POLYCRYSTAL SiC SELF-SUPPORTING MOLDING
By controlling CVD conditions, the polycrystalline SiC molded body achieves low nitrogen concentrations and gradients, addressing stability and cost issues in semiconductor manufacturing equipment, ensuring consistent wafer quality and cost-effectiveness.
Patent Information
- Application Number
- JP2023051538
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing polycrystalline SiC molded bodies used in semiconductor manufacturing equipment face challenges with high nitrogen concentration gradients and impurities, leading to unstable dopant concentrations and quality variations in semiconductor wafers, and are costly and difficult to manufacture in complex shapes.
A polycrystalline SiC free-standing molded body is produced through controlled CVD conditions and environment, achieving low nitrogen concentrations and gradients, with specific surface and gradient limits, ensuring stable dopant concentrations and reduced quality variations.
The solution provides a polycrystalline SiC member with significantly reduced nitrogen concentration gradients and impurities, enhancing the stability and consistency of semiconductor wafer production while being cost-effective and suitable for complex shapes.
Smart Images

Figure 2024140407000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a free-standing molded body of polycrystalline SiC formed by a CVD method. [Background technology]
[0002] Polycrystalline SiC compacts have excellent properties such as heat resistance, corrosion resistance, and strength, and are used in a variety of applications. In particular, when used as components for semiconductor manufacturing equipment, they are required to have high resistance and high purity.
[0003] The impurities contained in polycrystalline SiC compacts include N, B, Al, P, etc., which act as dopant sources for semiconductor elements, so a high impurity content poses problems in semiconductor manufacturing. Of these elements, N is present in large quantities in the atmosphere, making it difficult to reduce its content.
[0004] Regarding the reduction of the nitrogen concentration in a SiC film, for example, Patent Document 1 describes a SiC-coated carbon-based material having a carbon-based material and a SiC coating that coats the carbon-based material, in which the nitrogen content of the SiC coating measured by SIMS analysis is 5×10 16 atoms / cm 3 Patent Document 2 discloses a low-nitrogen-concentration carbon-based material having a nitrogen concentration of 100 ppm or less as measured by glow discharge mass spectrometry, and describes using the carbon-based material as a substrate for a SiC-coated graphite material. In the examples, the carbon-based material is coated with SiC by a CVD method, and the nitrogen content in the SiC is 2×10 15 atoms / cm 3 ~1.2×10 16 atoms / cm 3 It is stated that:
[0005] In addition, Patent Document 3 discloses a method for growing a crystal having a first end face and a second end face opposite to the first end face, the gradient of the nitrogen concentration in the growth direction, which is the direction in which the first end face and the second end face face each other, is 1×1016 cm -4 More than 1×10 18 cm -4 Disclosed is the following silicon carbide ingot. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-132637 A [Patent Document 2] JP 2002-249376 A [Patent Document 3] JP 2015-98420 A Summary of the Invention [Problem to be solved by the invention]
[0007] Here, coated products and free-standing molded bodies are used as the members made of polycrystalline SiC used in semiconductor manufacturing equipment. The coated product refers to a product in which the surface of a substrate is coated with SiC, and the free-standing molded body refers to a SiC molded body that does not include a substrate. Among these, the free-standing molded body of polycrystalline SiC, unlike the SiC film (coated product), has a problem of a nitrogen concentration gradient from the first main surface (growth surface) to the second main surface (substrate surface) in addition to a reduction in nitrogen concentration. For example, a semiconductor wafer (hereinafter, sometimes simply referred to as a wafer) is manufactured by a semiconductor manufacturing equipment using a member made of polycrystalline SiC. If the absolute value of the nitrogen concentration gradient from the first main surface to the second main surface of the polycrystalline SiC free-standing molded body is large, the concentration of nitrogen, which is a dopant source in the semiconductor wafer, is not stable in the thickness direction. Therefore, for example, in an etching application, as SiC is consumed, the nitrogen concentration and partial pressure in the vicinity of the wafer change over time.
[0008] The SiC described in Patent Documents 1 and 2 is a SiC film coated on the surface of a carbon material, not a free-standing SiC compact. Therefore, the effect of the nitrogen concentration gradient is not considered to be a problem, and Patent Documents 1 and 2 do not mention the issue of reducing the nitrogen concentration gradient in the direction from the first main surface (growth surface) to the second main surface (substrate surface).
