Cellulose acetate particles
Cellulose acetate particles with controlled acyl group substitution and specific coatings maintain softness and flexibility over time, addressing the issue of roughness in long-term storage.
Patent Information
- Application Number
- JP2023052436
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Cellulose acetate particles with low or high total substitution degrees of acyl groups remain soft but develop a rough texture over time, making them unsuitable for applications requiring flexibility and long-term storage stability.
Cellulose acetate particles with a controlled acyl group substitution of 0.05 to 0.70, combined with a coating layer containing fatty acids, fatty acid metal salts, amino acid compounds, lipid compounds, silicone compounds, fluorine compounds, or ceramide compounds, and optionally an intermediate layer and external inorganic particles, to enhance flexibility and prevent roughness.
The particles maintain softness and avoid roughness even after long-term storage, improving their suitability for applications like cosmetics by ensuring flexibility and biodegradability.
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose acetate particles. [Background technology]
[0002] Patent Document 1 proposes "particles containing cellulose acetate, the particles having an average particle diameter of 80 nm or more and 100 μm or less, a sphericity of 0.7 or more and 1.0 or less, a surface smoothness of 80% or more and 100% or less, and a surface contact angle with water of 100° or more, and a total acetyl substitution degree of the cellulose acetate of 0.7 or more and 2.9 or less."
[0003] Patent Document 2 proposes "cellulose derivative fine particles made of a cellulose derivative in which some of the hydroxyl groups of cellulose are substituted with a substituent, and characterized by having an average particle size of 9 to 1000 nm." [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 188698 [Patent Document 2] International Publication No. 2009 / 123148 Summary of the Invention [Problem to be solved by the invention]
[0005] The object of the present invention is to provide cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with cellulose acetate particles which contain cellulose acetate as a main component and have a total degree of substitution of acyl groups on cellulose acetate of less than 0.05 or 0.70 or more. [Means for solving the problem]
[0006] Means for solving the above problems include the following aspects. <1> The main component is cellulose acetate. The cellulose acetate particles have a total substitution degree of acyl groups substituted on the cellulose acetate of 0.05 or more and less than 0.70. <2> The acyl group of the cellulose acetate is only an acetyl group. <1> The cellulose acetate particles according to claim 1. <3> The total substitution degree of acyl groups substituted on the cellulose acetate is 0.15 or more and 0.6 or less. <1> or <2> The cellulose acetate particles according to claim 1. <4> The total degree of substitution of acyl groups on the cellulose acetate is 0.25 or more and 0.5 or less. <3> The cellulose acetate particles according to claim 1. <5> The volume average particle diameter of the cellulose acetate particles is more than 1 μm and not more than 100 μm. <1> ~ <4> 13. The cellulose acetate particles according to claim 12. <6> The volume average particle size of the cellulose acetate particles is 3 μm or more and 80 μm or less. <5> The cellulose acetate particles according to claim 1. <7> The base particles mainly composed of cellulose acetate; a coating layer that coats the base particles, the coating layer including at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, amino acid compounds, lipid compounds, silicone compounds, fluorine compounds, and ceramide compounds; have <1> ~ <6> 13. The cellulose acetate particles according to claim 12. <8> an intermediate layer between the base particle and the coating layer, The intermediate layer contains at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid. <7> The cellulose acetate particles according to claim 1. <9> Inorganic particles are added externally <1> ~ <7> 13. The cellulose acetate particles according to claim 12. Effect of the Invention
[0007] <1> According to the present invention, there is provided cellulose acetate particles which are soft and less likely to feel rough even when stored for a long period of time, compared with cellulose acetate particles which are mainly composed of cellulose acetate and have a total degree of substitution of acyl groups of less than 0.05 or 0.70 or more. <2> According to the invention described in the above, there is provided cellulose acetate particles which are soft and less prone to roughness even after long-term storage, as compared with cellulose acetate having an acyl group other than an acetyl group.
[0008] <3> According to the present invention, there is provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, as compared with cellulose acetate having a total substitution degree of acyl groups less than 0.15 or more than 0.6. <4> According to the present invention, there is provided cellulose acetate particles which are soft and less likely to feel rough even after long-term storage, compared with cellulose acetate having a total substitution degree of acyl groups less than 0.2 or more than 0.5. <5> According to the present invention, there is provided cellulose acetate particles which are soft and less likely to feel rough even when stored for a long period of time, as compared with cellulose acetate particles having a volume average particle size of 1 μm or less or 100 μm or less. <6> According to the present invention, there is provided cellulose acetate particles which are soft and less likely to feel rough even when stored for a long period of time, as compared with cellulose acetate particles having a volume average particle size of less than 3 μm or more than 80 μm.
[0009] <7> According to the present invention, there are provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with particles not having a coating layer on base particles mainly composed of cellulose acetate. <8> According to the present invention, there are provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, as compared with particles not having an intermediate layer between the base particles and the coating layer.
[0010] <9> According to the present invention, there are provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, as compared with particles not containing external inorganic particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0012] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0013] <Cellulose acetate particles> The cellulose acetate particles according to this embodiment contain cellulose acetate as a main component, and the total substitution degree of acyl groups substituted on the cellulose acetate is 0.05 or more and less than 0.70.
[0014] The cellulose acetate particles according to the present embodiment, due to the above-mentioned constitution, are soft and do not easily develop a rough feeling even when stored for a long period of time. The reason for this is presumed to be as follows.
[0015] Cellulose particles have a high elastic modulus and are hard, which makes them disadvantageous for applications requiring flexibility, such as cosmetic feel-improving particles. For example, a technique for improving the softness of cellulose particles is known in which the tactile feel is improved by using cellulose acetate with a total acetyl substitution degree controlled to 0.7 to 2.9 (Patent Document 1, etc.). However, in this technology, the introduction of these acyl groups makes cellulose more susceptible to plasticization and causes it to be eroded and hardened by low molecular weight components (esters, etc.), which leads to a deterioration in the texture and makes the material hard and rough when stored for a long period of time.
