. [5] The solder composition according to [4], The solder alloy in the component (G) contains at least one selected from the group consisting of tin, copper, zinc, silver, antimony, lead, indium, bismuth, nickel, gold, cobalt, and germanium. Solder composition. [6] A method for manufacturing an electronic substrate, comprising soldering using the solder composition according to [4] or [5], applying the solder composition onto an electronic substrate; placing an electronic component on the solder composition; a step of mounting the electronic component on the electronic board by heating under predetermined conditions in a reflow furnace; and cleaning the flux residue on the electronic substrate using a water-based cleaning agent. A method for manufacturing electronic boards. Effect of the Invention

[0007] According to one aspect of the present invention, it is possible to provide a flux composition and a solder composition, which have good ionic cleanliness, excellent cleaning properties for flux residues in an aqueous cleaner, and excellent solder melting properties in air reflow, and a method for producing an electronic substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Flux composition] First, the flux composition according to this embodiment will be described. The flux composition according to this embodiment is a component other than the solder powder in the solder composition, and contains (A) a rosin-based resin, (B) an activator, (C) a solvent, and (D) an imidazole compound, which will be described below. In addition, the (B) component contains (B1) at least one selected from the group consisting of tricarboxylic acids and tetracarboxylic acids, each having a molecular weight of 500 or less, the blending amount of the (B1) component is 1 mass% or more with respect to 100 mass% of the flux composition, and the mass ratio of the (D) component to the (B1) component ((D) / (B1)) is 0.25 or more.

[0009] The reasons why the flux composition according to the present embodiment has good ionic cleanliness, excellent cleaning properties for flux residues in an aqueous cleaner, and excellent solder melting properties in air reflow are not necessarily clear, but the inventors speculate as follows. That is, among the (B) activators, organic acids have a high activation effect and are effective in improving solder melting property in air reflow. Also, imidazole compounds are effective in improving solder melting property and solderability in air reflow. However, it has been found that an excess of organic acids or imidazole compounds deteriorates ionic cleanliness. And, by combining (B1) 1,2,3-propanetricarboxylic acid, which is a low molecular weight polycarboxylic acid, with (D) an imidazole compound in a predetermined ratio, it is possible to maintain good ionic cleanliness and sufficiently improve solder melting property in air reflow while maintaining cleaning properties of flux residue. The present inventors presume that the above-mentioned effects of the present invention are achieved in the above-mentioned manner.

[0010] [Component (A)] The rosin-based resin (A) used in this embodiment includes rosins and rosin-based modified resins. Examples of rosins include gum rosin, wood rosin, and tall oil rosin. Examples of rosin-based modified resins include disproportionated rosin, polymerized rosin, hydrogenated rosin, and derivatives thereof. Examples of hydrogenated rosin include fully hydrogenated rosin, partially hydrogenated rosin, and hydrogenated products of unsaturated organic acid-modified rosins (also called "hydrogenated acid-modified rosin"), which are modified rosins of unsaturated organic acids (aliphatic unsaturated monobasic acids such as (meth)acrylic acid, aliphatic unsaturated dibasic acids such as α,β-unsaturated carboxylic acids such as fumaric acid and maleic acid, unsaturated carboxylic acids having aromatic rings such as cinnamic acid, etc.). These rosin-based resins may be used alone or in combination of two or more. Among these rosin-based resins, it is preferable to use polymerized rosin and hydrogenated acid-modified rosin, and it is more preferable to use polymerized rosin and hydrogenated acid-modified rosin in combination. It is more preferable to use polymerized rosin in combination with other rosin-based resins (hydrogenated acid-modified rosin, formylated rosin, modified rosin, or the like).

[0011] The amount of the (A) component is preferably 30% by mass or more and 70% by mass or less, more preferably 35% by mass or more and 60% by mass or less, and particularly preferably 40% by mass or more and 50% by mass or less, based on 100% by mass of the flux composition. If the amount of the (A) component is more than the lower limit, the oxidation of the copper foil surface of the soldering land is prevented, making the surface more easily wetted with molten solder, and so-called solderability can be improved, and solder balls can be sufficiently suppressed. Also, if the amount of the (A) component is less than the upper limit, the amount of flux residue can be sufficiently suppressed.

