Aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, production method therefor, and method for producing active material for lithium secondary battery
An aqueous solution with niobium polyacid ions and phosphate ions stabilizes the lithium niobate coating on lithium ion battery electrodes, addressing interfacial resistance and specific surface area issues, thereby improving battery performance and stability.
Patent Information
- Application Number
- JP2024048652
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-09
AI Technical Summary
Existing lithium ion secondary batteries face issues with increased interfacial resistance and specific surface area after coating with lithium niobate, leading to performance deterioration and moisture absorption, which affects storage stability.
An aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is used to coat the positive electrode active material, with specific molar ratios and concentrations to stabilize the coating layer and suppress specific surface area increase, ensuring improved storage stability and ionic conductivity.
The solution provides a stable coating layer with reduced specific surface area, enhancing the performance and storage stability of all-solid-state lithium ion secondary batteries by minimizing moisture absorption and maintaining ionic conductivity.
Smart Images

Figure 2024139753000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions for coating the surfaces of positive electrode active material particles of a lithium ion secondary battery with lithium niobate as a solid electrolyte, a method for producing the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, and a method for producing an active material for lithium secondary batteries having a coating layer containing lithium niobate. [Background technology]
[0002] The positive electrode active material of lithium-ion secondary batteries has generally been composed of a composite oxide of lithium and a transition metal. Among them, lithium cobalt oxide (LiCoO2), a composite oxide containing Co, is widely used. Recently, lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), or ternary oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2) and their combinations are also on the rise.
[0003] The electrolyte for lithium ion secondary batteries is mainly made by dissolving lithium salts such as electrolyte LiPF6 and LiBF4 in a mixed solvent of cyclic carbonate esters such as PC (propylene carbonate) and EC (ethylene carbonate) and chain esters such as DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), and DEC (diethyl carbonate). Such organic solvents are weak in an oxidizing atmosphere, and are prone to oxidative decomposition reactions when they come into contact with transition metals such as Co, Ni, and Mn, especially on the positive electrode surface. Possible causes of this include the high potential of the positive electrode surface and the catalytic action of transition metals in a highly oxidized state. Therefore, it is effective to prevent contact between the electrolyte and the transition metals (e.g., one or more of Co, Ni, and Mn) that constitute the positive electrode active material as much as possible in order to maintain the performance of the electrolyte.
[0004] As a method for fundamentally solving the problems associated with the organic solvent-based electrolyte, an all-solid-state lithium ion secondary battery has been proposed in which the electrolyte is replaced with a non-flammable solid electrolyte. In general, the electrode reaction of a battery occurs at the interface between the electrode active material and the electrolyte. When a liquid electrolyte is used, the electrolyte penetrates the surface of the electrode active material present on the electrode, forming a reaction interface for charge transfer. In the case of an all-solid-state battery, a solid electrolyte having ion conductivity plays the role of the electrolyte, but since the solid electrolyte itself does not have the fluidity of a liquid, it is necessary to mix the powder that will become the electrode active material with the solid electrolyte or to coat the powder that will become the electrode active material with the solid electrolyte before constructing the secondary battery.
[0005] However, in the case of all-solid-state lithium-ion secondary batteries, there is a problem that the resistance (hereinafter, sometimes referred to as "interface resistance") that occurs when lithium ions move across the interface between the positive electrode active material and the solid electrolyte increases, and the performance of the all-solid-state lithium-ion secondary battery, such as the battery capacity, is likely to decrease. The increase in the interface resistance is believed to be caused by the reaction between the positive electrode active material and the solid electrolyte, resulting in the formation of high-resistance sites on the surface of the positive electrode active material, and it is known that the interface resistance can be reduced by coating the surface of lithium cobalt oxide, which is the positive electrode active material, with lithium niobate.
[0006] For example, Patent Document 1 discloses a technique for wet coating the surface of a positive electrode active material with a lithium ion conductive oxide containing niobium or tantalum and lithium by a wet method in order to improve the interface resistance between the positive electrode active material and the solid electrolyte. However, this coating technique uses alkoxides of niobium or tantalum as a source of niobium or tantalum, and absolute alcohol, a volatile organic compound, as a solvent, so there is a concern that the working environment may deteriorate. In addition, this coating technique also has cost problems, such as the need for explosion-proof measures for the device used for coating.
[0007] In order to solve these problems, for example, Patent Document 2 discloses a coating method for lithium niobate using water as a solvent. The coating solution for lithium niobate disclosed in Patent Document 2 is a solution in which niobium oxide, which is poorly soluble in water, is made water-soluble as a peroxo complex or an oxalate complex. For this reason, in the case of the coating solution for lithium niobate using the peroxo complex disclosed in Patent Document 2, it is necessary to add 8 moles or more of hydrogen peroxide to 1 mole of niobic acid, and since niobic acid does not dissolve in hydrogen peroxide water, it is necessary to further add 1 mole or more of ammonia to 1 mole of niobic acid. However, in the case of the coating solution, there is a problem that the storage stability is poor because the peroxo complex is chemically unstable. In addition, in the case of the coating solution, there is also a problem that the metal component of the positive electrode active material to be coated is eluted by the ammonia added to the coating solution.
[0008] As a technique for improving the chemical stability of a niobium peroxo complex, for example, Patent Document 3 discloses a technique of adding phosphate ions to a coating solution of lithium niobate. In this case, although it is not explicitly stated in Patent Document 3, it is considered that the phosphate ions act as a negative catalyst against the decomposition reaction of hydrogen peroxide. However, in the case of this coating solution, a large amount of hydrogen peroxide and ammonia are required to convert niobium into a peroxo complex, and the chemical stability is insufficient, and the problem of the metal components of the positive electrode active material being eluted is not solved.
