FORMATION METHOD FOR SiCN FILM AND PLASMA PROCESSING DEVICE
The method forms a SiCN film with high etching resistance by using plasma enhanced atomic layer deposition to inherit Si-C and Si-N bonds at low temperatures, addressing the challenge of forming high-quality SiCN films at 450°C or lower.
Patent Information
- Application Number
- JP2023050889
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods struggle to form SiCN films with high wet etching resistance at low temperatures (450°C or lower) by inheriting Si-C bonds without breaking them, leading to poor film quality.
A method involving plasma enhanced atomic layer deposition (PEALD) using a precursor gas with Si-C and Si-N bonds, suppressing dissociation, and exposing the substrate to hydrogen plasma to inherit these bonds while controlling temperature below 450°C, using a plasma processing apparatus with UHF wave power to form a SiCN film.
The method achieves a SiCN film with high density and etching resistance by inheriting Si-C and Si-N bonds, improving film quality and maintaining low processing temperatures.
Smart Images

Figure 2024139936000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for forming a SiCN film and a plasma processing apparatus. [Background technology]
[0002] For example, Patent Document 1 discloses a method for depositing a silicon carbide film on a substrate surface. The method includes, for example, the use of a gas-phase carbosilane precursor and employs a plasma-enhanced atomic layer deposition (PEALD) process by ALD (Atomic Layer Deposition). It is described that the method may be carried out at a temperature of less than 600°C, for example between about 23°C and about 200°C, or about 100°C.
[0003] For example, Patent Documents 2 and 3 disclose a method for forming a silicon-containing film by using a deposition method selected from an ALD deposition process or a cyclic CVD deposition process. The method discloses that a substrate is placed in a reactor, the reactor is heated to, for example, 700° C., at least one silane-based precursor having Si-N bond, Si-Si bond, and Si-H2 group is introduced, unreacted material is purged, a reducing agent (hydrogen plasma) is provided to react with the precursor to deposit a silicon-containing film, and unreacted material is purged, and the process is repeated.
[0004] For example, Patent Document 4 discloses a method for forming a silicon nitride film on a substrate at low temperature. The method discloses supplying a gas containing precursor gas molecules having an unstable Si-N bond, Si-C bond, or N-C bond, and forming a precursor material layer on the substrate by preferentially breaking the unstable bonds. It also discloses that when forming a precursor material layer on the substrate, activated precursor gas molecules bind to the surface of the substrate at the one or more reaction sites, and a plasma treatment process is performed on the precursor material layer to form a conformal silicon nitride film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] US Patent Application Publication No. 2012 / 0122302 [Patent Document 2] JP 2014-013888 A [Patent Document 3] JP 2015-15465 A [Patent Document 4] JP 2015-507362 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present disclosure provides techniques that can transfer Si-C bonds of a precursor gas to a film formed on a substrate. [Means for solving the problem]
[0007] According to one aspect of the present disclosure, there is provided a method for forming a SiCN film, comprising: (a) a step of preparing a substrate in a processing vessel; (b) a step of supplying a first gas containing a precursor gas having Si-N bonds and Si-C bonds into the processing vessel to form an adsorption layer on the substrate, the step not activating the Si-N bonds and the Si-C bonds in forming the adsorption layer; (c) a first purge step of purging the processing vessel after the step (b); (d) a second gas containing hydrogen gas and VHF or UHF power are supplied into the processing vessel to generate plasma, and the substrate is exposed to the plasma to react with the adsorption layer, thereby forming a SiCN film, the SiCN film inheriting at least a part of the Si-C bonds and the Si-N bonds of the adsorption layer; and (e) a second purge step of purging the processing vessel after the step (d), in which the steps (b) to (e) are repeated. Effect of the Invention
[0008] According to one aspect, the Si-C bonds of the precursor gas can be inherited by the film formed on the substrate. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing a configuration example of a plasma processing apparatus according to an embodiment; [Diagram 2] FIG. 1 is a diagram illustrating a precursor gas having Si-C bonds and the inheritance of bonds to a film. [Diagram 3] FIG. 13 shows an example of a precursor gas. [Figure 4] 1 is a flowchart illustrating an example of a method for forming a SiCN film according to an embodiment. [Diagram 5] 1A to 1C are diagrams showing an example of a method for forming a SiCN film according to an embodiment and a modification thereof; [Figure 6] FIG. 1 shows an example of an experimental result of the composition and pressure dependence of a SiCN film. [Figure 7] FIG. 1 is a graph showing the relationship between the carbon concentration in a SiCN film and the film density. [Figure 8] FIG. 1 shows an example of an XPS measurement result of a SiCN film. [Figure 9] A diagram showing an example of experimental results for H2 plasma and N2 plasma. [Figure 10] 1 is a flowchart showing an example of a method for forming a SiCN film used in an experiment. [Figure 11] 1A to 1C are diagrams showing an example of a method for forming a SiCN film used in an experiment. [Figure 12] FIG. 13 is a graph showing the relationship between the carbon concentration in a SiCN film and the film density in the experimental results. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated descriptions may be omitted.
[0011] [Plasma processing equipment] A configuration example of a plasma processing apparatus for performing a film forming method according to this embodiment will be described with reference to Fig. 1. Fig. 1 is a diagram showing a configuration example of a plasma processing apparatus 1 including a plasma source of UHF waves according to one embodiment.
[0012] The plasma processing apparatus 1 includes a processing vessel 10 and a plasma source 2. The processing vessel 10 is substantially cylindrical, made of a metal material such as aluminum, and is airtight, and is grounded. The plasma source 2 generates plasma by introducing UHF wave power into the processing vessel 10. The top wall 10a of the processing vessel 10 is configured by fitting a dielectric member (hereinafter, referred to as a dielectric window 56) connected to a plurality of radiation mechanisms 42 into a metal main body. Thus, the plasma source 2 introduces UHF waves into the processing vessel 10 through the plurality of dielectric windows 56 in the top wall 10a.