[0009] In addition, although the members made of polycrystalline SiC used in semiconductor manufacturing equipment are polycrystalline, Patent Document 3 is an invention of a single crystal SiC ingot, not polycrystalline SiC. Unlike polycrystalline SiC freestanding compacts, single crystal SiC ingots are expensive and have high manufacturing costs. In addition, it is not possible to manufacture in complex shapes, and it is difficult to manufacture large diameter ingots. For the above reasons, it is difficult to use single crystal SiC ingots as members for semiconductor manufacturing equipment. In addition, in the examples of Patent Document 3, the nitrogen concentration in the SiC ingot is 1.0×10 17 ~2.0×10 19 cm -3 The only ones that have been obtained are those with extremely high nitrogen concentrations.
[0010] Therefore, an object of the present invention is to provide a polycrystalline SiC free-standing molded body for semiconductor manufacturing equipment, which has a small nitrogen concentration gradient in the thickness direction, small quality variation, and is effective for processes requiring a small amount of dopant source (especially nitrogen). [Means for solving the problem]
[0011] As a result of extensive research, the inventors discovered that by controlling the CVD conditions and the growth environment of the SiC particles when forming polycrystalline SiC material, a polycrystalline SiC free-standing compact having a low nitrogen concentration and a small nitrogen concentration gradient in the direction from the first main surface to the second main surface can be obtained, and thus completed the present invention.
[0012] That is, the present invention provides (1) The thickness is 200 μm or more, The nitrogen concentration of the first main surface and the second main surface is 3.00×10 16 atoms / cm3 is as follows: The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is 3.00×10 17 atoms / cm 4 is as follows: The absolute value of the nitrogen concentration difference between the first main surface and the second main surface is 1.80×10 16 atoms / cm 3 That is: A polycrystalline SiC free-standing compact characterized by the above. (2) The nitrogen concentration of the first main surface and the second main surface is 0.50×10 16 atoms / cm 3 The polycrystalline SiC free-standing compact according to (1), characterized in that: (3) The polycrystalline SiC free-standing compact according to (1), wherein the thickness is 1000 μm or more. (4) the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is 3.00×10 16 atoms / cm 4 The polycrystalline SiC free-standing compact according to (1), characterized in that: (5) The absolute value of the nitrogen concentration difference between the first main surface and the second main surface is 0.40 × 10 16 atoms / cm 3 The polycrystalline SiC free-standing compact according to (1), characterized in that: This provides: Effect of the Invention
[0013] According to the present invention, it is possible to provide a polycrystalline SiC free-standing molded body for semiconductor manufacturing equipment, which can produce polycrystalline SiC components that are effective for processes requiring a small absolute value of the nitrogen concentration gradient in the thickness direction, small quality variation, and small amounts of dopant sources (especially nitrogen). [Brief description of the drawings]
[0014] [Figure 1] An example of a polycrystalline SiC free-standing compact is shown. [Diagram 2]1 is a graph showing the relationship between the residence time of methyltrichlorosilane gas in a furnace and the nitrogen concentration on the first main surface in Examples and Comparative Examples. [Diagram 3] 10 is a graph showing the relationship between the control of the environment in the furnace before CVD and the nitrogen concentration on the second main surface in the examples and comparative examples. [Figure 4] 1 is a graph showing the relationship between control of the environment in a furnace before CVD and the absolute value of the nitrogen concentration difference between the first main surface and the second main surface in an example and a comparative example. [Diagram 5] 1 is a graph showing the relationship between the control of the environment in a furnace before CVD and the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface in an example and a comparative example. [Figure 6] 1 is a graph showing the relationship between the control of the furnace environment and residence time before CVD and the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface in thick polycrystalline SiC freestanding bodies in the examples and comparative examples. [Figure 7] 10 is a graph showing the relationship between the control of the environment in the furnace before CVD and the nitrogen concentration on the second main surface in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.