[0009] As an aqueous solution-based lithium niobate coating liquid having excellent chemical stability, a precursor aqueous solution of lithium niobate using niobium polyacid ions and a method for producing the same are disclosed in Patent Document 4. In the case of this precursor aqueous solution, niobium is water-soluble in the form of polyacid ions, and ammonia is not used, so there is no problem of elution of metal components of the positive electrode active material. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. 2007 / 004590 [Patent Document 2] JP 2012-074240 A [Patent Document 3] JP 2017-191667 A [Patent Document 4] JP 2020-066570 A Summary of the Invention [Problem to be solved by the invention]
[0011] The aqueous precursor solution of lithium niobate disclosed in Patent Document 4 is a coating solution having excellent characteristics, such as excellent storage stability of the solution and suppressing dissolution of the positive electrode active material during coating. However, when the aqueous precursor solution is used to coat the surface of the positive electrode active material with lithium niobate, there is a problem in that the specific surface area of the lithium niobate-coated positive electrode active material becomes larger than that of the positive electrode active material before coating.
[0012] It is presumed that the increase in the specific surface area after coating is due to the formation of extremely fine pores in the coating layer of lithium niobate. If the coating layer becomes porous, moisture may be adsorbed onto the surface of the positive electrode active material through the pores, which may lead to deterioration of the positive electrode active material. In addition, if the coating layer becomes porous, the area of the interface between the coating layer, which is a solid electrolyte, and the positive electrode active material decreases, which is undesirable.
[0013] The present invention aims to provide an aqueous lithium niobate precursor solution that suppresses an increase in the specific surface area of a lithium niobate-coated positive electrode active material and has excellent storage stability when the surfaces of positive electrode active material particles of a lithium ion secondary battery are coated with lithium niobate, which is a solid electrolyte, and a method for producing the same. [Means for solving the problem]
[0014] [1] In order to achieve the above object, the present invention provides an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, in which the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution is 0.04 or more and less than 0.5, and the molar ratio Li / Nb of lithium to niobium is more than 0.6 and 2.0 or less. [2] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions in the above item [1] may further contain 0.01% by mass or more and 10% by mass or less of hydrogen peroxide. [3] The aqueous solution containing the niobium polyacid ion, lithium ion, and phosphate ion described in [2] above is dissolved in water at a ratio of 0.01 moles of hydrogen peroxide to niobium (PO C / Nb) is preferably 0.01 or more and 1 or less. [4] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [1] preferably has an absorbance of 0.1 or less at a wavelength of 660 nm. [5] Furthermore, the present invention provides a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, the method comprising the steps of: dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions; and adding phosphate ions to the aqueous solution containing niobium polyacid ions and lithium ions. [6] Furthermore, the present invention provides a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, the method comprising the steps of: dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions; and adding phosphate ions and hydrogen peroxide to the aqueous solution containing niobium polyacid ions and lithium ions. [7] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [5] or [6], it is preferable that the ratio of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus, P / (Nb+Li+P), is 0.04 or more and less than 0.5, and the molar ratio of lithium to niobium, Li / Nb, is more than 0.6 and 2.0 or less. [8] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [6], the concentration of hydrogen peroxide in the aqueous solution is preferably 0.01% by mass or more and 10% by mass or less. [9] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions as described in [6] above, the molar ratio of niobium to the amount of hydrogen peroxide added (PO A It is preferable that the value of Nb) is 0.1 or more and 1.0 or less.
[10] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [5] or [6], it is preferable to add phosphate ions at a rate of 0.07 mol / min or more and 3.07 mol / min or less per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions.
[11] The present invention further provides a method for producing a lithium secondary battery having a coating layer containing lithium niobate, comprising the steps of: coating a surface of an active material for lithium secondary batteries with an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions as described in any one of items [1] to [4] above; and heat treating the active material for lithium secondary batteries that has been coated. Effect of the Invention
[0015] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions obtained by the production method of the present invention has excellent storage stability, and even if the aqueous solution is used to form a coating layer on the surface of a positive electrode active material for a lithium ion secondary battery, an increase in the specific surface area is suppressed. Therefore, the present invention can contribute to improving the performance of all-solid-state lithium ion secondary batteries. [Brief description of the drawings]
[0016] [Figure 1] FT-IR spectra of the aqueous solutions obtained in Comparative Example 1 and Example 3.
BEST MODE FOR CARRYING OUT THE INVENTION
[0017] [Positive electrode active material] The positive electrode active material coated with the aqueous solution containing the polyacid ion of niobium, lithium ion and phosphate ion of the present invention is outside the scope of the present invention, but examples thereof include the following. The positive electrode active material is composed of a composite oxide of Li and transition metal M, and is a material conventionally used in lithium ion secondary batteries, such as lithium cobalt oxide (Li 1+X CoO2, -0.1 ≦ X ≦ 0.3), Li 1+X NiO2, Li 1+X Mn2O4, Li 1+X Ni 1 / 2 Mn 1 / 2 O2, Li 1+X Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (all -0.1 ≦ X ≦ 0.3), Li 1+X [Ni Y Li 1 / 3-2Y / 3 Mn 2 / 3-Y / 3 O2 (0 ≦ X ≦ 1, 0 < Y < 1 / 2), etc., lithium transition metal oxides in which a part of these Li or transition metal elements is substituted with Al or other elements, Li 1+X FePO4, Li 1+X MnPO4 (all -0.1 ≦ X ≦ 0.3), etc., phosphates having an olivine structure, and spinel-type compounds such as lithium manganate (LiMnO4) and those in which a part of Mn is substituted with Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Ni, Co, Fe, etc. (LiAl 0.1 Mn 0.9 O4, LiNi 0.5 Mn 1.5 O4, etc.).