[0013] However, the top wall 10a of the processing vessel 10 is not limited to the configuration in which a dielectric member connected to a plurality of radiation mechanisms 42 is fitted into a metal main body. For example, a dielectric member may be provided so as to cover the surface of the top wall 10a facing the substrate W, and UHF wave power may be introduced from one radiation mechanism 42, or a shower structure may be provided in which a predetermined gas is supplied in a shower-like manner to the surface of the top wall 10a facing the substrate W. The power introduced into the processing vessel 10 is not limited to UHF waves, and may be VHF wave power. The frequency of the VHF waves or UHF waves is within the range of 100 MHz to 3 GHz.
[0014] The plasma processing apparatus 1 has a control device 130. The control device 130 is, for example, a computer, and has a program storage unit (not shown). The program storage unit stores a program for controlling the processing of a substrate W, for example, a semiconductor wafer, in the plasma processing apparatus 1. The program may be recorded on a computer-readable storage medium, such as a computer-readable hard disk (HD), a flexible disk (FD), a compact disk (CD), a magnet optical disk (MO), or a memory card, and may be installed into the control device 130 from the storage medium.
[0015] A mounting table 11 for horizontally supporting a substrate W is provided in the processing vessel 10 and is supported by a cylindrical support member 12 that stands via an insulating member 12a at the center of the bottom of the processing vessel 10. The mounting table 11 and the support member 12 are made of a material such as a metal such as aluminum whose surface has been anodized (anodized), or an insulating material (such as ceramics) having a high-frequency electrode therein.
[0016] Although not shown, the mounting table 11 is also provided with a temperature control mechanism, a gas flow path for supplying a gas for heat transfer to the rear surface of the substrate W, lift pins for lifting and lowering to transport the substrate W, and the like. Furthermore, an electrostatic chuck for electrostatically adsorbing the substrate W may be provided.
[0017] An RF bias power supply 14 is electrically connected to the mounting table 11 via a matching box 13. When RF bias power is supplied from the RF bias power supply 14 to the mounting table 11, ions in the plasma are attracted to the substrate W side, which contributes to improving the film quality and the in-plane uniformity.
[0018] An exhaust pipe 15 is connected to the side of the bottom of the processing vessel 10, and an exhaust device 16 including a vacuum pump is connected to the exhaust pipe 15. By operating the exhaust device 16, the inside of the processing vessel 10 can be exhausted, and the inside of the processing vessel 10 can be reduced in pressure to a predetermined value. In addition, a side wall 10b of the processing vessel 10 is provided with a load / unload port 17 for loading / unloading the substrate W, and a gate valve 18 for opening / closing the load / unload port 17.
[0019] The plasma processing apparatus 1 also has a first gas shower unit 21 for discharging a predetermined gas into the processing vessel 10 from the ceiling wall 10a of the processing vessel 10, and a second gas shower unit 22 for introducing gas from a position between the ceiling wall 10a and the mounting table 11.
[0020] Although the first gas shower unit 21 and the second gas shower unit 22 are shown in Fig. 1 at radially shifted positions for convenience, they are actually provided alternately on the same circle. The first gas shower unit 21 supplies gas carried from a first gas supply unit 81 through a gas line 83 from the rear surface of the top wall 10a. The second gas shower unit 22 has a nozzle hanging down from the rear surface of the top wall of the processing vessel 10, and supplies gas carried from a second gas supply unit 82 through a gas line 84 from the tip of the nozzle to a position between the top wall 10a and the mounting table 11.
[0021] The plasma source 2 includes a UHF wave output unit 30 that distributes UHF waves to multiple paths and outputs them, and a UHF wave transmission unit 40 that transmits the UHF waves output from the UHF wave output unit 30. The UHF wave output unit 30 includes a UHF wave power supply, a UHF wave oscillator, an amplifier, and a distributor. The UHF wave power supply supplies power to the UHF wave oscillator. The UHF wave oscillator generates UHF waves of a predetermined frequency, for example, by PLL oscillation. The amplifier amplifies the oscillated UHF waves. The distributor distributes the UHF waves amplified by the amplifier while matching the impedance of the input side and the output side so as to minimize loss of the UHF waves. The frequency of the UHF waves is within a range of 300 MHz to 3 GHz.
[0022] The UHF wave transmission unit 40 has a plurality of amplifier units 41 and a plurality of radiation mechanisms 42 provided corresponding to the amplifier units 41. The radiation mechanisms 42 are arranged, for example, one at the center of the top wall 10a and six at equal intervals on a circumference centered on the central one, for a total of seven. In this example, these are arranged so that the distance between the central radiation mechanism 42 and the peripheral radiation mechanisms 42 is equal to the distance between the peripheral radiation mechanisms 42.
[0023] The amplifier unit 41 guides the UHF waves distributed by the distributor to each radiation mechanism 42. The radiation mechanism 42 has a coaxial tube 51. The coaxial tube 51 has a coaxial UHF wave transmission line consisting of a cylindrical outer conductor 51a and a rod-shaped inner conductor 51b provided at the center of the outer conductor 51a. The radiation mechanism 42 has a power feeding antenna (not shown) that feeds the UHF waves amplified by the amplifier unit 41 to the coaxial tube 51. Furthermore, the radiation mechanism 42 has a tuner that matches the impedance of the load to the characteristic impedance of the UHF wave power source, and an antenna unit that radiates the UHF waves from the coaxial tube into the processing vessel 10.