[0012] [(B) Component] The (B) activator used in this embodiment must contain (B1) at least one selected from the group consisting of tricarboxylic acids and tetracarboxylic acids, each having a molecular weight of 500 or less. This (B1) component has little adverse effect on the cleaning properties of flux residue. In addition, by combining this (B1) component with the (D) component described below, it is possible to improve the solder melting properties during air reflow while maintaining good ionic cleanliness. From the same viewpoint, the molecular weight of the (B1) component is preferably 400 or less, more preferably 300 or less, and particularly preferably 250 or less. Examples of the (B1) component include 1,2,3-propanetricarboxylic acid (molecular weight 176), 1,2,3,4-butanetetracarboxylic acid (molecular weight 234), trimellitic acid (molecular weight 210), etc. These may be used alone or in combination of two or more.

[0013] The blending amount of the (B1) component must be 1% by mass or more relative to 100% by mass of the flux composition. If the blending amount of the (B1) component is less than 1% by mass, the solder melting property during air reflow becomes insufficient. The blending amount of the (B1) component is preferably 1.2% by mass or more and 10% by mass or less relative to 100% by mass of the flux composition, more preferably 1.5% by mass or more and 7% by mass or less, and particularly preferably 1.5% by mass or more and 4% by mass or less. If the blending amount of the (B1) component is equal to or more than the lower limit, the solder melting property tends to be further improved, whereas if the blending amount is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.

[0014] The component (B) may contain an organic acid other than the component (B1) (hereinafter also referred to as the component (B2)). In addition, the component (B2) is preferably a dicarboxylic acid. Examples of the (B2) component include glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, eicosanedioic acid, and 8,13-dimethyl-8,12-eicosadienedioic acid. These may be used alone or in combination of two or more.

[0015] The blending amount of the (B2) component is preferably 1% by mass or more and 12% by mass or less, more preferably 2% by mass or more and 10% by mass or less, and particularly preferably 3% by mass or more and 8% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B2) component is equal to or more than the lower limit, the solder melting property tends to be further improved, while if it is equal to or less than the upper limit, the ionic cleanliness tends to be maintained at a good level.

[0016] In addition to the components (B1) and (B2), the component (B) may further contain another activator (hereinafter also referred to as the component (B3)) within the scope of the present invention. Examples of the component (B3) include halogen-based activators and amine-based activators.

[0017] The blending amount of the (B) component is preferably 2% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and particularly preferably 4% by mass or more and 12% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B) component is equal to or more than the lower limit, the activation action tends to be improved, whereas if it is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.

[0018] [(C) component] As the solvent (C) used in the present embodiment, a known solvent can be appropriately used. As such a solvent, it is preferable to use a solvent having a boiling point of 170° C. or higher. Examples of such solvents include diethylene glycol, dipropylene glycol, triethylene glycol, hexylene glycol, 1,5-pentanediol, methyl carbitol, butyl carbitol, 2-ethylhexyl diglycol, octanediol, phenyl glycol, diethylene glycol monohexyl ether (DEH), tetraethylene glycol dimethyl ether, dibutyl maleic acid, etc. These solvents may be used alone or in combination of two or more.

[0019] The blending amount of the (C) component is preferably 10% by mass or more and 60% by mass or less, and more preferably 20% by mass or more and 50% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the solvent is within the above range, the viscosity of the obtained solder composition can be appropriately adjusted to an appropriate range.

[0020] [(D) component] As the imidazole compound (D) used in the present embodiment, a known imidazole compound can be appropriately used. However, from the viewpoint of further reducing the adverse effect on the ionic cleanliness, the molecular weight of the imidazole compound is preferably 70 to 150, more preferably 70 to 120. Examples of component (D) include 2-methylimidazole (molecular weight 82.1), 2-ethylimidazole (molecular weight 96.1), 2-ethyl-4-methylimidazole (molecular weight 110.2), 1,2-dimethylimidazole (molecular weight 96.1), and 2-phenylimidazole (molecular weight 144.2).

[0021] In this embodiment, the mass ratio ((D) / (B1)) of the (D) component to the (B1) component must be 0.25 or more. If the mass ratio ((D) / (B1)) is less than 0.25, the solder melting property or ionic cleaning property becomes insufficient. From the same viewpoint, the mass ratio ((D) / (B1)) is preferably 0.3 to 5, more preferably 0.5 to 3, and particularly preferably 0.75 to 2.

