Method for manufacturing alloy substrate for creating nanocarbon, and method for producing nanocarbon

The method addresses the challenges of catalyst support uniformity and metal contamination in alloy substrates by using acid and thermal oxidation treatments to produce high-quality carbon nanotubes efficiently.

JP2024140623AInactive Publication Date: 2024-10-10TAIHEIYO MATERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051846
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing carbon nanotubes using alloy substrates face challenges in achieving industrial stability and quality due to issues with catalyst support uniformity, metal contamination, and unevenness, which affect the diameter and production efficiency.

Method used

A method involving an acid treatment, thermal oxidation, and reduction treatment of alloy substrates to create a uniform passivation layer, followed by reacting with hydrocarbons to produce high-quality carbon nanotubes.

Benefits of technology

The method enables the stable and efficient production of high-quality carbon nanotubes by ensuring uniform catalyst dispersion and reducing metal contamination, enhancing production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide an industrial and stable production method of an alloy substrate which is used for producing nanocarbon of excellent quality particularly a carbon nano-tube.SOLUTION: A method for producing an alloy substrate for creating nanocarbon is used for decomposing hydrocarbon to create nanocarbon, and the method comprises: (A) an acid treatment process of treating the alloy substrate by acid solution; (B) a thermal oxidation treatment process of performing heat treatment to an alloy substrate after the acid treatment process in an oxidizing atmosphere of 500 to 1200°C; (C) a reduction treatment process of performing heat treatment to the alloy substrate after the thermal oxidation treatment process in a reducing atmosphere of 400 to 800°C.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an alloy substrate for producing nanocarbon, and a method for producing nanocarbon. [Background technology]

[0002] As a manufacturing method of functional carbon including carbon nanotubes (hereinafter, also abbreviated as CNT), the substrate method is widely used in which carbon is generated using a substrate carrying a metal serving as a catalyst component as a catalyst. As a method for preparing a catalyst used in the substrate method, first, a metal oxide such as alumina or silica, or an alloy represented by stainless steel is used as a substrate or a carrier layer formed on a substrate. In particular, in the super growth method (see Non-Patent Document 1), which was devised as an efficient manufacturing method for single-walled CNT, alloys are sometimes used as substrates in recent years. Next, sputtering and coating methods have been studied as a method for supporting catalytic metals on a substrate and have been put to practical use. However, although the sputtering method allows precise control of the amount of metal supported and the particle size, it is not suitable for industrial use when considering mass production of catalysts and CNTs. For the coating method, it is also important to adjust the supporting conditions to ensure the dispersibility and strength of the metal, and these effects lead to a decrease in quality, such as the diameter of the CNT and metal contamination.

[0003] Meanwhile, a simple method for producing CNTs using an alloy substrate has been proposed, in which a metal oxide layer is formed on the surface of the alloy substrate by heat-treating the substrate in an oxidizing atmosphere, thereby producing high-density CNTs (Patent Document 1). However, the formation of the metal oxide layer and the state of catalyst metal support are greatly influenced by the combination of various conditions, such as the conditions for the oxidation treatment, the type of substrate material, and surface roughness, and this poses problems such as the aggregation and thickening of the metal and increased unevenness on the substrate surface. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-262509 A [Non-patent literature]

[0005] [Non-Patent Document 1] Kenji Hata et al,Water-Assisted Highly Efficient Synthesis of Impurity-Free Single-Walled Carbon Nanotubes, SCIENCE, 2004.11.19,VOl.30 6, p.1362-1364 Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above problems, the present invention provides an industrially and stably manufacturing method for an alloy substrate for producing high-quality nanocarbon, particularly carbon nanotubes. [Means for solving the problem]

[0007] Therefore, the present inventors conducted extensive research into a method for producing an alloy substrate for producing nanocarbon that produces high-quality nanocarbon, and as a result, discovered a method for producing a catalyst that can solve the above problems, thereby completing the present invention. That is, the present invention provides the following [1] to [4]. [1] A method for producing an alloy substrate for generating nanocarbon by decomposing hydrocarbons, comprising the steps of: (A) an acid treatment step of treating the alloy substrate with an acidic solution; (B) a thermal oxidation treatment step of heat-treating the alloy substrate after the acid treatment step in an oxidizing atmosphere at 500 to 1200°C; (C) a reduction treatment step of heat-treating the alloy substrate after the thermal oxidation treatment step in a reducing atmosphere at 400 to 800° C., [2] A method for producing an alloy substrate for generating nanocarbon according to [1], wherein the alloy substrate contains one or more catalytic metals selected from the group consisting of Fe, Ni, Cu, Pt, Au, Ru, Pd and Rh. [3] The method for producing an alloy substrate for generating nanocarbon according to [2], further comprising the step of: (a) forming a substrate on a substrate surface; (b) forming a substrate on a substrate surface; and (c) forming a substrate on a substrate surface. [4] A method for producing nanocarbon, comprising reacting an alloy substrate for generating nanocarbon produced by the method of [1] to [3] with a hydrocarbon to generate nanocarbon on the alloy substrate. Effect of the Invention