[0024] The antenna unit is provided at the lower end of the coaxial tube 51, and is fitted into a metal portion of the top wall 10a of the processing vessel 10. The antenna unit has a dielectric window 56, and a surface wave plasma is generated directly below the dielectric window 56 in the processing vessel 10 by the UHF wave that has passed through the dielectric window 56.
[0025] The multiple dielectric windows 56 are provided with one at the center of the ceiling and six on the outer periphery. Each of the multiple dielectric windows 56 can independently control the UHF wave power supplied from the plasma source 2. The UHF wave power supplied from the dielectric window 56 on the outer periphery may be higher than or the same as the UHF wave power supplied from the dielectric window 56 in the center.
[0026] The plasma processing apparatus 1 may have an ion trap function in the processing chamber 10, and may irradiate the substrate with hydrogen radicals in hydrogen plasma (H 2 plasma) described later.
[0027] [Overview of SiCN film formation] In the method for forming a SiCN film according to the present disclosure, a plasma-enhanced atomic layer deposition (PEALD) process by the ALD method is carried out in a plasma processing apparatus 1.
[0028] A precursor gas, which is a raw material gas, is supplied from the second gas shower unit 22. For example, when forming a SiCN film, a first gas containing a precursor gas having Si-N bonds and Si-C bonds is supplied from the second gas shower unit 22 to form an adsorption layer on the substrate W. In the process of forming the adsorption layer, no power is supplied and no plasma is used. By supplying the precursor gas to a position closer to the substrate W, dissociation of the precursor gas is suppressed and the precursor gas is adsorbed to the substrate W. In addition, in the process of forming the adsorption layer, the Si-N bonds and Si-C bonds are not activated. Therefore, the Si-N bonds and Si-C bonds of the adsorption layer are not broken.
[0029] The precursor gas may be selected from one of HMCTS, HMCTZ, TMSI, BTBAMS, BSBAMS, BTBAES, and BTBAVS (see FIG. 3). The precursor gas may have at least Si-N and Si-C bonds, but may not have Si-Si bonds.
[0030] The first gas may contain a carrier gas such as He gas. The first gas may also contain an inert gas such as Ar gas as a dilution gas. The carrier gas and dilution gas contained in the first gas may be supplied from the first gas shower unit 21. However, the dilution gas contained in the first gas may be supplied from the second gas shower unit 22.
[0031] A second gas containing H2 gas (hydrogen gas) is supplied from the first gas shower unit 21. UHF wave power is supplied to activate the H2 gas by plasma (plasma excitation). RF bias power may be optionally supplied from the RF bias power supply 14. C other than Si-C bonds contained in the precursor gas is included in group R that is easily broken with Si. By exposing the substrate W to plasma-excited H2 gas (H2 plasma) to react with the adsorption layer, the H2 plasma can break the bonds of group R. As a result, while the group R that deteriorates the properties of the SiCN film is desorbed from the adsorption layer, at least a part of the Si-N bonds and Si-C bonds of the adsorption layer are inherited by the SiCN film. According to this method, the SiCN film can be formed while controlling the temperature of the substrate W to a low temperature of 450° C. or less, and the film quality can be improved by inheriting the Si-C bonds to the SiCN film.
[0032] The second gas may include an inert gas. The inert gas may be selected from at least one of Ar gas, He gas, and N2 gas. The inert gas included in the second gas may be supplied from the first gas shower unit 21 and / or the second gas shower unit 22.
[0033] A purge process is provided between a process of supplying a first gas containing a precursor gas to form an adsorption layer on the substrate W and a process of supplying a second gas containing H2 gas to expose the substrate W to H2 plasma to react with the adsorption layer and form a SiCN film.
[0034] In the purge step, an inert gas such as Ar gas is supplied from the first gas shower unit 21 and / or the second gas shower unit 22. A purge step performed before a step of supplying a first gas containing a precursor gas into the processing vessel 10 to form an adsorption layer on the substrate W (hereinafter referred to as an "adsorption layer forming step") is referred to as a second purge step. A purge step performed before a step of supplying a second gas containing H2 gas and exposing it to H2 plasma to react with the adsorption layer to form a SiCN film (hereinafter referred to as an "SiCN film forming step") and after the adsorption layer forming step is referred to as a first purge step.
[0035] In the first and second purging steps, the gas inside the processing vessel 10 is replaced by supplying Ar gas or the like, and the gas supplied in the previous step is exhausted to the outside of the processing vessel 10 by the exhaust device 16 .
[0036] The first purge step, the adsorption layer forming step, the second purge step, and the SiCN film forming step are repeatedly performed, whereby the SiCN film can be formed on the substrate W by the ALD method while controlling the substrate W to a temperature of 450° C. or less using the plasma processing apparatus 1 of FIG.
[0037] [Low temperature deposition of SiCN film] SiN films are scraped off when exposed to etching liquids such as hydrofluoric acid used in the manufacturing process of electronic devices. Therefore, in recent years, SiCN films have been used in the manufacturing process of electronic devices as films with high wet etching resistance. In particular, with the increasing integration of devices, there is a demand for SiCN films with high wet etching resistance to be formed at low temperatures (for example, 450°C or lower).
[0038] As shown on the right side of Figure 2(a), when the substrate temperature during film formation is 600°C or higher, the Si contained in the gas bonds with C, forming Si-C bonds during film formation, and the desired SiCN film with improved film quality can be formed.
[0039] On the other hand, as shown on the left side of FIG. 2(a), when the substrate temperature is lower than 600° C. (for example, 450° C.), Si contained in the gas preferentially bonds with N in the processing vessel 10, making it difficult to bond Si and C at a low temperature, and low-temperature synthesis of Si-C bonds does not proceed. This causes a problem that a desired SiCN film cannot be formed and the film quality does not improve. In particular, when plasma is used, the Si-C bond is broken by ion energy, and ultimately, C disappears from the composition of the adsorption layer, resulting in an almost entirely SiN film.
