Cement based solidification material, production method, and solidification processing method using the cement based solidification method

A cement-based solidifying material with early-strength Portland cement, gypsum, thiosulfate, and blast furnace slag addresses strength and metal leaching issues in organic and volcanic ash clay soils, ensuring robust performance across temperature variations.

JP2024141056APending Publication Date: 2024-10-10MITSUBISHI UBE CEMENT CORP

Patent Information

Application Number
JP2023052495
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing cement-based solidifying materials face challenges in improving the strength of organic soil and volcanic ash clay soil, and they often lead to the leaching of heavy metals like hexavalent chromium and halogen elements, while being susceptible to temperature fluctuations.

Method used

A cement-based solidifying material comprising early-strength Portland cement, gypsum powder, thiosulfate, and blast furnace slag powder, with specific blending ratios, is used to enhance strength and suppress metal elution, maintaining effectiveness across varying temperatures.

Benefits of technology

The material effectively solidifies organic and volcanic ash clay soils, enhancing strength and reducing heavy metal elution, while being resilient to temperature changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141056000001
    Figure 2024141056000001
  • Figure 2024141056000002
    Figure 2024141056000002
  • Figure 2024141056000003
    Figure 2024141056000003
Patent Text Reader

Abstract

To provide a cement based solidification material exhibiting sufficient intensity by solidifying organic soft ground, and ash-based foundation, and suppressing elution of heavy metal or the like from the solidified foundation.SOLUTION: A cement based solidification material comprises: high early strength portland cement; gypsum powder; thiosulfate; and blast furnace slag powder satisfying any of Grade 80, Grade 100 and Grade 120 in ASTM C989 standard. A blended ratio of the high early strength portland cement is 40 mass% or more and 85 mass% or less. A blended ratio of the gypsum powder is 2 mass% or more and 10 mass% or less, in terms of SO3. A blended ratio of the thiosulfate is 0.15 mass% or more and 12 mass% or less. A blended ratio of the blast furnace slag powder is 5 mass% or more and 60 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement-based solidification material, a method for producing the same, and a soil solidification method using the cement-based solidification material. [Background technology]

[0002] As a method for solidifying soil contained in soft ground, a method of adding a solidifying material such as a cement-based solidifying material is known. Among the soils to be solidified, organic soils such as peat with a high water content contain a lot of humic substances such as humic acid and fulvic acid as organic matter. When solidifying such soils, calcium hydroxide produced in the hydration reaction of cement reacts with the humic substances, inhibiting the hydration of cement. In addition, when solidifying volcanic ash clay soil, since the volcanic ash clay soil contains a large amount of allophane, calcium hydroxide produced in the hydration reaction of cement is adsorbed by the allophane, inhibiting the hydration of cement. Thus, there is room for improvement in the solidification of organic soils and volcanic ash clay soils using a cement-based solidifying material.

[0003] Patent Document 1 proposes a cement-based solidification material containing cement, ground granulated blast furnace slag, and powdered gypsum as a solidification material for organic soil. Patent Document 2 proposes that potassium thiosulfate or sodium sulfite be contained in a cement-based solidification material used to solidify volcanic ash clay, in order to give the clay strength and suppress the elution of hexavalent chromium. Patent Document 3 proposes a ground improvement material containing cement and a ground improvement admixture of thiosulfate for the purpose of imparting high strength to low-viscosity ground. Patent Document 4 proposes that a cement-based solidification material for organic soil contain Portland cement, ground granulated blast furnace slag, gypsum, and acid sulfate. Patent Document 5 proposes that a sulfur oxide salt be contained in a cement-based solidification material intended for volcanic ash clayey soil and organic soil. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7185794 [Patent Document 2] JP 2019-178274 A [Patent Document 3] JP 2020-158710 A [Patent Document 4] JP 2022-055749 A [Patent Document 5] JP 2023-012126 A Summary of the Invention [Problem to be solved by the invention]

[0005] Compared to ordinary clayey soil, it is difficult to improve the strength of organic soil and volcanic ash clayey soil by solidification treatment, and it is particularly difficult to improve the strength of organic soil. In addition, when solidifying soil using a cement-based solidification material, there is a problem that heavy metals such as hexavalent chromium and halogen elements such as fluorine are likely to be eluted. With conventional cement-based solidification materials, it was not easy to achieve both strength improvement by solidification treatment and prevention of elution of heavy metals, etc. Furthermore, for soil types such as sandy soil and clayey soil, within the temperature range typically observed in temperate regions such as Japan (approximately 0°C to 40°C), the higher the temperature, the higher the strength at 7 days and 28 days of age. However, with some organic soils, there was a problem of a decrease in strength at high summer temperatures exceeding 35°C. Therefore, an object of the present invention is to provide a solidification material capable of simultaneously improving strength and suppressing the elution of heavy metals, etc., a method for producing the same, and a method for solidification treatment of soil using the solidification material. Another object of the present invention is to provide a solidification material that is not easily affected by changes in the temperature environment of the soil, a method for producing the same, and a method for solidifying soil using the solidification material. [Means for solving the problem]