[0008] By using the manufacturing method of the present invention, it is possible to obtain an alloy substrate that allows for the industrial and stable production of nanocarbon of excellent quality. By using this alloy substrate to decompose hydrocarbons, nanocarbon (especially carbon nanotubes) can be efficiently produced. [Brief description of the drawings]

[0009] [Figure 1] 1 shows a schematic diagram of a gas flow catalytic reactor. [Diagram 2] 1 shows the growth state of CNTs grown on an alloy substrate (Example 1). [Diagram 3] The image of the generated CNTs observed by a transmission electron microscope is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention is a method for producing an alloy substrate for generating nanocarbon, which generates nanocarbon by decomposing hydrocarbon. Specifically, the method for producing an alloy substrate for generating nanocarbon includes: (A) an acid treatment step of treating the alloy substrate with an acidic solution; (B) a thermal oxidation treatment step of heat treating the alloy substrate after the acid treatment step in an oxidizing atmosphere at 500 to 1200°C; and (C) a reduction treatment step of heat treating the alloy substrate after the thermal oxidation treatment step in a reducing atmosphere at 400 to 800°C. The method will be described in detail below.

[0011] <Alloy substrate> As the alloy substrate in the present invention, various alloys used as heat-resistant alloys can be widely used. In particular, it is preferable to include a metal that can be a catalyst for decomposing hydrocarbons to generate carbon (nanocarbon). Specifically, it is preferable to include one or more selected from the group of Fe, Ni, Cu, Pt, Au, Ru, Pd, and Rh. In particular, it is preferable to include Fe and / or Ni in industrial CNT production. In addition to the above metals, from the viewpoint of ensuring a good dispersion state of the catalyst metal, it is preferable to include one or more selected from the group of Al, Ti, Cr, Mg, Si, Mn, and Mo as a metal that can form a passivation layer. In particular, it is preferable to include Cr. Examples of such alloys include various SUSs, which are stainless steels, nickel alloys such as nichrome, various Inconels, Invar, and Permalloy. Among these, SUS304, 316, 310S, and Inconel 600 and 601 are preferable.

[0012] <(A) Acid treatment process> The acid treatment step in the present invention is a step of treating the alloy substrate with an acid solution. The acid solution is not particularly limited, and inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, and chromic acid, and organic acids such as citric acid, malic acid, and oxalic acid can be used, and two or more of these can be used in combination. By performing the acid treatment, scale such as metal oxide remaining on the substrate surface can be removed. In addition, a part of the passivation layer (metal oxide film) existing before the acid treatment can be removed, and a new passivation layer can be formed. An untreated alloy substrate usually has an uneven thickness of the passivation layer on the surface. By performing the acid treatment, the thickness of the passivation layer can be made uniform. It is considered that by removing the scale and making the thickness of the passivation layer uniform, a good dispersion state of the metal catalyst can be secured in the subsequent steps.

[0013] Specifically, this step is performed by immersing the alloy substrate in an acidic solution for a certain period of time. The concentration of the acidic solution used is not particularly limited, but is preferably adjusted to a pH of 0.2 to 3. The immersion time is also not particularly limited, and is appropriately adjusted depending on the type and concentration of the acidic solution. The immersion time is preferably 1 minute to 3 days.

[0014] In the acid treatment step of the present invention, an oxidizing agent such as hydrogen peroxide may be used in combination. By using an oxidizing agent in combination, the formation of a passivation layer can be promoted. In addition, in the acid treatment step, the formation of a passivation layer can also be promoted by passing a current through the alloy substrate as an anode while immersing it in an acidic solution.

[0015] <(B) Thermal oxidation treatment step> The thermal oxidation treatment step in the present invention is a step of heat treating the alloy substrate after the acid treatment step in an oxidizing atmosphere at 500 to 1200° C. It is believed that this step exposes the catalytic metal to the surface of the passivation layer on the surface of the alloy substrate, and forms oxides of the catalytic metal dispersed on the nano-order.