[0040] Therefore, in the method for forming a SiCN film of this embodiment, a precursor gas having Si-C bonds is used so that the Si-C bonds of the precursor gas are inherited by the SiCN film without being broken. Furthermore, a precursor gas having not only Si-C bonds but also Si-N bonds is used so that the Si-N bonds of the precursor gas are inherited by the SiCN film without being broken. In order to inherit the Si-C bonds and Si-N bonds in the precursor gas to the SiCN film, a raw material gas having the following characteristics (1) to (3) is used as the precursor gas. (1) There is a Si-C bond. (2) There is a Si-N bond. (3) C other than Si-C and Si-N bonds is in a group that is easily broken with Si (sometimes represented by the group R, such as "R" or "R'").
[0041] Regarding (3), for example, the "R" and "R'" in Si-NH-R, Si-NR2, and Si-NRR' contain C other than Si-C bonds and Si-N bonds. For example, groups containing carbon such as CH3, which has a negative effect on the SiCN film, are included in the group R, which is easily broken with Si.
[0042] The bond energy is about 400 kJ / mol for Si-N and about 200 to 300 kJ / mol for NR in Si-NH-R, and NR is easier to break than Si-N. Therefore, when the adsorption layer reacts with H2 plasma, Si-N of Si-NH-R remains, R is broken, Si-C bonds and Si-N bonds are inherited, and C in the set R, which has a negative effect on the SiCN film, is removed.
[0043] When the Si-C bond is not inherited, as shown in FIG. 2(c), the adsorption layer does not contain Si-C bonds, and a SiCN film cannot be formed with the temperature of the substrate W controlled to 450° C. or less. On the other hand, when the Si-C bond is inherited, as shown in FIG. 2(d), the adsorption layer contains Si-C bonds, and a SiCN film with high film quality can be formed. Furthermore, by using high-frequency plasma with high plasma density using the plasma processing apparatus 1 of FIG. 1, the film quality can be further improved. In order to improve the film quality by high-density plasma, high-frequency plasma with a VHF wave or UHF wave frequency in the range of 100 MHz to 3 GHz is used.
[0044] As described above, in the method for forming a SiCN film according to the present embodiment, the Si-C bond of the adsorption layer is inherited by the SiCN film. Also, the Si-N bond of the adsorption layer is inherited by the SiCN film. According to this method, a SiCN film having high density and high etching resistance can be formed while controlling the temperature of the substrate W to 450° C. or less.
[0045] Examples of precursor gases having the above characteristics (1) to (3) include the following. Aminosilanes: R I R II NR 2-x SiH x -NR III R IV (x is an integer between 0 and 1, R is C n H m Group, R I ,R II ,R III ,R IV are the same or different C n H m group or H). R I ,R II ,R III ,R IV is an example of group R where C other than Si-C bonds and Si-N bonds are easily broken by Si. Silazanes: Cyclic [-(CH3)2Si-NH-] n , cyclic [-(CH3)SiH-NH-]n , cyclic [-(CH3)SiH-N(CH3)-] n , for example, n=4~6.
[0046] 2,2,4,4,6,6-Hexamethylcyclotrisilazane (see Figure 3(a) HMCTS), linear (CH3)3Si-NH-Si(CH3)3, (CH3)3Si-[NH-Si(CH3)2] n -Si(CH3)3, for example n=1 to 3, is an example of a precursor gas containing Si-C bonds and Si-N bonds. Note that if there are Si-C bonds, some or all of the CH3 can be converted to H or C. x H y You may change it to. Silyl imidazoles: trimethylsilylimidazole (see Figure 3(c) TMSI).
[0047] The precursor gas may be selected from one of HMCTS (Figure 3(a)), HMCTZ (Figure 3(b)), TMSI (Figure 3(c)), BTBAMS (Figure 3(d)), BSBAMS (Figure 3(e)), BTBAES (Figure 3(f)), BTBAVS (Figure 3(g)).
[0048] [SiCN film formation method] A method for forming a SiCN film according to an embodiment will be described with reference to Fig. 4 and Fig. 5. Fig. 4 is a flow chart showing an example of the method for forming a SiCN film according to an embodiment. Fig. 5(a) is a diagram showing an example of the method for forming a SiCN film according to an embodiment. Fig. 5(b) is a diagram showing a modified example of the method for forming a SiCN film according to an embodiment.
[0049] The method for forming the SiCN film is, for example, an atomic layer deposition (ALD) process executed in the plasma processing apparatus 1 of Fig. 1 and is controlled by the control device 130. In the method for forming the SiCN film according to an embodiment shown in Fig. 4, in step S1, the control device 130 opens the gate valve 18, loads the substrate W into the processing chamber 10 of the plasma processing apparatus 1 through the load / unload port 17, and places the substrate W on the mounting table 11.
[0050] Next, in step S3, the controller 130 purges the inside of the processing vessel 10 (purge step ST1 in FIG. 5(a)). The controller 130 controls the supply of an inert gas such as Ar gas into the processing vessel 10 and purging the inside of the processing vessel 10 while exhausting the gas by the exhaust device 16 for 0.1 to 60 seconds. This allows the gas in the processing vessel 10 to be exhausted, thereby adjusting the condition inside the processing vessel 10. This purge step is an example of a second purge step that purges the inside of the processing vessel 10 after the second or later repetitive process described below, after the "H2 plasma processing step (ST4)" and before the "precursor gas adsorption step (ST2)". The "precursor gas adsorption step (ST2)" is an example of a "step of forming an adsorption layer", and the "H2 plasma processing step (ST4)" is an example of a "step of forming a SiCN film".