[0018] [Nb source] Since anhydrous niobium oxide (Nb2O5) is poorly soluble in water, the manufacturing method of the present invention uses amorphous, water-soluble niobium oxide as the Nb source. Niobium oxide hydroxide is a substance represented by the general formula Nb2O5·nH2O (n is not 0, for example, 3≦n≦16).
[0019] [Polyacid ion] Polyacids are anionic species formed by the condensation of oxoacids, and polyacids of transition metal elements can be considered to be molecular ionic species of metal oxides. When there is only one type of metal element, they are called isopolyacids, and when there are multiple metal elements, they are called heteropolyacids.
[0020] The potential-pH diagram for niobium has not been established at present, but since niobium hydroxide precipitates in the neutral region, it is thought that solid phases such as Nb(OH)5 or HNbO3 are stable species in the relevant pH region. When an alkali is added to an aqueous solution containing these solid phases to raise the pH of the system, the excess OH - The presence of ions causes niobium to react with e.g. Nb(OH)6 - and NbO3 - etc. When the pH of the system is further increased, it is considered that the soluble niobium oxide will take various condensation states depending on the pH of the system, but in this specification, it is considered that the niobium oxide solubilized on the alkaline side will collectively become a polyacid ion of niobium. Note that the polyacid ion of niobium once solubilized on the alkaline side will maintain the form of a polyacid even if phosphoric acid is added and the pH of the system is lowered to about 4. The aqueous solution of the present invention containing the polyacid ion of niobium, lithium ion, and phosphate ion contains niobium in the form of a polyacid, and therefore has excellent storage stability. The form of niobium may be a soluble polyacid ion, and its structure is not particularly limited. The fact that niobium in an aqueous solution is in the form of a polyacid ion can be confirmed by FT-IR measurement. When niobium in an aqueous solution is in the form of a polyacid ion, the FT-IR spectrum is at a wave number of 850 cm -1 ±20cm -1 An absorption peak due to Nb-O bonds is observed near the
[0021] [Li source] In the manufacturing method of the present invention, lithium hydroxide (LiOH) is used as the Li source. The LiOH may be either anhydrous or hydrated. The LiOH added to the aqueous solution is Li + and OH - and exhibits strong alkalinity. In the method for producing a precursor aqueous solution of lithium niobate described in Patent Documents 2 and 3, niobic acid and hydrogen peroxide are reacted first, then ammonia water is added to increase the pH, and finally a Li salt is added to adjust the precursor aqueous solution. In contrast, the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention is characterized in that LiOH is first added to an aqueous solution containing niobic acid to dissolve the niobic acid.
[0022] LiOH is itself a strong alkali, so when LiOH is added to an aqueous solution containing niobic acid, the pH of the system rises, dissolving the niobium oxide and forming a stable polyoxygen ion of niobium. Hydrogen peroxide is then added to the alkaline aqueous solution containing the polyoxygen ion of niobium and lithium ions, but the effect of hydrogen peroxide will be described later.
[0023] Since a coating layer of a solid electrolyte having ion conductivity is ultimately formed, the amount of lithium added is preferably set to a molar ratio Li / Nb of more than 0.6 and not more than 2.0 relative to 1 mole of niobium contained in the niobium polyacid ion. If Li / Nb is 0.6 or less, lithium ion conductivity is deteriorated due to lithium deficiency, which is not preferable. Also, if Li / Nb exceeds 2.0, storage stability is deteriorated due to an increase in pH caused by excess lithium hydroxide, which is not preferable. From the viewpoint of ion conductivity, Li / Nb is preferably 0.9 or more, more preferably 0.95 or more. From the viewpoint of ion conductivity, Li / Nb is preferably 1.5 or less, more preferably 1.4 or less.
[0024] The reason why the storage stability of the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention is better than that of the aqueous precursor solutions obtained by the techniques described in Patent Documents 2 and 3 is presumed to be as follows. In the techniques described in Patent Documents 2 and 3, niobium exists in the form of a peroxo complex in an aqueous solution, and it is known that the peroxo ion coordinated to niobium is easily released and is unstable. In contrast, the niobium in the aqueous solution containing the polyacid ions, lithium ions, and phosphate ions of the present invention is considered to be mainly in the form of a relatively stable polyacid. Adding hydrogen peroxide to the aqueous solution further improves the storage stability. The aqueous solution of the present invention does not contain organic matter, unlike the coating solution described in Non-Patent Document 1, and therefore a coating layer with a low volume resistivity can be obtained in the end.
[0025] [Phosphate ion] The greatest technical feature of the present invention is that phosphate ions are made to coexist in an aqueous solution containing niobium polyphosphate ions and lithium ions. The source of phosphate ions is water-soluble phosphoric acid (PO4 3- ) salts can be used. Phosphoric acid is a tribasic acid that dissociates in three stages in an aqueous solution, and therefore can exist in various forms in the aqueous solution, such as phosphate ion, monohydrogen phosphate ion, dihydrogen phosphate ion, and pyrophosphate ion, but the form is determined by the pH of the aqueous solution, not by the type of chemical used as the phosphate ion source, and therefore the above ions containing a phosphate group are collectively referred to as phosphate ions. In the case of the aqueous solution containing the niobium polyacid ion, lithium ion and phosphate ion of the present invention, the FT-IR measurement shows that -1 An absorption peak due to phosphate ions is observed.
[0026] The reason why the coexistence of niobium polyacid ions and phosphate ions in an aqueous lithium ion solution suppresses the increase in the specific surface area of the coated positive electrode active material is unclear at present, but the inventors speculate as follows. That is, possible mechanisms include the presence of phosphate ions contained in the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions of the present invention improving the wettability of the aqueous solution to the surface of the positive electrode active material, the action of the phosphate ions contained in the aqueous solution changing the double layer structure at the interface, thereby changing the structure of the coating layer, or a trace amount of phosphate ions contained in the coating layer suppresses the generation of pores in the coating layer during drying.
