Processing method for molten metal and continuous casting method
By adjusting slag composition with chromium oxide and controlling weir thickness, slag infiltration is suppressed, improving durability and recyclability in molten metal processing.
Patent Information
- Application Number
- JP2023051937
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing methods fail to effectively suppress slag infiltration into tundish weirs, leading to deformation and reduced durability, which affects the recyclability and cleanliness of molten metal processing.
Adjust the composition of slag components to include chromium oxide, which suppresses infiltration, and control the thickness of the tundish weir refractories to maintain integrity.
Prevents slag infiltration, enhances weir durability, and maintains high cleanliness and recyclability of refractories, ensuring stable continuous casting operations.
Smart Images

Figure 2024140671000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for treating molten metal in which the infiltration of refractories by slag is suppressed, and in particular, to a method for treating molten metal in a continuous casting process in which the infiltration of a gate provided in a tundish by slag is suppressed to improve the durability. [Background technology]
[0002] In the treatment of molten metal, for example, molten pig iron or molten steel, a treatment vessel equipped with a refractory material or a functional material made of a refractory material is used. Refractories are used in blast furnace ladles, charging ladles, ladles, impellers for desulfurization treatment, tundishes, their covers, weirs, long nozzles, sliding nozzle plates, etc. For example, continuous casting of steel is performed by pouring molten steel from a ladle into a tundish and then pouring it into a mold from a submerged nozzle. In this case, a weir is provided between the molten steel injection part in the tundish that receives the molten steel from the ladle and the tundish nozzle that discharges the molten steel into the mold. As an effect of such a weir, it is expected that the flow of molten steel in the tundish can be controlled, such as preventing a short-circuit flow from the molten steel injection part toward the tundish nozzle, and thus promoting the floating and separation of inclusions. Then, the inclusions can be removed to produce a cast slab with high cleanliness.
[0003] The gate of the tundish is often in contact with slag flowing from the ladle, and is usually made of aluminum for corrosion resistance. 2 O 3 It is composed of refractories mainly composed of Al and MgO. 2 O 3 When the content of a single component such as SiO or MgO is high, cracks are likely to occur due to thermal shock. 2In many cases, tundish weirs are manufactured with a composite composition that contains raw materials with low volume expansion coefficients such as refractory materials. For these reasons, the component ratio of refractory materials has been determined for tundish weirs. Tundish weirs using such component systems have a limit to the amount that can be recycled, so they may have to be disposed of as industrial waste. For example, Patent Document 1 discloses a technology for reusing weirs with the aim of reducing the amount of refractory materials used.
[0004] In addition, when pouring molten steel from a ladle into a tundish, ladle slag inevitably gets mixed into the tundish. Such ladle slag does not have a suitable composition for absorbing and removing the inclusions that float and separate in the tundish. In addition, the SiO 2 and lower oxides (Fe x O y , MnO) may contaminate the molten steel. Therefore, it is necessary to control the slag composition in the tundish or to cover the molten steel with flux to prevent contact between the molten steel and air. For example, Patent Document 2 discloses a technique for adding flux to the tundish to achieve this purpose. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-183586 A [Patent Document 2] JP 2012-110946 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the above-mentioned conventional techniques have the following problems. That is, according to Patent Document 1, the weir refractory of a tundish recovered after use is exposed to various stresses due to heating, cooling, infiltration of oxides, etc. Therefore, it is damaged and deformed, and in particular, it tends to deform convexly from the ladle molten steel injection side toward the outflow side to the mold due to molten steel pressure. Patent Document 1 describes the limit deformation amount for reuse when the tundish weir deforms convexly. However, it does not describe a technology for suppressing the infiltration of oxides into the weir refractory to suppress the deformation.
[0007] Patent Document 2 also describes a technique for controlling the slag composition by adding flux into the tundish, taking into consideration the component fluctuations caused by ladle slag and packing sand that flows out from the ladle when pouring starts. However, the techniques in Patent Document 2 all aim to prevent contamination of molten steel by absorbing and removing inclusions or reducing the degree of slag oxidation. However, there is no mention of a technique for suppressing oxide infiltration into the tundish gate. In other words, there is currently no technique that takes into consideration the effects of slag components on slag infiltration into refractories.