[0051] Next, in step S5, the controller 130 supplies a first gas containing a precursor gas into the processing vessel 10 and causes it to be adsorbed onto the substrate W (FIG. 5(a) ST2). For example, TMCTS is supplied as the precursor gas, and at least one of Ar gas, He gas, and N2 gas is supplied into the processing vessel 10 as a gas other than the precursor gas contained in the first gas for 0.1 to 60 seconds. This causes the precursor to be adsorbed onto the substrate W, and an adsorption layer having Si-N bonds and Si-C bonds is formed on the substrate W.
[0052] Next, in step S7, the controller 130 purges the inside of the processing vessel 10 (purge step ST3 in FIG. 5(a)). The controller 130 controls the process to supply an inert gas such as Ar gas into the processing vessel 10 and purge the inside of the processing vessel 10 while exhausting the gas by the exhaust device 16 for 0.1 to 60 seconds. This allows the gas in the processing vessel 10 to be exhausted, thereby adjusting the condition inside the processing vessel 10. This purge step is an example of a first purge step that is performed after the "step of forming an adsorption layer (ST2)" and before the "H2 plasma processing step (ST4)" to purge the inside of the processing vessel 10.
[0053] Next, in step S9, the control device 130 supplies a second gas containing H2 gas into the processing vessel 10, supplies UHF wave power, and exposes the substrate W to H2 plasma to react with the adsorption layer to form a SiCN film (FIG. 5(a) ST4). For example, H2 gas is supplied as the second gas, and at least one of Ar gas, He gas, and N2 gas is further supplied into the processing vessel 10 for 0.1 to 60 seconds. As a result, the second gas containing H2 gas is supplied and exposed to H2 plasma to react with the adsorption layer, and the Si-C bond and Si-N bond are inherited to form a SiCN film. In addition, the set R containing C other than Si-C bond and Si-N bond is cut by ion energy in the H2 plasma. As a result, the adsorption layer reacts with the H2 plasma, leaving Si-N of Si-NH-R, and the set R is cut and the C contained in the set R is removed. As a result, the SiCN film inherits Si--C bonds and Si--N bonds from the precursor gas, and a high-quality SiCN film can be formed.
[0054] Next, in step S11, the control device 130 determines whether the set number of times has been reached, and repeats steps S3 to S9 until the set number of times n is reached, and ends this process when it is determined in step S11 that the set number of times has been reached.
[0055] (Modification) Fig. 5(b) shows a modified example of the method for forming a SiCN film according to one embodiment. Steps ST1, ST2, ST3-1, and ST4 in Fig. 5(b) are the same as steps ST1, ST2, ST3, and ST4 in Fig. 5(a). In this modified example, in addition to these steps ST, step ST3-2, which is not shown in Fig. 5(a), is also performed.
[0056] That is, a step of evacuating the inside of the processing vessel 10 in ST3-2 may be further performed after the purge step in ST3-1 and before the H2 plasma processing step in ST4. In the evacuation step, the supply of purge gas is stopped, and the pressure inside the processing vessel 10 is controlled by the exhaust device 16 to a desired degree of vacuum. The steps ST1, ST2, ST3-1, ST3-2, and ST4 may be repeated a set number of times (e.g., 100 times, etc.) (repetition of (1) in FIG. 5(b)). In this case, each time the steps ST1, ST2, ST3-1, ST3-2, and ST4 are repeated once, the steps ST3-1 and ST3-2 may be repeated a predetermined number of times (e.g., twice, etc.) (repetition of (2) in FIG. 5(b)).
[0057] The process conditions in the method for forming the SiCN film shown in Figures 5(a) and 5(b) are as follows: However, the process conditions shown below are merely examples and are not limited to these.
[0058] [Experiment 1] An experiment was carried out on the quality of the SiCN film formed by the above-mentioned method for forming a SiCN film, changing the pressure and the type of precursor gas.
[0059] <Process conditions> First gas: HMCTS, HMCTZ, BTBAS-MS, TMSI (precursor gas) Second gas: at least one of H2 gas, Ar gas, He gas, and N2 gas Substrate temperature: 100℃~450℃ Pressure inside the processing vessel: 10Pa to 400Pa Gap between the top wall 10a and the mounting table 11: 10 mm to 100 mm UHF wave frequency: 40MHz~3GHz UHF wave power: 50W~5000W
[0060] [Experimental Results] The film quality of the SiCN film formed by the SiCN film forming method will be described with reference to Fig. 6 to Fig. 9. Fig. 6 is a diagram showing an example of an experimental result of the composition and pressure dependence of the SiCN film formed by the SiCN film forming method of Fig. 4 using HMCTS as a precursor gas.
[0061] 6, the horizontal axis indicates the pressure inside the processing vessel 10, and the vertical axis indicates the composition of the formed SiCN film. The pressure inside the processing vessel 10 was set to 20 Pa, 40 Pa, and 133 Pa in the process of forming an adsorption layer using a first gas containing at least a precursor and the process of forming a SiCN film.
[0062] As a result, it was found that C (carbon) was contained in the film at all pressures of 20 Pa, 40 Pa, and 133 Pa. In the SiCN film formation method shown in Figure 4, C in set R was removed during film formation, so the presence of C in the film indicated that the Si-C bond contained in the precursor gas was inherited by the SiCN film.
[0063] It was also found that N (nitrogen) was contained in the film at all pressures of 20 Pa, 40 Pa, and 133 Pa. In other words, it was found that the Si-N bonds contained in the precursor gas were inherited by the SiCN film.
[0064] In addition, the concentration of C contained in the SiCN film changed depending on the pressure inside the processing vessel 10. From the results shown in Fig. 6, it was found that when the pressure inside the processing vessel 10 becomes low at about 20 Pa, ions collide with the substrate W in a state of strong ion energy, and therefore the probability of breaking the Si-C bond increases.