[0016] In contrast, in this embodiment, cellulose acetate particles mainly composed of cellulose acetate are used. The degree of substitution of acetyl groups in cellulose acetate is 0.05 or more, so that the strong molecular structure derived from cellulose is broken, the touch is improved, and the product is soft and less likely to have roughness. On the other hand, the degree of substitution of acyl groups in cellulose acetate is less than 0.70, so that the erosion by low molecular weight components is suppressed, and the product maintains its touch even after long-term storage, and is soft and less likely to have roughness.
[0017] From the above, it is presumed that the cellulose acetate particles according to this embodiment remain soft and are unlikely to develop a rough feel even when stored for a long period of time.
[0018] The cellulose acetate particles according to this embodiment will be described in detail below.
[0019] (Cellulose Acetate) The cellulose acetate particles according to this embodiment contain cellulose acetate as a main component. Here, "containing cellulose acetate as a main component" means that the content of cellulose acetate in the cellulose acetate is 90% by mass or more. However, when the cellulose particles have a coating layer and an intermediate layer described below, "containing cellulose acetate as a main component" means that the content of cellulose acetate in the base particles is 90% by mass or more.
[0020] Cellulose acetate is a cellulose derivative in which at least a portion of the hydroxyl groups in cellulose are substituted with acetyl groups (acetylation). In the cellulose acetate, at least a part of the hydroxyl groups in the cellulose may be substituted with an acyl group other than the acetyl group.
[0021] Here, in the acyl group other than an acetyl group, the hydrocarbon group in the acyl group may be any of linear, branched, and cyclic, but is preferably linear or branched, and more preferably linear. In the acyl group other than an acetyl group, the hydrocarbon group in the acyl group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group, but is more preferably a saturated hydrocarbon group. The acyl group other than the acetyl group is preferably an acyl group having 2 to 6 carbon atoms. In the acyl group other than an acetyl group, the hydrogen atom in the acyl group may be substituted with a halogen atom (e.g., a fluorine atom, a bromine atom, an iodine atom), an oxygen atom, a nitrogen atom, or the like, but an unsubstituted acyl group is preferable. Examples of acyl groups other than acetyl groups include propionyl groups, butyryl groups (butanoyl groups), propenoyl groups, hexanoyl groups, etc. Among these, from the viewpoint of improving the biodegradation rate, acyl groups having from 2 to 4 carbon atoms are more preferred, and acyl groups having 2 or 3 carbon atoms are even more preferred.
[0022] Examples of cellulose acetate include cellulose monoacetate, cellulose diacetate (DAC), cellulose triacetate, cellulose acetate propionate (CAP), and cellulose acetate butyrate (CAB).
[0023] The cellulose acetate may be used alone or in combination of two or more kinds.
[0024] The total substitution degree of acyl groups substituted on cellulose acetate is from 0.05 to less than 0.70, but from the viewpoint of improving softness and suppressing roughness after long-term storage, it is preferably from 0.15 to 0.6, more preferably from 0.25 to 0.5.
[0025] The acyl group of cellulose acetate is preferably only acetyl group. If the acyl group of cellulose acetate is only acetyl group, the strong molecular structure derived from cellulose is easily broken. Also, erosion by low molecular weight components is easily suppressed. Therefore, even if stored for a long period of time, it becomes softer and less likely to have a rough feeling.
[0026] In cellulose acetate, the degree of substitution is an index showing the degree to which hydroxyl groups in cellulose are substituted with acyl groups. In other words, the degree of substitution is an index showing the degree of acylation of cellulose acetate. Specifically, the degree of substitution means the intramolecular average number of substitutions in which three hydroxyl groups in a D-glucopyranose unit of cellulose acetate are substituted with acyl groups. The degree of substitution is determined from the intensity ratio of the cellulose-derived peak to the acyl group-derived peak in an infrared absorption spectrum (Spotlight400 / PerkinElmer).
[0027] The number average molecular weight of cellulose acetate is preferably 37,000 or more, and more preferably 45,000 or more. The upper limit of the number average molecular weight of cellulose acetate is not particularly limited, but may be, for example, 100,000 or less.
[0028] By setting the number average molecular weight of cellulose acetate to 37,000 or more, the material becomes highly biodegradable, soft, and less prone to roughness. The reasons for this are presumed to be as follows. By making the number average molecular weight 37,000 or more, the number of terminal hydroxyl groups is less likely to increase, and the number of hydroxyl groups per unit volume is suppressed. Therefore, the number and bond strength of intramolecular and extramolecular hydrogen bonds are less likely to become strong, hardness is reduced, and flexibility is increased. As a result, the product becomes soft and less likely to have a rough feel.
[0029] The number average molecular weight of cellulose acetate was measured by gel permeation chromatography (differential refractometer Optilab T-rEX / Wyatt Technology, multi-angle light scattering detector) The measurement is performed using a DAWN HELEOS II (Wyatt Technology) and columns (TSKgel α-M, α-3000, Tosoh) in dimethylacetamide (with 0.1M lithium chloride added) as the solvent.
[0030] (Other Ingredients) The cellulose acetate particles according to the present embodiment may contain other components. However, when the cellulose acetate particles have a coating layer described below, the other components are contained in the base particles that are coated with the coating layer.
[0031] Examples of other components include plasticizers, flame retardants, compatibilizers, release agents, light resistance agents, weather resistance agents, colorants, pigments, modifiers, anti-drip agents, antistatic agents, hydrolysis inhibitors, fillers, reinforcing agents (glass fibers, carbon fibers, talc, clay, mica, glass flakes, milled glass, glass beads, crystalline silica, alumina, silicon nitride, aluminum nitride, boron nitride, etc.), acid acceptors for preventing release of acetic acid (oxides such as magnesium oxide and aluminum oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, aluminum hydroxide, and hydrotalcite; calcium carbonate; talc; etc.), and reactive trapping agents (for example, epoxy compounds, acid anhydride compounds, carbodiimides, etc.). The content of the other components is preferably 0% by mass or more and 5% by mass or less based on the total amount of the cellulose acetate particles (or base particles), where "0% by mass" means that no other components are included.