[0008] An object of the present invention is to solve the above-mentioned conventional problems and to provide a technique for suppressing the infiltration of refractories by slag and improving their durability. [Means for solving the problem]
[0009] The method for treating molten metal according to the present invention, which advantageously solves the above problems, is a method for treating molten metal in which a refractory used for holding or treating the molten metal comes into contact with slag on the molten metal, and at least one of a component that promotes the infiltration of the slag into the refractory and a component that inhibits the infiltration of the slag is adjusted in the composition of the slag, so that the refractory after use is provided with a thickness t of the slag that has not been infiltrated. e The present invention is characterized in that a predetermined amount of
[0010] The method for treating molten metal according to the present invention comprises the steps of: (a) The refractory material is Al 2 O3 and SiO 2 containing, (b) The refractory material is Al 2 O 3 : 45% by mass or more, and SiO 2 : Contains 10% by mass or more, (c) the components that promote the infiltration of the slag into the refractory are iron oxide and manganese oxide in the slag, and the component that inhibits the infiltration of the slag into the refractory is chromium oxide in the slag; This may be a more preferable solution.
[0011] The continuous casting method of the present invention which advantageously solves the above-mentioned problems is characterized in that, when continuous casting is performed using any of the above-mentioned molten metal treatment methods, the refractory material is a weir provided in a molten steel flow path in a tundish between a supply section through which molten steel flows from a ladle and a discharge section through which molten steel flows out into a mold.
[0012] The continuous casting method according to the present invention is as follows: (d) The initial thickness of the weir is t 0 The thickness t of the slag not yet infiltrated at the end of operation is calculated from the sum of the iron oxide content and manganese oxide content in the slag as components that promote the infiltration of the slag into the refractory of the gate and the chromium oxide content in the slag as a component that inhibits the infiltration of the slag into the refractory of the gate. e and adjusting the slag components so that the amount is a predetermined amount. (e) The thickness t of the slag that is not yet infiltrated e The following formula (1) (where t 0 : initial thickness of the weir (mm), t e : Thickness of the weir without slag penetration (mm), (Fe x O y +MnO): The sum of the iron oxide content and manganese oxide content in the slag (mass%), (Cr 2 O 3 ): the content of chromium oxide in the slag (mass%), a, b, c: coefficients and constants. This may be a more preferable solution. t e =t 0 -{a×(Fe x O y +MnO)-b×(Cr 2 O 3 )}+c (1) Effect of the Invention
[0013] According to the method for treating molten metal and the method for continuous casting of the present invention, the thickness of the refractory that is not infiltrated with slag can be secured by adjusting the slag composition after use, so that the durability of the refractory can be improved. In addition, the deformation of the weir can be prevented, and the durability of the weir can be improved. In addition, the recyclability of the refractory can be improved, and the high cleanliness of the molten metal can be maintained, which is industrially useful. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic cross-sectional view showing a tundish according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional conceptual diagram illustrating a state in which slag has infiltrated into a dam of a tundish in use in the above embodiment. [Diagram 3] 1 is a graph comparing the amount of slag infiltration into the gate of a tundish after use with and without composition adjustment of the tundish slag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiments of the present invention will be described in detail. Note that the drawings are schematic and may differ from the actual ones. Furthermore, the following embodiments are merely examples of devices and methods for embodying the technical idea of the present invention, and are not intended to limit the configuration to the following. In other words, the technical idea of the present invention can be modified in various ways within the technical scope described in the claims.
[0016] 1 is a schematic cross-sectional view showing the configuration of a tundish used in a continuous casting method according to one embodiment of the present invention. The tundish 10 used in this embodiment has a refractory lining 2 on the inside of a steel shell 1. Molten steel 3 is poured from a ladle (not shown) into a molten metal supply section 4 through a long nozzle 11, and the molten steel 3 is poured into a mold (not shown) from a nozzle (not shown) installed at the bottom of a molten metal discharge section 5.
[0017] The tundish 10 shown in Fig. 1 is provided with a weir 8 that separates the slag 6, 7 in the tundish between the slag 6 on the supply side and the slag 7 on the discharge side. When continuous casting of steel is performed using such a tundish 10, the slag penetrates the weir 8 from both sides, the slag 6 on the supply side and the slag 7 on the discharge side.