[0022] The blending amount of component (D) is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 7% by mass, and particularly preferably 2% by mass to 5% by mass, based on 100% by mass of the flux composition. If the blending amount of component (D) is equal to or more than the lower limit, the solder melting property tends to be improved, while if it is equal to or less than the upper limit, the cleaning property of the flux residue tends to be maintained.

[0023] [(E) component] From the viewpoint of solder melting properties, the flux composition according to the present embodiment may further contain (E) a hindered phenol-based antioxidant. Examples of the hindered phenol antioxidant include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], N,N'-bis[2-[2-(3,5-di-tert-butyl-4-hydroxyphenyl)ethylcarbonyloxy]ethyl]oxamide, and N,N'-bis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl}hydrazine.

[0024] The blending amount of the (E) component is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.5% by mass or more and 4% by mass or less, and particularly preferably 1% by mass or more and 3% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (E) component is equal to or more than the lower limit, the solder melting property tends to be improved, whereas if the blending amount is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.

[0025] [Component (F)] The flux composition according to the present embodiment may further contain (F) a hindered amine antioxidant. The (F) component has a structure represented by the following general formula (F1). The (F) component can improve the solder melting property during air reflow.

[0026] [ka]

[0027] In general formula (F1), R 1 are independently a methyl group or an ethyl group, and are preferably a methyl group. X is hydrogen, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. When X is hydrogen, the structure is represented by the following general formula (F1-1). When X is an alkyl group having 1 to 12 carbon atoms, the structure is represented by the following general formula (F1-2). When X is an alkoxy group having 1 to 12 carbon atoms, the structure is represented by the following general formula (F1-3). In addition, in component (F), the structure of the portion beyond the wavy line is not particularly limited. The number of structures represented by general formula (F1) in one molecule of the component (F) is preferably 1 or more and 10 or less, and more preferably 2 or more and 4 or less.

[0028] [ka]

[0029] In general formula (F1-1), R 1 are independently a methyl group or an ethyl group, and are preferably a methyl group. Examples of compounds having a structure represented by general formula (F1-1) include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, and 2,2,6,6-tetramethyl-4-piperidyl methacrylate.

[0030] [ka]

[0031] In general formula (F1-2), R 1 are independently a methyl group or an ethyl group, and are preferably a methyl group. R 2 is an alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group. Examples of compounds having a structure represented by general formula (F1-2) include bis(1,2,2,6,6-pentamethyl-4-piperidyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]ethyl]butyl malonate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate.

[0032] [ka]

[0033] In general formula (F1-3), R 1 are independently a methyl group or an ethyl group, and are preferably a methyl group. R 3 is an alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 4 to 11 carbon atoms, more preferably an alkyl group having 8 to 11 carbon atoms, and particularly preferably an octyl group or an undecyl group. Examples of compounds having a structure represented by general formula (F1-3) include bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate and bis(1-undecaoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate.

[0034] The blending amount of the (F) component is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 3% by mass, and particularly preferably 1% by mass to 2% by mass, based on 100% by mass of the flux composition. If the blending amount of the (F) component is equal to or more than the lower limit, the solder melting property during air reflow tends to be improved, especially when the time to reach the melting temperature during reflow is long, while if the blending amount is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.

[0035] [Thixilation agent] The flux composition of the present embodiment may further contain a thixotropic agent from the viewpoint of printability, etc. Examples of the thixotropic agent used here include hardened castor oil, amides, kaolin, colloidal silica, organic bentonite, and glass frit. These may be used alone or in combination of two or more.

[0036] The amount of the thixotropic agent is preferably 1% by mass or more and 20% by mass or less, and more preferably 2% by mass or more and 12% by mass or less, based on 100% by mass of the flux composition. If the amount is less than the lower limit, thixotropy is not obtained and sagging tends to occur easily, while if the amount is more than the upper limit, the thixotropy is too high and printing defects tend to occur easily.

[0037] [Other ingredients] In addition to the (A), (B), (C), (D), (E), and (F) components and the thixotropic agent, other additives and even other resins can be added to the flux composition used in this embodiment as necessary. Examples of the other additives include antioxidants other than the (E) and (F) components, antifoaming agents, modifiers, matting agents, and foaming agents. The amount of these additives to be added is preferably 0.01% by mass or more and 5% by mass or less with respect to 100% by mass of the flux composition. Examples of the other resins include acrylic resins and polybutadiene.

