All-solid battery
By integrating an expanded metal mesh with specified dimensions and flexibility into the electrode layers of all-solid-state batteries, the internal resistance is reduced, enhancing ion transfer and conductivity.
Patent Information
- Application Number
- JP2023051283
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
All-solid-state batteries exhibit excessively high internal resistance, necessitating a reduction to enhance performance.
Incorporating an expanded metal mesh with specific dimensions and flexibility into the electrode layers, combined with a solid electrolyte, to form a dense electrode layer that reduces internal resistance.
The solution results in an all-solid-state battery with lower internal resistance, ensuring effective ion transfer and electrical conductivity despite expansion and contraction during charging and discharging.
Smart Images

Figure 2024140240000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery. [Background technology]
[0002] In recent years, electronics technology has made remarkable progress, and efforts are being made to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for electronic devices, to be smaller, lighter, thinner, and more reliable. Thus, attention is being paid to all-solid-state batteries that use a solid electrolyte as the electrolyte. Conventionally, oxide-based solid electrolytes, complex hydride-based solid electrolytes, and the like are known as solid electrolytes for all-solid-state batteries (for example, Patent Document 1).
[0003] In Patent Document 1, a non-flammable solid electrolyte having the general formula Li 1+x M III x Ti IV 2-x (PO4)3 (where 0≦x≦0.6, M III An all-solid-state battery is disclosed that includes a solid electrolyte represented by the formula (I): at least one metal ion selected from the group consisting of Al, Y, Ga, In, and La). This all-solid-state lithium secondary battery includes an active material layer and a solid electrolyte layer bonded to the active material layer by sintering, the active material layer includes a crystalline first material capable of absorbing and releasing lithium ions, and the solid electrolyte layer includes a crystalline second material having lithium ion conductivity. It is also disclosed that the packing rate of the solid electrolyte layer is preferably more than 70%, and the battery is manufactured by sequentially stacking the materials constituting each layer and then sintering them.
[0004] As disclosed in Patent Document 1, it is considered preferable that the solid electrolyte included in the all-solid-state battery is dense.
[0005] On the other hand, it is known that expansion and contraction occurs during charging and discharging of an all-solid-state battery. A method for suppressing cracks in the electrode material of the all-solid-state battery caused by such expansion and contraction during charging and discharging has been studied (for example, Patent Document 2).
[0006] Patent Document 2 discloses a configuration in which a porous metal sheet, which is a metal foam or a sintered metal fiber compact, is provided on a solid electrolyte layer. The all-solid-state battery of Patent Document 2 is produced by a manufacturing method including a step of filling a porous metal sheet with an electrode material. Patent Document 2 discloses that the provision of this configuration can suppress cracks in the electrode material. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2007-005279 A [Patent Document 2] JP 2010-40218 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the all-solid-state batteries disclosed in Patent Documents 1 and 2, the internal resistance is excessively high, and there has been a demand for reducing the internal resistance. The present invention has been made in view of the above circumstances, and has an object to provide an all-solid-state battery with low internal resistance. [Means for solving the problem]
[0009] The present inventors have conducted intensive research to solve the above problems. As a result, in the method of using a porous metal sheet in Patent Document 2, it cannot be said that other materials are densely formed in the voids inside the porous electrode sheet and around it. The same was true when the porous electrode sheet was replaced with an expanded metal. However, by selecting an expanded metal with a predetermined mesh size, setting the thickness of the electrode layer to a certain value or less, and incorporating a solid electrolyte having appropriate flexibility in the electrode layer, it was found that when an all-solid-state battery is produced by a powder compaction method, an all-solid-state battery in which an electrode mixture constituting the electrode layer is densely formed around the expanded metal can be obtained, and the internal resistance can be reduced.
[0010] That is, in order to solve the above problems, the present invention provides the following means.
[0011] (1) An all-solid-state battery according to one embodiment of the present invention includes a laminate in which a positive electrode mixture layer including a positive electrode active material and a negative electrode mixture layer including a negative electrode active material are laminated with a solid electrolyte layer interposed therebetween, at least one of the positive electrode mixture layer and the negative electrode mixture layer is an electrode mixture layer including an expanded metal and solid electrolyte particles, and a product SW × LW of a center-to-center distance SW in a short direction and a center-to-center distance LW in a long direction of the expanded metal satisfies formula (1), 0.5mm 2 ≦SW×LW≦2mm 2 (1) The Young's modulus of the solid electrolyte particles contained in the electrode mixture layer is 20 GPa or less, and the thickness of the electrode mixture layer is 300 μm or less.
[0012] (2) In the all-solid-state battery described above in (1), a ratio of a volume of the expanded metal to a volume of the electrode mixture layer may be 5% or more and 80% or less.
[0013] (3) In the all-solid-state batteries of (1) and (2) above, the expanded metal may contain one or more selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon.
[0014] (4) In the all-solid-state batteries described above in (1) to (3), both the positive electrode mixture layer and the negative electrode mixture layer may contain the expanded metal and the solid electrolyte particles.
[0015] (5) In the all-solid-state batteries according to any one of (1) to (4) above, the expanded metal may form an angle of 1° or more and 15° or less with respect to the interface between the electrode mixture layer and the solid electrolyte layer.
[0016] (6) In the all-solid-state batteries described above in (1) to (5), the Young's modulus of the solid electrolyte particles contained in the electrode mixture layer may be 20 GPa or less. Effect of the Invention
[0017] According to the present invention, it is possible to provide an all-solid-state battery having low internal resistance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a perspective view showing an example of a configuration of an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view of the all-solid-state battery of FIG. 1 cut along the stacking direction of the power storage element. [Diagram 3] FIG. 3 is an enlarged view of a region R1 surrounded by a dashed line in the all-solid-state battery of FIG. 2. [Figure 4] 3 is a plan view showing an example of the configuration of an expanded metal provided in a positive electrode mixture layer in the all-solid-state battery of FIG. 2. [Diagram 5] FIG. 3 is an enlarged view of a region R2 surrounded by a dashed line in the all-solid-state battery of FIG. 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the cathode active material layer, the cathode, and the all-solid-state battery of this embodiment will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may be enlarged to show the characteristic parts of the present invention for the sake of convenience in order to make the characteristics of the present invention easier to understand. Therefore, the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are examples, and the present invention is not limited to them, and can be appropriately changed and implemented within the scope that does not change the gist of the present invention.