[0018] Although Fig. 1 shows an example of a tundish for a single-strand continuous casting machine, it may have multiple discharge sections so as to supply to multiple strands. In that case, a weir 8 can be provided in any of the molten steel flow paths from the supply section to the discharge section. The shape of the weir 8 is not limited to the plate shape shown in Fig. 1, and may be any shape as long as it comes into contact with the slag in the tundish. The weir 8 is fixed by a wedge 9 and resists the molten steel flow and buoyancy.
[0019] The composition of the refractory material constituting the gate 8 of the tundish 10 is Al, taking into consideration the operating environment. 2 O 3 and SiO 2 The refractory composition is preferably a refractory containing Al. 2 O 3 : 45% by mass or more, and SiO 2 It is preferable that the content is 10 mass % or more. More preferably, Al 2 O 3 : 45% by mass or more, and SiO 2 : 30 mass % or more. This composition provides excellent corrosion resistance and thermal shock resistance. Other refractory components may include SiC and FC.
[0020] As shown in FIG. 2, the thickness of the weir 8 of the tundish 10 is defined as the vertical dimension from the surface in contact with the slag 6, 7 in the tundish. The initial thickness t 0 The slag 6 on the supply side and the slag 7 on the discharge side permeate the refractory of the weir 8 to form a permeation layer 8a. 2 O 3 Or SiO 2 The slag reacts with the infiltrated slag to form a eutectic phase, and a liquid phase is formed at the molten steel temperature. Such a infiltrated layer 8a does not contribute to the material strength of the weir 8 of the tundish 10. The thickness of the infiltrated layer 8a is classified into two areas, the molten metal supply section 4 side and the molten metal discharge section 5 side, and the thickness of each area is t m , t h Then, the effective thickness of the barrier that contributes to the material strength, that is, the thickness of the unpermeated slag, t e is expressed by the following equation (2). t e =t 0 -(t m +t h ) ···(2)
[0021] Effective thickness of the barrier that contributes to material strength t e When the effective weir thickness t of the weir 8 becomes 0, the slag has infiltrated the entire thickness of the weir 8. When the strength of the weir 8 of the tundish 10 in the full thickness infiltrated state becomes lower than the dynamic pressure from the molten steel 3, the dynamic pressure of the molten steel 3 causes the weir 8 to deform into a convex shape toward the molten metal discharge section 5, which may lead to problems such as the collapse of the weir 8. Furthermore, if a through hole occurs in the weir 8, the slag 6 on the molten metal supply section 4 side may flow out to the molten metal discharge section 5 side, which may cause quality problems. Therefore, the effective weir thickness t of the weir 8 is e It is required to perform continuous casting in a state where the initial thickness t of the gate 8 is t ≥ 10 mm, that is, in a state where the thickness of the gate 8 without slag infiltration is secured. 0 When is 100mm, the effective thickness of the weir t e The distance between the gap and the surface of the substrate should be ≧40mm.
[0022] As described above, slag infiltration into the refractory material that constitutes the weir 8 proceeds when the infiltrated slag forms a eutectic phase with the material of the main body of the weir 8. The lower the melting point and viscosity of the slag in contact with the weir 8, the deeper the slag infiltration will proceed. Therefore, by controlling the composition of the slag in contact with the weir 8 so that it has a high melting point and high viscosity, it is possible to suppress the infiltration of slag into the weir 8.
[0023] In this embodiment, the composition of the slags 6 and 7 in the tundish 10 is such that the iron oxide (Fe x O y ) and manganese oxide (MnO) have the effect of lowering the melting point and viscosity of the slag, and are therefore components that promote the penetration of the slag into the refractory material of the gate 8. Similarly, chromium oxide (Cr 2 O 3 ) has the effect of increasing the melting point and viscosity of the slag, and is therefore a component that inhibits the infiltration of the slag into the refractory material of the gate 8.