[0038] [Solder composition] Next, the solder composition of the present embodiment will be described. The solder composition of the present embodiment contains the flux composition of the present embodiment described above and the solder powder (G) described below. The amount of the flux composition is preferably 5% by mass or more and 35% by mass or less, more preferably 7% by mass or more and 18% by mass or less, and particularly preferably 8% by mass or more and 15% by mass or less, relative to 100% by mass of the solder composition. When the amount of the flux composition is less than 5% by mass (when the amount of the solder powder is more than 95% by mass), the flux composition as a binder is insufficient, so that it tends to be difficult to mix the flux composition and the solder powder. On the other hand, when the amount of the flux composition is more than 35% by mass (when the amount of the solder powder is less than 65% by mass), when the obtained solder composition is used, it tends to be difficult to form a sufficient solder joint.

[0039] [(G) component] The solder powder (G) used in the present invention is preferably made of only lead-free solder powder, but may be lead-containing solder powder. The solder alloy in the solder powder preferably contains at least one selected from the group consisting of tin (Sn), copper (Cu), zinc (Zn), silver (Ag), antimony (Sb), lead (Pb), indium (In), bismuth (Bi), nickel (Ni), gold (Au), cobalt (Co) and germanium (Ge). The solder alloy in the solder powder is preferably an alloy mainly composed of tin. More preferably, the solder alloy contains tin, silver, and copper. Furthermore, the solder alloy may contain at least one of antimony, bismuth, and nickel as an additive element. According to the flux composition of the present embodiment, even when a solder alloy containing an additive element that is easily oxidized, such as antimony, bismuth, and nickel, is used, the generation of voids can be suppressed. Here, lead-free solder powder refers to a powder of solder metal or alloy to which no lead is added. However, the presence of lead as an unavoidable impurity in the lead-free solder powder is permitted, but in this case, the amount of lead is preferably 300 ppm by mass or less.

[0040] Specific examples of alloy systems for lead-free solder powder include Sn-Ag-Cu systems, Sn-Cu systems, Sn-Ag systems, Sn-Bi systems, Sn-Ag-Bi systems, Sn-Ag-Cu-Bi systems, Sn-Ag-Cu-Ni systems, Sn-Ag-Cu-Bi-Sb systems, Sn-Ag-Bi-In systems, and Sn-Ag-Cu-Bi-In-Sb systems.

[0041] The average particle size of component (G) is usually 1 μm or more and 40 μm or less, but from the viewpoint of being compatible with electronic boards having narrow pitches of solder pads, it is more preferably 1 μm or more and 35 μm or less, even more preferably 2 μm or more and 35 μm or less, and particularly preferably 3 μm or more and 32 μm or less. The average particle size can be measured by a dynamic light scattering type particle size measuring device.

[0042] [Method of manufacturing solder composition] The solder composition of this embodiment can be produced by blending the above-described flux composition and the above-described (G) solder powder in the above-described predetermined ratio, and stirring and mixing them.

[0043] [Electronic board manufacturing method] Next, a method for manufacturing an electronic board according to the present embodiment will be described. The method for manufacturing an electronic board according to the present embodiment is characterized by using the solder composition described above. According to the method for manufacturing an electronic board according to the present embodiment, an electronic board can be manufactured by mounting electronic components on an electronic board (such as a printed wiring board) using the solder composition. The solder composition of the present embodiment described above has excellent cleaning properties for flux residues with an aqueous cleaner, so that the flux residues can be easily cleaned with an aqueous cleaner after soldering. In the method for producing an electronic substrate according to the present embodiment, first, a solder composition is applied onto the electronic substrate by a coating device. Examples of the coating device used here include a screen printer, a metal mask printer, a dispenser, and a jet dispenser. In addition, an electronic component can be mounted on an electronic board by a reflow process in which an electronic component is placed on the solder composition applied by the application device and heated under specified conditions in a reflow furnace to mount the electronic component on a printed wiring board.