[0006] The present invention relates to a cement-based solidification material comprising high-early-strength Portland cement, gypsum powder, thiosulfate, and blast furnace slag powder satisfying any one of Grade 80, Grade 100, and Grade 120 of the ASTM C989 standard, The blending ratio of the high-early-strength Portland cement is 40% by mass or more and 85% by mass or less, The mixing ratio of the gypsum powder is SO 3 The converted amount is 2% by mass or more and 10% by mass or less, The blending ratio of the thiosulfate is 0.1% by mass or more and 7.5% by mass or less, The above problem is solved by providing a cement-based solidification material in which the blending ratio of the blast furnace slag powder is 5% by mass or more and 60% by mass or less.

[0007] The present invention also provides a method for solidifying soil, which comprises mixing the cement-based solidification material with soil to solidify the soil. Effect of the Invention

[0008] According to the present invention, it is possible to solidify weak organic ground or volcanic ash ground to develop sufficient strength and to suppress the elution of heavy metals and the like from the solidified ground. In addition, according to the present invention, a cement-based solidification material that is not easily affected by changes in the soil temperature environment is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The cement-based solidification material of the present invention will be described below based on preferred embodiments thereof. The cement-based solidification material of the present invention contains high-early-strength Portland cement, gypsum powder, thiosulfate, and blast furnace slag powder. Each of the materials will be described below.

[0010] High-early-strength Portland cement, which is one of the materials constituting the cement-based solidification material of the present invention, is the main material in the solidification material. As the high-early-strength Portland cement, for example, one specified in JIS R5210:2019 can be used. High-early-strength Portland cement has a Blaine specific surface area of ​​3300 cm 2 By using high early strength Portland cement as the cement component, the cement-based solidification material of the present invention can have an increased early strength. Although it is possible to use ordinary Portland cement as the cement component, in that case, a large amount of ordinary Portland cement must be used to sufficiently increase the early strength, which makes it disadvantageous in comparison with high-early-strength Portland cement.

[0011] The mixing ratio of high-early-strength Portland cement in the cement-based solidification material is preferably 40% by mass or more and 85% by mass or less relative to the cement-based solidification material, in order to improve the initial strength expression of the cement-based solidification material. From the viewpoint of making this advantage more prominent, the mixing ratio of high-early-strength Portland cement is more preferably 45% by mass or more and 85% by mass or less, and even more preferably 60% by mass or more and 70% by mass or less relative to the cement-based solidification material.

[0012] The gypsum powder, which is one of the materials constituting the cement-based solidification material of the present invention, may be, for example, anhydrous gypsum powder, hemihydrate gypsum powder, dihydrate gypsum powder, etc. From the viewpoint of effectively performing the solidification treatment of organic soil and volcanic ash clayey soil, the gypsum powder is preferably either anhydrous gypsum powder or dihydrate gypsum powder, and more preferably anhydrous gypsum powder.

[0013] The mixing ratio of gypsum powder in the cement-based solidification material is set so that all sulfur elements contained in the cement-based solidification material are converted to SO 3 It is preferable that the amount of gypsum powder is 2% by mass or more and 10% by mass or less of the cement-based solidification material in terms of effective solidification treatment of organic soil and volcanic ash clayey soil. In order to make this advantage more prominent, the mixing ratio of gypsum powder is set to 10% by mass or more. 3Expressed in converted form, the content is more preferably 3% by mass or more and 9% by mass or less, and even more preferably 4% by mass or more and 8% by mass or less, based on the cement-based solidification material.

[0014] Thiosulfate, one of the materials constituting the cement-based solidification material of the present invention, is used for the purpose of improving the strength development of soil that is the target of solidification treatment. In particular, it is used for the purpose of improving the strength development of organic soil or volcanic ash clayey soil. Furthermore, by using thiosulfate, the cement-based solidification material of the present invention exhibits high strength development during solidification treatment, regardless of changes in the temperature environment of the soil. Since organic soil has a problem of decreasing in strength under high temperatures in summer, for example, the cement-based solidification material of the present invention is extremely effective in this respect.

[0015] Other advantages of the cement-based solidification material of the present invention containing thiosulfate are as follows. When the cement in the cement-based solidification material comes into contact with the water in the soil, calcium hydroxide is produced, and the soil pH rises to a high alkaline range. For example, if the soil to be solidified is organic soil, the humic substances contained in the organic soil tend to dissolve in large amounts due to the high alkalinity. Dissolved humic substances are one of the factors that inhibit the hydration of cement, so by adding thiosulfate to the cement-based solidification material, the hardening of the cement and the reaction of the blast furnace slag are promoted, and the strength of the soil, especially its initial strength, is increased. When the soil to be solidified is volcanic ash clay, the allophane contained in the soil is one of the factors that inhibits the hydration of cement. However, by incorporating thiosulfate into the cement-based solidification material, the hardening of the cement and the reaction of the blast furnace slag are promoted, just as in the case of organic soil, and the strength of the soil, especially its initial strength, is increased.