[0016] The polycrystalline SiC freestanding compact of the present invention has a thickness of 200 μm or more, The nitrogen concentration of the first main surface and the second main surface is 3.00×10 16 atoms / cm 3 is as follows: The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is 3.00×10 17 atoms / cm 4 is as follows: The absolute value of the nitrogen concentration difference between the first main surface and the second main surface is 1.80×10 16 atoms / cm3 That is: In the present invention, the first main surface refers to the surface (growth surface) of the polycrystalline SiC material on the growth side in forming the polycrystalline SiC material by a CVD (chemical vapor deposition) method, and the second main surface refers to the surface (substrate surface) on the substrate side.
[0017] The polycrystalline SiC free-standing molded body of the present invention is manufactured by forming a film using a CVD method (chemical vapor deposition method). For example, as shown in Fig. 1, the polycrystalline SiC free-standing molded body 10 is plate-shaped or cylindrical, has a first main surface 1 and a second main surface 2, and has a thickness that allows easy handling.
[0018] The polycrystalline SiC free-standing molded body of the present invention has a thickness of 200 μm or more. From the viewpoint of ensuring the strength as a free-standing molded body, the polycrystalline SiC free-standing molded body of the present invention has a thickness of at least 200 μm or more, preferably 350 μm or more, and more preferably 500 μm or more.
[0019] Furthermore, when the polycrystalline SiC free-standing molded body of the present invention is used as, for example, a member of a semiconductor manufacturing device, the thicker the polycrystalline SiC free-standing molded body is, the longer it will last as a member of the semiconductor manufacturing device and the smaller the quality variation of the manufactured semiconductor wafers will be, which is preferable. From the above viewpoints, the thickness of the polycrystalline SiC free-standing molded body of the present invention is preferably 1000 μm or more, more preferably 2000 μm or more.
[0020] There is no particular upper limit to the thickness of the polycrystalline SiC freestanding compact of the present invention, but a polycrystalline SiC freestanding compact having a thickness of 10,000 μm or less can be produced by a normal CVD method.
[0021] In the polycrystalline SiC freestanding compact of the present invention, the nitrogen concentration of both the first main surface and the second main surface is 3.00×10 16 atoms / cm 3 Less than or equal to 2.00×10 16 atoms / cm 3 Less than or equal to 1.00×10 16 atoms / cm 3Less than 0.50×10, particularly preferably 16 atoms / cm 3 According to the method for producing a polycrystalline SiC freestanding compact of the present invention, the nitrogen concentration is 3.00×10 16 atoms / cm 3 The polycrystalline SiC free-standing compact was obtained with a lower melting point than the conventional one, especially at 0.50×10 16 atoms / cm 3 Since the nitrogen concentration is one order of magnitude lower than that of the conventional product, the polycrystalline SiC freestanding molded body of the present invention can provide a polycrystalline SiC member with an extremely low nitrogen concentration.
[0022] In the polycrystalline SiC freestanding compact of the present invention, the lower limit of the nitrogen concentration of the first main surface and the second main surface is not particularly limited, but the nitrogen concentration of the first main surface and the second main surface is, for example, 0.020 × 10 16 atoms / cm 3 That's all.
[0023] In the polycrystalline SiC freestanding compact of the present invention, the absolute value of the nitrogen concentration gradient from the first main surface to the second main surface (absolute value of (nitrogen concentration of the first main surface - nitrogen concentration of the second main surface) / thickness) is 3.00 × 10 17 atoms / cm 4 The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface of the polycrystalline SiC freestanding compact is 3.00 × 10 17 atoms / cm 4 By setting the absolute value of the nitrogen concentration gradient from the first main surface to the second main surface of the polycrystalline SiC freestanding body to 3.00×10 or less, the concentration of nitrogen, which is a dopant source in the wafer, is stabilized in the thickness direction, and the change over time in the nitrogen concentration and partial pressure in the vicinity of the wafer when the SiC is consumed can be suppressed. 17 atoms / cm 4 If the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface of the polycrystalline SiC freestanding molded body of the present invention exceeds 1.00×10, the concentration of nitrogen, which is a dopant source in the wafer, becomes unstable in the thickness direction, and the nitrogen concentration and partial pressure change over time. 17atoms / cm 4 Less than or equal to 3.00×10, more preferably 16 atoms / cm 4 The following is the result.
