Antibacterial / antiviral glass composition
A lead-free low-melting glass composition with vanadium and phosphorus oxides, enhanced with silver or copper, addresses the challenge of maintaining antibacterial and antiviral efficacy while preserving material integrity, effectively inhibiting virus and bacteria spread.
Patent Information
- Application Number
- JP2023050821
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing antibacterial and antiviral resin compositions face challenges in maintaining effective antibacterial and antiviral properties while preserving material integrity and cost-effectiveness, as increasing the amount of antibacterial agents often deteriorates resin composition properties.
A lead-free low-melting glass composition incorporating vanadium oxide, phosphorus oxide, and optionally silver or copper oxide, with specific mole percentages, along with optional additives like iron, barium, tungsten, or zinc oxides, to achieve high-density antibacterial and antiviral effects, combined with polymers for sustained performance.
The glass composition exhibits excellent antibacterial and antiviral effects, maintaining material properties and longevity, even when used with polymers, and effectively inhibits the spread of viruses and bacteria, including coronaviruses and influenza viruses.
Smart Images

Figure 2024139884000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an antibacterial and antiviral glass composition that can inactivate viruses or kill bacteria, and suppress or prevent their spread. [Background technology]
[0002] 2. Description of the Related Art Conventionally, resin compositions and coating compositions containing materials that exhibit antibacterial or antiviral properties have been developed for the purpose of inhibiting bacterial proliferation or suppressing viruses in parts of building materials, home electrical appliances, and the like that are likely to be touched by human hands.
[0003] For example, Patent Document 1 discloses an antibacterial resin composition containing antibacterial silver zeolite in which a fluororesin film is formed on the surface of zeolite carrying antibacterial metal ions, mainly silver ions.
[0004] Patent Document 2 discloses a polyester resin sheet obtained by molding a resin composition containing a polyester resin (a) consisting of specific components, a polyester resin (b) consisting of specific components, a lubricant, and an antibacterial and antifungal agent such as an inorganic silver-based agent.
[0005] Furthermore, Patent Document 3 discloses an antibacterial and antiviral paint capable of forming an antibacterial and antiviral coating film having excellent water resistance, which is made by blending a quaternary ammonium salt and a polyvalent carboxylic acid having a hydrocarbon group with 6 or more carbon atoms and 2 or more carboxyl groups into an acrylic-melamine paint. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-045410 [Patent Document 2] JP 2007-031586 A [Patent Document 3] International Publication No. 2015 / 046372 Summary of the Invention [Problem to be solved by the invention]
[0007] In the resin compositions of Patent Documents 1 and 2, a general-purpose antibacterial agent is added to the resin composition to obtain antibacterial properties, but the antibacterial agent is, so to speak, an impurity, and while increasing the amount of the antibacterial agent improves the antibacterial function, there is a problem that the physical properties of the resin composition are reduced. Therefore, the amount of the antibacterial agent added to the resin composition is kept low within the range in which antibacterial properties are expressed. That is, in the resin compositions of Patent Documents 1 and 2, the amount of the antibacterial agent added is adjusted near the lower limit of the range in which antibacterial properties are expressed in order to more stably express antibacterial properties. In addition, in Patent Document 3, it was a difficult task to achieve both antiviral properties and material properties while suppressing costs.