[0032] (Cellulose acetate particles having a coating layer) The cellulose acetate particles according to this embodiment are preferably cellulose acetate particles having a base particle mainly composed of cellulose acetate (hereinafter also referred to as a cellulose acetate base particle) and a coating layer covering the base particle, the coating layer including at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, amino acid compounds, lipid compounds, silicone compounds, fluorine compounds, and ceramide compounds (hereinafter also referred to as a "cellulose acetate particle having a coating layer").
[0033] By configuring the cellulose acetate particles according to the present embodiment as described above, the cellulose acetate particles tend to be soft and less prone to roughness even after long-term storage. In addition, the decrease in biodegradability is suppressed. The reason for this is presumed to be as follows.
[0034] In fatty acids and fatty acid metal salts, the aliphatic groups repel each other due to repulsive forces, forming a pseudo-foam structure, i.e., a sponge-like action, emphasizing the flexibility of the surface of the particles themselves. Therefore, even after long-term storage, the product becomes soft and is less likely to feel rough. In addition, fatty acids and fatty acid metal salts themselves have strong water repellency and become highly hydrophobic, which suppresses hydrolysis of cellulose acetate and prevents surface defects due to initial biodegradation of the particles, allowing biodegradation to proceed uniformly. On the other hand, these compounds are prone to partial aggregation, which creates gaps on the surface through which microorganisms can penetrate, achieving excellent biodegradability.
[0035] Amino acid compounds have strong affinity and binding properties with cellulose acetate, and are easily fixed to the surface of cellulose acetate particles. In addition, they have a bent molecular structure, which enhances the flexibility of the cellulose acetate to which they are bound. Therefore, even after long-term storage, the product remains soft and is less likely to become rough. In addition, amino acid compounds tend to form flat crystals after coating, and the large specific surface area suppresses the initial contact of microorganisms with cellulose acetate, slowing down biodegradation and minimizing changes in texture over time. Also, gaps are formed between the crystals, allowing microorganisms to slowly penetrate, allowing biodegradation to proceed uniformly, and achieving excellent biodegradability.
[0036] The lipid compound has a strong bond with cellulose acylate and is easily fixed to the surface of the cellulose acylate particles. In addition, the lipid compound has a function of lowering the friction coefficient of the particle surface. Therefore, even if the surface is stored for a long period of time, the surface becomes soft and does not easily become rough. Silicone compounds have strong bonding properties with cellulose acylate and are easily fixed to the surface of cellulose acylate particles. They also act to reduce the coefficient of friction of the particle surface, so that the surface becomes soft and less prone to roughness even after long-term storage. Fluorine compounds have strong bonding properties with cellulose acylate and are easily fixed to the surface of cellulose acylate particles. They also have the effect of lowering the coefficient of friction of the particle surface, so that the surface becomes soft and does not easily become rough even after long-term storage. The ceramide compound has a strong bond with cellulose acylate and is easily fixed to the surface of cellulose acylate particles. It also has a function of lowering the coefficient of friction of the particle surface. Therefore, even after long-term storage, the surface becomes soft and does not easily become rough.
[0037] From the above, it is presumed that the product will remain soft and less likely to develop a rough texture even after long-term storage.
[0038] -Mother particle- The base particles are mainly composed of cellulose acetate. The cellulose acetate contained in the base particles has the same meaning as the cellulose acetate described above, and the preferred range is also the same.
[0039] -Coating layer- The coating layer preferably contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, amino acid compounds, lipid compounds, silicone compounds, fluorine compounds, and ceramide compounds.
[0040] ·fatty acid The fatty acids are linear or branched, saturated or unsaturated fatty acids. The fatty acids may also be mixtures of saturated and unsaturated fatty acids. From the viewpoint of improving softness and suppressing roughness after long-term storage, the fatty acid is preferably a fatty acid having 16 to 22 carbon atoms (preferably 18 to 20 carbon atoms). Specific examples of linear fatty acids having 16 to 22 carbon atoms include behenic acid, arachidic acid, palmitic acid, etc.
[0041] Fatty acid metal salts The fatty acid metal salt is a linear or branched, saturated or unsaturated fatty acid metal salt. From the viewpoint of improving the softness and suppressing the occurrence of roughness after long-term storage, the fatty acid metal salt may be a mixture of a saturated fatty acid metal salt and an unsaturated fatty acid metal salt. Examples of the metal salt of a fatty acid include metal salts of fatty acids having 16 to 22 carbon atoms (preferably 18 to 20 carbon atoms). Examples of the metal salt of a fatty acid having 16 to 22 carbon atoms include metal salts of stearic acid, metal salts of behenic acid, and metal salts of palmitic acid. The metal in the fatty acid metal salt may be a divalent metal. Examples of metals in the straight-chain fatty acid metal salts include magnesium, calcium, aluminum, barium, and zinc.
[0042] Here, in the fatty acid and fatty acid metal salt, if the number of carbon atoms is 16 or more, the fatty acid group is short and the sponge effect is sufficient. On the other hand, if the number of carbon atoms is 22 or less, the repulsion of the fatty acid group is reduced, the affinity with cellulose acetate is sufficient, and it is difficult to peel off from the cellulose acetate particles. Therefore, even if stored for a long period of time, it becomes soft and does not easily become rough. In addition, biodegradability is also sufficient.
[0043] Amino acid compounds The amino acid compound refers to amino acids and amino acid derivatives. Examples of the amino acid compound include lauryl leucine, lauryl arginine, and myristyl leucine.
[0044] ·Lipid compounds Representative examples of lipid compounds include phospholipids (lecithin and hydrogenated products thereof, phosphatidic acid and / or its salts, phosphatidylinositol, phosphatidylethanolamine, phosphatidylglycerol, soybean-derived phospholipids, soybean-derived hydrogenated phospholipids, egg yolk-derived phospholipids, egg yolk-derived hydrogenated phospholipids, etc.). Lipids also include glycolipids (rice bran glycosphingolipids, glycosphingolipids, etc.) and complex lipids.