[0024] In the polycrystalline SiC freestanding compact of the present invention, the lower limit of the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is not particularly limited, but the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is, for example, 1.00 × 10 16 atoms / cm 4 That's all.
[0025] In the polycrystalline SiC freestanding compact of the present invention, the absolute value of the difference in nitrogen concentration between the first main surface and the second main surface (absolute value of (nitrogen concentration of the first main surface - nitrogen concentration of the second main surface)) is 1.80 × 10 16 atoms / cm 3 The absolute value of the nitrogen concentration difference between the first and second main surfaces of the polycrystalline SiC freestanding compact is 1.80 × 10 16 atoms / cm 3 By setting the absolute value of the nitrogen concentration difference between the first and second main surfaces of the polycrystalline SiC freestanding body to 1.80×10 or less, the concentration of nitrogen, which is a dopant source in the wafer, is stabilized in the thickness direction, and the change over time in the nitrogen concentration and partial pressure in the vicinity of the wafer when the SiC is consumed can be suppressed. 16 atoms / cm 3 If the absolute value of the difference in nitrogen concentration between the first and second main faces of the polycrystalline SiC freestanding molded body of the present invention exceeds 0.60×10, the concentration of nitrogen, which is a dopant source in the wafer, becomes unstable in the thickness direction, and the nitrogen concentration and partial pressure change over time. 16 atoms / cm 3 Less than or equal to 0.40×10, more preferably 16 atoms / cm 3 The following is the result.
[0026] In the polycrystalline SiC freestanding compact of the present invention, the lower limit of the absolute value of the nitrogen concentration difference between the first main surface and the second main surface is not particularly limited, but the absolute value of the nitrogen concentration difference between the first main surface and the second main surface is, for example, 0.10 × 1016 atoms / cm 3 That's all.
[0027] In addition, the polycrystalline SiC freestanding molded body of the present invention is not particularly limited in terms of light transmittance, but generally, the higher the nitrogen concentration, the lower the light transmittance. The light transmittance per unit thickness of the polycrystalline SiC freestanding molded body of the present invention at wavelengths of 390 to 900 nm is 3.00×10 16 atoms / cm 3 In the following cases, the light transmittance is 0.5% / mm or more, and the nitrogen concentration is 2.00×10 16 atoms / cm 3 In the following cases, the light transmittance is 5.0% / mm or more, and the nitrogen concentration is 1.00×10 16 atoms / cm 3 In the following cases, the light transmittance is 10.0% / mm or more, and the nitrogen concentration is 0.50×10 16 atoms / cm 3 In the following cases, the light transmittance is 15.0% / mm or more. 16 atoms / cm 3 In the above cases, the polycrystalline SiC freestanding compact of the present invention has a light transmittance per unit thickness of 17.0% / mm or less at a wavelength of 390 to 900 nm.
[0028] The polycrystalline SiC free-standing molded body of the present invention can be obtained by selecting the reaction conditions and reaction environment in a method for producing a polycrystalline SiC free-standing molded body using a CVD method.
[0029] In the method for producing a polycrystalline SiC free-standing compact of the present invention, a CVD process is performed to obtain a polycrystalline SiC material formed on a graphite substrate by generating polycrystalline SiC on the graphite substrate by the CVD method. For example, a carrier gas and a raw material gas serving as a supply source of SiC are first mixed in a mixer to generate a mixed gas, and then the mixed gas is supplied from the mixer to a CVD furnace. A graphite substrate is placed in the CVD furnace, and the mixed gas is supplied to the CVD furnace to generate polycrystalline SiC on the graphite substrate by the CVD method, thereby obtaining a polycrystalline SiC material formed on the graphite substrate. The raw material gas used to produce SiC may be a one-component system (gas containing Si and C) or a two-component system (gas containing Si and gas containing C).
[0030] In the manufacturing method of the present invention for producing a polycrystalline SiC free-standing compact, after performing the CVD process, the polycrystalline SiC material formed on the graphite base material is removed and separated by oxidative combustion, mechanical grinding, etc., and then the separated polycrystalline SiC material is ground with diamond abrasive grains, etc., to obtain a polycrystalline SiC free-standing compact.