[0008] Therefore, an object of the present invention is to provide an antibacterial and antiviral glass composition having antibacterial and antiviral effects. [Means for solving the problem]
[0009] An example of the aspect of the present embodiment for solving the above problems is as follows: A composition comprising vanadium oxide, phosphorus oxide, and at least one of silver oxide and copper oxide, wherein the vanadium oxide, the phosphorus oxide, the silver oxide, and the copper oxide are present in the following oxide-equivalent mole percentages: 25≦[V2O5]≦35, 15≦[P2O5]≦30, 1≦[Ag2O]+[CuO]≦50 1. An antibacterial and antiviral glass composition comprising:
[0010] The antibacterial and antiviral glass composition further contains iron oxide or barium oxide, and the vanadium oxide, silver oxide, copper oxide, iron oxide and barium oxide are contained in the following oxide-equivalent mole percentages: 5≦[Fe2O3]≦15, [Ag2O]+[CuO]+3[Fe2O3]≦2[V2O5] or 5≦[BaO]≦30, [Ag2O]+[CuO]+[BaO]≦2[V2O5] A preferred example of the antibacterial and antiviral glass composition is
[0011] The antibacterial and antiviral glass composition further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, tungsten oxide and zinc oxide are contained in the following mole % calculated as oxide: [WO3]≦15, [ZnO]≦10, [Ag2O]+[CuO]+[ZnO]≦2[V2O5] A preferred example of the antibacterial and antiviral glass composition is
[0012] Further, another aspect of this embodiment is as follows: A composition comprising the antibacterial and antiviral glass composition and at least one component selected from a polymer and a monomer. Effect of the Invention
[0013] According to the present invention, it is possible to provide an antibacterial and antiviral glass composition capable of storing silver and other elements having excellent antibacterial and antiviral properties at high density. Furthermore, by using the antibacterial and antiviral glass composition together with a material such as a polymer, it is possible to rapidly exert the antibacterial and antiviral properties of the antibacterial and antiviral glass composition while maintaining the material properties, and this antibacterial and antiviral properties can be maintained for a long period of time. [Brief description of the drawings]
[0014] [Figure 1] An example of a typical differential thermal analysis (DTA) result of glass is shown below. [Diagram 2]2A shows a schematic diagram of an aluminum alloy plate having a glass firing coating film, and FIG. 2B shows a schematic diagram of an aluminum alloy plate having a layer formed from a composition containing a glass composition and a polymer, in an example and a comparative example. [Diagram 3] FIG. 3A shows a glass firing temperature profile, FIG. 3B shows a polypropylene heating temperature profile, and FIG. 3C shows an acrylic heating temperature profile in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The following description shows a specific example of the contents of the present invention, and the present invention is not limited to these descriptions. Various changes and modifications can be made by those skilled in the art within the scope of the technical ideas disclosed in this specification. In addition, in all the drawings for explaining the present invention, parts having the same functions are given the same reference numerals, and repeated explanations thereof may be omitted.
[0016] In this specification, the word "to" is used to mean that the numerical values before and after it are included as the upper and lower limits. In the numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value described in another stage. The upper or lower limit value of the numerical ranges described in this specification may be replaced with the value shown in the examples.
[0017] When selecting a material from the group of materials exemplified below, a single material may be selected or a combination of multiple materials may be selected, provided that it does not contradict the contents disclosed in this specification. Furthermore, a material other than the group of materials exemplified below may be selected, provided that it does not contradict the contents disclosed in this specification.
[0018] The antibacterial and antiviral glass composition according to the present embodiment contains vanadium oxide, phosphorus oxide, and at least one of silver oxide and copper oxide, and the vanadium oxide, the phosphorus oxide, the silver oxide, and the copper oxide are contained in the following oxide-equivalent mole percentages: 25≦[V2O5]≦35, 15≦[P2O5]≦30, 1≦[Ag2O]+[CuO]≦50 It is characterized in that:
[0019] Glass compositions generally have a transition temperature T g , yield point M g , softening point T s Strictly speaking, there is a transition point T g , yield point M g and softening point T s is defined by the viscosity of the glass composition, T g is 10 13.3 poise, M g is 10 11.0 poise, T s is 10 7.65 The lower these characteristic temperatures are, the better the softening and fluidity at low temperatures is, and glass coating and joining at low temperatures are possible. 4 ~10 6 The viscosity must be about poise. s The softening temperature T s and crystallization temperature T cry The closer these values are, the greater the tendency for crystallization is, and the more likely the glass is to crystallize during heating and firing. When glass crystallizes, its softening and fluidity deteriorates, making it difficult to obtain good adhesion and density.
[0020] The antibacterial and antiviral glass composition (lead-free low-melting glass composition) contains vanadium oxide and phosphorus oxide as main components, and further contains silver oxide or copper oxide for antibacterial and antiviral effects. The structure of this glass composition has a layered structure consisting of VO5 pyramids, with PO4 tetrahedrons and Ag oxide between the layers. + ion or Cu 2+It is believed that silver oxide (Ag) is present in the glass composition of the present invention. The phosphorus oxide (P2O5) contained in the glass composition is a vitrification component for vitrifying vanadium oxide (V2O5). + In the form of ions or copper oxide, Cu 2+ By introducing ions into the glass structure, we found that V2O5-P2O5-based lead-free low-melting glass compositions have antibacterial and antiviral effects.
[0021] In general SiO2-Na2O-based glass compositions and SiO2-B2O3-based glass compositions, Ag + It is known that Ag can contain 1,2-dichlorophenyl ether and have antibacterial and antiviral properties. + However, the glass composition of the present invention contains a large amount of Ag. + Ion and Cu 2+ It can contain ions, which is extremely useful from the standpoint of antibacterial and antiviral effects.