[0044] In the reflow process, the electronic component is placed on the solder composition and heated under predetermined conditions in a reflow furnace. This reflow process allows sufficient solder bonding between the electronic component and the printed wiring board. As a result, the electronic component can be mounted on the printed wiring board. The atmosphere during reflow may be a nitrogen atmosphere, but since the solder composition of the present embodiment described above has excellent solder melting properties in air reflow, it may be left in air. The reflow conditions may be appropriately set according to the melting point of the solder. For example, the preheat temperature is preferably 140°C or higher and 200°C or lower, and more preferably 150°C or higher and 160°C or lower. The preheat time is preferably 60 seconds or higher and 120 seconds or lower. The peak temperature is preferably 230°C or higher and 270°C or lower, and more preferably 240°C or higher and 255°C or lower. The holding time at a temperature of 220°C or higher is preferably 20 seconds or higher and 60 seconds or lower.

[0045] After the reflow process, flux residues on the electronic substrate are cleaned using a water-based cleaner. The cleaning method may be a dipping method, a jet method, or the like. For example, in the immersion method, the electronic substrate is immersed in a water-based cleaning agent, and ultrasonic waves may be applied at this time. As the water-based cleaner, a known water-based cleaner for flux residue can be used. Here, water-based refers to a cleaner whose main component is water (water is 50% by mass or more). Commercially available products include "VIGON US" manufactured by Zestron Japan Co., Ltd. The temperature of the aqueous cleaner during cleaning is, for example, 30° C. or higher and 70° C. or lower. The cleaning time is, for example, from 1 minute to 10 minutes. After cleaning with the aqueous cleaner, rinsing may be performed. The conditions for rinsing are not particularly limited, and the rinsing may be performed with water at 20° C. to 50° C. for 0.5 minutes to 5 minutes. Rinsing may be performed two or more times.

[0046] Furthermore, the solder composition and electronic substrate of the present embodiment are not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. For example, in the manufacturing method of the electronic board, the printed wiring board and the electronic component are bonded by a reflow process, but the present invention is not limited thereto. For example, instead of the reflow process, the printed wiring board and the electronic component may be bonded by a process of heating the solder composition using a laser beam (laser heating process). In this case, the laser light source is not particularly limited and can be appropriately adopted according to the wavelength that matches the absorption band of the metal. Examples of the laser light source include solid lasers (ruby, glass, YAG, etc.), semiconductor lasers (GaAs, InGaAsP, etc.), liquid lasers (dye, etc.), and gas lasers (He-Ne, Ar, CO2, excimer, etc.). EXAMPLES

[0047] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples. The materials used in the examples and comparative examples are shown below. (Component (A)) Rosin-based resin A: Polymerized rosin, product name "China Polymerized Rosin 140", manufactured by Arakawa Chemical Industries Co., Ltd. Rosin resin B: Acrylic acid modified hydrogenated rosin, product name "Pine Crystal KE-604", manufactured by Arakawa Chemical Industries Co., Ltd. Rosin-based resin C: Formylated rosin, trade name "FORAL-AX", manufactured by Eastman Chemical Company Rosin-based resin D: Special modified rosin, product name "Haritac FG-90", manufactured by Harima Chemicals Co., Ltd. ((B1) component) Organic acid A: 1,2,3-propanetricarboxylic acid (molecular weight 176), trade name "Rikacid TCR-100", manufactured by New Japan Chemical Co., Ltd. Organic acid B: 1,2,3,4-butanetetracarboxylic acid (molecular weight 234), trade name "Rikacid BT-W", manufactured by New Japan Chemical Co., Ltd. Organic acid C: Trimellitic acid (molecular weight 210) ((B2) component) Organic Acid D: Glutaric Acid Organic Acid E: Adipic Acid Organic acid F: Sebacic acid Organic acid G: Dodecanedioic acid Organic acid H: Eicosanedioic acid, trade name "SL-20", manufactured by Okamura Oil Mills ((C) component) Solvent: Diethylene glycol monohexyl ether (DEH, hexyl diglycol) ((D) component) Imidazole compound A: 2-ethyl-4-methylimidazole (molecular weight 110.2), trade name "2E4MZ", manufactured by Shikoku Chemical Industry Co., Ltd. Imidazole compound B: 2-methylimidazole (molecular weight 82.1), trade name "2MZ", manufactured by Shikoku Chemical Industry Co., Ltd. Imidazole compound C: 2-ethylimidazole (molecular weight 86.1), trade name "2EZ", manufactured by Shikoku Chemical Industry Co., Ltd. Imidazole compound D: 2-phenylimidazole (molecular weight 144.2), trade name "2PZ", manufactured by Shikoku Chemical Industry Co., Ltd. ((E) component) Hindered phenol antioxidant: bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], trade name "Irganox 245", manufactured by BASF (Component (F)) Hindered amine antioxidant: a compound having two structures represented by the general formula (F1-2) in one molecule, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]ethyl]butylmalonate, trade name "Tinuvin PA144", manufactured by BASF (Other ingredients) Thixotropic agent A: Product name "Slipax H", manufactured by Nippon Kasei Co., Ltd. Thixotropic agent B: Trade name "Himako", manufactured by KF Trading Co., Ltd. Additive: Polybutadiene, product name "BI-2000", manufactured by Nippon Soda Co., Ltd. ((G) component) Solder powder: alloy composition is Sn-3.0Ag-0.5Cu, particle size distribution is 20~38μm, solder melting point is 217~220℃