[0031] In the CVD process, a feed gas containing a raw material gas is supplied to a reactor, and while exhaust gas after the reaction is discharged from the reactor, the inside of the reactor is heated to generate polycrystalline SiC on the graphite substrate, and the polycrystalline SiC layer is grown in the growth direction to obtain a polycrystalline SiC material.
[0032] In the CVD process, the supply gas used to produce polycrystalline SiC contains a raw material gas and a carrier gas. The carrier gas is not particularly limited as long as it does not contain N, B, Al, P, etc., but examples of the carrier gas include hydrogen gas, Ar gas, etc.
[0033] The source gas is not particularly limited as long as it contains a Si source and a C source. Examples of the source gas include (A) a gas containing Si and C in the molecule, and (B) a mixed gas of a Si source gas containing Si in the molecule and a hydrocarbon gas as a C source. When the source gas (A) is used, it is a one-component system, and examples of such one-component source gases include methyltrichlorosilane, trichlorophenylsilane, dichloromethylsilane, dichlorodimethylsilane, and chlorotrimethylsilane. When the source gas (B) is used, it is a two-component system, and examples of such two-component source gases include a mixture of a silane-containing gas such as trichlorosilane or monosilane and a hydrocarbon gas. Of these, methyltrichlorosilane is used as the source gas in the embodiment because it has a stable Si to C ratio of 1:1 at the molecular level and is preferable in terms of the uniformity of the film quality and the molar ratio of Si atoms to C atoms of the polycrystalline SiC free-standing molded body, but this is just one example and is not limited thereto.
[0034] In the CVD process, the concentration of the raw material gas in the supply gas is 14.0 to 25.0 volume %, preferably 20.0 to 25.0 volume %. By keeping the concentration of the raw material gas in the supply gas within the above range, the time required for film formation can be shortened even for a free-standing molded body with a film thickness of 200 μm or more. This reduces the amount of nitrogen in the atmosphere taken in the CVD process, and allows the polycrystalline SiC free-standing molded body of the present invention to be obtained.
[0035] Generally, the reaction temperature in the CVD process is 1100 to 1600°C, preferably 1200 to 1450°C, and more preferably 1200 to 1350°C.
[0036] In the method for producing a polycrystalline SiC free-standing molded body of the present invention, (I) before the reaction, the inside of the reactor is depressurized with a graphite base material placed in the reactor, and then the inside of the reactor is depressurized and then restored with hydrogen gas, (II) before the reaction, the inside of the reactor is held in a hydrogen gas atmosphere at a predetermined temperature for a predetermined time, and (III) by adjusting the relationship between the residence time of the supply gas during the reaction and the thickness of the polycrystalline SiC material to be formed, a polycrystalline SiC material having a required thickness as a free-standing molded body, a low nitrogen concentration, a small absolute value of the nitrogen concentration gradient from the first main surface to the second main surface, and a small absolute value of the nitrogen concentration difference between the first main surface and the second main surface can be formed. Thus, in the method for producing a polycrystalline SiC free-standing molded body of the present invention, the polycrystalline SiC free-standing molded body of the present invention can be obtained by carrying out the above (I), (II), and (III).
[0037] In the method for producing a polycrystalline SiC free-standing compact of the present invention, (I) before the reaction, the inside of the reactor is depressurized with the graphite substrate placed in the reactor and then repressurized with hydrogen gas, and then the inside of the reactor is depressurized and repressurized with hydrogen gas, thereby removing nitrogen molecules present on the surface of the graphite substrate and in the atmosphere of the reactor, thereby lowering the nitrogen concentration on the second main surface (substrate surface). The pressure when depressurizing the inside of the reactor is 80 to 200 Pa, preferably 80 to 90 Pa, in absolute pressure. When the inside of the reactor is repressurized with hydrogen gas, the pressure after repressurization is 70×10 absolute pressure. 3 ~100×10 3 Pa, preferably 90 x 10 3 ~100×10 3 The pressure in the reactor is -5 Pa. The temperature in the reactor during the depressurization and repressurization is -5 to 45°C. If the operations of "depressurization → repressurization with hydrogen gas → depressurization → repressurization with hydrogen gas" are performed before the reaction, operations of depressurization and repressurization with nitrogen gas or operations of depressurization and repressurization with hydrogen gas may be performed before the series of operations.