[0022] The lead-free low melting glass composition of the present invention may further contain iron oxide (Fe2O3) or potassium oxide (K2O). These are considered to be present between layers of the layered structure, and Fe2O3 is effective in improving the water resistance and salt water resistance of the V2O5-P2O5-based lead-free low melting glass composition, while K2O is effective in increasing the thermal expansion to match the thermal expansion with the base material. However, if the content is too large, Fe2O3 may deteriorate the softening fluidity due to an increased tendency to crystallize, and K2O may deteriorate the water resistance and salt water resistance, and for example, when barium oxide is contained, it may cause the elution of barium. When the glass composition contains potassium oxide, it is preferable that the mole % of the oxide is 5≦[K2O]≦20.
[0023] The lead-free low melting glass composition of the present invention may further contain barium oxide (BaO). Barium oxide is added especially when iron oxide is not contained, and serves as a vitrification component for vitrifying vanadium oxide (VO). In terms of mole percent of oxide, it is preferable that 5≦[BaO]≦30, and particularly 15≦[BaO]≦30.
[0024] From the above viewpoint, the vanadium oxide, the phosphorus oxide, the silver oxide, and the copper oxide contained in the glass composition are, in mole % in terms of oxide, as follows: 25≦[V2O5]≦35, 15≦[P2O5]≦30, 1≦[Ag2O]+[CuO]≦50 It is.
[0025] In one embodiment of the glass composition, the glass composition further contains iron oxide or barium oxide, and the vanadium oxide, the silver oxide, the copper oxide, the iron oxide, and the barium oxide are contained in the following oxide-equivalent mole percentages: 5≦[Fe2O3]≦15, [Ag2O]+[CuO]+3[Fe2O3]≦2[V2O5] or 5≦[BaO]≦30, [Ag2O]+[CuO]+[BaO]≦2[V2O5] In this embodiment, it is preferable that the composition contains the iron oxide and is substantially free of the barium oxide, or contains the barium oxide and is substantially free of the iron oxide.
[0026] In one embodiment of the glass composition, the glass composition further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, tungsten oxide, and zinc oxide are contained in the following oxide-equivalent mole percents: [WO3]≦15, [ZnO]≦10, [Ag2O]+[CuO]+[ZnO]≦2[V2O5] In this embodiment, it is preferable that the composition contains the iron oxide and is substantially free of the barium oxide, or contains the barium oxide and is substantially free of the iron oxide.
[0027] In one embodiment of the glass composition, the glass composition contains the iron oxide and further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, iron oxide, tungsten oxide, and zinc oxide are present in the following oxide-equivalent mole percentages: [WO3]≦15, [ZnO]≦10, [Ag2O]+[CuO]+3[Fe2O3]+[ZnO]≦2[V2O5] or The composition contains the barium oxide and further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, barium oxide, tungsten oxide, and zinc oxide are contained in the following oxide equivalent mole %: [WO3]≦15, [ZnO]≦10, [Ag2O]+[CuO]+[BaO]+[ZnO]≦2[V2O5] In this embodiment, it is preferable that the composition contains the iron oxide and is substantially free of the barium oxide, or contains the barium oxide and is substantially free of the iron oxide.
[0028] In the present disclosure, "substantially free of a certain component" means that the component is present at 0.01 mol % or less, in mol %, calculated as oxide, and preferably at 0.001 mol % or less.
[0029] The glass composition is preferably in the form of a plate or film, and is a powder having an average particle size (D50) of 3 to 50 μm. If it is in the form of a plate, the thickness is preferably 0.1 to 30 mm, and more preferably 1.8 to 5 mm. If it is in the form of a film, the thickness is preferably 10 to 100 μm, and more preferably 50 to 100 μm. Within the above ranges, the glass can fully exhibit its functions and can maintain its effects for a long period of time.
[0030] The method for producing the glass composition is not particularly limited, and the glass composition can be produced by referring to a conventionally known method for producing lead-free low-melting glass using vanadium oxide (V2O5) and phosphorus oxide (P2O5). For example, oxides containing each element as raw materials, such as V2O5, P2O5, Ag2O, AlPO4, Fe2O3, BaO, K2CO3, KVO3, CuO, WO3 and ZnO, are blended and mixed according to the composition of a desired glass composition, placed in a container such as a platinum crucible, heated at 850 to 1300°C for 0.5 to 3.0 hours, and the molten material in the container is appropriately stirred to produce a glass composition in the form of cullet, plate, etc. When the glass composition is obtained as a powder (particle), the glass composition in the form of cullet, plate, etc. is then granulated by a method such as crushing to produce a powdered glass composition. The powdered glass composition is also referred to as glass particles or glass powder.