[0065] FIG. 7 is a graph showing the relationship between the carbon concentration in the SiCN film and the film density formed by the method of forming a SiCN film of FIG. 4 using HMCTS and other precursor gases.
[0066] 7, the horizontal axis indicates the pressure in the process vessel 10 for each type of precursor gas, the left vertical axis indicates the carbon concentration in the formed SiCN film, and the right vertical axis indicates the film density of the formed SiCN film. The pressure in the process vessel 10 was set to 20 Pa and 40 Pa in the process of forming an adsorption layer using at least the first gas containing a precursor and the process of forming a SiCN film.
[0067] As a result, it was found that the carbon concentration in the film was higher at 40 Pa than at 20 Pa, regardless of which precursor gas was used. In the SiCN film formation method shown in Figure 4, C in set R was removed during film formation, and therefore, the presence of C in the film indicated that the Si-C bond contained in the precursor gas was inherited by the SiCN film.
[0068] It was also found that, regardless of the precursor gas used, when the pressure was reduced (20 Pa), the carbon concentration in the film decreased and the film density decreased.
[0069] Therefore, in the process of forming an adsorption layer by the first gas containing a precursor and the process of forming a SiCN film, it is preferable to control the pressure in the processing vessel 10 within a range of 10 Pa to 400 Pa. This allows at least a part of the Si-C bonds and Si-N bonds contained in the precursor gas to be inherited. As a result, a SiCN film with high film quality can be formed because of the presence of Si-C bonds in the SiCN film. In addition, it is preferable to control the pressure to an appropriate level within the above pressure range and reduce the ion energy so as not to break the Si-C bonds. Furthermore, it is preferable to use a frequency of 40 MHz or more for the UHF wave to generate high-density plasma. This allows the film quality of the SiCN film to be further improved.
[0070] Fig. 8 is a diagram showing an XPS spectrum measured by X-ray photoelectron spectroscopy (XPS) of a SiCN film formed using HMCTS as a precursor gas by the SiCN film formation method of Fig. 4. In the experiment of Fig. 8, a SiCN film was formed by the SiCN film formation method of Fig. 4 using the above process conditions.
[0071] 8, the horizontal axis indicates binding energy (eV), and the vertical axis indicates XPS spectrum intensity (CPS). Line A in the figure indicates the state of binding energy in the XPS spectrum of a film, with a SiCN film formed by controlling the inside of processing vessel 10 to 40 Pa as the base. Line B indicates the state of binding energy in the XPS spectrum of a SiCN film formed by controlling the inside of processing vessel 10 to 20 Pa. Line C indicates the state of binding energy in the XPS spectrum of a SiCN film formed by controlling the inside of processing vessel 10 to 133 Pa.
[0072] According to this, at the binding energy of the XPS spectrum when the inside of the processing vessel 10 of line C is 133 Pa, the peak of the XPS spectrum indicating the Si-C bond of the measured SiCN film is at a high position similar to the Base of line A, and it was found that many Si-C bonds are inherited in the SiCN film similar to the Base of line A. It was also found that the bonding state of C in the SiCN film is mainly Si-C bonding, with some being C-C bonding and / or C-H bonding (CC(H) in the figure). It was found that the peak of C-C(H) of the SiCN film of line C is lower than the Base of line A, and the film quality is even better than that of the Base.
[0073] On the other hand, the peaks of the XPS spectrum for line B are low for both the Si-C bond and CC(H) of the measured SiCN film, and it was found that the number of Si-C bonds inherited in the SiCN film is smaller than those of lines A and C. It was also found from the results shown in Fig. 8 that when the pressure inside the processing vessel 10 becomes low at about 20 Pa, ions collide with the substrate with strong ion energy, increasing the probability of breaking the Si-C bond.
[0074] Fig. 9 is a diagram showing an example of an experimental result of the composition and film characteristics of a SiCN film formed using HMCTS as a precursor gas by the SiCN film formation method of Fig. 4. In the experiment of Fig. 9, a SiCN film was formed by the SiCN film formation method of Fig. 4 using the above process conditions.
[0075] Fig. 9 shows the pressure in the processing vessel 10 during film formation, the composition, composition ratio, RI, film density, and WER (wet etch rate) of the SiCN film. As shown in the results of Fig. 9, according to the method for forming the SiCN film in Fig. 4, the Si-C bond and Si-N bond of the precursor gas could be inherited by the SiCN film as shown in the composition and composition ratio of the SiCN film at any pressure. In addition, the RI was roughly the same at any pressure and did not change.
[0076] Furthermore, when the pressure was 40 Pa and 133 Pa, the C content in the SiCN film was 20% or more, which was more than three times that when the pressure was 20 Pa. Therefore, it was found that the pressure in the processing vessel 10 during film formation should be controlled within the range of 10 Pa to 400 Pa, but it is more preferable to control it to 40 Pa or more.
[0077] Generally, the higher the C content in the SiCN film, the lower the film density. The higher the film density, the better the film quality. For example, in an ALD apparatus that performs batch-type heat treatment, when the C content in the SiCN film is about 12%, the film density is about 2.6. In contrast, in the method of forming a SiCN film in FIG. 4, when the pressure inside the processing vessel 10 is 40 Pa and 133 Pa, the film density (g / cm 3 ) was more than 2.8, and a high-density SiCN film could be produced.
[0078] WER (Wet Etch Rate) indicates the amount (Å / min) of etching that occurs in one minute when hydrofluoric acid has a concentration of 0.5%. The SiCN film was hardly removed when the pressure inside the processing vessel 10 was 20 Pa, 40 Pa, or 133 Pa. In other words, the SiCN film formed by the SiCN film forming method of FIG. 4 had sufficient film properties including etching resistance (hydrofluoric acid resistance).