[0020] [All-solid battery] Fig. 1 is a perspective view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention. The all-solid-state battery 100 shown in Fig. 1 includes an energy storage element 10 and an exterior body 20. The energy storage element 10 is accommodated in an accommodation space K within the exterior body 20. For ease of understanding, Fig. 1 illustrates a state immediately before the energy storage element 10 is accommodated in the exterior body 20. The energy storage element 10 has external terminals 12, 14 that are electrically connected to the outside.
[0021] The exterior body 20 has, for example, a metal foil and a resin layer 24 laminated on both sides of the metal foil 22 (see FIG. 2). The exterior body 20 is a metal laminate film in which a metal foil is coated on both sides with a polymer film (resin layer). The metal foil 22 is, for example, an aluminum foil. The resin layer 24 is, for example, a polymer film such as polypropylene. The resin layer 24 may be different on the inside and outside. For example, the outside resin layer may be made of a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inside resin layer may be made of a material with high heat resistance, oxidation resistance, and reduction resistance, such as polyethylene (PE) or polypropylene (PP).
[0022] Fig. 2 is a cross-sectional view of the all-solid-state battery of Fig. 1 cut along the stacking direction of the power storage element. The all-solid-state battery 100 shown in Fig. 2 includes a laminate in which a positive electrode mixture layer 11B containing a positive electrode active material and a negative electrode mixture layer 13B containing a negative electrode active material are stacked via a solid electrolyte layer 15, at least one of the positive electrode mixture layer 11B and the negative electrode mixture layer 13B is an electrode mixture layer containing an expanded metal and solid electrolyte particles, the product SW × LW of the center-to-center distance SW in the short direction of the expanded metal and the center-to-center distance LW in the long direction satisfies formula (1), the Young's modulus of the solid electrolyte particles contained in the electrode mixture layer is 10 GPa or more and 20 GPa or less, and the thickness of the electrode mixture layer is 300 μm or less. 0.5mm 2 ≦SW×LW≦2mm 2 (1)
[0023] The all-solid-state battery 100 includes an energy storage element 10 and an exterior body 20. The exterior body 20 covers the periphery of the energy storage element 10. The energy storage element 10 is connected to the outside via a pair of connected external terminals 12, 14. The all-solid-state battery 100 may have any other shape as long as it is a laminated battery. For example, the all-solid-state battery 100 can be applied to a laminated battery, a square battery, a coin battery, a button battery, etc.
[0024] <Electricity storage element> The energy storage element 10 includes a solid electrolyte layer 15, a positive electrode layer 11, and a negative electrode layer 13. The energy storage element 10 is charged or discharged by the exchange of ions between the positive electrode layer 11 and the negative electrode layer 13 via the solid electrolyte layer 15 and the exchange of electrons via an external circuit.
[0025] (Positive electrode layer) 2, the positive electrode layer 11 has, for example, a plate-shaped (foil-shaped) positive electrode current collector 11A and a positive electrode mixture layer 11B. The positive electrode mixture layer 11B is formed, for example, so as to be in contact with at least one surface of the positive electrode current collector 11A.
[0026] ·Positive electrode current collector The positive electrode current collector 11A may be made of any electronically conductive material that is resistant to oxidation during charging and is not easily corroded. The positive electrode current collector 11A may be made of, for example, a metal such as aluminum, stainless steel, nickel, or titanium, or a conductive resin. The positive electrode current collector 11A may be in any form such as powder, foil, punching, or expanded metal.
[0027] Positive electrode mixture layer Fig. 3 is an enlarged view of a region R1 surrounded by a dashed line in the all-solid-state battery of Fig. 2. As shown in Fig. 3, the positive electrode mixture layer 11B is provided between the positive electrode current collector 11A and the solid electrolyte layer 15, and contains a positive electrode mixture 1 and an expanded metal 2. The positive electrode mixture 1 contains a positive electrode active material and solid electrolyte particles, and may further contain one or both of a binder and a conductive assistant. The binder and the conductive assistant may be known ones.
[0028] The thickness of the positive electrode mixture layer 11B is 300 μm or less, preferably 30 μm or more, or 40 μm or more and 295 μm or less, preferably 50 μm or more, or 100 μm or more and 260 μm or less, and more preferably 150 μm or more and 200 μm or less. The thickness of the positive electrode mixture layer 11B is measured using a cross-sectional SEM image in the direction perpendicular to the surface of the positive electrode mixture layer 11B.
[0029] The positive electrode active material is not particularly limited as long as it can reversibly absorb and release, and insert and remove (intercalate and deintercalate) lithium ions, and any positive electrode active material used in known lithium ion secondary batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.
[0030] Lithium-containing metal oxides include, for example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and lithium manganese oxides represented by the general formula: LiNi x Co y Mn zO2 (x+y+z=1), lithium vanadium compounds (LiVOPO4, Li3V2(PO4)3), olivine-type LiMPO4 (where M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li4Ti5O 12 ) etc.
[0031] The positive electrode active material may not contain lithium. Examples of such positive electrode active materials include non-lithium-containing metal oxides (MnO2, V2O5, etc.), non-lithium-containing metal sulfides (MoS2, etc.), non-lithium-containing fluorides (FeF3, VF3, etc.), and sulfur-modified polyacrylonitrile. When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.
[0032] The solid electrolyte may have a Young's modulus in the range of 20 GPa or less, preferably 10 GPa or more and 20 GPa or less, and more preferably 12 GPa or more and 16 GPa or less. Such a solid electrolyte may include one or more selected from halide-based solid electrolytes and sulfide-based solid electrolytes. With a Young's modulus of 20 GPa or less, the expanded metal is formed in the positive electrode mixture layer 11B, and a configuration with a large contact area between the expanded metal 2 and the solid electrolyte can be realized.