[0031] The composition of the present embodiment is characterized in that it contains an antibacterial / antiviral glass composition and at least one component selected from a polymer and a monomer. Since the glass composition has antibacterial / antiviral activity, the composition can also exhibit antibacterial / antiviral activity. In one preferred embodiment of the composition, the antibacterial / antiviral glass composition is in the form of a powder, and it is preferable that the antibacterial / antiviral glass composition is in the form of a powder with an average particle size (D50) of 3 to 50 μm, since an antiviral effect is exhibited due to an increased specific surface area, and the effect is maintained for a long period of time.
[0032] The polymer used in the composition is not particularly limited, and may be a polymer of a resin material, a rubber material, etc. Examples of the polymer include polyvinyl alcohol, polyvinyl acetal (butyral resin, etc.), cellulose, acrylic urethane resin, acrylic resin, urethane resin, vinyl chloride resin, vinylidene chloride resin, polyolefin resin, polyethylene terephthalate, polyester resin, polystyrene, polyamide resin, polycarbonate resin, and ABS resin.
[0033] The monomer is not particularly limited, and for example, a monomer that can be polymerized to the above-mentioned polymer can be used. The monomer may also be a macromonomer (a high molecular weight monomer having a polymerizable functional group).
[0034] In the composition of the present embodiment, the content of the glass composition in the composition is preferably 5% by volume or more and 50% by volume or less, more preferably 5% by volume or more and 30% by volume or less, and particularly preferably 5% by volume or more and 25% by volume or less. In addition, in the composition of the present embodiment, the content of at least one component selected from the polymer and the monomer in the composition is 50% by volume or more and 95% by volume or less, preferably 70% by volume or more and 95% by volume or less, and more preferably 75% by volume or more and 95% by volume or less. Within the above range, antibacterial and antiviral effects can be sufficiently exhibited, which is preferable.
[0035] The composition of the present embodiment may contain other components. Examples of the other components include various additives. Examples of the additives include plasticizers, stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, curing agents, crosslinking agents, lubricants, antistatic agents, fillers, pigments, dyes, and waxes (e.g., natural waxes such as plant-based, animal-based, and mineral-based). The additives may be contained alone or in combination.
[0036] The method for producing the composition is not particularly limited. For example, the polymer and the glass particles are mixed and then dried to obtain a composition containing the polymer and the glass composition. When the polymer and the glass composition are mixed, it is preferable to use a solvent or a dispersion medium capable of dissolving or dispersing the polymer. As the solvent or the dispersion medium, either an organic solvent or an aqueous solvent may be used. For example, a glass composition can be obtained by preparing a solution in which a polymer is dissolved in a solvent, mixing the solution with glass particles (glass composition), and removing the solvent by drying or the like. As another method, a composition containing the monomer and the glass composition can be obtained by mixing a monomer with the glass composition. Also, a composition containing the polymer and the glass composition can be obtained by polymerizing the monomer in the composition containing the monomer and the glass composition.
[0037] The use of the composition of the present embodiment will be described. When the composition contains a polymer and a glass composition, it can be used for various applications as an antibacterial and antiviral molded product. Examples of the molded product include a plate, a sheet, a fiber, a woven fabric, and a nonwoven fabric. When the composition contains a monomer and a glass composition, the composition may be a paint. The molded product may be a single-layered molded product or a multi-layered molded product. In the case of a multi-layered molded product, at least one layer is formed from the composition. In the case of a multi-layered molded product, it is preferable that at least a part of the part that comes into contact with air or the part that comes into contact with a person or the like is formed from the composition. In addition, the paint may be a one-component paint, or a multi-component paint in which multiple agents are mixed and used. When the sheet has a single layer structure, the thickness is preferably in the range of 20 to 500 μm, and more preferably in the range of 30 to 100 μm. When the sheet has a multi-layer structure, it is preferable that the thickness of each layer is 20 μm or more from the viewpoint of producing a uniform sheet. The molded article may have three or more layers of nonwoven fabric. As for the fibers, it is assumed that the composition is molded into a fibrous form, the composition is mixed with polymer fibers, etc., and the composition is attached to the surface of any fiber, and it can be used in any thickness. As for the woven fabric, it can be appropriately applied to objects such as clothing. As for the molded article having three or more layers of nonwoven fabric, the inner layer may have a nonwoven fabric formed