[0079] [Experiment 2] Next, an experiment was conducted to control the carbon concentration in the SiCN film. Fig. 10 is a flow chart showing an example of a method for forming a SiCN film used in this experiment. Fig. 11 is a diagram showing an example of a method for forming a SiCN film used in this experiment.
[0080] In the method for forming a SiCN film shown in Fig. 10, when ST1 to ST4 in Fig. 11 are repeated a first set number of times, an H2 plasma treatment step (ST4) is performed once every second set number of times, which is less than the first set number, followed by a purge step (ST5) and an N2 plasma treatment step (ST6). The N2 plasma treatment is an example of a modification step in which a third gas containing N2 gas and VHF or UHF wave power are supplied into the processing vessel 10 to generate plasma, and the substrate W is exposed to the N2 plasma for modification. This modification step is performed at a predetermined frequency while the steps ST1 to ST4 in Fig. 11 are repeated.
[0081] First, in step S1, the controller 130 opens the gate valve 18, loads the substrate W through the load / unload port 17, and places it on the mounting table 11. Next, in step S3, the controller 130 purges the inside of the processing vessel 10 (FIG. 11, ST1). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the inside of the processing vessel 10 is purged while being exhausted by the exhaust device 16 for 0.1 to 60 seconds. This adjusts the condition inside the processing vessel 10. This purging process is an example of a second purging process.
[0082] Next, in step S5, the controller 130 supplies a first gas containing a precursor gas into the processing chamber 10 and causes it to be adsorbed onto the substrate W (FIG. 11 ST2). For example, TMCTS is supplied as the precursor gas, and at least one of Ar gas, He gas, and N2 gas is supplied into the processing chamber 10 as a gas other than the precursor gas contained in the first gas for 0.1 to 60 seconds. This causes the precursor to be adsorbed onto the substrate W, and an adsorption layer having Si-N bonds and Si-C bonds is formed on the substrate.
[0083] Next, in step S7, the controller 130 purges the inside of the processing vessel 10 (ST3 in FIG. 11). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the inside of the processing vessel 10 is purged while being exhausted by the exhaust device 16 for 0.1 to 60 seconds. This adjusts the condition inside the processing vessel 10. This purging process is an example of a first purging process.
[0084] Next, in step S9, the control device 130 supplies a second gas containing H2 gas into the processing vessel 10, supplies UHF wave power, and exposes the substrate W to H2 plasma to react with the adsorption layer to form a SiCN film (FIG. 11 ST4). For example, H2 gas is supplied as the second gas, and further, for example, at least one of Ar gas, He gas, and N2 gas is supplied into the processing vessel 10 for 0.1 to 60 seconds. As a result, the second gas containing H2 gas is supplied and exposed to H2 plasma to react with the adsorption layer, and the Si-C bond and Si-N bond are inherited to form a SiCN film. In addition, the set R containing C other than the Si-C bond is broken by the ion energy in the H2 plasma. As a result, the adsorption layer reacts with the H2 plasma, leaving Si-N of Si-NH-R, and R is broken to remove C other than the Si-C bond. As a result, the carbon of the SiCN film becomes Si-C bond, and a SiCN film with high film quality can be formed.
[0085] Next, in step S13, the control device 130 determines whether the first set number of times has been reached, and if the first set number of times has not been reached, the process immediately returns to step S3, and the processes from step S3 onwards are repeated.
[0086] When the first set number of times is reached in step S13 and the process proceeds to step S15, the controller 130 purges the inside of the processing vessel 10 (ST5 in FIG. 11). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the inside of the processing vessel 10 is purged while being exhausted by the exhaust device 16 for 0.1 to 60 seconds. This allows the condition inside the processing vessel 10 to be adjusted. This purge process is an example of a third purge process.
[0087] Next, in step S17, the control device 130 supplies a third gas containing N2 gas into the processing vessel 10, supplies UHF wave power, and exposes the substrate to N2 plasma to modify the SiCN film (FIG. 11 ST6). As the third gas, at least one of Ar gas, He gas, and N2 gas is supplied into the processing vessel 10 for 0.1 to 60 seconds as a gas other than N2 gas. As a result, the third gas containing N2 gas is supplied to expose the substrate W to N2 plasma to react with the adsorption layer, and the SiCN film is modified. Note that the N2 plasma is not limited to UHF wave power, and may be, for example, VHF wave power.
[0088] Next, in step S19, the control device 130 determines whether the second set number of times has been reached. The second set number of times is set to a number of times less than the first set number of times. As an example, the first set number of times is set to 5 to 300 times, and the second set number of times is set to 1 to 30 times. However, this is not limited to this, and step S17 may be executed at a predetermined frequency while the processes of steps S3 to S9 are repeated. If the second set number of times has not been reached, the process immediately returns to step S3, and the processes from step S3 onwards are repeated. If it is determined that the second set number of times has been reached, this process ends.
[0089] The main process conditions for the SiCN film formed by the above-mentioned SiCN film forming method are as follows.
[0090] <Process conditions> First gas: THMCTS, HMCTZ, BTBAS-MS, TMSI (precursor gas) Second gas: H2 gas and at least one of Ar gas, He gas, and N2 gas Third gas: N2 gas Substrate temperature: 100℃~450℃ Pressure inside the processing vessel: 10Pa to 400Pa Gap between the top wall 10a and the mounting table 11: 10 mm to 100 mm UHF wave frequency: 40MHz~3GHz UHF wave power: 50W~5000W
[0091] [Experimental Results] FIG. 12 is a diagram showing the relationship between the carbon concentration in the SiCN film and the film density formed by the SiCN film forming method of FIG. 10 using precursor gases of HMCTS, HMCTZ, BTBAS-MS, and TMSI.