[0033] As the halide-based solid electrolyte, for example, one represented by the following formula (2) can be used. Li a E b G c X d (2)
[0034] In the halide-based solid electrolyte represented by formula (2), when E is Al, Sc, Y, or a lanthanoid, it is preferable that 2.0 ≦ a ≦ 4.0, and more preferably 2.5 ≦ a ≦ 3.5. When E is Zr or Hf, it is preferable that 1.0 ≦ a ≦ 3.0, and more preferably 1.5 ≦ a ≦ 2.5. In the solid electrolyte represented by formula (2), since 0.5 ≦ a < 6, the content of Li contained in the compound becomes appropriate, and the ionic conductivity increases.
[0035] In the halide-based solid electrolyte represented by formula (2), E is an essential element and is an element that forms the skeleton of the halide-based solid electrolyte represented by formula (2). E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). By including E, a solid electrolyte having a wide potential window and high ionic conductivity is obtained. As E, in order to obtain a solid electrolyte with higher ionic conductivity, it is preferable to include Al, Sc, Y, Zr, Hf, and La, and particularly preferably to include Zr and Y.
[0036] In the halide-based compound represented by formula (2), 0 < b < 2. Since the effect of including E can be obtained more effectively, it is preferable that 0.6 ≦ b. Further, E is an element that forms the skeleton of the halide-based solid electrolyte in the positive electrode mixture layer 11B represented by formula (2) and is an element with relatively high density. When b ≦ 1, a solid electrolyte with low density is obtained, which is preferable.
[0037] In the halide-based solid electrolyte represented by formula (2), G is an optional group. G is, for example, OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , Si6O 18 , PO3, PO4, P2O7, P3O 10, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, CH3COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-COO, C6H5SO3, OOC-CH=CH-COO, C(OH)(CH2COOH)2COO, AsO4, BiO4, CrO4, MnO4, PtF6, PtCl6, PtBr6, PtI6, SbO4, SeO4, TeO4, and at least one group selected from the group consisting of HCOO. G is preferably at least one group selected from the group consisting of OH, SO4, CH3COO, CF3COO, HCOO, and O, and since G has a strong covalent bond with E, and thus becomes a compound in which E ions are difficult to reduce, it is preferably at least one group selected from the group consisting of SO4, BO2, CO3, BF4, and PF6, and is particularly preferably SO4 or O. When G is contained, the potential window on the reduction side of the halide-based solid electrolyte becomes wider, and reduction becomes difficult.
[0038] In the halide-based solid electrolyte represented by formula (2), c satisfies 0≦c≦6. c is preferably 0.1≦c, and more preferably 0.5≦c, because the effect of widening the potential window on the reduction side by including G becomes more pronounced. c is preferably c≦3 so that the ionic conductivity of the solid electrolyte is not reduced due to an excessively high G content.
[0039] In the halide-based solid electrolyte represented by formula (2), X is an essential component. X is at least one selected from the group consisting of F, Cl, Br, and I. X has a large ionic radius per valence. Therefore, when the halide-based solid electrolyte represented by formula (2) contains X, lithium ions can flow easily, and the effect of increasing the ionic conductivity is obtained. As X, it is preferable to contain Cl in order to obtain a solid electrolyte with high ionic conductivity. Further, when X contains F, since X becomes a solid electrolyte with high ionic conductivity, it is preferable to contain F and two or more selected from the group consisting of Cl, Br, and I.
[0040] When X is F, it becomes a solid electrolyte with sufficiently high ionic conductivity and excellent oxidation resistance. When X is Cl, it becomes a solid electrolyte with high ionic conductivity and a good balance between oxidation resistance and reduction resistance. When X is Br, it becomes a solid electrolyte with sufficiently high ionic conductivity and a good balance between oxidation resistance and reduction resistance. When X is I, it becomes a solid electrolyte with high ionic conductivity.
[0041] In the halide-based solid electrolyte represented by formula (2), d satisfies 0 < d ≦ 6.1. It is preferable that 1 ≦ d. When 1 ≦ d, when the solid electrolyte is pressure-molded into a pellet shape, the strength of the pellet increases. Also, when 1 ≦ d, the ionic conductivity of the solid electrolyte increases. Further, it is preferable that d ≦ 5 so that the potential window of the solid electrolyte does not become narrow due to an excessive content of X causing a shortage of G.
[0042] The halide-based solid electrolyte represented by formula (2) is, for example, Li2ZrCl6, Li2ZrSO4Cl4, Li2ZrCO3Cl4, Li2Zr((COO)2) 0.5 Cl5, Li2Zr(CH3COO) 0.2 Cl 5.8 , Li2Zr(CF3COO) 0.2 Cl 5.8 , Li2Zr(HCOO) 0.4 Cl 5.6, Li2ZrBO2Cl5, Li2ZrBF4Cl5, Li3YSO4Cl4, Li3YCO3Cl4, Li3YBO2Cl5, Li3YBF4Cl5, Li2ZrOCl4.
[0043] The solid electrolyte may be a sulfide-based solid electrolyte, and a compound containing Li, S, Si and / or P may be used as the sulfide-based solid electrolyte. The sulfide-based solid electrolyte may further contain Ge, Cl, Br, or I. The sulfide-based solid electrolyte may be amorphous, crystalline, or of the argyrodite type. Examples of sulfide-based solid electrolytes include Li2S-P2S5-based solid electrolytes (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 solid electrolytes (Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x (1.0≦x≦1.9).
[0044] As the sulfide-based solid electrolyte, one represented by the following formula (3) can be used. Li q M r P s O t X u S v (3) In formula (3), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, X is at least one selected from the group consisting of F, Cl, Br, and I, and q, r, s, t, u, and v are numbers that satisfy 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×stu / 2. M is preferably Si or Ge.
[0045] Conductive additives The conductive assistant contained in the positive electrode mixture 1 is not particularly limited as long as it improves the electronic conductivity of the positive electrode mixture layer 11B, and a known conductive assistant can be used. Examples of the conductive assistant include carbon-based materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO, and mixtures thereof. The conductive assistant may be in the form of powder or fiber. In addition, from the viewpoint of not lowering the current collecting function of the conductive assistant, it is preferable to dehydrate the conductive assistant by heating and vacuum drying in a glove box in which argon gas is circulated, and then store the conductive assistant in a glass bottle or an aluminum laminate bag. The dew point in the glove box is preferably -30°C or lower and -90°C or higher.