[0045] Silicone compounds A silicone compound is a compound having a siloxane chain. Examples of silicone compounds include dimethylpolysiloxane, methylphenylsiloxane, methylhydrogenpolysiloxane, decamethylpolysiloxane, dodecamethylpolysiloxane, tetramethyltetrahydrogenpolysiloxane, triethoxysilylethyl polydimethylsiloxyethyl dimethicone, triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone, acrylic-silicone graft polymer, organic silicone resin partially crosslinked organopolysiloxane polymer, tetramethyltetrahydrogencyclotetrasiloxane, trimethylsiloxysilicate, amino-modified silicone, carboxylic acid-modified silicone, fluorinated silicone, silicone gum, acrylic silicone, silicone resin, triethoxysilylethyl polydimethylsiloxyethyl dimethicone, triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone, and the like.
[0046] Fluorine compounds A fluorine compound is a compound that contains fluorine atoms. Examples of the fluorine compound include perfluoropolyether, perfluoroalkyl phosphate ester (a mixture of diethanolamine salt of monoperfluoroalkylethyl phosphate ester and diethanolamine salt of diperfluoroalkylethyl phosphate ester, fluoro(C9-15)alcohol phosphate, etc.), perfluoroalkylalkoxysilane (perfluorooctyltriethoxysilane, perfluorocaprylyltriethoxysilylethylmethicone, etc.), fluorine-modified silicone, fluorine-modified polymer (copolymer of diethylaminoethyl methacrylate / 2-hydroxyethyl methacrylate / perfluorohexylethyl methacrylate, etc.), perfluoroalkylsilane, perfluoroalkyl group-containing ester, perfluoroalkyl phosphate ester salt, perfluoropolyether, fluorosilicone, fluorinated silicone resin, trimethoxy(3,3,3-trifluoropropyl)silane, tridecafluorooctyltriethoxysilane, etc.
[0047] Ceramide compounds Ceramide is a compound in which sphingosine and a fatty acid are bonded via an amide bond. Examples of ceramides include natural ceramides, plant ceramides, human ceramides, and synthetic ceramides (pseudoceramides). Examples of natural ceramides include ceramide 1, ceramide 2, ceramide 3, ceramide 4, ceramide 5, ceramide 6, and ceramide 7. Examples of plant ceramides include ceramides extracted from rice bran, rice, corn, konjac, pineapple, and the like. Examples of human ceramides include ceramide 1 (ceramide EOP), ceramide 2 (ceramide NG), ceramide 3 (ceramide NP), ceramide 4 (ceramide EOH), ceramide 5 (ceramide AG), ceramide 6II (ceramide AP), ceramide 7 (ceramide AH), ceramide 8, ceramide 9, and ceramide 10. Synthetic ceramides are hydroxypropyl bispalmitamide MEA, hydroxypropyl bislauramide MEA, and hydroxypropyl bisisostearamide MEA. etc.
[0048] The amount of the coating layer on the base particles is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 9% by mass or less, and even more preferably 1% by mass or more and 8% by mass or less, from the viewpoint of improving softness after long-term storage and suppressing the occurrence of roughness. Here, the content of the coating material in the entire coating layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.
[0049] -Middle class- In the cellulose acetate particles having a coating layer, it is preferable that an intermediate layer is provided between the base particle and the coating layer, and the intermediate layer preferably contains at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid.
[0050] By configuring the cellulose acetate particles according to the present embodiment as described above, the cellulose acetate particles tend to be soft and less prone to roughness even after long-term storage. In addition, the biodegradability is improved. The reason for this is presumed to be as follows.
[0051] The polyamine compound has a high affinity with cellulose acetate and with the carboxylic acid portion of the coating layer, such as fatty acid or fatty acid metal salt, and can selectively direct the aliphatic group of the fatty acid or fatty acid metal salt to the surface side of the coated particle, thereby enabling the effect of the coating layer to be more fully exhibited. Therefore, even if stored for a long period of time, the product becomes soft and is less likely to have a rough feel. In addition, the decrease in biodegradability is also suppressed. Polyquaterniums, like polyamine compounds, also make the material soft and less prone to roughness even after long-term storage, and also inhibit the deterioration of biodegradability. Since polysaccharide compounds have a structure very similar to that of cellulose acetate, the entire molecule covers a large portion of the cellulose acetate, but creates a cushion state with some voids, on which a coating layer such as an aliphatic acid or an aliphatic acid metal salt can adhere. Therefore, even if stored for a long period of time, the material remains soft and is less likely to feel rough. In addition, the deterioration of biodegradability is suppressed. Polyacrylic acid has a moderate water absorption property, so by incorporating water into the molecule, it becomes compatible with the surface of cellulose acetate that has absorbed a certain amount of water without reducing its flexibility, and for example, it has affinity with fatty acids and fatty acid metal salts because of its similar polarity, and the effect of the coating layer can be further enhanced. Therefore, even if stored for a long period of time, it becomes soft and is unlikely to develop a rough feeling. In addition, the decrease in biodegradability is also suppressed.
[0052] From the above, it is presumed that the cellulose acetate particles tend to be soft and less prone to roughness even after long-term storage, and that the decrease in biodegradability is also suppressed.
[0053] A polyamine compound is a general term for an aliphatic hydrocarbon having two or more primary amino groups. Examples of the polyamine compound include polyalkyleneimine, polyallylamine, polyvinylamine, and polylysine. From the viewpoint of improving biodegradability, the polyalkyleneimine is preferably a polyalkyleneimine having a structural unit with an alkylene group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms), and more preferably polyethyleneimine. Examples of polyallylamine include homopolymers or copolymers of allylamine, allylamine amide sulfate, diallylamine, dimethylallylamine, and the like. An example of the polyvinylamine is one produced by hydrolyzing poly(N-vinylformamide) with an alkali, and a specific example thereof is "PVAM-0595B" manufactured by Mitsubishi Chemical Corporation. The polylysine may be one extracted from a natural product, one produced by a transformed microorganism, or one chemically synthesized.
[0054] Examples of polyquaterniums include polyquaternium-6, polyquaternium-7, polyquaternium-10, polyquaternium-11, polyquaternium-51, polyquaternium-61, and polyquaternium-64.
[0055] The coverage of the intermediate layer on the base particles is preferably from 0.1% by mass to 20% by mass, more preferably from 1% by mass to 10% by mass, from the viewpoint of preventing softness and roughness after long-term storage. The content of the intermediate material in the entire intermediate layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.