[0048] [Example 1] 25 mass% rosin-based resin A, 15 mass% rosin-based resin B, 1 mass% organic acid A, 8 mass% organic acid H, 35 mass% solvent, 1.5 mass% imidazole compound A, 2 mass% hindered phenol-based antioxidant, 1 mass% hindered amine-based antioxidant, 4 mass% additive, 7 mass% thixotropic agent A, and 0.5 mass% thixotropic agent B were charged into a container and mixed using a planetary mixer to obtain a flux composition. Thereafter, 12% by mass of the obtained flux composition and 88% by mass of the solder powder (total of 100% by mass) were placed in a container and mixed with a planetary mixer to prepare a solder composition.

[0049] [Examples 2 to 18] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1. [Comparative Examples 1 to 5] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1.

[0050] <Evaluation of solder composition> The solder compositions were evaluated (ionic cleanliness, cleaning properties, solder melting properties (air reflow), and wetting effectiveness) by the following methods. The results are shown in Table 1. (1) Ionic cleanliness A solder composition was printed on a JIS2-type comb-shaped substrate, and the solder composition was melted in a reflow furnace (manufactured by Tamura Manufacturing Co., Ltd.) to obtain a substrate for evaluation. The reflow conditions were a preheat temperature of 130 to 180°C (about 100 seconds), a time at a temperature of 220°C or higher for about 60 seconds, a peak temperature of 240°C, and a nitrogen atmosphere with an oxygen concentration of 1000 ppm. The substrate for evaluation was set in an omegameter, and a 75% IPA solution was injected into the test cell as a test liquid, and the change in the resistance value of the test liquid was obtained to calculate the eluted ions of the specimen. The amount of eluted ions was converted into a NaCl equivalent value to be the ionic cleanliness. The ionic cleanliness was evaluated according to the following criteria. ○: Ionic cleanliness is 1.50μgNaCl / cm 2 is less than. △: Ionic cleanliness is 1.50μgNaCl / cm 2 More than 1.60μgNaCl / cm 2 is less than. ×: Ionic cleanliness is 1.60 μg NaCl / cm 2 That's all. (2) Cleanability A solder composition was printed on a substrate capable of mounting chip components, chip components (size: 1.6 mm x 0.8 mm) were mounted, and the solder composition was melted and soldered in a reflow furnace (manufactured by Tamura Corporation) to obtain a substrate for evaluation. The reflow conditions were a preheat temperature of 130 to 180°C (approximately 100 seconds), a time at a temperature of 220°C or higher for approximately 60 seconds, a peak temperature of 240°C, and a nitrogen atmosphere with an oxygen concentration of 1000 ppm. Next, the obtained evaluation substrate was immersed in a container containing a water-based cleaning agent (Zestron Japan's "VIGON US", 20% concentration) and cleaned with ultrasonic waves (liquid temperature: 60°C, cleaning time: 5 minutes). After that, the liquid was removed with an air knife, and the substrate was immersed in a container containing pure water at room temperature for a first rinse (rinsing time: 1 to 2 minutes), and further immersed in a container containing pure water at 45°C for a second rinse (rinsing time: 1 to 2 minutes). After that, the liquid was removed with an air gun, and the substrate was dried in a hot air drying furnace (furnace temperature: 70°C) for 10 minutes. After cleaning with the aqueous cleaner, all chips were removed from the evaluation board and the presence or absence of flux residue under the chips was observed. The number of chips with residual flux and the ratio to the total number of chips (residual ratio) were then measured, and the cleaning performance was evaluated based on the residual ratio according to the following criteria. ◯: The residual ratio is less than 25%. △: The residual ratio is 25% or more and less than 50%. ×: The residual ratio is 50% or more. (3) Solder melting property (air reflow) A solder composition was printed on a substrate capable of mounting chip components, a 1005 chip component (size: 1.0 mm x 0.5 mm) was mounted, and the solder composition was melted and soldered in a reflow furnace (manufactured by Tamura Corporation) to obtain a substrate for evaluation. The reflow conditions were air reflow, a preheat temperature of 130 to 180°C (approximately 100 seconds), a time at a temperature of 220°C or higher for approximately 60 seconds, and a peak temperature of 240°C. The number of unmelted portions in the chip bonding portions of the evaluation board was then counted, and the solder melting property (air reflow) was evaluated according to the following criteria. ◯: The unmelted ratio is less than 50%. △: The unmelted ratio is 50% or more and less than 70%. ×: The unmelted ratio is 70% or more. (4) Wetting Efficiency The solder wettability (dewetting) test is performed according to the method described in JIS Z 3284 (2014). That is, two types of metal plates A (brass, size: 30 mm x 30 mm, thickness: 0.3 mm) and metal plate B (42 alloy, size: 30 mm x 30 mm, thickness: 0.3 mm) are prepared and polished with an abrasive. A solder composition is printed on the metal plate using a metal mask having a thickness of 0.2 mm and a circular pattern hole with a diameter of 6.5 mmφ to obtain a test plate. The test plate is heated in a solder bath maintained at 270°C and melted for 5 seconds. The test plate is observed under a microscope, the wet spread area ratio is measured, and the wettability (brass, 42 alloy) is evaluated according to the following criteria. ◯: The wet spread area ratio is 70% or more. Δ: The wet spread area ratio is 50% or more and less than 70%. ×: The wet spread area ratio is less than 50%.