[0046] ·binder The binder contained in the positive electrode mixture 1 bonds the positive electrode current collector 11A and the positive electrode mixture layer 11B, the positive electrode mixture layer 11B and the solid electrolyte layer, and various materials constituting the positive electrode mixture layer 11B.
[0047] It is preferable to use a binder within a range that does not impair the function of the positive electrode mixture layer 11B. The binder may be any binder capable of the above-mentioned bonding, and examples thereof include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). In addition to the above, examples of the binder may include cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, and the like. In addition, a conductive polymer having electronic conductivity or an ion conductive polymer having ion conductivity may be used as the binder. Examples of the conductive polymer having electronic conductivity include polyacetylene. In this case, the binder also functions as the conductive assistant particles, so that it is not necessary to add a conductive assistant. Examples of the ion conductive polymer having ion conductivity include those that conduct lithium ions, etc., and include monomers of polymer compounds (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) and LiClO4, LiBF4, LiPF 6、 Examples of the polymerization initiator used for the composite include a photopolymerization initiator or a thermal polymerization initiator that is compatible with the above-mentioned monomers. The properties required for the binder include resistance to oxidation and reduction and good adhesiveness.
[0048] The content of the binder in the positive electrode mixture layer 11B is preferably 0.5 to 30% by volume of the positive electrode mixture layer 11B in order to reduce the resistance of the positive electrode mixture layer 11B. Moreover, in order to improve the energy density, the content of the binder in the positive electrode mixture layer 11B is preferably 0% by volume.
[0049] The content of the solid electrolyte in the positive electrode mixture layer 11B is, for example, 5% by volume to 70% by volume, preferably 20% by volume to 60% by volume, and more preferably 40% by volume to 55% by volume. The content of the positive electrode active material in the positive electrode mixture layer 11B is, for example, 25% by volume to 95% by volume, and preferably 55% by volume to 40% by volume.
[0050] 4 is a plan view showing an example of the configuration of an expanded metal provided in an electrode mixture layer in the all-solid-state battery of FIG. 2. The expanded metal 2 has a strand 51 formed to surround a void G, and a bond 52 to which the strands 51 are bonded. The expanded metal 2 has a shape in which, for example, the length in one direction in the in-plane direction of the void G is longer than the direction perpendicular to the direction. In FIG. 4, the center-to-center distance between the nearest bonds 52 in the long direction in which the length of the void G is longer is represented by the symbol LW, and the center-to-center distance between the nearest bonds 52 in the short direction perpendicular to the long direction is represented by the symbol SW. The product SW×LW of the center-to-center distance SW in the short direction of the expanded metal and the center-to-center distance LW in the long direction satisfies formula (1). 0.5mm 2 ≦SW×LW≦2mm 2 (1) In addition, the above area SW × LW is 1 mm 2 More than 2mm 2 It is preferable that:
[0051] The center-to-center distance SW in the short direction of the expanded metal 2 is, for example, 0.4 mm or more and 1.5 mm or less, and preferably 0.5 mm or more and 1.0 mm or less. The center-to-center distance LW in the short direction of the expanded metal is, for example, 0.5 mm or more and 3.0 mm or less, and preferably 1.0 mm or more and 2.0 mm or less.
[0052] The interval width w of the expanded metal 2 is, for example, not less than 0.05 mm and not more than 0.3 mm, and preferably not less than 0.1 mm and not more than 0.2 mm.
[0053] The thickness of the expanded metal 2 is, for example, not less than 10 μm and not more than 300 μm, and preferably not less than 15 μm and not more than 200 μm.
[0054] By making the expanded metal 2 have the above-mentioned size, the expanded metal 2 can be formed inside the positive electrode mixture layer 11B by a powder compaction method for the positive electrode mixture layer 11B including the above-mentioned positive electrode mixture 1 containing a solid electrolyte, thereby realizing an all-solid-state battery in which the positive electrode mixture 1 is densely formed around the expanded metal 2. The expanded metal 2 is sandwiched by the positive electrode mixture 1 on both sides in the direction perpendicular to the surface, for example, and is separated from the positive electrode current collector 11A. The gap G of the expanded metal 2 is filled with the positive electrode mixture 1.
[0055] The expanded metal 2 may contain, for example, one or more materials selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon, and is preferably a material selected from the group consisting of Al, Ni, and Ti.
[0056] The expanded metal 2 is preferably formed so as to be inclined with respect to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15. The inclination angle θ1 of the expanded metal 2 with respect to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15 is preferably 0.5° or more and 20° or less, more preferably 1° or more and 15° or less, and even more preferably 10° or less. When the inclination angle θ1 of the expanded metal 2 is within the above range, an all-solid-state battery having excellent conductivity in the stacking direction and particularly excellent internal resistance is obtained.
[0057] The ratio of the volume of the expanded metal 2 to the volume of the positive electrode mixture layer 11B is, for example, 1% to 85%, preferably 5% to 80%, more preferably 65% or 50%, even more preferably 30%, and particularly preferably 10% to 20%. The ratio of the volume of the expanded metal 2 to the volume of the positive electrode mixture layer 11B is observed as an average value based on cross-sectional SEM images of multiple locations along the direction indicated by the two-dot chain line in FIG. 4. The ratio of the volume of the expanded metal 2 to the volume of the positive electrode mixture layer 11B is calculated by averaging the area ratio of the expanded metal 2 to the positive electrode mixture layer 11B in each SEM image obtained by obtaining 20 cross-sectional SEM images along the direction indicated by the two-dot chain line in FIG. 4 at equal intervals between the centers of two bonds 52 provided to sandwich one gap G.
[0058] (Negative electrode layer) The negative electrode layer 13 has, for example, a plate-shaped (foil-shaped) negative electrode current collector 13A and a negative electrode mixture layer 13B. The negative electrode mixture layer 13B is formed, for example, so as to be in contact with at least one surface of the negative electrode current collector 13A. In the following description of the negative electrode layer, description of components common to the positive electrode layer may be omitted.
[0059] ·Negative electrode current collector The negative electrode current collector 13A may have electronic conductivity. The negative electrode current collector 13A may be made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 13A may be in the form of a powder, a foil, a punching, or an expanded metal.