[0056] -External additives- The cellulose acetate particles according to the present embodiment may have inorganic particles added thereto. When inorganic particles are added thereto, secondary aggregation between particles is suppressed, and the particles are more likely to exhibit their inherent properties. Therefore, it is assumed that the cellulose acetate particles tend to be soft and less likely to have a rough feel even after long-term storage. It is also assumed that the decrease in biodegradability is suppressed.
[0057] The external additive may be at least one selected from the group consisting of silicon-containing compound particles and metal oxide particles.
[0058] The silicon-containing compound particles refer to particles that contain silicon. The silicon-containing compound particles may be particles containing only silicon, or may be particles containing silicon and other elements.
[0059] The silicon-containing compound particles are preferably silica particles. The silica particles may be crystalline or amorphous as long as they are particles that are mainly composed of silica, i.e., SiO2. The silica particles may be particles manufactured from silicon compounds such as water glass and alkoxysilane as raw materials, or may be particles obtained by crushing quartz. As the metal oxide, oxides of metals other than silicon can be used. Examples of metal oxides include zinc oxide, magnesium oxide, iron oxide, and aluminum oxide.
[0060] The volume average particle size of the external additive is preferably from 1 nm to 100 nm, more preferably from 5 nm to 30 nm, from the viewpoint of texture (specifically, feel on the skin). The volume average particle size of the external additive is measured in the same manner as the volume average particle size of the cellulose acetate particles.
[0061] The amount of the external additive added is preferably 0.1% by mass or more and 5% by mass or less based on the total mass of the cellulose acetate particles (cellulose acetate particles to which no external additive has been added).
[0062] (Volume average particle size and large particle size distribution index GSDv) The volume average particle diameter of the cellulose acetate particles according to this embodiment is preferably more than 1 μm and not more than 100 μm, and more preferably 3 μm or more and not more than 80 μm.
[0063] By setting the volume average particle diameter of the cellulose acetate particles according to the present embodiment to be more than 1 μm and 100 μm or less, the cellulose acetate particles tend to be soft and less prone to roughness even after long-term storage. In addition, the decrease in biodegradability is also suppressed. The reason for this is presumed to be as follows. If the volume average particle size is more than 1 μm, the particles are less likely to be affected by the hard core and tend to have excellent flexibility. Therefore, even if stored for a long period of time, the particles will remain soft and less likely to feel rough. In addition, if the volume average particle size is 100 μm or less, the flexibility tends to be excellent because the flexibility can be exhibited by the water absorption of the extreme surface. Therefore, even if stored for a long period of time, it becomes soft and is unlikely to develop a rough feeling. In addition, since the surface area is appropriately increased, biodegradation that occurs from the surface tends to proceed uniformly, resulting in excellent biodegradability.
[0064] The volume average particle size of the cellulose acetate particles is measured as follows. The particle size is measured using an LS particle size distribution analyzer "Beckman Coulter LS13 320 (manufactured by Beckman Coulter)" and the cumulative particle size distribution is plotted from the smallest diameter side on a volume basis. The particle size at 50% of the cumulative distribution is determined as the volume average particle size.
[0065] <Method of producing cellulose acetate particles> The method for producing the cellulose acetate particles according to this embodiment is, for example, as follows.
[0066] - Cellulose acetate particle (mother particle) manufacturing process - (1) First, cellulose acetate is dissolved in a water-soluble organic solvent A to prepare a cellulose acylate solution A. (2) Next, the cellulose acylate solution A is added to a calcium carbonate dispersion obtained by dispersing calcium carbonate in water, and the mixture is stirred to prepare a cellulose acylate solution B. (3) Next, the cellulose acylate solution B is added to a mixed solution of carboxymethyl cellulose, the water-soluble organic solvent B, and water, and the mixture is stirred at high speed to prepare a cellulose acylate solution C. (4) Next, sodium hydroxide is added to the cellulose acylate solution C. The cellulose acylate dispersion C is heated to remove the water-soluble organic solvents A and B, and hydrochloric acid is added to form cellulose acylate particles. The cellulose acylate particles are then filtered, and the filtered cellulose acylate particles are dispersed in water to prepare a cellulose acylate particle dispersion. (5) Next, sodium hydroxide is added to the cellulose acylate particle dispersion, and the cellulose acylate particle dispersion is heated and stirred in a weak alkaline environment to saponify the cellulose acylate particles. (6) Next, hydrochloric acid is added to the cellulose acylate particle suspension with the adjusted substitution degree to adjust the pH of the suspension to near neutral (for example, in the range of 6.5 to 7), and the cellulose acetate particles are repeatedly filtered and washed with pure water. After the electrical conductivity of the filtrate reaches 10 μs / cm or less, the filtered cellulose acylate particles are dried.
[0067] In the above manufacturing process, cellulose acetate particles having the above-mentioned degree of substitution can be obtained by (A) adjusting the saponification temperature and saponification time, and (B) carrying out a treatment to increase the alkali permeability of the cellulose acylate particles during saponification (e.g., a treatment of adding water-soluble organic solvent D to a cellulose acylate particle dispersion liquid before saponification).
[0068] Here, the water-soluble organic solvent A is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate and butyl acetate. The water-soluble organic solvent B is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include methyl ethyl ketone and acetone. The water-soluble organic solvent D is a solvent in which 0.1% by mass or more to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate, butyl acetate, methyl ethyl ketone, and acetone.
[0069] The cellulose acylate particles (base particles) having the above-mentioned specific degree of substitution of the acetyl group in this embodiment are not limited to the above-mentioned manufacturing method, but may be obtained in advance by the following manufacturing method, etc., using cellulose acylate having the above-mentioned specific degree of substitution of the acetyl group. 1) A kneading and crushing method in which raw materials are kneaded, and the resulting kneaded material is crushed and classified to obtain granules; 2) A dry manufacturing method in which the shape of granules obtained by the kneading and grinding method is changed by mechanical impact force or thermal energy to obtain granules. 3) Agglomeration and coalescence method in which the raw material particle dispersion is mixed, the particles in the dispersion are aggregated, and then heat-fused to obtain granules. 4) A dissolution suspension method in which the organic solvent in which the raw materials have been dissolved is suspended in an aqueous solvent to produce granules containing each component.