[0024] The inventors have investigated the amount (thickness) of slag infiltration into the refractory of the gate 8 during the use of the tundish 10 in continuous casting within a range of 9 to 11 hours. m +t h As a result, the relationship in formula (3) below was derived. t m +t h =a×(Fe x O y +MnO)-b×(Cr 2 O 3 )-c (3) Where: t m +t h : Slag infiltration thickness into the refractory of gate 8 (mm), (Fe x O y +MnO): content of iron oxide and manganese oxide in the slag (mass%), (Cr 2 O 3 ): chromium oxide content in the slag (mass%), a, b, c: coefficients and constants Represents.
[0025] From the above equations (2) and (3), the effective weir thickness t e In order to ensure this, the following equation (4) must be satisfied. t 0 ≧a×(Fe x O y +MnO)-b×(Cr 2 O 3 )-c+t e (4)
[0026] In the continuous casting method according to the present embodiment, the initial thickness t of the gate 8 of the tundish 10 is set to satisfy the above formula (4). 0 and adjust the slag composition in the tundish 10. For example, a reducing material such as metallic Al can be added to the slag in the tundish to reduce and reduce low-grade oxides such as FeO and MnO. Also, chromium oxide can be added to suppress slag infiltration. The timing for adjusting the slag composition can be selected from among adding a reducing material such as Al to the slag above the molten steel in the ladle at the time of tapping, scattering a reducing material or chromium oxide, etc., on the slag above the molten steel in the ladle during secondary refining, and scattering a reducing material or chromium oxide, etc., on the slag above the molten steel in the tundish. In adjusting the slag composition, the composition of the ladle slag is estimated or measured from past results, and the slag composition in the tundish is estimated or measured, and the amount of slag infiltration (thickness) t m +t h In this embodiment, it is preferable to calculate the thickness of the uninfiltrated slag t e The initial thickness t of the weir is set to 10 mm or more, preferably 40 mm or more. 0 or adjust the slag composition.
[0027] By adjusting the slag composition in the tundish according to the present embodiment, the thickness of the slag that is not infiltrated into the weir 8 after use is t e Therefore, the deformation of the weir 8 can be suppressed and the fixation of the weir 8 by the wedges 9 can be maintained.
[0028] In the above embodiment, the method for continuous casting of steel has been described by taking the weir of a tundish as an example, but the present invention can also be applied to the refractory material constituting the vessel of the tundish, the long nozzle for pouring molten steel from a ladle, and the sliding nozzle plate. The present invention can also be applied to the treatment of other molten metals. For example, the present invention can be applied to refractories that come into contact with slag, such as refractories of blast furnace ladles and charging ladles used in the preliminary treatment of molten pig iron, and the impeller of a mechanical stirring desulfurization device. EXAMPLES
[0029] Continuous casting of steel was carried out using the tundish shown in Figure 1. The processing time was 9 to 11 hours, and the amount of molten steel passing through was about 3,000 to 4,000 tons. The relationship between the various slag compositions in the tundish and the amount of slag infiltrated into the gate is summarized in Table 1. The initial thickness of the gate t 0 The slag composition in the tundish was iron oxide (Fe x O y ), manganese oxide (MnO) and chromium oxide (Cr 2 O 3 The content (mass%) of slag (t m +t h ) was calculated. In the formula, a = 2.89, b = 10.38, and c = -61.19 were used. The gate of the tundish retrieved after casting was inspected, and the measured value of the amount of slag infiltration was used. From the results in Table 1, it can be seen that the calculated value of the amount of slag infiltration is in good agreement with the measured value.
[0030] [Table 1]
[0031] In treatment No. 1, the amount of slag infiltration was greater than the initial thickness of the weir t 0 The thickness of the weir reached 100 mm, the same as the previous year, and the weakened weir was pushed by the dynamic pressure of the molten steel flow and deformed into a convex shape toward the drainage area. A crack caused by the deformation caused part of the weir to fall off.