[0092] The horizontal axis of FIG. 12 indicates the modification frequency by N2 plasma treatment for each type of precursor gas, and the vertical axis on the left indicates the carbon concentration in the SiCN film formed. The vertical axis on the right indicates the film density of the SiCN film formed. The modification frequency was set to 0 (no N2 plasma treatment), 1 / 50, and 1 / 8 as the ratio of the number of times of N2 plasma treatment to H2 plasma (second set number of times / first set number of times, see FIG. 10). The first set number of times is the number of times (1) of repetition of the H2 plasma treatment step (ST4) shown in FIG. 11, and the second set number of times is the number of times (2) of repetition of the N2 plasma treatment step (ST6).
[0093] As a result, it was found that the carbon concentration in the SiCN film can be adjusted and controlled by changing the frequency of the modification treatment using N2 plasma.
[0094] In addition, by performing the modification process using N2 plasma (S17 in FIG. 10), the quality of the SiCN film can be improved compared to the case where the modification process using N2 plasma is not performed. It was found that these processes enable the carbon concentration in the SiCN film to be controlled to a desired concentration while maintaining the film quality.
[0095] As described above, according to the first and second embodiments of the method for forming a SiCN film, the Si-C bond of the precursor gas can be inherited by the SiCN film formed on the substrate. This allows the formation of a high-quality SiCN film. In addition, the quality of the SiCN film can be further improved by generating high-frequency plasma with high plasma density by VHF waves or UHF waves with a frequency of 100 MHz to 3 GHz.
[0096] Furthermore, according to the method for forming a SiCN film by performing modification treatment with N2 plasma, N2 plasma treatment is performed at a predetermined frequency to adjust the C content in the SiCN film, which makes it possible to adjust the N and C concentrations in the SiCN film while improving the film quality of the SiCN film.
[0097] The SiCN film forming method and plasma processing apparatus according to the presently disclosed embodiments should be considered as illustrative and not restrictive in all respects. The embodiments can be modified and improved in various forms without departing from the scope and spirit of the appended claims. The matters described in the above embodiments can be configured in other ways without any contradiction, and can be combined without any contradiction.
[0098] The plasma processing apparatus of the present disclosure can be applied to any type of apparatus, including Capacitively Coupled Plasma (CCP), Inductively Coupled Plasma (ICP), Radial Line Slot Antenna (RLSA), Electron Cyclotron Resonance Plasma (ECR), and Helicon Wave Plasma (HWP). [Explanation of symbols]
[0099] 1. Plasma processing equipment 2. Plasma Source 10 Processing vessel 11 Placement table 130 Control device
Claims
1. (a) providing a substrate in a processing chamber; (b) supplying a first gas containing a precursor gas having a Si—N bond and a Si—C bond into the processing vessel to form an adsorption layer on the substrate, the Si—N bond and the Si—C bond not being activated in the formation of the adsorption layer; (c) a first purging step of purging the inside of the processing vessel after the step (b); (d) supplying a second gas containing hydrogen gas and VHF or UHF power into the processing vessel to generate plasma, and exposing the substrate to the plasma to react with the adsorption layer, thereby forming a SiCN film, the SiCN film inheriting at least a portion of the Si—C bonds and Si—N bonds of the adsorption layer; (e) a second purging step of purging the processing vessel after the step (d), The method for forming a SiCN film comprises repeating the steps (b) to (e).
2. The precursor gas does not have a Si-Si bond; The method for forming a SiCN film according to claim 1 .
3. The frequency of the VHF wave or UHF wave is within the range of 100 MHz to 3 GHz. The method for forming a SiCN film according to claim 1 .
4. In the steps (b) and (d), the pressure in the processing vessel is within a range of 10 Pa to 400 Pa; The method for forming a SiCN film according to any one of claims 1 to 3.
5. The second gas comprises an inert gas. The method for forming a SiCN film according to any one of claims 1 to 3.
6. The inert gas is Ar gas, He gas, N 2 At least one of the gases, The method for forming a SiCN film according to claim 5 .
7. The method further includes a step of (f) evacuating the processing vessel after the step (c) and before the step (d). The method for forming a SiCN film according to any one of claims 1 to 3.
8. repeating the steps (c) and (f) a predetermined number of times, and then carrying out the step (d); The method for forming a SiCN film according to claim 7.
9. The precursor gas is selected from one of HMCTS, HMCTZ, TMSI, BTBAMS, BSBAMS, BTBAES, BTBAVS; The method for forming a SiCN film according to any one of claims 1 to 3.
10. The temperature of the substrate is 450° C. or less. The method for forming a SiCN film according to any one of claims 1 to 3.
11. (g) further comprising a modification step of generating plasma by supplying a third gas containing nitrogen gas and VHF or UHF electric power into the processing vessel, and exposing the substrate to the plasma for modification; The method for forming a SiCN film according to any one of claims 1 to 3.
12. The step (g) is performed at a predetermined frequency while the steps (b) to (e) are repeated. The method for forming a SiCN film according to claim 11.
13. A processing vessel and a control device are provided. The control device is a plasma processing apparatus that controls the method of forming a SiCN film according to any one of claims 1 to 13.
Citation Information
Patent Citations
Organic aminodisilane precursor and method for depositing film containing the same
JP2014013888A
Aza-polysilane precursor and process of depositing film including the same
JP2015015465A
Low-temperature plasma chemical vapor deposition of conformal silicon nitride carbon films and conformal silicon nitride films
JP2015507362A
Apparatus And Methods For Deposition Of Silicon Carbide And Silicon Carbonitride Films