[0070] - Intermediate layer and covering layer formation process - When producing cellulose acetate particles having a coating layer, it is preferable to include a step of forming a coating layer (a coating layer forming step) after the above-mentioned cellulose acetate particle (base particle) production step. Here, when the coating layer forming step is carried out, the coating layer is formed using the particles obtained in the above-mentioned cellulose acetate particle (base particle) production step as base particles.
[0071] First, an aqueous dispersion of the base particles is prepared. Before preparing the aqueous dispersion, it is preferable to wash the base particles with an acid.
[0072] Next, the aqueous dispersion in which the base particles are dispersed is mixed with an aqueous solution containing the intermediate material that constitutes the intermediate layer. As a result, for example, the hydroxyl groups of the cellulose acetate contained in the base particles react with the functional groups (amine sites, carboxyl groups, amino groups, etc.) of the intermediate material that constitutes the intermediate layer, or the hydroxyl groups form hydrogen bonds to form the intermediate layer. Then, the aqueous dispersion in which the base particles with the intermediate layer formed are dispersed is mixed with an emulsion that contains the coating material that constitutes the coating layer. As a result, the coating layer is formed. Here, when no intermediate layer is formed, the coating layer is formed by mixing an aqueous dispersion in which the base particles obtained by the above-mentioned cellulose acetate particle (base particle) manufacturing process are dispersed with an emulsion containing a compound that constitutes the coating layer.
[0073] Then, the cellulose acetate particles having a coating layer are taken out from the mixture. The cellulose acetate particles having a coating layer are taken out, for example, by filtering the mixture. The taken out cellulose acetate particles having a coating layer are preferably washed with water. This makes it possible to remove unreacted surface treatment polymer. Then, the cellulose acetate particles having a coating layer are dried to obtain the cellulose acetate particles according to the present embodiment.
[0074] -External addition process- An external additive may be added to the obtained cellulose acetate particles. The external addition step may be, for example, a process in which an external additive is added to cellulose acetate particles using a mixing mill, a V-type blender, a Henschel mixer, a Loedige mixer, or the like.
[0075] <Application> Applications of the cellulose acetate particles according to this embodiment include granular materials such as cosmetics, rolling agents, abrasives, scrubbing agents, display spacers, materials for forming beads, light diffusing particles, resin reinforcing agents, refractive index control agents, biodegradation promoters, fertilizers, water absorbing particles, toner particles, and antiblocking particles.
[0076] The cellulose acetate particles according to this embodiment are preferably used in cosmetics. Among these, the cellulose acetate particles according to the present embodiment are preferably used as a cosmetic additive. The cellulose acetate particles according to this embodiment have excellent flexibility, and therefore when used as a cosmetic additive, the cosmetic spreads well and does not easily slide on the skin when applied to the skin.
[0077] The cellulose acetate particles according to this embodiment can be used as a cosmetic additive in, for example, base makeup cosmetics (e.g., makeup base, concealer, foundation, face powder, etc.); makeup cosmetics (e.g., lipstick, gloss, lip liner, blush, eye shadow, eyeliner, mascara, eyebrow, nail, nail care cosmetics, etc.); skin care cosmetics (e.g., facial cleanser, cleanser, lotion, emulsion, serum, pack, face mask, eye and mouth care cosmetics, etc.); etc. In particular, since cosmetic additives for makeup cosmetics are required to be flexible and biodegradable, the resin particles according to this embodiment are preferably used as cosmetic additives for makeup cosmetics. EXAMPLES
[0078] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0079] <Preparing each ingredient> The following materials were prepared:
[0080] (Cellulose Acylate) CA-1: Diacetyl cellulose, Daicel Corporation "L50", number average molecular weight 58,000 CA-2: Diacetyl cellulose, Daicel Corporation "L20, number average molecular weight 47000 CA-3: Cellulose acetate propionate, Eastman Chemical "CAP482-0.5", number average molecular weight 25000
[0081] (covering material) ST-1: Calcium stearate (fatty acid metal salt), NOF Corp. "Calcium stearate vegetable oil" ST-2: Behenic acid (fatty acid), NOF "NAA-222S" ST-3: Lauroyl lysine (amino acid compound), Ajinomoto Co., Inc. "Amihope LL" ST-4: Hydrogenated lecithin (lipid compound). Nikko Chemicals Co., Ltd. "NIKKOL Lecithinol S-10 Nikko Chemicals" ST-5: Hydrogen dimethicone (silicone compound), Shin-Etsu Chemical Co., Ltd. KF-9901 ·ST-6: Perfluorooctyltriethoxysilane (fluorine-based compound) Fuluorochem "Perfluorooctyltriethoxysilane" ST-7 Hydroxypropylbispalmitamide MEA (ceramide compound), MACROCARE "Pacificos CRM" ·ST-8 Polyvinylpyrrolidone, Nippon Shokubai "PVP"
[0082] (Intermediate material) AA-1: Polyethyleneimine (polyamine compound), Nippon Shokubai Co., Ltd. "PEI-1500" AA-2: Polyquaternium 11 (Polyquaternium), BASF Japan "Rubycut PQ11AT1" AA-3: Cationic guar gum (polysaccharide), Sumitomo Pharma Food & Chemical Co., Ltd. "Labor Gum CG-M" AA-4: Polyacrylic acid, Toagosei Co., Ltd. "Jurimer AC-10H" ·AA-5: Carbomer, Nikko Chemicals "NTC-CARBOMAER 380"
[0083] EA-1: Dimethylsilylated silica, Nippon Aerosil Co., Ltd. "AEROSIL R972", volume average particle size = 16 nm EA-2: Dimethicone silicate, Nippon Aerosil Co., Ltd. "AEROSIL RY200S", volume average particle size = 16 nm
[0084] <Examples 1 to 22 and Comparative Examples 1 to 4> - Formation of mother particles - 130g of cellulose acylate of the type shown in Table 1 was dissolved in 870g of ethyl acetate. This was added to a dispersion of 50g of calcium carbonate dispersed in 500g of pure water, and stirred for 3 hours. 4g of carboxymethylcellulose and 200g of methyl ethyl ketone were added to a dispersion of 600g of pure water, and stirred for 5 minutes with a high-speed emulsifier. 10g of sodium hydroxide was added to this, and stirred at 80°C for 3 hours to remove ethyl acetate and methyl ethyl ketone. 10g of dilute hydrochloric acid was added to this to dissolve calcium carbonate. The residue was filtered and dispersed again in pure water to obtain a mother particle slurry. According to Table 1, 10g of ethyl acetate or 30g of methyl ethyl ketone (MKE) solvent was added to this mother particle slurry before saponification.