[0051] [Table 1]

[0052] As is clear from the results shown in Table 1, the solder compositions of the present invention (Examples 1 to 18) were confirmed to have good results in all aspects of ionic cleanliness, cleaning properties, solder melting properties (air reflow), and wetting effectiveness. Therefore, it was confirmed that the solder composition of the present invention has good ionic cleanliness, is excellent in cleaning ability for flux residues with an aqueous cleaner, and is excellent in solder melting property during air reflow. [Industrial Applicability]

[0053] The flux composition and solder composition of the present invention can be suitably used as a technique for mounting electronic components on electronic substrates such as printed wiring boards of electronic devices.

Claims

1. A flux composition comprising: (A) a rosin-based resin; (B) an activator; (C) a solvent; and (D) an imidazole compound, The component (B) contains (B1) at least one selected from the group consisting of tricarboxylic acids and tetracarboxylic acids, each having a molecular weight of 500 or less, The blending amount of the (B1) component is 1 mass% or more with respect to 100 mass% of the flux composition, a mass ratio ((D) / (B1)) of the component (D) to the component (B1) is 0.25 or more; Flux composition.

2. 2. The flux composition according to claim 1, Further, (E) a hindered phenol-based antioxidant is contained, Flux composition.

3. The flux composition according to claim 1 or 2, Further, (F) a hindered amine-based antioxidant is contained. Flux composition.

4. A flux composition according to claim 1 or 2, and (G) a solder powder. Solder composition.

5. The solder composition according to claim 4, The solder alloy in the component (G) contains at least one selected from the group consisting of tin, copper, zinc, silver, antimony, lead, indium, bismuth, nickel, gold, cobalt, and germanium. Solder composition.

6. A method for manufacturing an electronic substrate by soldering using the solder composition according to claim 4, comprising the steps of: applying the solder composition onto an electronic substrate; placing an electronic component on the solder composition; a step of mounting the electronic component on the electronic board by heating under predetermined conditions in a reflow furnace; and cleaning the flux residue on the electronic substrate using a water-based cleaning agent. A method for manufacturing electronic boards.

Citation Information

Patent Citations

  • Air pressure spot coating soldering paste for connector

    CN101992361A

  • Soldering flux

    JP1986501377A

  • Flux for soldering

    JP1992037497A

  • Solder composition and electronic substrate

    JP2019018210A

  • Flux and solder paste

    JP2021130115A