[0038] In the method for producing a polycrystalline SiC free-standing compact of the present invention, after the operation (I) is performed, and before the reaction (II), the inside of the reactor is kept in a hydrogen gas atmosphere at a predetermined temperature for a predetermined time to desorb the nitrogen molecules adsorbed on the heat insulating material in the reactor, and then hydrogen gas is supplied into the reactor to discharge the gas in the reactor to the outside of the reactor, or while supplying hydrogen gas into the reactor, the reactor is kept at a predetermined temperature for a predetermined time to desorb the nitrogen molecules adsorbed on the heat insulating material in the reactor, and the gas in the reactor is discharged to the outside of the reactor to remove the nitrogen molecules adsorbed on the heat insulating material in the reactor, thereby lowering the nitrogen concentration on the second main surface (substrate surface). The temperature at which the temperature in the reactor is kept is preferably 1100°C or higher, and from the viewpoint of industrial efficiency, 1200 to 1450°C is more preferable. The time at which the temperature in the reactor is kept is preferably 0.5 hours or higher, and from the viewpoint of industrial efficiency, 0.5 to 1.5 hours is more preferable.
[0039] In the method for producing a polycrystalline SiC free-standing compact of the present invention, (III) the relationship between the residence time of the supply gas during the reaction and the thickness of the polycrystalline SiC material to be formed can be adjusted to lower the nitrogen concentration of the first main surface (growth surface), reduce the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface, and reduce the absolute value of the nitrogen concentration difference between the first main surface and the second main surface. In addition, when the thickness of the polycrystalline SiC material, the reaction temperature, and other manufacturing conditions are the same, the shorter the residence time, the less the amount of nitrogen taken in, and the lower the nitrogen concentration of the first main surface (growth surface). On the other hand, the shorter the residence time, the greater the heterogeneity of the structure of the polycrystalline SiC material to be obtained. In light of the above, the residence time of the supply gas during the reaction is preferably selected appropriately within the range of 2 to 50 seconds depending on the thickness of the polycrystalline SiC material to be formed, and more preferably selected appropriately within the range of 4 to 12 seconds.
[0040] The residence time of the supply gas is a parameter that indicates the time during which the source gas resides in the CVD reaction chamber and is involved in the reaction when a CVD reaction is carried out, and is a value calculated by the following formula.
[0041]
number
[0042] The thickness of the polycrystalline SiC material formed in the CVD process is selected to be 200 μm or more, preferably 500 μm or more, more preferably 2000 μm or more. The thickness of the polycrystalline SiC material formed in the CVD process is appropriately selected within the range of 10000 μm or less, preferably 8000 μm or less.
[0043] In the manufacturing method of the present invention for producing a polycrystalline SiC free-standing compact, the growth rate of the SiC layer in the CVD process is 60 μm / hour or more, and from the viewpoint of being able to reduce the nitrogen concentration in the polycrystalline SiC free-standing compact, it is preferably 500 μm / hour or more, and more preferably 1000 μm / hour or more.
[0044] In the method for producing a polycrystalline SiC free-standing body of the present invention, the reaction time in the CVD step is 0.17 to 1.67 hours, and from the viewpoint of increasing the thickness of the polycrystalline SiC free-standing body and decreasing the nitrogen concentration, it is preferably 0.50 to 1.33 hours, and more preferably 1.00 to 1.33 hours.
[0045] In the manufacturing method of the present invention for producing a polycrystalline SiC free-standing compact, in the CVD process, when the formation of the polycrystalline SiC material by the CVD method is completed, the graphite base material on which the polycrystalline SiC material has been formed is removed from the CVD furnace, and then processed so as to remove only the polycrystalline SiC free-standing compact. EXAMPLES
[0046] The invention will now be illustrated by the following examples.