[0085] -Saponification of mother particles- 17.5 parts by mass of 20% NaOH was added to 500 parts by mass of the base particle slurry (solid concentration 10%) and stirred at the saponification temperature and time shown in Table 1 to saponify the base particles. Hydrochloric acid was added to the base particle slurry after saponification to adjust the pH to 7. Thereafter, filtration and washing were repeated until the filtrate had an electrical conductivity of 10 μs / cm or less. The obtained base particles were dried at 80° C. for 3 hours to remove the solvent. This resulted in a base particle cake.
[0086] -Surface treatment- The washed base particle cake was reslurried with ion-exchanged water to adjust the weight to 500 g, and then an intermediate material was added in an amount corresponding to the type and coating amount shown in Table 1 and mixed for 1 hour, and then a coating material was added in an amount corresponding to the type and coating amount shown in Table 1 and stirred for 24 hours. As a result, an intermediate layer and a coating layer were formed on the base particles. Thereafter, the base particles having the intermediate layer and the coating layer formed thereon were repeatedly filtered and washed until the filtrate had a filtrate conductivity of 10 μs / cm or less. After washing, the resulting cake was dried to obtain cellulose acetate particles having an intermediate layer and a coating layer. The obtained particles were mixed in an FM mixer (FM40, manufactured by Nippon Coke and Engineering Co., Ltd.) for 2000 min while maintaining the mixer temperature at 25°C. -1 The mixture was stirred at a rotation speed of 1000 for 3 hours to tan the surface of the coating layer.
[0087] -External additive treatment- Next, external additives of the types and amounts (parts) shown in Table 1 were added to 100 parts of cellulose particles having an intermediate layer and a coating layer, and mixed in a mixing mill (Wonder Crusher, manufactured by Osaka Chemical Co., Ltd.) to obtain cellulose acetate particles having external additives.
[0088] In addition, as shown by "-" in Table 1, in some examples, cellulose acetate particles were produced without performing any one or more of the formation of an intermediate layer, the formation of a coating layer, and the external addition of an external additive. In some cases, cellulose acetate particles were prepared without adding a solvent of 10 g of ethyl acetate or 30 g of methyl ethyl ketone (MKE) to the base particle slurry before saponification. In some cases, cellulose acetate particles were prepared without saponifying the base particles.
[0089] [Table 1]
[0090] <Physical property evaluation> (Particle properties) For the cellulose acetate particles obtained in each example, the following particle properties were measured according to the methods already described. Degree of substitution of acetyl groups in cellulose acetate Degree of substitution of cellulose acetate other than acetyl group Volume average particle size (referred to as "particle size" in the table)
[0091] <Cosmetics evaluation> (Making cosmetics) Among the cellulose particles of each example, the cellulose particles shown in Table 3 were used to prepare various types of cosmetics. Specifically, the procedures are as follows.
[0092] -Liquid foundation- A liquid foundation was obtained according to the formulation shown in Table 2-1 by a known method.
[0093] [Table 2-1]
[0094] -Emulsion- An emulsion was obtained by a known method according to the formulation shown in Table 2-2.
[0095] [Table 2-2]
[0096] -Loose powder- The formulation shown in Table 2-3 was mixed in a blender, pulverized in a grinder, and then sieved through a sieve with 250 μm openings to obtain a loose powder.
[0097] [Table 2-3]
[0098] -Powder foundation- According to the recipe shown in Table 2-4, the particles and powder were mixed, and a binder was separately mixed. The mixture of particles and powder was gradually added to the binder while stirring, and mixed to obtain a powder foundation.
[0099] [Table 2-4]
[0100] -Sunscreen cream- According to the recipe shown in Table 2-5, oil phase (1) was heated to 50°C and dissolved, and then oil phase (2) was added and mixed. Meanwhile, water phase (2) was dissolved and mixed. Particles and powder were added to the mixture of oil phases (1) and (2), dispersed and mixed, and then the mixture of water phases (1) and (2) was gradually added and emulsified to obtain a sunscreen cream.
[0101] [Table 2-5]
[0102] -All-in-one gel- According to the recipe shown in Table 2-6, aqueous phase (1) and aqueous phase (2) were mixed. Next, oil phase (1) was mixed and added to the mixture of aqueous phase (1) and aqueous phase (2). Oil phase (2) was heated to 70°C, and then particles were added to obtain a dispersion. The obtained dispersion was added to the mixture of aqueous phase (1), aqueous phase (2) and oil phase (1), and emulsified by stirring and mixing. A neutralizer was added to this, and the mixture was stirred and cooled to obtain an all-in-one gel.
[0103] [Table 2-6]
[0104] -Makeup base- According to the recipe shown in Table 2-7, the particles were dispersed in component A and stirred. Component B was added to this and stirred to obtain a makeup base.
[0105] [Table 2-7]
[0106] -Lipstick base- According to the recipe shown in Table 2-8, component B was heated to 60°C and mixed. Particles were dispersed in this, and component A was added. The mixture was heated and dissolved in a microwave oven, mixed, poured into a mold, and cooled. This was placed in a lipstick container to obtain a lipstick base.
[0107] [Table 2-8]
[0108] -Body powder- The formulation shown in Table 2-9 was mixed in a laboratory mixer to obtain a body powder.
[0109] [Table 2-9]
[0110] -Solid powder eyeshadow- According to the recipe shown in Table 2-10, the particles and powder were mixed, the binder was uniformly dissolved, added to the powder mixture, further mixed, and then compression molded to obtain a solid powder eye shadow.
[0111] [Table 2-10]
[0112] (evaluation) The cellulose acetate particles of each example and the resulting cosmetic product were evaluated for softness and roughness as follows.