from the composition of this embodiment. Since nonwoven fabrics are usually capable of passing air, they can exert antibacterial and antiviral effects even when the inner layer is a nonwoven fabric formed from the composition. As layers other than the inner layer, known nonwoven fabrics can be used, and for example, masks and the like can be manufactured. In addition, the molded article may be subjected to a mesh treatment using the composition. Specific examples of the shape of the mesh include a lattice shape, a polka dot shape, a polygonal shape, etc., but are not limited thereto. The nonwoven fabric obtained from the composition can be laminated with a substrate such as another nonwoven fabric, if necessary, and / or subjected to various processes such as embossing and pleating, and can be suitably used for various applications such as a filter for filtering gas or liquid.Examples of applications of the composition containing the polymer and glass composition include clothing (medical clothing) (masks, white coats, protective clothing, gloves, etc.); bedding (medical bedding) (futon / pillow covers, curtains, patient amenities, etc.); handrails and door knobs in hospitals, touch buttons for elevators and automatic doors, escalator belts, medical equipment terminals, etc.; air conditioning filters in hospitals; tents for temporary medical sites; mosquito nets for home recuperation; floor wax; hanging rings, handrails, and touch buttons for trains, buses, airplanes, ships, elevators, taxis, etc. Examples of such applications include door knobs, floors, walls, ceilings, sheets, and air conditioning filters; building materials (floors, walls, doors, and ceilings) and furniture (tables, desks, chairs, curtains, and the like) for schools, libraries, companies, supermarkets, detached houses, and apartment buildings; air conditioning filters; shopping cart grips and shopping basket handles; medical equipment; vehicles; elevators; escalators (belts); home appliances; odor-resistant underwear; socks for preventing athlete's foot; odor-resistant sportswear; odor-resistant shoe insoles; and water-related (sanitary) areas (kitchens, toilets, baths, washbasins, and the like). The composition of the present embodiment can be used as a component constituting all or part of these applications. EXAMPLES
[0038] The present embodiment will be described below with reference to examples, but the present disclosure is not limited to these examples.
[0039] [Example 1] In this example, the influence and effect of the glass composition of the glass composition on glass properties, and the effect of the composition were examined. Tables 1 to 6 show the glass compositions and properties of the glass compositions of the examples and comparative examples (V2O5-P2O5-based lead-free low-melting glass compositions and V2O5-TeO2-based lead-free low-melting glass compositions).
[0040] (Preparation of lead-free low melting glass composition) The lead-free low melting glass compositions having the compositions shown in Tables 1 to 6 were prepared by the following method. As the glass raw materials in Table 1, powders of V2O5, P2O5, Ag2O, AlPO4, Fe2O3, BaO, K2CO3, KVO3, CuO, WO3, and ZnO were used. The glasses in Table 4 were comparative examples using conventional vanadium glass, zinc-based glass, and silica-based glass. The glass raw materials were mixed and mixed in a predetermined amount in the ratios shown in Tables 1 or 4 so that the total amount of glass raw materials was about 200 g, and then placed in a platinum crucible. The platinum crucible was heated to about 900°C in an electric furnace at a heating rate of about 10°C / min in the atmosphere and held for 1 to 2 hours. During the holding period, the molten material in the platinum crucible was stirred at intervals of 20 to 30 minutes using an alumina rod to make it into a uniform glass. After this holding, the platinum crucible was removed from the electric furnace, and the molten material in the platinum crucible was poured onto a thick stainless steel plate to obtain glass cullet of a lead-free low melting point glass composition.
[0041] (Evaluation of vitrification state) The glass cullet of the obtained lead-free low melting point glass composition was observed visually and by an optical microscope to confirm the presence or absence of surface devitrification, crystallization, phase separation, and undissolved matter, thereby evaluating the vitrification state. In addition, when it was unclear, the glass cullet was crushed and the presence or absence of a sharp diffraction peak was confirmed by powder X-ray diffraction to evaluate the vitrification state. When the obtained glass cullet did not exhibit any of surface devitrification, crystallization, phase separation, and undissolved matter, or when no sharp diffraction peak was observed by powder X-ray diffraction, it was judged to be in a uniform vitrification state and was evaluated as good (◯). On the other hand, when the obtained glass cullet exhibited any of surface devitrification, crystallization, phase separation, and undissolved matter, or when a sharp diffraction peak was observed by powder X-ray diffraction, it was evaluated as not being in a uniform vitrification state, and was evaluated as poor (×).
[0042] (Preparation of glass particles) The glass cullet obtained above (production of lead-free low melting point glass composition) was pulverized by a Raikai mill and a jet mill to an average particle size (D50) of about 20 μm to obtain glass particles (glass powder).
