Laminate, antenna
A laminate with a boron nitride and graphene layer configuration addresses the need for high electron mobility and transparency, enabling the development of efficient antennas with a wide resonant frequency range.
Patent Information
- Application Number
- JP2023051137
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a demand for new devices that utilize the properties of graphene, particularly in developing laminates and antennas, but existing methods for producing graphene do not effectively enhance electron mobility and other desired characteristics.
A laminate configuration is developed with a substrate, a boron nitride layer, and a graphene layer, where the graphene layer exhibits an electron mobility of 6000 cm²/Vs or higher, featuring a turbostratic structure, low surface roughness, and specific sheet resistance, enabling high electron mobility and transparency.
The laminate provides enhanced electron mobility and transparency, allowing for the development of novel antennas with a resonant frequency range of 0.3 to 50 GHz, leveraging the unique properties of graphene for improved device performance.
Smart Images

Figure 2024140133000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate, and more particularly to a laminate having a graphene layer. The present invention also relates to an antenna comprising the laminate described above. [Background technology]
[0002] Graphene is a material in which the carbon atoms are sp 2 Graphene is a sheet-like substance that is bound together by bonds, and graphite is made up of stacked graphene sheets. In graphene, carbon atoms and their bonds form a hexagonal lattice structure (hexagonal mesh surface).
[0003] Patent Document 1 discloses a method for producing graphene, in which a surface of a silicon carbide (SiC) substrate is heated while being supplied with C2H2 gas and O2 gas, and a buffer layer selected from the group consisting of SiOC and a single layer of graphene are formed. Patent Document 1 also discloses peeling off the produced graphene and transferring it to another substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-056749 A Summary of the Invention [Problem to be solved by the invention]
[0005] Due to the above-mentioned structure, graphene exhibits properties that make it applicable to various devices. In recent years, there has been a demand for the development of new devices that take advantage of the properties of graphene.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a novel laminate having a graphene layer. Another object of the present invention is to provide an antenna using the above laminate. [Means for solving the problem]
[0007] As a result of extensive investigation into the above problems, the present inventors have found that the above problems can be solved by the following configuration. [1] A semiconductor device comprising a substrate, a boron nitride layer, and a graphene layer in this order, the graphene layer having an electron mobility of 6000 cm 2 / Vs or more, stack. [2] The laminate according to [1], wherein the boron nitride layer contains hexagonal boron nitride. [3] The laminate according to [1] or [2], wherein the graphene layer has 1 to 20 graphene sheets. [4] The laminate according to any one of [1] to [3], wherein the graphene layer has a turbostratic structure. [5] The laminate according to any one of [1] to [4], wherein the surface roughness of the surface of the graphene layer opposite to the substrate is 0.1 to 2.0. [6] The laminate according to any one of [1] to [5], wherein the graphene layer has a sheet resistance of 15 Ω / sq. or less. [7] In the Raman spectrum of the laminate, E originating from hexagonal boron nitride 2g The peaks are observed above E 2g The average half-width of the peak is 10 to 50 cm -1 The laminate according to [1], [8] The laminate according to [1], having a total light transmittance of 50% or more. [9] The laminate according to [1], wherein the substrate is a transparent substrate.
[10] An antenna comprising the laminate according to any one of [1] to [9].
[11] The antenna according to the above, having a resonant frequency of 0.3 to 50 GHz. Effect of the Invention
[0008] According to the present invention, a novel laminate having a graphene layer can be provided. Moreover, according to the present invention, there can be provided an antenna using the above laminate. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing an example of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The following description of the configuration may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment.
[0011] The meaning of each description in this specification is as follows. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0012] In this specification, graphene includes not only single-layer graphene consisting of a single graphene sheet, but also multi-layer graphene consisting of stacked single-layer graphene sheets. The number of layers of the graphene sheets in the multi-layer graphene is preferably 2 to 10, more preferably 2 to 5. The graphene sheet is sp 2 Graphene is a sheet of carbon atoms bonded together in a plane by bonds, with a thickness of one carbon atom. A graphene sheet has a carbon atom at each vertex of the hexagonal mesh plane.
[0013] <Laminate> The laminate of the present invention has a substrate, a boron nitride layer (hereinafter also referred to as a "BN layer"), and a graphene layer in this order, and the graphene layer has an electron mobility of 6000 cm 2 / Vs or more. The laminate of the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view of a laminate 10, which is an example of the laminate of the present invention. The laminate 10 shown in Figure 1 includes a substrate 12, a BN layer 14, and a graphene layer 16, in that order. The electron mobility of the graphene layer 16 is 6000 cm 2 / Vs or more.