[0060] Negative electrode mixture layer Fig. 5 is an enlarged view of a region R2 surrounded by a dashed line in the all-solid-state battery in Fig. 2. As shown in Fig. 5, the negative electrode mixture layer 13B is provided between the negative electrode current collector 13A and the solid electrolyte layer 15, and includes the negative electrode mixture 3 and the expanded metal 4.
[0061] The negative electrode mixture 3 includes a negative electrode active material and a solid electrolyte having a Young's modulus of 10 GPa or more and 20 GPa or less, and may further include one or both of a binder and a conductive assistant. Known binders and conductive assistants can be used. The type and amount of the binder and conductive assistant in the negative electrode mixture layer 13B may be the same as the type and amount of the binder and conductive assistant in the positive electrode mixture layer 11B.
[0062] The thickness of the negative electrode mixture layer 13B is 300 μm or less, preferably 30 μm or more, or 40 μm or more and 295 μm or less, preferably 50 μm or more, or 100 μm or more and 260 μm or less, and more preferably 150 μm or more and 200 μm or less. The thickness of the negative electrode mixture layer 13B is measured using a cross-sectional SEM image in the direction perpendicular to the surface of the negative electrode mixture layer 13B.
[0063] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. The negative electrode active material may be any negative electrode active material used in known lithium ion secondary batteries.
[0064] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies; metals that can be combined with lithium, such as Si, SiOx, Sn, and aluminum; alloys of these; composite materials of these metals and carbon materials; and lithium titanate (Li4Ti5O 12 ), oxides such as SnO2, sulfur-modified polyacrylonitrile, metallic lithium, etc. The negative electrode active material is natural graphite or lithium titanate (Li4Ti5O 12 ) is preferred.
[0065] The content of the solid electrolyte in the negative electrode mixture layer 13B is, for example, 5 volume % to 70 volume % or less, preferably 30 volume % to 65 volume % or less, and more preferably 40 volume % to 55 volume % or less. The content of the negative electrode active material in the negative electrode mixture layer 13B is, for example, 30 volume % to 70 volume % or less, and preferably 40 volume % to 60 volume % or less.
[0066] The solid electrolyte may have a Young's modulus in the range of 10 GPa to 20 GPa, and preferably in the range of 12 GPa to 16 GPa. Such a solid electrolyte may include one or more selected from halide-based solid electrolytes and sulfide-based solid electrolytes. With a Young's modulus of 20 GPa or less, the expanded metal is formed in the positive electrode mixture layer 11B, and a configuration with a large contact area between the expanded metal 2 and the solid electrolyte can be realized.
[0067] The halide-based solid electrolyte may be one represented by the above formula (2), and the sulfide-based solid electrolyte may be one represented by the above formula (3). Two or more of the halide-based solid electrolyte represented by the above formula (2) and the sulfide-based solid electrolyte represented by the above formula (3) may be used in combination. The solid electrolyte contained in the negative electrode mixture layer 13B may be the same as the solid electrolyte contained in the positive electrode mixture layer 11B.
[0068] The shape and material of the expanded metal 4 may be the same as those of the expanded metal 2. That is, in the expanded metal 4, the product SW×LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction of the expanded metal 4 satisfies formula (1). 0.5mm 2 ≦SW×LW≦2mm 2 (1)
[0069] The expanded metal 4 is preferably formed so as to be inclined with respect to the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15. The inclination angle θ2 of the expanded metal 4 with respect to the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15 is preferably 0.5° or more and 20° or less, more preferably 1° or more and 15° or less, and even more preferably 10° or less. When the inclination angle θ2 of the expanded metal 4 is within the above range, an all-solid-state battery having excellent conductivity in the stacking direction and particularly excellent internal resistance is obtained.
[0070] The ratio of the volume of the expanded metal 4 to the volume of the negative electrode mixture layer 13B is, for example, 1% or more and 85% or less, preferably 5% or more and 80% or less, more preferably 65% or less or 50% or less, further preferably 30% or less, and particularly preferably 10% or more and 20% or less. The ratio of the volume of the expanded metal 4 to the volume of the negative electrode mixture layer 13B is measured in the same manner as the ratio of the volume of the expanded metal to the volume of the positive electrode mixture layer 11B.
[0071] The expanded metal 4 may be inclined in the same direction as the expanded metal 2 with respect to the solid electrolyte layer 15, or may be inclined in a different direction.
[0072] (Solid electrolyte layer) The solid electrolyte layer 15 is sandwiched between the positive electrode layer 11 and the negative electrode layer 13. The solid electrolyte layer 15 includes a solid electrolyte that can move ions by an externally applied voltage. For example, the solid electrolyte conducts lithium ions and inhibits the movement of electrons.
[0073] The solid electrolyte constituting the solid electrolyte layer 15 contains, for example, lithium. The solid electrolyte may be, for example, an oxide-based material, a sulfide-based material, a halide-based material, or a complex hydride-based material. As the solid electrolyte provided in the solid electrolyte layer 15, it is preferable to use one or both of a halide-based material and a sulfide-based material. As the halide-based solid electrolyte, one represented by the above formula (2) may be used. As the sulfide-based solid electrolyte, one represented by the above formula (3) may be used.
[0074] [Manufacturing method of all-solid-state batteries] Next, a method for manufacturing the all-solid-state battery according to the present embodiment will be described. The all-solid-state battery according to the present embodiment is manufactured by, for example, a powder molding method. The powder molding method is performed in a glove box.
[0075] The method for producing the all-solid-state battery according to this embodiment includes a solid electrolyte layer forming step of forming a solid electrolyte layer by powder compaction, a positive electrode mixture forming step of synthesizing a positive electrode mixture containing one or both of a halide-based solid electrolyte and a sulfide-based solid electrolyte, a negative electrode mixture forming step of forming a negative electrode mixture containing one or both of a halide-based solid electrolyte and a sulfide-based solid electrolyte, a positive electrode mixture layer forming step of placing the positive electrode mixture on one surface of the solid electrolyte layer, further placing an expanded metal thereon, and compacting the mixture using a punch or the like, and a negative electrode mixture layer forming step of placing the negative electrode mixture on one surface of the solid electrolyte layer, further placing an expanded metal thereon, and compacting the mixture using a punch or the like.