[0043] (Measurement of glass characteristic temperature) The characteristic temperatures (transition point, yield point, softening point, etc.) of the glass particles (lead-free low melting point glass composition) were measured by differential thermal analysis (DTA). The glass powder (glass particles) was placed in an aluminum DTA cell and heated in air from room temperature to 550°C at a heating rate of 5°C / min to obtain a DTA curve. Figure 1 shows an example of a typical differential thermal analysis (DTA) result of glass. As shown in Figure 1, when the glass powder (glass particles) is heated, the transition point T g The endothermic heat begins to be absorbed from the sag point M g Then, the amount of heat absorbed decreases once and then increases again. The temperature corresponding to the second endothermic peak is the softening point T s If it is heated further, the crystallization temperature T cry The amount of heat generated increases rapidly from this temperature, and reaches an exothermic peak. This exothermic peak is due to the crystallization of glass, and the temperature at which heat generation begins is called the crystallization temperature T cry The temperature at which the exothermic peak reaches its maximum value is called the crystallization peak temperature T cry-p Usually, each characteristic temperature is calculated by the tangent method.
[0044] (Evaluation of glass softening fluidity) The softening fluidity of the glass particles (lead-free low melting point glass composition) was evaluated by a button flow test. As an evaluation sample, a powder compact having a diameter of 10 mm and a thickness of 5 mm was obtained using the glass powder (glass particles). This powder compact was placed on an aluminum plate and heated in air at a heating rate of 10° C. / min until the softening point T s The softening and fluidity state was observed by heating the sample to a temperature 30 to 40°C higher than the sample temperature and holding the temperature for 30 minutes. A sample that exhibited good softening and fluidity was rated as "Good", whereas a sample that did not exhibit good softening and fluidity due to surface devitrification, crystallization, phase separation, etc. was rated as "Poor".
[0045] (chemical stability) Samples were created by mixing α-terpineol and glass powder on an aluminum plate measuring 50 mm x 50 mm x 1 mm and firing the mixture at 170°C for 30 minutes and at 390°C for 30 minutes. The fired aluminum plate was immersed in water or 3.5 wt% salt water and left for over a day. Those that did not elute any glass components other than silver into the solution were marked with an ◯, and those in which other components were detected were marked with an ×.
[0046] (comprehensive evaluation) The overall evaluation of the glass was that it was not crystallized, and in the chemical stability test, no substances other than silver were eluted, and the amount of eluted silver was within the required amount (5 × 10 -7 g / cm 3 ) or more was marked with an O, and those that did not meet the required value in any item were marked with an X.
[0047] (Firing onto the surface of an alloy substrate (production of a film-like glass composition)) 25 g of the glass particles (lead-free low melting point glass composition) was added to a solvent (5 g) and kneaded for about 30 minutes using a mortar and pestle to prepare a paste. The paste was applied to an aluminum alloy plate, dried, and fired as described below, and the coating state of the coating film was observed to evaluate the properties. α-Terpineol (α-T) was used as the solvent.
[0048] As shown in FIG. 2A, each paste was applied to an aluminum alloy plate of 50×50×2 mm in a thickness of 0.1 mm in an area of 50×50 mm. The aluminum alloy plate was A6501. The aluminum alloy plate to which the paste was applied was dried in air at 150-170°C for 30 minutes. After drying, the aluminum alloy plate was further heated in air at a temperature increase rate of 10°C / min as shown in the glass firing temperature profile in FIG. 3A, held at a temperature about 30-40°C higher than the softening point of the glass for 30 minutes, and cooled in a furnace to form a glass firing coating film (film-like glass composition) on the aluminum alloy plate, thereby obtaining a sample.
[0049] (Mixing into polymer (resin material) (production of glass composition and composition containing polymer)) 25g of the glass particles (lead-free low melting point glass composition) was added to a solution (15g polypropylene, 18g solvent) in which a resin binder (powdered polypropylene) was dissolved in a solvent, and the mixture was kneaded for about 30 minutes using a mortar and pestle to prepare a paste. The paste was applied to an aluminum alloy plate as described below, dried, and evaluated by observing the coating state of the coating film. The volume ratio of glass differs depending on the glass components used, but the glass particles and polypropylene were used in amounts such that the glass particles were 5 to 20 volume % and the polypropylene was 80 to 95 volume % in the composition after drying. α-Terpineol (α-T) was used as the solvent.