[0032] Of the slag compositions in the tundish, the iron oxide and manganese oxide are thought to originate from the converter slag. On the other hand, the chromium oxide is thought to originate from the packing sand that flows in when pouring from the ladle begins. In treatment No. 2, slag modification was insufficient, and the remaining effective weir thickness was less than 10 mm. In treatments No. 3 to 6, slag modification ensured that the remaining effective weir thickness was 10 mm or more. In treatments No. 4 to 6, metallic Al was added to the slag above the molten steel tapped from the converter to the ladle to reduce low-grade oxides. In treatments No. 3, 5, and 6, chromium oxide was added. In treatments No. 5 and 6 (inventive examples), in which the slag composition was adjusted, the (Fe x O y + MnO) could be reduced to 9 mass% or less. As shown in Fig. 3, in the inventive examples corresponding to treatments No. 5 and 6, the amount of slag infiltration was less than 60 mm, that is, the thickness of the remaining effective weir was 40 mm or more, and a sound weir shape could be maintained.
[0033] In this embodiment, the composition was controlled by adding metallic Al to the slag above the molten steel tapped into the ladle. However, this method is not limited to this method as long as it reduces low-grade oxides. In addition, it is also useful to control the slag composition by adding flux to the tundish. For example, Cr 2 O 3 The infiltration of slag can also be suppressed by a method of adding a flux containing [Industrial Applicability]
[0034] According to the continuous casting method of the present invention, the durability of the gate of the tundish is improved, so that the continuous casting can be operated stably and without trouble, and the quality of the steel can be maintained, which is industrially useful. [Explanation of symbols]
[0035] 1 Ironhide 2 Refractory lining 3. Molten Steel 4. Hot water supply section (from ladle) 5. Drainage section (for the mold) 6 (Hot water supply side) Slag 7 (Drain side) Slag 8. Weir (of a tundish) 8a (slag) infiltration layer 9 Wedge 10 Tundish 11 Long nozzle
Claims
1. 1. A method for treating molten metal in which a refractory material used to hold or treat the molten metal contacts a slag above the molten metal, comprising the steps of: In the composition of the slag, at least one of a component that promotes the infiltration of the slag into the refractory and a component that inhibits the infiltration of the slag is adjusted to obtain a thickness t of the refractory that is not infiltrated by the slag after use. e A method for treating molten metal that ensures a predetermined amount of
2. The refractory material is Al 2 O 3 and SiO 2 2. The method of claim 1, comprising:
3. The refractory material is Al 2 O 3 : 45% by mass or more, and SiO 2 3. The method for treating molten metal according to claim 2, comprising: 10 mass % or more of ZnO.
4. The components that promote the infiltration of the slag into the refractory material are iron oxide and manganese oxide in the slag, 2. The method for treating molten metal according to claim 1, wherein the component that inhibits the infiltration of the slag into the refractory is chromium oxide in the slag.
5. When performing continuous casting using the molten metal treatment method according to any one of claims 1 to 4, a dam provided in a molten steel flow path in a tundish between a supply section through which molten steel flows from a ladle and a discharge section through which the molten steel flows into a mold.
6. The initial thickness of the dam is t 0 year, the sum of the iron oxide content and the manganese oxide content in the slag as components that promote the infiltration of the slag into the refractory of the gate; The thickness t of the slag that is not infiltrated at the end of operation is calculated from the content of chromium oxide in the slag as a component that suppresses the infiltration of the slag into the refractory of the gate. e 6. The continuous casting method according to claim 5, further comprising the step of adjusting the slag components so that the amount of the slag is a predetermined amount.
7. The thickness of the slag that has not yet infiltrated is t e The continuous casting method according to claim 6, wherein the above formula (1) is used to calculate the melting point. t e =t 0 -{a×(Fe x O y +MnO)-b×(Cr 2 O 3 )}+c (1) Where: t 0 : initial thickness of the weir (mm), t e : thickness of the weir not infiltrated with slag (mm), (Fe x O y + MnO): the sum of the iron oxide content and manganese oxide content in the slag (mass%), (Cr 2 O 3 ): chromium oxide content in the slag (mass%), a, b, c: coefficients and constants Represents.
Citation Information
Patent Citations
Method for suppressing erosion of castable refractories in ladle
JP1994248319A
Method for refining steel by utilizing mgo in slag in electric furnace for steelmaking or combination of electric furnace for steelmaking and ladle arc refining apparatus
JP1999172320A
Molten metal receiver and production method of the same
JP2015116571A
Method of refining molten metal
JP5463644B2
Continuous casting method of steel of high cleanliness
JP2012110946A