[0014] In the laminate of the present invention, the mechanism by which the electron mobility of the graphene layer is increased is not necessarily clear, but the present inventors speculate as follows. In the laminate of the present invention, the graphene layer is provided in contact with the surface of the BN layer, so that the graphene layer is less susceptible to phonon scattering originating from the substrate. In addition, since the lattice constants of the graphene layer and the BN layer are close to each other, stress is less likely to act on the graphene layer, and the electron mobility of the graphene layer is less likely to decrease. As a result, it is believed that the electron mobility of the graphene layer is increased in the laminate of the present invention.
[0015] Preferred properties of the laminate of the present invention and the layers constituting the laminate of the present invention will be described in detail below.
[0016] [substrate] The laminate of the present invention has a substrate. The substrate in the laminate of the present invention is not particularly limited, and any conventionally known substrate can be used. The substrate has a first main surface on which the BN layer and the graphene layer are formed. The first main surface may be a flat surface or a curved surface.
[0017] The material constituting the substrate is not particularly limited, and may be an organic material or an inorganic material. Preferred examples of the organic material include resins, such as polyester resins, polyimide resins, polyurethane resins, polyalkylene resins, and fluorine-containing resins. Inorganic materials include materials containing metal elements and semiconductor elements. In this case, specific examples of materials constituting the substrate include silicon oxide, silicon carbide, titanium oxide, aluminum oxide, metallic silicon, metallic germanium, silicon-germanium alloy, gallium arsenide, zinc oxide, indium phosphide, and gallium nitride. The inorganic material may be glass, such as common glass containing silicon dioxide as a main component, for example, soda-lime silicate glass, aluminosilicate glass, borosilicate glass, alkali-free glass, and quartz glass. The substrate has a thermal expansion coefficient of 1.0×10 -5 ~5.0×10 -7 K -1 It is preferable that:
[0018] The substrate is also preferably a transparent substrate. A transparent substrate refers to a substrate having a total light transmittance of 60% or more in the visible light region (wavelength 400 to 760 nm). The total light transmittance of the transparent substrate in the visible light region is preferably 70% or more, and more preferably 80% or more. The total light transmittance of the transparent substrate can be measured with a spectrophotometer. When the substrate is a transparent substrate, examples of the material constituting the substrate include the above-mentioned glass.
[0019] The thickness of the substrate is not particularly limited, but is preferably from 100 μm to 5 mm, and more preferably from 0.5 to 1 mm.
[0020] [Boron nitride layer] The laminate of the present invention has a boron nitride layer (BN layer). The BN layer in the laminate of the present invention is not particularly limited as long as it contains boron nitride, but it is preferable that it contains hexagonal boron nitride (h-BN). Hereinafter, the boron nitride layer containing hexagonal boron nitride is also referred to as "h-BN layer". Hexagonal boron nitride has a structure in which boron nitride sheets are stacked at the vertices of the hexagonal mesh planes such that nitrogen atoms and boron atoms are bonded to each other. In the h-BN layer, the stacked structure of the boron nitride sheets is not particularly limited, but a turbostratic structure is preferred. A turbostratic h-BN layer means that the unit lattice vectors in the in-plane direction of two adjacent boron nitride sheets are not parallel to each other. A turbostratic h-BN layer can be obtained by the method described below.
[0021] It is preferable that the crystallinity of the h-BN layer is high in order to increase the electron mobility of the graphene layer. The crystallinity of the h-BN layer can be measured, for example, by Raman spectroscopy. The measurement method of Raman spectroscopy will be described later.
[0022] The crystallinity of the h-BN layer may be analyzed by analyzing the ultraviolet absorption peak corresponding to the band gap of hexagonal boron nitride. In other words, the laminate of the present invention preferably has a maximum absorption wavelength of 205 to 280 nm, in order to increase the electron mobility of the graphene layer.
[0023] The thickness of the BN layer is not particularly limited, but is preferably 1 nm or more, more preferably 8 nm or more, and is preferably 50 nm or less.
[0024] [Graphene layer] The laminate of the present invention has a graphene layer. The graphene layer in the laminate of the present invention contains graphene sheets and has an electron mobility of 6000 cm 2 There is no particular limitation as long as it is equal to or greater than / Vs. The graphene layer may be a single-layer graphene consisting of a single graphene sheet, or a multi-layer graphene consisting of multiple graphene sheets. The number of graphene sheets in the multi-layer graphene is preferably 2 to 20, more preferably 2 to 10. That is, the total number of graphene sheets in the graphene layer is preferably 1 to 20, more preferably 1 to 10. The number of graphene sheets in the graphene layer can be determined by a known method. For example, a Raman spectrum of the graphene layer is obtained, and -1 The number of layers of graphene sheets can be determined by peak analysis of the so-called 2D band observed around 1590 cm. -1 The number of layers of the graphene sheets may be determined by peak analysis of the so-called G band observed in the vicinity of the graphene sheet. The number of graphene sheets in the graphene layer may be determined by measuring the thickness through microscopic observation.