[0016] The heat treatment temperature is appropriately adjusted according to the heat resistance temperature (maximum use temperature) of the alloy substrate used. It is sufficient if the temperature is equal to or higher than the temperature at which the metal contained in the alloy used usually starts to oxidize and is lower than the melting point of the alloy. Specifically, it is preferable to perform heat treatment at ±200°C of the heat resistance temperature of the alloy substrate. For example, in the case of an alloy substrate with a heat resistance temperature of 700°C, 500 to 900°C is preferable, and in the case of an alloy substrate with a heat resistance temperature of 1000°C, 800 to 1200°C is preferable. It is more preferable that the heat resistance temperature of the alloy substrate is ±100°C, and further preferable that the heat resistance temperature of the alloy substrate is ±50°C. As the oxidizing atmosphere, it is sufficient if the oxygen concentration is about 10 to 30% by volume, and it can be preferably treated in air. The treatment time is not particularly limited, but is preferably 10 minutes to 3 hours.

[0017] <(C) Reduction Treatment Step> The reduction treatment step in the present invention is a step of heat treating the alloy substrate after the thermal oxidation treatment step in a reducing atmosphere at 400 to 800 ° C. By reducing the alloy substrate after the thermal oxidation treatment, the oxide of the catalytic metal on the substrate is preferentially reduced and becomes a metallic state having catalytic activity. The reducing atmosphere is not particularly limited as long as it can sufficiently reduce the oxide of the catalytic metal, and examples thereof include a reducing atmosphere in a gas such as hydrogen, carbon monoxide, hydrocarbon, inert gas, or a mixed gas thereof. In this step, the alloy substrate after the thermal oxidation treatment is placed in a gas flow catalyst reaction tube for nanocarbon production, and a reduction treatment is performed in a reducing atmosphere containing a hydrocarbon gas as a pre-step, followed by the production of nanocarbon.

[0018] <Other processing> In addition, the alloy substrate may be subjected to physical polishing such as buffing, chemical polishing such as electrolytic polishing, or a polishing treatment combining chemical polishing and physical polishing as a pretreatment for the acid treatment step. In particular, when an alloy substrate with a large surface roughness is used, it is preferable to perform a polishing treatment. The surface roughness is preferably 1 μmRa or less, more preferably 0.5 μmRa or less, and even more preferably 0.2 μmRa or less.

[0019] <Production of carbon by decomposition of hydrocarbons> Nanocarbon can be efficiently produced by decomposing hydrocarbons using the alloy substrate for producing nanocarbon produced by the method of the present invention. Here, nanocarbon means carbon of nanometer size, and specific examples include carbon nanotubes, carbon nanofibers, graphene, fullerene, etc. In particular, the present invention can efficiently produce carbon nanotubes of excellent quality.

[0020] The method of reacting the nanocarbon generating alloy substrate with the hydrocarbon is not particularly limited, but it is preferable to flow a gas containing a hydrocarbon over the nanocarbon generating alloy substrate and react at a temperature of 500 to 1000°C. As the hydrocarbon, a chain or cyclic hydrocarbon or an unsaturated hydrocarbon can be used, and is not particularly limited, but ethylene and acetylene are preferable from the viewpoint of reactivity. In addition, as the gas containing a hydrocarbon, it is preferable to use hydrogen, argon, nitrogen, etc. in addition to the hydrocarbon. Furthermore, in order to promote the generation of nanocarbon, it is preferable to include a small amount of water vapor, carbon monoxide, carbon dioxide, oxygen, or a compound containing an oxygen atom such as an alcohol such as ethanol or a ketone such as acetone. EXAMPLES

[0021] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0022] Example 1 The alloy substrate used was Alloy600 (manufactured by Standard Test Piece Co., Ltd.; equivalent to Inconel 600) (□25×2mm). One side of the substrate was buffed with #800, ultrasonically cleaned in acetone for 80 minutes, and then ultrasonically cleaned in ethanol for 40 minutes before being used for testing. The surface roughness of the polished surface was 0.2μmRa or less. This alloy substrate was immersed in a citric acid aqueous solution adjusted to a pH of 1.0 at 40°C for 30 minutes. After immersion, it was ultrasonically cleaned in distilled water for 15 minutes, and then ultrasonically cleaned in acetone for 5 minutes. Next, it was subjected to thermal oxidation treatment at 1100°C for 2 hours in a box-type electric furnace with a dry air flow rate of 2 L / min. After that, it was subjected to reduction treatment at 600°C for 1 hour with a mixed gas of hydrogen and argon (hydrogen concentration 90%, argon concentration 10%) flowing at 4 L / min to obtain an alloy substrate with catalytic activity. This alloy substrate was placed in a gas flow catalyst reaction tube as shown in the schematic diagram of Figure 1, and a mixed gas containing hydrocarbons (ethylene concentration 5%, hydrogen concentration 75%, argon concentration 20%) was passed through at 2 L / min and the reaction was carried out at 780°C for 30 minutes, producing carbon nanotubes (CNTs) on the alloy substrate. Figure 2 shows the state of CNT production. An aggregate of CNTs with a height of about 2 mm was produced on the alloy substrate, and the production state was extremely good. The results of observation of the CNTs using a transmission electron microscope are shown in Figure 3. This shows that six-walled multi-walled carbon nanotubes were produced.