[0113] Ten female monitors were asked to place 5 g of each sample of the cellulose acetate particles and the cosmetic on the back of their hands, spread them, and score the softness and roughness on a 10-point scale, with 10 being the best and 0 being the worst. The scores of the 10 monitors were then averaged to evaluate the results. This operation was carried out on untreated cellulose acetate particles and cosmetics (indicated as "initial" in the table) and on cellulose acetate particles and cosmetics that had been stored stationary at room temperature for three months (indicated as "stored" in the table).
[0114] [Table 3-1]
[0115] [Table 3-2]
[0116] From the above results, it is evident that the cellulose acetate particles of this Example are softer and less prone to develop roughness even after long-term storage, as compared with the cellulose acetate particles of the Comparative Example.
[0117] The present embodiment includes the following aspects. (((1))) The main component is cellulose acetate. The cellulose acetate particles have a total substitution degree of acyl groups substituted on the cellulose acetate of 0.05 or more and less than 0.70. (((2))) The cellulose acetate particles according to (((1))), wherein the acyl group of the cellulose acetate is only an acetyl group. (((3))) The cellulose acetate particles according to (((1))) or (((2))), wherein the total substitution degree of the acyl groups substituted on the cellulose acetate is 0.15 or more and 0.6 or less. (((4))) The cellulose acetate particles according to (((3))), wherein the total substitution degree of the acyl groups substituted on the cellulose acetate is 0.25 or more and 0.5 or less. (((5))) The cellulose acetate particles according to any one of (((1))) to (((4))), wherein the volume average particle size of the cellulose acetate particles is more than 1 μm and not more than 100 μm. (((6))) The cellulose acetate particles according to (((5))), wherein the volume average particle size of the cellulose acetate particles is 3 μm or more and 80 μm or less. (((7))) The base particles mainly composed of cellulose acetate; a coating layer that coats the base particles, the coating layer including at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, amino acid compounds, lipid compounds, silicone compounds, fluorine compounds, and ceramide compounds; The cellulose acetate particles according to any one of ((1))) to (((6))), having (((8))) an intermediate layer between the base particle and the coating layer, The cellulose acetate particles according to (((7))), wherein the intermediate layer contains at least one intermediate material selected from the group consisting of polyamine compounds, polyquaterniums, polysaccharide compounds, and polyacrylic acids. (((9))) The cellulose acetate particles according to any one of ((1))) to (((7))), wherein inorganic particles are externally added.
[0118] The advantages of the above aspect are as follows. According to the invention (((1))), there is provided cellulose acetate particles which are soft and less likely to feel rough even after long-term storage, compared with cellulose acetate particles which contain cellulose acetate as a main component and have a total degree of substitution of acyl groups of less than 0.05 or 0.70 or more for the cellulose acetate particles substituted with cellulose acetate. According to the invention described in (((2))), there is provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, as compared with cellulose acetate particles in which the acyl groups of the cellulose acetate have acyl groups other than acetyl groups.
[0119] According to the invention (((3))), there is provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with cellulose acetate having a total substitution degree of acyl groups less than 0.15 or more than 0.6. According to the invention related to (((4))), there is provided a cellulose acetate particle which is soft and less likely to develop a rough feeling even after long-term storage, compared with a case in which the total substitution degree of acyl groups substituted on the cellulose acetate is less than 0.2 or exceeds 0.5. According to the invention (((5))), there is provided cellulose acetate particles which are soft and less likely to feel rough even when stored for a long period of time, compared with cellulose acetate particles having a volume average particle size of 1 μm or less or 100 μm or less. According to the invention (((6))), there is provided cellulose acetate particles which are soft and less likely to feel rough even after long-term storage, compared with cellulose acetate particles having a volume average particle size of less than 3 μm or more than 80 μm.
[0120] According to the invention related to (((7))), there is provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with particles having no coating layer on base particles mainly composed of cellulose acetate. According to the invention (((8))), there are provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with particles not having an intermediate layer between the base particles and the coating layer.
[0121] According to the invention (((9))), there are provided cellulose acetate particles which are soft and less likely to develop a rough feel even after long-term storage, compared with particles not containing external inorganic particles.
Claims
1. The main component is cellulose acetate. The cellulose acetate particles have a total substitution degree of acyl groups substituted on the cellulose acetate of 0.05 or more and less than 0.
70.
2. 2. The cellulose acetate particles according to claim 1, wherein the acyl groups of the cellulose acetate are only acetyl groups.
3. 3. The cellulose acetate particles according to claim 1, wherein a total substitution degree of acyl groups substituted on the cellulose acetate is from 0.15 to 0.
6.
4. 4. The cellulose acetate particles according to claim 3, wherein the total degree of substitution of acyl groups on the cellulose acetate is from 0.25 to 0.
5.
5. 3. The cellulose acetate particles according to claim 1, wherein the volume average particle size of the cellulose acetate particles is more than 1 μm and not more than 100 μm.
6. 6. The cellulose acetate particles according to claim 5, wherein the volume average particle size of the cellulose acetate particles is 3 [mu]m or more and 80 [mu]m or less.
7. The base particles mainly composed of cellulose acetate; a coating layer that coats the base particle, the coating layer including at least one coating material selected from the group consisting of a fatty acid, a fatty acid metal salt, an amino acid compound, a lipid compound, a silicone compound, a fluorine compound, and a ceramide compound; The cellulose acetate particles according to claim 1 or 2, which have the formula:
8. an intermediate layer between the base particle and the coating layer, 8. The cellulose acetate particles according to claim 7, wherein the intermediate layer contains at least one intermediate material selected from the group consisting of polyamine compounds, polyquaterniums, polysaccharide compounds, and polyacrylic acids.
9. 3. The cellulose acetate particles according to claim 1, further comprising inorganic particles added thereto.
Citation Information
Patent Citations
Cellulose derivative fine particles, fluid dispersions of the same, solid dispersions thereof, and diagnostic drugs
WO2009123148A1
Cellulose acetate-containing particles, cosmetic composition, and method for producing cellulose acetate-containing particles
WO2020188698A1