[0025] When the graphene layer is made of multilayer graphene, the stacked structure of the graphene sheets is not particularly limited. In particular, the multilayer graphene preferably has a turbostratic structure, in that the graphene layer has a higher electron mobility. The term "turbostratic multilayer graphene" means that the unit lattice vectors in the in-plane direction of two adjacent graphene sheets are not parallel to each other. Turbostratic multilayer graphene can be obtained by the method described below.
[0026] The electron mobility in the graphene layer is 6000 cm 2 / Vs or more. The electron mobility in the graphene layer can be measured by the van der Pauw method at a measurement temperature of 23°C. The electron mobility in the graphene layer is 6300 cm 2 / Vs or more is preferable, 7500cm 2 The upper limit of the electron mobility is not particularly limited, but is, for example, 20,000 cm 2 / Vs are mentioned.
[0027] The graphene layer may contain elements other than carbon. Examples of elements that the graphene layer may contain include hydrogen, boron, nitrogen, oxygen, sulfur, and transition metal elements. Among these, boron or sulfur is preferable. The graphene layer may also contain a compound other than graphene, such as bis(trifluoromethanesulfonyl)amine, nitric acid, and iron(III) chloride.
[0028] It is also preferable that the surface roughness of the graphene layer on the side opposite to the substrate is 0.1 to 2.0 nm. If the surface roughness is 2.0 nm or less (more preferably 0.5 nm or less), the graphene layer has better electron mobility. The surface roughness is obtained by observing and analyzing the surface of the graphene layer using an atomic force microscope, and refers to the arithmetic mean roughness (Ra) calculated from a roughness curve obtained by observation using an atomic force microscope.
[0029] The sheet resistance of the graphene layer is preferably 100 Ω / sq. or less, more preferably 30 Ω / sq. or less, and even more preferably 15 Ω / sq. or less. The lower limit of the sheet resistance of the graphene layer is not particularly limited, but may be 0.01 Ω / sq. The sheet resistance of the graphene layer can be measured by a known method, for example, by a four-terminal method.
[0030] [Other layers] The laminate of the present invention may have layers (other layers) other than those explained above. The other layer may be a protective layer. The protective layer is preferably disposed on the side opposite to the substrate side of the graphene layer. The protective layer is preferably made of an insulating material. The protective layer may preferably be a hexagonal boron nitride layer separate from the BN layer, or a substrate separate from the substrate. It is also preferable that the laminate of the present invention does not have a hexagonal boron nitride layer, separate from the BN layer, on the side of the graphene layer opposite the substrate side.
[0031] [Transmittance of laminate] The total light transmittance in the visible light region of the laminate of the present invention is preferably 50% or more, and more preferably 60% or more. The total light transmittance of the laminate can be measured with a spectrophotometer.
[0032] [Raman spectrum of laminate] In the laminate of the present invention, when the Raman spectrum was obtained, E originating from hexagonal boron nitride was 2g A peak was observed, E 2g The average half-width of the peak is 10 to 50 cm -1 It is also preferable that: E 2g A small average half-width of the peak indicates that the crystallinity of the hexagonal boron nitride contained in the BN layer is high. E 2g The peak is usually at 1320-1420 cm -1 Observed nearby.
[0033] In addition, when the Raman spectrum of the laminate of the present invention was obtained, a peak derived from the graphene layer was observed at 2700 cm -1 The half-width of the so-called 2D band observed near the -1 It is preferable that the half-width of the 2D band is 40 cm or less. -1 The electron mobility of the graphene layer is likely to be higher when the 2D band width is less than 20 cm. -1 In many cases it is more than that.
[0034] <Method of manufacturing laminate> The method for producing the laminate of the present invention is not particularly limited as long as the above-mentioned laminate can be obtained. For example, a method for producing the laminate of the present invention includes a method in which a separately prepared BN layer is transferred to a substrate, and then a separately prepared graphene layer is transferred to the substrate. Moreover, as a method for producing the laminate of the present invention, a method in which a separately prepared BN layer is transferred onto a substrate, and a graphene layer is formed on the surface of the BN layer by a vapor phase method can be mentioned. Further, as a method for producing the laminate of the present invention, a method in which a BN layer is formed on one surface of a substrate by a vapor phase method or the like, and a separately prepared graphene layer is transferred to the substrate can be mentioned. Further, a method for producing the laminate of the present invention may include a method in which a BN layer is formed on one surface of a substrate by a vapor phase method or the like, and a graphene layer is formed on the surface of the BN layer by a vapor phase method. Among these, it is preferable to apply one or more of the manufacturing methods described below, since the electron mobility of the graphene layer can be further improved.
[0035] In manufacturing the laminate, the BN layer (preferably an h-BN layer) is preferably prepared by chemical vapor deposition. In addition, if an h-BN layer is transferred onto an h-BN layer having one or more already formed hexagonal boron nitride sheets, a turbostratic h-BN layer can be formed.