[0027] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention, the phosphate ion aqueous solution is added to an aqueous solution containing lithium and niobium polyacid in which niobium polyacid ions are stably formed, thereby suppressing the precipitation of niobic acid in the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions. In this case, a large amount of precipitate (colloid) mainly composed of Li3PO4 and the like may be generated due to a sudden increase in the phosphate ion concentration. If the concentration of colloid particles in the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is high, it is not preferable because it causes an increase in the specific surface area of the coated positive electrode active material.
[0028] In order to prevent the generation of colloids, it is preferable to adjust the rate of addition of the aqueous phosphate ion solution to the aqueous solution containing niobium polyacid ions and lithium ions. In order to prevent the generation of colloids, the rate of addition of the aqueous phosphate ion solution is preferably 3.07 mol / min or less of phosphate ions per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions. More preferably, it is 2 mol / min or less, and even more preferably, it is 1 mol / min or less or 0.6 mol / min or less. The lower limit of the addition rate is not particularly limited, but may be, for example, 0.07 mol / min or more from the viewpoint of production time.
[0029] The occurrence of the colloid can be confirmed by the absorbance value at a wavelength of 660 nm in an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions. This is because the absorbance at a wavelength of 660 nm indicates the intensity of scattered light caused by colloidal particles present in an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions. Therefore, high absorbance in the precursor solution according to the present invention suggests that the concentration of particles present in the aqueous solution is high (see, for example, JIS-K0101).
[0030] If the positive electrode active material is coated with an aqueous solution having a high concentration of the fine particles, the fine particles will adhere to the surface of the positive electrode active material, making the coating layer uneven, and the thickness of the coating layer will be non-uniform, which may cause an increase in the specific surface area. According to the study by the present inventors, if the absorbance value at a wavelength of 660 nm of an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is 0.1 or less, even if colloidal fine particles are present in the aqueous solution, the amount of the fine particles is small, and the coating layer thickness is prevented from becoming non-uniform, and the increase in the specific surface area is also suppressed. More preferably, the absorbance value is 0.08 or less, and even more preferably, 0.07 or less. In the present invention, the lower limit of the absorbance is not particularly specified, but it may be, for example, 0.001 or more.
[0031] The content of phosphate ions in an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is preferably such that the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution is 0.04 or more and less than 0.5. If the ratio is less than 0.04, the effect of adding phosphate ions is insufficient. From the viewpoint of ionic conductivity, P / (Nb+Li+P) is preferably 0.08 or more. If the value of P / (Nb+Li+P) is 0.5 or more, the effect of adding phosphate ions is saturated. From the viewpoint of ionic conductivity, P / (Nb+Li+P) is preferably 0.35 or less. The range of P / (Nb+Li+P) is more preferably 0.1 or more and 0.4 or less, and even more preferably 0.2 or more and 0.4 or less.
[0032] The sum of the contents of lithium, niobium and phosphorus in the aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions is preferably 1% by mass or more and 20% by mass or less. More preferably, it is 3% by mass or more and 10% by mass or less. Even more preferably, it is 5% by mass or more and 8% by mass or less. If the sum of the contents of lithium, niobium and phosphorus is less than 1% by mass, it is necessary to increase the amount of the aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions in order to obtain the required thickness of the coating layer, and the water content increases, which is disadvantageous in terms of cost. If the concentration is low, the water content increases to achieve the required coating thickness, which is not economical. If the sum of the contents of lithium, niobium and phosphorus exceeds 20% by mass, the viscosity of the aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions increases, which may cause clogging of thin piping in the device used for the coating process.
[0033] The amount of impurity elements other than lithium, niobium, phosphorus, oxygen, and hydrogen in the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is preferably 10% by mass or less. More preferably, it is 1% by mass or less. Carbonate ions and the like are considered as inevitable impurities. Here, the impurities refer to impurities contained in the evaporation residue when the precursor aqueous solution is evaporated to dryness at 200°C. When evaporated to dryness at 200°C, the carbonate ions combine with counter cations and precipitate as carbonate salts.
[0034] [hydrogen peroxide] The aqueous solution of the present invention may further contain hydrogen peroxide to improve storage stability. In this case, hydrogen peroxide is preferably added so that the concentration of the aqueous solution is 0.01% by mass or more and 10% by mass or less. If the concentration of hydrogen peroxide is less than 0.01% by mass, the generated niobium polyacid reacts with hydroxide ions and is easily decomposed. If the concentration of hydrogen peroxide is more than 10% by mass, the generated niobium polyacid may react with hydrogen peroxide to form an unstable peroxo complex. The concentration of hydrogen peroxide in the aqueous solution is preferably 0.05% by mass or more and 5% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less.
[0035] The ratio of the moles of hydrogen peroxide to the moles of niobium added (PO A The molar ratio (PO / Nb) is preferably in the range of 0.1 to 1. A ratio of 0.1 or more is advantageous in avoiding decomposition of the niobium polyacid through reaction with hydroxide ions. A ratio of 1 or less is advantageous in avoiding the formation of an unstable peroxo complex through reaction of the generated niobium polyacid with hydrogen peroxide. A / Nb) is preferably 0.05 or more and 0.5 or less, and more preferably 0.1 or more and 0.35 or less. From the viewpoint of reactivity, the hydrogen peroxide is preferably added after dissolving hydrous niobium oxide with LiOH to form stable polyoxygen ions of niobium. Note that the addition of the phosphate ions and the hydrogen peroxide in this section may be added in any order.