[0023] Comparative Example 1 Except for carrying out the thermal oxidation treatment without the immersion treatment in an aqueous citric acid solution (acid treatment), the test was carried out in the same manner as in Example 1. CNTs were formed in a spotty form on the substrate, and the formation state was poor.

[0024] Comparative Example 2 Except for not carrying out the thermal oxidation treatment at 1100° C., the test was carried out in the same manner as in Example 1. Only a small amount of CNTs, about 100 μm in size, was observed to be formed on the alloy substrate, and the formation state was poor.

[0025] Example 2 Except for using a nitric acid aqueous solution (pH: 1) instead of the citric acid aqueous solution as the acidic solution, the test was carried out in the same manner as in Example 1. CNTs with a height of about 1 mm were produced on the alloy substrate, and the production state was good.

[0026] Example 3 After immersing in an aqueous citric acid solution as in Example 1, the alloy substrate was further immersed in an aqueous hydrogen peroxide solution adjusted to 3.5% by weight at 40° C. for 2 hours. Except for this, the test was carried out in the same manner as in Example 1. An aggregate of CNTs with a height of about 1 mm was formed on the alloy substrate, and the formation state was good.

[0027] Comparative Example 3 The test was carried out in the same manner as in Example 1, except that the thermal oxidation treatment was carried out at 450° C. The CNTs grown on the alloy substrate were only slightly grown, about 50 μm in size, and the growth state was poor.

[0028] Example 4 A SUS304 substrate (□25×2 mm) was used as the alloy substrate. One side of the substrate was buffed with #800, ultrasonically cleaned in acetone for 80 minutes, and then ultrasonically cleaned in ethanol for 40 minutes, and then subjected to the test. The surface roughness of the polished surface was 0.2 μmRa or less. This alloy substrate was immersed in a citric acid aqueous solution prepared to have a pH of 1.0 for 30 minutes at 40°C. After immersion, it was ultrasonically cleaned in distilled water for 15 minutes, and then ultrasonically cleaned in acetone for 5 minutes. Next, a thermal oxidation treatment was performed in a box-type electric furnace at 850°C for 2 hours under a flow condition of 2 L / min of dry air. Thereafter, the test was performed in the same manner as in Example 1. An aggregate of CNTs with a height of about 1 mm was generated on the alloy substrate, and the generation condition was good.

[0029] The test results are summarized in Table 1. It was found that when an alloy substrate that had been subjected to an acid treatment process and a thermal oxidation process and then a reduction process was used as a catalyst, CNTs could be produced efficiently.

[0030] [Table 1]

Claims

1. A method for producing an alloy substrate for generating nanocarbon by decomposing hydrocarbons, comprising the steps of: (A) an acid treatment step of treating the alloy substrate with an acidic solution; (B) a thermal oxidation treatment step of heat-treating the alloy substrate after the acid treatment step in an oxidizing atmosphere at 500 to 1200° C.; (C) a reduction treatment step of heat-treating the alloy substrate after the thermal oxidation treatment step in a reducing atmosphere at 400 to 800° C.

2. 2. The method for producing an alloy substrate for generating nanocarbon according to claim 1, wherein the alloy substrate contains one or more catalytic metals selected from the group consisting of Fe, Ni, Cu, Pt, Au, Ru, Pd and Rh.

3. The method for producing an alloy substrate for generating nanocarbon according to claim 2, wherein the alloy substrate further contains one or more metals selected from the group consisting of Al, Ti, Cr, Mg, Si, Mn and Mo.

4. A method for producing nanocarbon, comprising reacting an alloy substrate for producing nanocarbon produced by the method according to any one of claims 1 to 3 with a hydrocarbon to produce nanocarbon on the alloy substrate.

Citation Information

Patent Citations

  • Alloy substrate for producing carbon nanotube, manufacturing method therefor, alloy substrate having carbon nanotube formed thereon by using the same, production method therefor, and application thereof

    JP2007262509A