[0047] Example 1 A graphite substrate with a diameter of 300 mm and a thickness of 4 mm was placed in the CVD furnace. Then, the pressure was reduced to 80 to 90 Pa, and the furnace was filled with nitrogen gas at 100 × 10 3 The pressure was then reduced to 80-90 Pa, and hydrogen gas was added to the reactor to restore the pressure to 100×10 Pa.3 The operation of restoring the pressure to 10 Pa was repeated three times. Next, the inside of the reactor was heated to 1300° C. for 60 minutes while supplying hydrogen gas. Next, a supply gas containing 25% by volume of methyltrichlorosilane (raw material gas, purity 99.5%) was introduced into the CVD furnace at the supply gas flow rate shown in Table 1, and a reaction was carried out at 1300°C and the furnace pressure shown in Table 1 to obtain a polycrystalline SiC material formed on the graphite substrate. The residence time of the supply gas at this time is shown in Table 1. After the CVD process, the graphite substrate was removed from the CVD furnace and a polycrystalline SiC free-standing molded body was obtained. The evaluation results of the obtained polycrystalline SiC free-standing molded body are shown in Table 2.
[0048] (Examples 2 to 7) The same procedure as in Example 1 was carried out except that in the CVD process, the source gas was supplied at the supply gas flow rate shown in Table 1, so that the residence time of the supply gas was set to the value shown in Table 1. In Example 5, the graphite substrate used was one that had been purified at 2400°C in a CF4 atmosphere and then ultra-purified at 2000°C or higher under reduced pressure.
[0049] (Comparative Examples 1 to 3) A graphite substrate with a diameter of 300 mm and a thickness of 4 mm was placed in a CVD furnace. Next, a supply gas containing 25 volume % of methyltrichlorosilane (raw material gas, purity 99.5%) was introduced into the CVD furnace at the supply gas flow rate shown in Table 1, and a reaction was carried out at 1300°C and the furnace pressure shown in Table 1 to obtain a polycrystalline SiC material formed on the graphite substrate. The residence time of the supply gas at this time is shown in Table 1. In Comparative Example 3, the graphite substrate used was one that had been purified at 2400°C in a CF4 atmosphere and then ultra-purified at 2000°C or higher under reduced pressure. After the CVD process, the graphite substrate was removed from the CVD furnace and a polycrystalline SiC free-standing molded body was obtained. The evaluation results of the obtained polycrystalline SiC free-standing molded body are shown in Table 2. That is, in Comparative Examples 1 to 3, the operations of reducing pressure before the reaction and restoring the pressure with hydrogen gas, and the operations of heating and maintaining the hydrogen gas atmosphere in the reactor were not performed.
[0050] (Analysis of nitrogen concentration, nitrogen concentration gradient, and nitrogen concentration difference) The nitrogen concentration of the polycrystalline SiC free-standing molded body obtained in each Example and Comparative Example was measured in the thickness range of 0.1 to 8.0 μm using dynamic SIMS. The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface of the polycrystalline SiC free-standing molded body was calculated using the thickness measured by a thickness meter. Regarding the nitrogen concentration distribution in the thickness direction, the thickness was measured by a thickness meter after machining, and the nitrogen concentration was measured by dynamic SIMS. The nitrogen concentration difference was calculated from the difference between the nitrogen concentrations of the first main surface and the second main surface measured by dynamic SIMS. (Volume resistivity) The volume resistivity was measured by the four-probe method using a Loresta GP manufactured by Mitsubishi Chemical Analytech.
[0051] [Table 1]
[0052] [Table 2]
[0053] In the table, the first main surface nitrogen concentration means the nitrogen concentration of the first main surface (growth surface), the second main surface nitrogen concentration means the nitrogen concentration of the second main surface (substrate surface), the nitrogen concentration difference between the first and second main surfaces means the absolute value of the nitrogen concentration difference between the first and second main surfaces, and the nitrogen concentration gradient means the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface.
[0054] <Residence time> As shown in Table 3 and Fig. 2, in the relationship between the residence time of the source gas in the reactor and the nitrogen concentration on the first main surface when the thickness of the polycrystalline SiC freestanding compact formed is 500 µm, the nitrogen concentration on the first main surface is low for the residence times of Examples 1, 2 and 6, and the shorter the residence time, the lower the nitrogen concentration on the first main surface. On the other hand, when the residence time is extended to the same extent as Comparative Example 1, the nitrogen concentration on the first main surface becomes high. These results show that the shorter the gas residence time in the CVD process, the less nitrogen is taken in.