[0036] Here, the added hydrogen peroxide decomposes over time, but it is preferable that the aqueous solution contains 0.01% by mass or more and 6.7% by mass or less of hydrogen peroxide. If the hydrogen peroxide content is less than 0.01% by mass, the effect of maintaining the stability of the precursor aqueous solution is small. If the hydrogen peroxide content exceeds 6.7% by mass, the effect of adding hydrogen peroxide becomes saturated. The concentration of hydrogen peroxide in the aqueous solution is preferably 0.05% by mass or more and 5% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less.
[0037] In addition, the ratio of the number of moles of hydrogen peroxide to 1 mole of niobium (PO C The ratio of hydrogen peroxide to hydrogen peroxide is preferably in the range of 0.01 to 1. If the amount of hydrogen peroxide exceeds the above range, not only will the effect of hydrogen peroxide be saturated, but if the hydrogen peroxide is used as a coating liquid, the positive electrode active material may be dissolved. If the amount of hydrogen peroxide is too small, the niobium polyacid reacts with hydroxide ions and is easily decomposed. C A more preferable range for / Nb is 0.05 or more and 0.5 or less, and a more preferable range is 0.1 or more and 0.35 or less.
[0038] [pH] In the manufacturing method of the present invention, the pH of the aqueous solution when forming the niobium polyacid ion is almost automatically determined by the amount of LiOH, which is a strong alkali, the amount of phosphoric acid, and the amount of hydrogen peroxide, so there is no need to adjust the pH, but it is alkaline, 7.5 to 12.5. Since the niobium polyacid ion is stably formed, the pH is more preferably 9.0 to 12.0. When phosphoric acid is added to the solution containing this niobium polyacid and lithium, the pH of the system decreases, but it has been confirmed that the niobium polyacid exists stably at a pH of 3 or more. The pH of the solution to which phosphoric acid is added is preferably 12.5 or less. More preferably, it is 12 or less. The pH value here is a value measured using a glass electrode with a pH meter equipped with a temperature compensation electrode, calibrated with an appropriate buffer solution according to the pH range to be measured based on JIS Z8802.
[0039] [Manufacturing method] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention, as described above, hydrous niobium oxide is used as the starting material for niobium. Hydrous niobium oxide and LiOH are dissolved in water to obtain an aqueous solution containing niobium polyacid ions and lithium, and then phosphate ions are added to the aqueous solution to obtain an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions. In this case, it is preferable that the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus is 0.04 or more and less than 0.5, and the molar ratio Li / Nb of niobium to lithium is more than 0.6 and 2.0 or less. In addition, it is preferable that the total concentration of niobium is 1% by mass or more and 20% by mass or less as niobium. When hydrogen peroxide is added, it is preferable to add hydrogen peroxide so that the concentration of hydrogen peroxide in the aqueous solution is 0.01% by mass or more and 10% by mass or less.
[0040] [Coating treatment] The following is an embodiment of the coating treatment for a positive electrode active material for a lithium ion secondary battery using an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the present invention. The positive electrode active material to be coated must have a specific surface area of 0.1 to 2 m 2 Since the specific surface area of the positive electrode active material is inversely proportional to the particle size, the specific surface area of the positive electrode active material is appropriately selected depending on the application of the lithium ion secondary battery. The thickness of the coating layer that coats the positive electrode active material is preferably 3 to 20 nm, and more preferably 5 to 15 nm. The coating treatment can be carried out by a known method such as a tumbling fluidized bed coating method or a high-velocity air current collision shear method, and the positive electrode active material can be brought into contact with an aqueous solution containing the niobium polyacid ions of the present invention, lithium ions, and phosphate ions, followed by a heat treatment such as drying, to obtain a positive electrode active material having a coating layer. EXAMPLES
[0041] [Qualitative evaluation of aqueous solutions] Qualitative evaluation of the dissolved chemical species in the aqueous solution was performed by Fourier transform infrared spectroscopy (FT-IR) using a NICOLET7600 manufactured by Thermo Fisher Scientific. In order to remove the peak on the low wave number side of the water solvent, water was used for background measurement, and the measurement was performed by the attenuated total reflection (ATR) method. A germanium prism was used for the measurement, and the incident angle was set to 45°. By performing the FT-IR measurement, it can be confirmed that niobium exists as a polyacid ion and phosphorus exists as a phosphate ion in the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention.
[0042] [Determination of Li, Nb and P in aqueous solutions] The components of the aqueous solution were analyzed using an inductively coupled plasma atomic emission spectrometer (ICP-AES, Agilent Technology 700 Series). 0.1 g of sample was taken from the precursor solution and weighed, and 15 mL of pure water and 5 mL of hydrochloric acid were added to it, heated, and then allowed to cool. 2 mL of hydrogen peroxide was added and allowed to cool, after which the liquid volume was adjusted to 100 mL and ICP-AES analysis was performed. The moles of the present invention were calculated from the contents of niobium, lithium, and phosphorus obtained by the quantitative analysis using ICP.
[0043] [Method for determining hydrogen peroxide in aqueous solution] Prior to the quantitative operation, prepare a Ti-PAR solution by mixing 20 mL of Ti solution with a titanium concentration of 1 mmol / L prepared using a commercially available titanium standard solution with 15 mL of PAR solution in which 11 mg of PAR (4-(2-pyridylazo)-resorcinol) is dissolved in a 1% by mass aqueous sodium hydroxide solution and adjusted to 50 mL with ultrapure water. Add 0.1 mL of the aqueous solution as a sample to a plastic container that already contains 0.05 mL of special-grade nitric acid and 20 mL of special-grade methanol, shake gently, and filter using a 0.45 μm filter after the precipitate has settled. Note that it is preferable to wait about 1 minute from the time the solution is added until the start of filtration. 0.25 mL of the filtrate was taken, and 5 mL of methanol, 1 mL of Ti-PAR solution, 5 mL of 1 mol / L ammonia water, and 40 mL of 1 mol / L ammonium chloride were mixed to prepare a pH 8.6 buffer solution, which was added in sequence, and the measurement solution was adjusted to 10 mL with methanol and allowed to stand at 40 to 45 ° C for 30 minutes. The absorbance was measured at a wavelength of 520 nm using a spectrophotometer U-2800 manufactured by Hitachi High-Technologies. The hydrogen peroxide concentration was quantified using the standard addition method, and was measured from the relative intensity of absorbance with respect to a standard solution of hydrogen peroxide. The moles of the present invention were calculated from the content of hydrogen peroxide obtained by this quantitative analysis.