[0076] The expanded metal that can be used is one in which the product SW×LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction satisfies formula (1). 0.5mm 2 ≦SW×LW≦2mm 2 (1)
[0077] According to the all-solid-state battery 100 of this embodiment, by providing the expanded metals 2, 4 in at least one of the positive electrode mixture layer 11B and the negative electrode mixture layer 13B, even if a void or the like is generated due to a crack in the electrode mixture layer due to the expansion and contraction of the all-solid-state battery, if the region in which the void is formed is around the expanded metals 2, 4, the expanded metals 2, 4 will become a path, and electrical conduction will be ensured.
[0078] Moreover, according to the all-solid-state battery 100 of this embodiment, by using an expanded metal having a predetermined shape and a Young's modulus in an optimal range for a solid electrolyte, the expanded metals 2, 4 are inserted into the electrode mixture layer by a powder compaction method (powder compaction method), the expanded metals 2, 4 are not exposed to the outside, and the electrode mixture is densely formed around the expanded metals 2, 4. Therefore, the contact area between the expanded metals 2, 4 and the electrode mixture is large, and it is possible to realize an all-solid-state battery having a large area that exhibits excellent internal resistance.
[0079] In the above embodiment, both the positive electrode mixture layer 11B and the negative electrode mixture layer 13B include the predetermined expanded metals 2, 4, have a thickness of 300 μm or less, and include a solid electrolyte with a Young's modulus of 10 GPa or more and 20 GPa or less. However, it is sufficient that at least one of the positive electrode mixture layer 11B and the negative electrode mixture layer 13B has the above configuration.
[0080] 3 and 4 show a configuration in which the expanded metals 2 and 4 are inclined with respect to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15 and the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15, respectively. However, the expanded metals 2 and 4 may be arranged parallel to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15 and the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15.
[0081] 2, 3, and 5 show all-solid-state batteries including the positive electrode current collector 11A and the negative electrode current collector 13A, but the present invention is not limited to the above examples. For example, when the expanded metal 2 and the expanded metal 4 are formed on the positive electrode mixture layer 11B and the negative electrode mixture layer 13B, respectively, these expanded metals also function as current collectors by bonding with the external terminals 12 and 14, so the positive electrode current collector 11A and the negative electrode current collector 13A shown in FIG. 2, 3, and 5 may not be provided.
[0082] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES
[0083] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0084] [Example 1] -Synthesis of solid electrolyte- In a glove box with argon gas circulating at a dew point of -90°C, an oxygen concentration of 1 ppm, and atmospheric pressure, the synthesis of solid electrolyte, the mixing of the positive electrode mixture layer material, the mixing of the negative electrode mixture layer material, and the preparation of an all-solid-state battery were carried out. First, Li2SO4 and ZrCl4 were weighed out as raw material powder so that the molar ratio was 1:1. Next, the weighed raw material powder was placed in a Zr container together with a Zr ball having a diameter of 5 mm, and mechanochemical milling was carried out using a planetary ball mill. The treatment was carried out at a rotation speed of 500 rpm for 50 hours, and then sieved through a 200 μm mesh sieve. As a result, a powder of Li2ZrSO4Cl4 was obtained as a solid electrolyte.
[0085] -Synthesis of positive electrode mixture- Next, the positive electrode mixture was weighed and mixed in a glove box with argon gas circulating at a dew point of -85°C and an oxygen concentration of 1 ppm. The materials were weighed out so that the ratio of lithium cobalt oxide (LiCoO2):Li2ZrSO4Cl4:carbon black was 77:18:5 parts by weight, and mixed in an agate mortar for 5 minutes to obtain a positive electrode mixture.
[0086] -Synthesis of negative electrode mixture- Next, the negative electrode mixture was weighed and mixed in a glove box with argon gas circulating at a dew point of -85°C and an oxygen concentration of 1 ppm. 12 ): Li2ZrSO4Cl4: carbon black = 72:22:6 parts by weight, and mixed in an agate mortar for 5 minutes to obtain a negative electrode mixture.
[0087] -Molding process- Next, using the above solid electrolyte, positive electrode mixture, negative electrode mixture, and expanded metal, a power storage element composed of a positive electrode current collector / positive electrode mixture layer / electrolyte layer / negative electrode mixture layer / negative electrode current collector was produced by a powder molding method.
[0088] First, a die made of SKD11 material with a 30 x 40 mm through hole in the center was prepared, along with a lower punch and an upper punch made of the same material, measuring 29.9 x 39.9 mm. The lower punch was inserted into the through hole of the die, and 400 mg of solid electrolyte was added from the opening side. The upper punch was then inserted on top of the solid electrolyte. This first unit was placed in a press machine and pressed at a pressure of 373 MPa to form a solid electrolyte layer. The first unit was removed from the press machine, and the upper punch was removed.
[0089] Next, 750 mg of the negative electrode mixture was poured onto the solid electrolyte layer (upper punch side) from the open side of the resin holder.
[0090] Next, an expanded metal made of aluminum was placed on the negative electrode mixture. The expanded metal had a center-to-center distance SW between the nearest bonds in the short direction, which is the shortest length in the gap, of 1 mm, a center-to-center distance LW between the nearest bonds in the long direction perpendicular to the short direction, a pitch width of 150 μm, and a thickness of 50 μm. That is, the product SW×LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction of the expanded metal used in Example 1 was 2 mm. 2 It is.
[0091] Next, an upper punch was inserted on top of it. This second unit was placed in a press and molded at a pressure of 373 MPa. Next, the second unit was removed, turned upside down, and the lower punch was removed.
[0092] Next, 750 mg of a positive electrode mixture was placed on the solid electrolyte layer (on the lower punch side).
[0093] Next, an expanded metal made of aluminum was placed on the positive electrode mixture. The expanded metal had a center-to-center distance SW between the nearest bonds in the short direction where the gap length is small, of 1 mm, and a center-to-center distance LW between the nearest bonds in the long direction perpendicular to the short direction, of 2 mm, a pitch width of 150 μm, and a thickness of 50 μm. That is, the product SW×LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction of the expanded metal used in Example 1 was 2 mm. 2 It is.
[0094] Next, a lower punch was inserted onto the third unit, and the third unit was placed in a press and molded at a pressure of 373 MPa.