[0036] In the production of the laminate, the formation of the graphene layer preferably includes a step of transferring a graphene sheet. A graphene layer having a turbostratic structure can be formed by transferring a graphene sheet onto a graphene layer having one or more graphene sheets already formed. The number of graphene sheets transferred in one transfer is preferably 1 to 3 layers, more preferably 1 or 2 layers, and even more preferably 1 layer. The preferred number of graphene sheets in the graphene layer is as described above.
[0037] The graphene sheet to be transferred can be formed by a known method, for example, a method in which a hydrocarbon gas is supplied to a catalyst substrate having an exposed copper (111) surface, and the catalyst substrate is heated. Specific examples of the hydrocarbons used in the hydrocarbon gas include saturated hydrocarbons such as methane, ethane, propane, butane, pentane, hexane, and cyclohexane; unsaturated hydrocarbons such as ethylene, acetylene, propylene, butadiene, pentene, and cyclopentadiene; and aromatic hydrocarbons such as benzene and toluene. These may be used alone or in combination of two or more. Among these, hydrocarbons having 10 or less carbon atoms are preferred, and hydrocarbons having 5 or less carbon atoms are more preferred. The heating temperature is preferably from 300 to 1200° C., and more preferably from 500 to 1000° C., in that a graphene layer with few defects can be obtained. The heating time is preferably from 1 to 300 minutes, and more preferably from 10 to 60 minutes. Although copper has been shown as the catalyst substrate in the above, the catalyst substrate may be, for example, a catalyst substrate in which the (111) plane of nickel is exposed.
[0038] In producing the laminate, when the graphene layer is formed by transfer, a known transfer method can be applied. In order to increase the electron mobility of the graphene layer, the transfer method is preferably a method in which the graphene sheet to be transferred does not come into contact with water (dry transfer). A specific example of the dry transfer method is a method of transferring a graphene sheet onto a tape whose adhesive strength decreases when exposed to heat or ultraviolet light, heating the tape or irradiating it with ultraviolet light, and transferring the graphene sheet onto a substrate or an already formed graphene layer. Another specific example of the dry transfer method is a method of transferring the graphene sheet under a reduced pressure environment.
[0039] <Antenna> In the laminate of the present invention, since the graphene layer functions as a conductor, the laminate of the present invention can be used, for example, as an antenna. An antenna using the laminate of the present invention (antenna of the present invention) will be described below.
[0040] The resonant frequency of the antenna of the present invention is preferably 0.3 to 50 GHz. In order to use the laminate of the present invention as an antenna, the shape of the graphene layer in the laminate may be adjusted to match the desired resonant frequency. When the graphene layer in the laminate of the present invention is processed into a rectangular shape having sides of about λ / 2, where λ is the wavelength of radio waves at the above-mentioned resonant frequency, it can function as an antenna with a wavelength of λ. The graphene layer may also be processed into a linear shape having sides of λ / 4. The graphene layer may also be processed to match the type of a conventionally known antenna. In order to operate the laminate of the present invention as an antenna, an electrode electrically connected to the graphene layer may be formed, and a predetermined alternating current may be supplied from the electrode, or a current generated in the graphene layer may be detected by the electrode. The electrode may be formed by a known means. [Explanation of symbols]
[0041] 10 Laminate 12 Substrate 14 BN layer (boron nitride layer) 16 graphene layers
Claims
1. The present invention comprises a substrate, a boron nitride layer, and a graphene layer in this order, and the graphene layer has an electron mobility of 6000 cm 2 / Vs or more.
2. The laminate of claim 1 , wherein the boron nitride layer comprises hexagonal boron nitride.
3. 2. The laminate according to claim 1, wherein the number of graphene sheets in the graphene layer is 1 to 20.
4. The laminate according to claim 1 , wherein the graphene layer has a turbostratic structure.
5. 2. The laminate according to claim 1, wherein a surface roughness of the surface of the graphene layer opposite to the substrate side is 0.1 to 2.
0.
6. The laminate according to claim 1 , wherein the graphene layer has a sheet resistance of 15 Ω / sq. or less.
7. In the Raman spectrum of the laminate, E originating from hexagonal boron nitride 2g A peak was observed, and the E 2g The average half-width of the peak is 10 to 50 cm -1 The laminate according to claim 1 ,
8. The laminate according to claim 1 , having a total light transmittance of 50% or more.
9. The laminate according to claim 1 , wherein the substrate is a transparent substrate.
10. An antenna comprising the laminate according to any one of claims 1 to 9.
11. The antenna according to claim , wherein the resonant frequency is 0.3 to 50 GHz.
Citation Information
Patent Citations
Graphene production method and stack for graphene production
JP2022056749A