[0044] [Absorbance measurement] 3.5 mL of the solution was dispensed into a quartz cell (10 mm x 10 mm x 45 mm), and the absorbance was measured at wavelengths of 400 to 700 nm using a Hitachi High-Technologies Corporation U-2800 spectrophotometer. The temperature of the precursor solution during the measurement was kept at 25°C. The zero point of the absorbance was the absorbance measured when ultrapure water with an electrical conductivity of 17 MΩ cm or more and 25°C was placed in the measurement cell. The absorbance at a wavelength of 660 nm indicates the intensity of scattered light caused by the particles in the precursor aqueous solution, and high absorbance suggests a high particle concentration (see JIS-K0101).
[0045] [Measurement of BET specific surface area] The BET specific surface area of the positive electrode active material before and after coating was determined by a single-point BET method using 4Sorb US manufactured by Yuasa Ionics Co., Ltd. The increase rate of the BET specific surface area before and after coating is defined by the following formula (1). BET specific surface area increase rate = 100 × (BET A -BET B ) / BET B …(1) BET HERE A is the BET specific surface area after coating, BET B is the BET specific surface area before coating. In the present invention, when the BET specific surface area increase rate is 100% or less, it is determined that the increase in the specific surface area is suppressed.
[0046] [Evaluation of ionic conductivity] The ionic conductivity of the coating layer obtained from the aqueous solution of the present invention was evaluated using a bulk powder formed from the aqueous solution. The aqueous solution was evaporated to dryness in a dryer set at 100°C, and the obtained powder was further fired in air at 300°C for 12 hours. 0.5 g of the fired powder was placed in a mold with a diameter of 10 mm and pressed at 20 MPa by a press to obtain a green compact. The obtained green compact was subjected to impedance measurement in a frequency range of 100 Hz to 4 MHz under an Ar atmosphere at a temperature of 25°C using a potentio / galvanostat (1470E manufactured by Solartron) and a frequency response analyzer (1255B manufactured by Solartron). The resistance value of the oxide powder sample was obtained from the intercept of the Cole-Cole plot (complex impedance plane plot) of the measured value, and the ionic conductivity was calculated from the obtained resistance value.
[0047] [Calculation of coating layer thickness] The thickness of the coating layer obtained by the above coating process is calculated on the assumption that the entire amount of the aqueous solution used in the coating process is used to form the coating layer. In this case, the lithium, niobium, and phosphorus contained in the aqueous solution are considered to have changed to Li2O, Nb2O5, and P2O5, respectively, and the volume of the mixture is calculated. The thickness of the coating layer is defined by the following formula (2). [Coating layer thickness (nm)] = 103 × [Volume of mixture of Li2O, Nb2O5 and P2O5 (cm 3 )] / [amount of positive electrode active material × specific surface area of positive electrode active material (m 2 / g)] …(2) Here, the volume of the above mixture is calculated as follows. If the Li content in the aqueous solution is a (mass%), the Nb content is b (mass%), and the P content is c (mass%), then from the atomic weights of Li, Nb, and P and the molecular weights of Li2O, Nb2O5, and P2O5, Li2O content (mass%) a' = a × molecular weight of Li2O / (atomic weight of Li × 2) Nb2O5 content (mass%) b' = b × molecular weight of Nb2O5 / (atomic weight of Nb × 2) P2O5 content (mass%) c' = c × molecular weight of P2O5 / (atomic weight of P × 2) The amount of aqueous solution used in the coating process is x (g), and the density of LiO is 2.0 g / cm 3 , the density of Nb2O5 is 4.6g / cm 3 , density of P2O5 is 2.4g / cm 3 Then, Volume (cm) of a mixture of Li2O, Nb2O5 and P2O5 3 )=(a' / 2.0+b' / 4.6+c' / 2.4)×x / 100 It becomes.
[0048] [Comparative Example 1] In a 0.5L beaker, 81.6g of pure water and 4.195g of lithium hydroxide monohydrate (LiOH·H2O) were added, and the lithium hydroxide was dissolved by stirring. Then, 13.84g of hydrous niobium oxide (Nb2O5·nH2O, Nb concentration: 67.4 mass%) dried at 300°C was added, and the mixture was stirred at 70°C for 8 hours to solubilize the hydrous niobium oxide, and a clear aqueous solution containing niobium polyacid ions and lithium ions was obtained. The pH of the resulting aqueous solution was 11.8. In this case, the amount of lithium added was 1.0, and the molar ratio Li / Nb to 1 mole of niobium contained in the niobium polyacid ions was 1.0. While keeping the aqueous solution containing niobium and lithium at 20°C, 3.2g of a 30% aqueous solution of hydrogen peroxide was added, and 71g of pure water was added for the final concentration adjustment to obtain an aqueous solution containing niobium polyacid ions and lithium ions. In this case, the hydrogen peroxide concentration in the aqueous solution was 0.49 mass%. No cloudiness was observed visually in the aqueous solution. When the aqueous solution of Comparative Example 1 was subjected to absorbance measurement, the absorbance value was 0.01 at a wavelength of 660 nm. The preparation conditions of the aqueous solution of this Comparative Example are shown in Table 1, and the calculated values of the concentrations of each element in the aqueous solution and the hydrogen peroxide concentration are shown in Table 2. When the aqueous solution of this Comparative Example was subjected to FT-IR measurement, the absorbance value was 0.01 at a wavelength of 850 cm. -1 ±20cm -1 An absorption peak due to Nb-O bonds was observed near the FT-IR spectrum of the aqueous solution obtained in this comparative example, and it is believed that the solubilized hydrous niobium oxide exists in the form of niobium polyacid ions.