[0095] Next, the electricity storage element composed of the positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer was removed from the die.
[0096] -Containment process- Next, the obtained electricity storage element was housed in an outer casing. An aluminum laminate bag was prepared as an exterior body to be enclosed. In addition, an aluminum foil (width 4 mm, length 40 mm, thickness 100 μm) wrapped with maleic anhydride grafted polypropylene (PP) was welded to the negative electrode current collector (aluminum foil, 30 × 40 mm, thickness 20 μm) and the positive electrode current collector (aluminum foil, 30 × 40 mm, thickness 20 μm) as an external terminal. The layers were laminated to form a positive electrode current collector / positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer / negative electrode current collector, and inserted into the aluminum laminate bag. Finally, the opening was heat sealed while the inside of the exterior body was evacuated, to produce the all-solid-state battery of Example 1.
[0097] [Examples 2 and 3] An all-solid-state battery was produced in the same manner as in Example 1, except that the expanded metal used was changed. In Example 2, the distance SW between the closest bond centers in the short direction is 0.5 mm, the distance LW between the closest bond centers in the long direction is 1 mm, and the area SW × LW is 1 mm. 2 The above was used. In Example 3, SW is 1 mm, LW is 1 mm, and the area SW×LW is 0.5 mm. 2 The above was used.
[0098] [Examples 4 to 6] An all-solid-state battery was produced under the same conditions as in Example 1, except that the solid electrolyte used for producing the all-solid-state battery was changed. In Example 4, Li6PS5Cl4 was used. In Example 5, Li2ZrCl6 was used. In Example 6, Li2ZrOCl4 was used.
[0099] [Examples 7 to 9] An all-solid-state battery was produced in the same manner as in Example 1, except that the amounts of the positive electrode mixture and the negative electrode mixture used were changed, the thicknesses of the positive electrode mixture layer and the negative electrode mixture layer were changed, and the thickness of the expanded metal was changed to maintain the ratio of the volume of the expanded metal to the volume of the electrode mixture layer. In Example 7, the thickness of the positive electrode mixture layer and the negative electrode mixture layer was set to 45 μm. In Example 8, the thickness of the positive electrode mixture layer and the negative electrode mixture layer was set to 200 μm. In Example 8, the thickness of the positive electrode mixture layer and the negative electrode mixture layer was set to 260 μm. In Example 8, the thickness of the positive electrode mixture layer and the negative electrode mixture layer was set to 295 μm.
[0100] [Examples 11 to 14] An all-solid-state battery was produced in the same manner as in Example 1, except that the expanded metals formed in the positive electrode mixture layer and the negative electrode mixture layer were changed to different materials. In Example 11, an expanded metal made of Ni (nickel) was used. In Example 12, an expanded metal made of Ti (titanium) was used. In Example 13, an expanded metal made of Cu (copper) was used. In Example 14, an expanded metal made of stainless steel (SUS316L) was used.
[0101] [Example 15] An all-solid-state battery was produced in the same manner as in Example 1, except that no expanded metal was used when forming the negative electrode mixture layer, and the expanded metal was contained only in the positive electrode mixture layer.
[0102] [Example 16] An all-solid-state battery was produced in the same manner as in Example 1, except that no expanded metal was used when forming the positive electrode mixture layer, and the expanded metal was contained only in the negative electrode mixture layer.
[0103] [Examples 17 to 26] All-solid-state batteries were produced in the same manner as in Example 1, except that expanded metals of different thicknesses were used, and the ratio of the volume of the expanded metal to the volume of the positive electrode mixture layer and the ratio of the volume of the expanded metal to the volume of the negative electrode mixture layer were changed. In Example 17, the volume ratio was 2%, in Example 18, 5%, in Example 19, 11.8%, in Example 19, 19.7%, in Example 20, 29.6%, in Example 21, 43%, in Example 22, 64.5%, in Example 23, 75.5%, in Example 24, 79.9%, and in Example 25, 85%.
[0104] [Examples 27 to 34] The electrode mixture was placed on the solid electrolyte layer, and the expanded metal was placed on the electrode mixture, and the orientation of the expanded metal was adjusted when the surface of the electrode mixture powder was leveled before the punch was inserted. In this way, an all-solid-state battery was produced in the same manner as in Example 1, except that the inclination θ1 of the expanded metal with respect to the interface between the positive electrode mixture layer and the solid electrolyte layer, and the inclination θ2 of the expanded metal with respect to the interface between the negative electrode mixture layer and the solid electrolyte were changed. In Example 27, the angles θ1 and θ2 were set to 0.5°, in Example 28 to 1°, in Example 29 to 5°, in Example 30 to 8°, in Example 31 to 10°, in Example 32 to 12°, in Example 33 to 15°, and in Example 34 to 20°.
[0105] [Comparative Example 1 to Comparative Example 3] An all-solid-state battery was produced in the same manner as in Example 1, except that the expanded metal used was changed. In Comparative Example 1, the distance SW between the closest bond centers in the short direction is 2 mm, the distance LW between the closest bond centers in the long direction is 3 mm, and the area SW × LW is 6 mm. 2 The above was used. In Comparative Example 2, SW is 1.5 mm, LW is 3 mm, and the area SW×LW is 4.5 mm. 2 The above was used. In Comparative Example 3, SW was 0.46 mm, LW was 0.48 mm, and the area SW×LW was 0.22 mm. 2 The above was used.
[0106] [Comparative Example 4] The solid electrolyte used in the production of the all-solid-state battery was Li 10GeP2S 12 An all-solid-state battery was produced under the same conditions as in Example 1, except for the above change.
[0107] [Comparative Example 5] An all-solid-state battery was produced in the same manner as in Example 1, except that the amounts of the positive electrode mixture and the negative electrode mixture used were increased, the thicknesses of the positive electrode mixture layer and the negative electrode mixture layer were changed to 340 μm, and the thickness of the expanded metal was changed to maintain the ratio of the volume of the expanded metal to the volume of the electrode mixture layer.
[0108] (Internal resistance measurement) The internal resistance of the all-solid-state batteries of Examples 1 to 34 and Comparative Examples 1 to 5 was measured by electrochemical impedance spectroscopy (EIS) under the following conditions. Specifically, the all-solid-state batteries were held in a thermostatic chamber at 25° C., and the real component Z′ of the impedance at a measurement frequency of 1 kHz was measured as the internal resistance [Ω].