[0055] [Table 3]
[0056] <Pressure reduction before reaction, pressure recovery with hydrogen gas, and heating and maintaining the inside of the furnace in a hydrogen gas atmosphere> As shown in Table 4 and Figs. 3 to 5, in Examples 5 to 7, the nitrogen concentration of the second main surface can be reduced by reducing the pressure before the reaction, restoring the pressure with hydrogen gas, and heating and holding the furnace in a hydrogen gas atmosphere. In addition, by adjusting the relationship between the formation thickness of the polycrystalline SiC material and the residence time, the nitrogen concentration of the first main surface can be reduced, the absolute value of the nitrogen concentration difference between the first main surface and the second main surface can be reduced, and the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface can be reduced. On the other hand, in Comparative Example 3, the nitrogen concentration of the second main surface was high, the nitrogen concentration of the first main surface was high, and the absolute value of the nitrogen concentration difference between the first main surface and the second main surface was large, resulting in a large absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface. From Comparative Example 3, it can be seen that the nitrogen concentration of the second main surface cannot be reduced simply by using a graphite base material that has been purified with CF4.
[0057] [Table 4]
[0058] <Manufacturing of thick polycrystalline SiC free-standing compacts> As shown in Table 5 and Fig. 6, by reducing the pressure before the reaction, restoring the pressure to hydrogen gas, and heating and holding in the furnace in a hydrogen gas atmosphere, and selecting the residence time according to the case of a large thickness, it is possible to obtain a polycrystalline SiC freestanding molded body having a small absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface, even though the thickness is as large as 2000 µm, in Examples 3 and 4. On the other hand, in Comparative Example 2, since reducing the pressure before the reaction, restoring the pressure to hydrogen gas, and holding in the furnace in a hydrogen gas atmosphere are not performed, the absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface cannot be reduced by adjusting the residence time alone when the thickness is as large as 2000 µm.
[0059] [Table 5]
[0060] <Pressure reduction before reaction, pressure recovery with hydrogen gas, and heating and maintaining the inside of the furnace in a hydrogen gas atmosphere> 7, in Example 4, the nitrogen concentration of the second main surface is as low as that of Example 5, which uses a graphite base material purified with CF4, even though the graphite base material does not use a graphite base material purified with CF4. On the other hand, it is understood from Comparative Example 3 that the nitrogen concentration of the second main surface cannot be reduced by simply using a graphite base material purified with CF4.
[0061] [Table 6] [Explanation of symbols]
[0062] 1 First main surface 2 Second main surface 10 Polycrystalline SiC free-standing molded body
Claims
1. The thickness is 200 μm or more, The nitrogen concentration of the first main surface and the second main surface is 3.00×10 16 atoms / cm 3 is as follows: The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is 3.00×10 17 atoms / cm 4 is as follows: The absolute value of the nitrogen concentration difference between the first main surface and the second main surface is 1.80×10 16 atoms / cm 3 That is: A polycrystalline SiC free-standing compact, characterized by:
2. The nitrogen concentration of the first main surface and the second main surface is 0.50×10 16 atoms / cm 3 2. The polycrystalline SiC free-standing compact according to claim 1, wherein:
3. 2. The polycrystalline SiC free-standing compact according to claim 1, wherein the thickness is 1000 μm or more.
4. The absolute value of the nitrogen concentration gradient in the direction from the first main surface to the second main surface is 3.00×10 16 atoms / cm 4 2. The polycrystalline SiC free-standing compact according to claim 1, wherein:
5. The absolute value of the nitrogen concentration difference between the first main surface and the second main surface is 0.40×10 16 atoms / cm 3 2. The polycrystalline SiC free-standing compact according to claim 1, wherein:
Citation Information
Patent Citations
Low nitrogen concentration carbonaceous material and method for producing the same
JP2002249376A
SiC-COATED CARBONACEOUS MATERIAL AND CARBONACEOUS MATERIAL TO BE COATED WITH SiC
JP2005132637A
Silicon carbide ingot and production method of silicon carbide substrate
JP2015098420A