[0049] Using a rolling fluidized coating device (MP-micro manufactured by Powrex Corporation), a coating with a BET specific surface area of 0.636 m 2 / g of positive electrode active material (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 25.2 g of the aqueous solution obtained in this comparative example was sprayed onto a tumbler (EQ-Lib-LNCM111, manufactured by MTI) while drying the aqueous solution in parallel to coat the surface of the positive electrode active material. The operating conditions of the rolling fluidized coating device were: intake gas: atmospheric air, intake temperature: 100°C, intake air volume: 0.1 m 3 / h, rotor speed: 1000 rpm, spray rate: 0.5 g / min. The amount of the aqueous solution was equivalent to a coating layer thickness of 10 nm. The BET specific surface area after coating was 1.91 m 2 / g, and the increase in the BET specific surface area when the coating treatment was carried out using the aqueous solution of this comparative example was 200%. The coating treatment conditions and the increase in the BET specific surface area are shown in Table 3.
[0050] [Example 1] The procedure was the same as that of Comparative Example 1 up to the addition of hydrogen peroxide, and 1.0 g of phosphoric acid (manufactured by Wako Pure Chemical Industries, Ltd., 80 mass%) was further added, and then 75 g of pure water for adjusting the concentration was added to obtain an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of Example 1. When phosphoric acid was added, phosphate ions were added at a rate of 0.25 mol / min per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions while stirring the solution. In this case, P / (Nb+Li+P) was 0.04, and no generation of white colloids was observed. When the absorbance of the aqueous solution of Example 1 was measured, the absorbance value at a wavelength of 660 nm was 0.01.
[0051] The aqueous solution obtained in this example was subjected to FT-IR measurement, and the wave number was 850 cm -1 ±20cm -1 An absorption peak due to Nb-O bonds was observed around 1000 to 1150 cm, which suggests that solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed at 1.225×10 -8S / cm. When 25.2 g of the aqueous solution obtained in this example was used to carry out a coating treatment under the same conditions as in Comparative Example 1, the thickness of the coating layer was 10 nm, the BET specific surface area increase rate was 90%, and the effect of suppressing the increase in the BET specific surface area was observed compared to Comparative Example 1. The preparation conditions of the aqueous solution in this example are shown in Table 1, the calculated concentrations of each element in the aqueous solution and the hydrogen peroxide concentration in Table 2, the coating treatment conditions and the BET specific surface area increase rate in Table 3, and the ionic conductivity of the powder obtained by evaporation to dryness in Table 4.
[0052] [Examples 2 to 5] The procedure was the same as in Example 1 up to the addition of hydrogen peroxide, and the amounts of phosphoric acid and pure water for adjusting the concentration and the rate of addition of phosphate ions were variously changed as shown in Table 1 to obtain aqueous solutions containing niobium polyacid ions, lithium ions, and phosphate ions in Examples 2 to 5. In this case, P / (Nb+Li+P) was set to 0.10 to 0.40, but no white colloid was observed to be produced in any of the Examples. The results of absorbance measurements performed in the same manner as in Example 1 for each Example are also shown in Table 2. FT-IR measurements were performed in all of the Examples, and the results were: -1 ±20cm -1 An absorption peak due to Nb-O bonds was observed around 1000 to 1150 cm, which suggests that solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed. FIG. 3 also shows the FT-IR spectrum of the aqueous solution obtained in this example. Using the aqueous solutions obtained in Examples 2 to 5, coating treatment was performed under the same conditions as in Comparative Example 1. When the amount of aqueous solution used was adjusted so that the thickness of the coating layer was 10 nm in each case, the BET specific surface area increase rate was -1% to 27%. Table 1 shows the preparation conditions of the aqueous solutions in Examples 2 to 5, Table 2 shows the calculated values of the concentrations of each element and the hydrogen peroxide concentration in the aqueous solutions, Table 3 shows the conditions of the coating treatment and the BET specific surface area increase rate, and Table 4 shows the ionic conductivity of the powder obtained by evaporation to dryness. From the results in Table 4, it can be said that from the viewpoint of ionic conductivity, the P / (Li+Nb+P) ratio is preferably 0.35 or less, and more preferably 0.08 or more.
[0053] [Examples 6 to 9] In the same procedure as in Example 1, the amounts of lithium hydroxide, phosphoric acid, and pure water for adjusting the concentration and the rate of addition of phosphate ions were changed as shown in Table 1 to obtain aqueous solutions containing niobium polyacid ions, lithium ions, and phosphate ions in Examples 6 to 9 in which the values of Li / Nb and P / (Nb+Li+P) were changed. In this case, Li / Nb was 0.78 to 2.00, and P / (Nb+Li+P) was 0.20 to 0.40. No white colloid was observed in any of the Examples. The results of absorbance measurements performed in the same manner as in Example 1 for each Example are also shown in Table 2. FT-IR measurements were performed for all of the Examples, and the results were: -1 ±20cm -1 An absorption peak due to Nb-O bonds was observed around 1000 to 1150 cm, which suggests that solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed. Using the aqueous solutions obtained in Examples 6 to 9, coating treatment was performed under the same conditions as in Comparative Example 1. When the amount of aqueous solution used was adjusted so that the thickness of the coating layer was 10 nm in all cases, the BET specific surface area increase rate was -2% to -3%. Table 1 shows the preparation conditions of the aqueous solutions in Examples 6 to 9, Table 2 shows the calculated values of the concentrations of each element in the aqueous solutions and the hydrogen peroxide concentrations, Table 3 shows the coating treatment conditions and the BET specific surface area increase rate, and Table 5 shows the ionic conductivity of the powder obtained by evaporation to dryness for Examples 6 and 7. From the results in Table 5, it can be said that from the viewpoint of ionic conductivity, the Li / Nb ratio is preferably 0.9 or more, and more preferably 0.95 or more.