[0109] (Cross-section observation of an all-solid-state battery) The all-solid-state batteries of Examples 1 to 34 and Comparative Examples 1 to 5 were cut along the short side direction of the expanded metal, and cross-sectional SEM images were taken. From each cross-sectional SEM image, the thickness of the positive electrode mixture layer and the negative electrode mixture layer, the angle of the expanded metal provided on the positive electrode mixture layer relative to the interface between the positive electrode mixture layer and the solid electrolyte layer, and the angle of the expanded metal provided on the negative electrode mixture layer relative to the interface between the negative electrode mixture layer and the solid electrolyte layer were measured.
[0110] In addition, 20 SEM images of the above cross section were prepared at equal intervals between the centers of the closest bonds arranged to sandwich one gap in the expanded metal, and the ratio of the area of the expanded metal to the area of the positive electrode mixture layer was obtained in each SEM image, and the ratio of the volume of the expanded metal to the volume of the positive electrode mixture layer was calculated by calculating the average value. In addition, the ratio of the volume of the expanded metal to the volume of the negative electrode mixture layer was calculated in a similar manner.
[0111] (Measuring Young's modulus of solid electrolyte) In addition, a scanning probe microscope (SPM) was used to measure the Young's modulus of the solid electrolyte in the batteries produced in Examples 1 to 34 and Comparative Examples 1 to 5. Specifically, a fall curve was measured using an SPM (manufactured by Bruker, Bruker AXS), and the Young's modulus was calculated from the obtained force curve. Such measurements were performed based on the manual provided by the manufacturer of the device.
[0112] Tables 1 and 2 summarize the configurations and internal resistance measurement results of the all-solid-state batteries of Examples 1 to 16.
[0113] [Table 1]
[0114] [Table 2]
[0115] Tables 3 and 4 summarize the configurations of the all-solid-state batteries of Examples 17 to 34 and Comparative Examples 1 to 5, as well as the measurement results of the internal resistance.
[0116] [Table 3]
[0117] [Table 4]
[0118] As can be seen from Tables 1 to 4, the product SW × LW [mm 2It was confirmed that an all-solid-state battery having a Young's modulus [GPa] of 0.5 to 2, a solid electrolyte particle contained in an electrode mixture layer having a Young's modulus [GPa] of 10 to 20, and an electrode mixture layer having a thickness of 300 μm or less has superior effects compared to the all-solid-state batteries of Comparative Examples 1 to 5 not having any of the above configurations. By comparing Example 1 with Examples 7 to 10, it has been confirmed that when the positive electrode mixture layer thickness and the negative electrode mixture layer thickness are from 50 μm to 260 μm, particularly excellent internal resistance is exhibited, and when they are from 150 μm to 200 μm, even more remarkably excellent internal resistance is exhibited. By comparing Example 1 and Examples 11 to 14, it was confirmed that the expanded metal, which is composed of one or more elements selected from the group consisting of Al, Ni, and Ti, exhibits particularly excellent internal resistance.
[0119] It was confirmed from Examples 15 and 16 that excellent internal resistance was exhibited even if the electrode mixture layer in which a predetermined expanded metal was formed was either the positive electrode mixture layer or the negative electrode mixture layer.
[0120] By comparing Example 1 and Examples 17 to 26, it was confirmed that a particularly excellent internal resistance was exhibited when the volume ratio of the expanded metal to the electrode mixture layer was 3% or more and 50% or less, and an even better internal resistance was exhibited when the volume ratio of the expanded metal to the electrode mixture layer was 5% or more and 20% or less. By comparing Example 1 and Examples 27 to 34, it was confirmed that a particularly excellent internal resistance was exhibited when the inclination of the expanded metal with respect to the interface between the electrode mixture layer and the solid electrolyte layer was 1° or more and 10° or less, and an even better internal resistance was exhibited when the inclination was 2° or more and 5° or less. [Explanation of symbols]
[0121] 1: Positive electrode mixture, 2, 4: Expanded metal, 3: Negative electrode mixture, 10: energy storage element, 11: positive electrode layer, 11A: positive electrode current collector, 11B: positive electrode mixture layer, 13: negative electrode layer, 13A: negative electrode current collector, 13B: negative electrode mixture layer, 15: solid electrolyte layer, 12, 14: external terminal, 20: exterior body, 22: metal foil, 24: resin layer, 51: strand, 52: bond, 100: all-solid-state battery
Claims
1. a positive electrode mixture layer including a positive electrode active material and a negative electrode mixture layer including a negative electrode active material are laminated with a solid electrolyte layer interposed therebetween; At least one of the positive electrode mixture layer and the negative electrode mixture layer is an electrode mixture layer including an expanded metal and solid electrolyte particles, The product SW × LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction of the expanded metal satisfies formula (1), 0.5mm 2 ≦SW×LW≦2mm 2 ・・・(1) the Young's modulus of the solid electrolyte particles contained in the electrode mixture layer is 20 GPa or less; The electrode mixture layer has a thickness of 300 μm or less.
2. 2. The all-solid-state battery according to claim 1, wherein a ratio of a volume of the expanded metal to a volume of the electrode mixture layer is 5% or more and 80% or less.
3. 2. The all-solid-state battery according to claim 1, wherein the expanded metal contains one or more selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon.
4. 2. The all-solid-state battery according to claim 1, wherein both the positive electrode mixture layer and the negative electrode mixture layer contain the expanded metal and the solid electrolyte particles.
5. 2. The all-solid-state battery according to claim 1, wherein an angle of the expanded metal with respect to an interface between the electrode mixture layer and the solid electrolyte layer is 1° or more and 15° or less.
6. The all-solid-state battery in accordance with claim 1 , wherein the Young's modulus of the solid electrolyte particles contained in the electrode mixture layer is 10 GPa or more.
Citation Information
Patent Citations
Laminate including active material layer and solid electrolyte layer, and all solid lithium secondary battery using it
JP2007005279A
Electrode material sheet for lithium battery, solid lithium battery, and device with the solid lithium battery
JP2010040218A