[0050] The paste was applied to a 50×50×2 mm aluminum alloy plate with a thickness of 0.1 mm over a 50×50 mm area, as shown in FIG. 2B. The aluminum alloy plate used was A6501. As shown in FIG. 3B, the polypropylene heating temperature profile was then shown, and the plate was heated in air at a temperature increase rate of 10° C. / min, held at 200° C. for 1 hour, and cooled in a furnace to form a layer made of a composition containing a glass composition and a polymer (polypropylene) on the plate, thereby obtaining a sample.
[0051] (Mixing with monomer (preparation of composition (paint) containing glass composition and monomer) and curing (production of composition containing glass composition and polymer)) The glass particles (lead-free low melting point glass composition) and acrylic powder were added to α-terpineol and kneaded for about 30 minutes with a mortar and pestle to prepare a paste. The paste was applied to an aluminum alloy plate as described below, dried, and evaluated by observing the coating state of the coating film. The glass particles and acrylic powder were used in amounts such that the glass particles were 5 to 20 volume % and the acrylic powder was 80 to 95 volume % in the paste state (mixture of glass particles, acrylic-containing composition precursor, and solvent), calculated excluding the solvent. The glass particles and acrylic powder were used in amounts such that the glass particles were 5 to 20 volume % and the acrylic resin was 80 to 95 volume % in the coating film (composition containing glass particles and acrylic resin).
[0052] The paste was applied to a 50×50×2 mm aluminum alloy plate with a thickness of 0.1 mm over a 50×50 mm area, as shown in FIG. 2B. The aluminum alloy plate used was A6501. As shown in FIG. 3C, the acrylic heating temperature profile was then shown, and the plate was heated at a temperature increase rate of 10° C. / min in air, held at 80° C. for 3 hours, and cooled in a furnace to form a layer made of a composition containing a glass composition and a polymer (acrylic) on the alloy plate, thereby obtaining a sample.
[0053] Next, antiviral tests were conducted using the prepared samples. The antiviral tests were conducted based on ISO 21702 (measurement of antiviral activity of plastics and other non-porous surfaces). In this test, the results of the tests using enveloped SARS-COV-2 and influenza A viruses are summarized and shown in Tables 7 to 12. These results take into account the antiviral properties of the material and cell poisoning in the human body. The test items in Tables 7 to 12 were measured as follows.
[0054] (Immediate effect) Antiviral activity value (R): Indicates the difference in logarithmic value (R=Ut-At) between the viral infectivity value (Ut) after 2 hours for an untreated test piece (no drug added) and the viral infectivity value (At) after 2 hours for a treated test piece (with antiviral drug added). An R of 2 or more is considered to be a pass.
[0055] According to the results shown in Tables 7 to 12, the test pieces of Examples A-1 to A-31 and B-1 showed good results against both SARS-COV-2 and influenza A virus. In contrast, the antiviral activity values (R) of the test pieces of Comparative Examples B-2 to B-5 did not reach the pass value. In addition, a test was conducted to confirm the antibacterial effect according to JIS-Z2911. It was confirmed that the number of bacteria was reduced in all the test pieces of the Examples.
[0056] (Sustainability) Each sample was immersed in pure water for 744 hours, and the duration of silver ion elution into water was evaluated. If the amount of Ag ion elution after 744 hours could be maintained for 10 years, it was considered to have passed. The following evaluation was performed using linear approximation, and samples that met the requirements were evaluated as ◯, and samples that did not meet the requirements were evaluated as ×. Amount of Ag ions dissolved in 744 hours / total amount of Ag ions contained in glass < 0.0085 (= 744 / (24 × 365 × 10))
[0057] (Non-cytotoxic) Materials that do not contain elements that have adverse effects on the human body (e.g., Ni, Te, Hg, Co) are marked with a 〇, and materials that do contain these elements are marked with an ×.
[0058] [Table 1]
[0059] [Table 2]
[0060] [Table 3]
[0061] [Table 4]
[0062] [Table 5]
[0063] [Table 6]
[0064] [Table 7]
[0065] [Table 8]
[0066] [Table 9]
[0067] [Table 10]
[0068] [Table 11]
[0069] [Table 12]
[0070] The glass composition and compositions containing the glass composition and a polymer have antibacterial and antiviral effects, and have been shown to be particularly effective against coronaviruses and influenza viruses. However, it goes without saying that the same can be applied to all viruses and bacteria for which silver ions and copper ions are effective, including other viruses and bacteria.