[0054] [Example 10] Using 36.3 g of the aqueous solution containing the niobium polyacid ions, lithium ions, and phosphate ions obtained in Example 4, a niobium polyacid having a BET specific surface area of 1.085 m was 2 When a coating treatment was performed on a positive electrode active material of 0.1 g / g, the increase in the BET specific surface area was -1%.
[0055] [Example 11] An aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions was obtained by the same procedure as in Example 2, except that the rate of addition of phosphate ions was set to 3.38 mol / min. In this example, when phosphoric acid was added, a small amount of white colloid was generated, but no cloudiness of the aqueous solution was observed by visual inspection. The absorbance measured for this example is shown in Table 2. Using the aqueous solution obtained in this example, a coating treatment was carried out under the same conditions as in Comparative Example 1. When the amount of the aqueous solution used was adjusted so that the thickness of the coating layer was 10 nm in each case, the BET specific surface area increase rate was 73%, and the effect of suppressing the increase in the BET specific surface area was observed compared to the above-mentioned Comparative Example 1. From the results of comparing Example 2 and Example 11, it was found that by setting the phosphate ion addition rate to 3.07 mol / min or less of phosphate ions per mol of lithium in an aqueous solution containing niobium polyacid ions and lithium ions, it is possible to suppress the generation of colloidal particles and further suppress the increase in the BET specific surface area due to coating.
[0056] [Comparative Example 2] The procedure was the same as that of Comparative Example 1 up to the addition of hydrogen peroxide, and 24.5 g of phosphoric acid was further added at a phosphate ion addition rate of 0.24 mol / min per mol of lithium in an aqueous solution containing niobium polyacid ions and lithium ions, resulting in the generation of a large amount of white colloid. In this case, P / (Nb+Li+P) was 0.50. The white colloid did not redissolve even when diluted with pure water for concentration adjustment, and the aqueous solution became cloudy with the naked eye, so a coating treatment using this comparative example was not performed.
[0057] [Comparative Example 3] The procedure was the same as that of Comparative Example 1, except that the amount of lithium hydroxide added was 2.517 g and Li / Nb was 0.50, and after the addition of hydrogen peroxide, 4.9 g of phosphoric acid was further added at a phosphate ion addition rate of 0.24 mol / min per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions, and a large amount of white colloid was generated. The white colloid did not redissolve even when diluted with pure water for concentration adjustment, and the aqueous solution became cloudy with the naked eye, so a coating treatment using this comparative example was not performed.
[0058] As described above, by coating the positive electrode active material of a lithium ion battery positive electrode with an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions as defined in the present invention, it is possible to suppress an increase in the BET specific surface area due to the coating.
[0059] [Table 1]
[0060] [Table 2]
[0061] [Table 3]
[0062] [Table 4]
[0063] [Table 5]
Claims
1. An aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, in which the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution is 0.04 or more and less than 0.5, and the molar ratio Li / Nb of lithium to niobium is more than 0.6 and 2.0 or less.
2. The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to claim 1, further containing hydrogen peroxide at a concentration of 0.01% by mass or more and 10% by mass or less.
3. The ratio of the number of moles of hydrogen peroxide to the number of moles of niobium present in the aqueous solution (PO C 3. The aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 2, wherein the value of (Nb) is 0.01 or more and 1 or less.
4. 2. The aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 1, wherein the aqueous solution has an absorbance of 0.1 or less at a wavelength of 660 nm.
5. A step of dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing a polyacid ion of niobium and a lithium ion; adding phosphate ions to the aqueous solution containing the niobium polyacid ions and lithium ions; The present invention relates to a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, the method comprising the steps of:
6. A step of dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing a polyacid ion of niobium and a lithium ion; adding phosphate ions and hydrogen peroxide to the aqueous solution containing the niobium polyacid ions and lithium ions; The present invention relates to a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, the method comprising the steps of:
7. 7. The method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 5 or 6, wherein the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium and phosphorus is 0.04 or more and less than 0.5, and the molar ratio Li / Nb of lithium to niobium is more than 0.6 and 2.0 or less.
8. The method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to claim 6, wherein the concentration of hydrogen peroxide in the aqueous solution is 0.01% by mass or more and 10% by mass or less.
9. The ratio of the moles of hydrogen peroxide added to the moles of niobium (PO A 7. The method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 6, wherein the value of (Nb) is 0.1 or more and 1.0 or less.
10. 7. The method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 5 or 6, wherein phosphate ions are added at a rate of 0.07 mol / min or more and 3.07 mol / min or less per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions.
11. A step of coating a surface of an active material for a lithium secondary battery with an aqueous solution containing the niobium polyacid ion according to any one of claims 1 to 4, lithium ions, and phosphate ions; a step of heat-treating the coated active material for lithium secondary batteries; The present invention relates to a method for producing an active material for a lithium secondary battery having a coating layer containing lithium niobate.
Citation Information
Patent Citations
Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery
JP2012074240A
Active material coating solution
JP2017191667A
Precursor aqueous solution of lithium niobate and manufacturing method thereof
JP2020066570A
All-solid lithium battery
WO2007004590A1
Cited By
Nb complex aqueous solution, method for manufacturing positive electrode active material for all-solid-state lithium ion battery, method for manufacturing positive electrode for all-solid-state lithium ion battery, and method for manufacturing all-solid-state lithium ion battery
JP7774761B1