[0071] The present invention is not limited to the above-mentioned embodiment and examples, and any configuration that has substantially the same technical idea as the technical concept described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention, and includes various modifications. For example, the above-mentioned embodiment and examples have been described in detail to explain the present invention in an easy-to-understand manner, and the present invention is not necessarily limited to those having all the described configurations. In addition, it is possible to replace a part of the configuration of one embodiment and example with the configuration of another embodiment and example, and it is also possible to add the configuration of another embodiment and example to the configuration of one embodiment and example. In addition, it is possible to add, delete, or replace other configurations with respect to a part of the configuration of each embodiment and example.
Claims
1. The composition contains vanadium oxide, phosphorus oxide, and at least one of silver oxide and copper oxide, and the vanadium oxide, the phosphorus oxide, the silver oxide, and the copper oxide are contained in the following oxide-equivalent mole percentages: 25≦[V 2 O 5 ]≦35, 15≦[P 2 O 5 ]≦30, 1≦[Ag 2 O]+[CuO]≦50 1. An antibacterial and antiviral glass composition comprising:
2. The antibacterial and antiviral glass composition according to claim 1, The vanadium oxide, the silver oxide, the copper oxide, the iron oxide, and the barium oxide are contained in the following oxide-equivalent mole percentages: 5≦[Fe 2 O 3 ]≦15, [Ag 2 O]+[CuO]+3[Fe 2 O 3 ]≦2[V 2 O 5 ] or 5≦[BaO]≦30, [Ag 2 O]+[CuO]+[BaO]≦2[V 2 O 5 ] 1. An antibacterial and antiviral glass composition comprising:
3. The antibacterial and antiviral glass composition according to claim 1, The composition further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, tungsten oxide, and zinc oxide are contained in the following oxide-equivalent mole percentages: [W.O. 3 ]≦15, [ZnO]≦10, [Ag 2O]+[CuO]+[ZnO]≦2[V 2 O 5 ] 1. An antibacterial and antiviral glass composition comprising:
4. The antibacterial and antiviral glass composition according to claim 2, The composition contains the iron oxide and further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, the silver oxide, the copper oxide, the iron oxide, the tungsten oxide, and the zinc oxide are contained in the following oxide-equivalent mole percentages: [W.O. 3 ]≦15, [ZnO]≦10, [Ag 2 O]+[CuO]+3[Fe 2 O 3 ]+[ZnO]≦2[V 2 O 5 ] or The composition contains the barium oxide and further contains at least one of tungsten oxide and zinc oxide, and the vanadium oxide, silver oxide, copper oxide, barium oxide, tungsten oxide, and zinc oxide are contained in the following oxide-equivalent mole percentages: [W.O. 3 ]≦15, [ZnO]≦10, [Ag 2 O] + [CuO] + [BaO] + [ZnO]≦2[V 2 O 5 ] 1. An antibacterial and antiviral glass composition comprising:
5. The antibacterial and antiviral glass composition according to claim 2, comprising said iron oxide and being substantially free of said barium oxide; or An antibacterial and antiviral glass composition comprising the barium oxide and substantially free of the iron oxide.
6. The antibacterial and antiviral glass composition according to claim 4, comprising said iron oxide and being substantially free of said barium oxide; or An antibacterial and antiviral glass composition comprising the barium oxide and substantially free of the iron oxide.
7. The antibacterial and antiviral glass composition according to claim 1, An antibacterial and antiviral glass composition characterized in that it is in the form of a plate or film and is in the form of a powder having an average particle size (D50) of 3 to 50 μm.
8. A composition comprising the antibacterial and antiviral glass composition according to any one of claims 1 to 7 and at least one component selected from the group consisting of polymers and monomers.
9. 9. The composition according to claim 8, The antibacterial and antiviral glass composition is in the form of a powder having an average particle size (D50) of 3 to 50 μm.
10. 9. The composition according to claim 8, A composition, comprising the antibacterial and antiviral glass composition in an amount of 5% by volume or more and 50% by volume or less.
Citation Information
Patent Citations
Antibacterial phosphate glass with adjusted refractive index
JP2005255517A
Vanadium phosphate base glass
JP2006342044A
Vanadium phosphate glass composition and sealing material
JP2019073403A
Vanadium phosphate glass composition and sealing material
JP2019089685A
Glass composition and sealing material
JP2019089689A
Cited By
Antibacterial / antiviral polymer composition
JP2024139934A
Antibacterial and antiviral polymer compositions
JP7819145B2
Glass particle-containing pellet, method for producing glass particle-containing pellet, and molded article made from glass particle-containing pellet
WO2026220916A1