[0016] From the above viewpoints, the mixing ratio of thiosulfate in the cement-based solidification material is preferably 0.1% by mass or more and 7.5% by mass or less with respect to the cement-based solidification material. From the viewpoint of further increasing the strength development of the soil to be solidified, particularly organic soil and volcanic ash clayey soil, the mixing ratio of thiosulfate is preferably 0.13% by mass or more and 6.4% by mass or less with respect to the cement-based solidification material.

[0017] As the thiosulfate, it is preferable to use an alkali metal salt or an alkaline earth metal salt of thiosulfate from the viewpoint of high strength development and economic efficiency. Examples of the alkali metal salt of thiosulfate include sodium thiosulfate and potassium thiosulfate. Examples of the alkaline earth metal salt of thiosulfate include magnesium thiosulfate. Thiosulfate may be anhydrous or a hydrate such as a monohydrate, tetrahydrate, pentahydrate, or heptahydrate. In this specification, the term "thiosulfate" refers to anhydrous thiosulfate unless otherwise specified.

[0018] The thiosulfate is preferably in a powder form. The average particle size of the particles constituting the thiosulfate powder is preferably 5 μm or more and 40 μm or less, and more preferably 5 μm or more and 20 μm or less. Thiosulfate particles having such an average particle size suppress the dissolution of humic substances caused by high alkali. At the same time, the supply of sulfate ions proceeds at an appropriate rate, resulting in improved strength development. For example, commercially available thiosulfate having such an average particle size can be used. Alternatively, the average particle size can be adjusted by crushing or sieving. The average particle size of the thiosulfate can be measured, for example, using a laser diffraction particle size distribution analyzer. The average particle size is the volume cumulative particle size D at 50% cumulative volume. 50 It is.

[0019] Blast furnace slag powder, one of the materials constituting the cement-based solidification material of the present invention, is made by water-cooling and pulverizing slag generated as a by-product in the blast furnaces of steelworks to a powder shape with an average particle size of about 5 μm to 20 μm. Blast furnace slag powder contains a large amount of alumina, which contributes to the alumina source for increasing the amount of ettringite produced. Therefore, by blending blast furnace slag powder with the cement-based solidification material, the strength of the soil after solidification can be improved.

[0020] The blast furnace slag powder used in the present invention advantageously satisfies any one of Grade 80, Grade 100 and Grade 120 of the ASTM C989 standard. In ASTM C989, blast furnace slag is classified into Grade 80, Grade 100 and Grade 120 according to its activity index, and any one or more of these three types can be used in the present invention. The activity index specified in ASTM C989 is a value expressed as a percentage of the compressive strength at a given age of a reference mortar made using ordinary Portland cement, the compressive strength at the same age of a test mortar made by replacing 50% of ordinary Portland cement with an admixture. Each grade is classified as follows: Grade 80: No specific regulations at 7 days old. Activity index is 75 or more at 28 days old. Grade 100: Activity index of 75 or more at 7 days of age, and activity index of 95 or more at 28 days of age. Grade 120: Activity index of 95 or more at 7 days of age, and activity index of 115 or more at 28 days of age. By using blast furnace slag powder that satisfies the above-mentioned standards, it is possible to achieve a good balance between the latent hydraulic properties of the blast furnace slag powder and the alkaline hydration reaction of the cement, thereby enabling the soil to develop high strength after solidification treatment.

[0021] In particular, from the viewpoint of solidifying organic soil and volcanic ash clayey soil to develop sufficient strength and suppressing the leaching of heavy metals from the soil after solidification treatment, the mixing ratio of blast furnace slag powder in the cement-based solidification material is preferably 5% by mass or more and 60% by mass or less, more preferably 10% by mass or more and 50% by mass or less, and even more preferably 15% by mass or more and 45% by mass or less, relative to the cement-based solidification material. In this specification, the term "heavy metal" is a broad concept that includes not only heavy metal elements in the narrow sense, such as arsenic, selenium, lead, hexavalent chromium, mercury, and cadmium, but also elements such as fluorine and boron specified in the Soil Contamination Countermeasures Act.

[0022] Blast furnace slag powder has latent hydraulic properties that harden when stimulated by alkali contained in cement, etc., and as a result, by solidifying water-containing organic soil or volcanic ash clayey soil, the strength of the soil after solidification can be improved. To make this advantage even more pronounced, the blast furnace slag powder is preferably selected so that its Blaine specific surface area is 2500 cm or more. 2 / g or more, and 2 / g or more, and 2 The Blaine specific surface area value of the blast furnace slag powder can be measured in accordance with JIS R5201:2015 "Physical testing methods for cement."

[0023] Basicity is generally known as a measure of reactivity when blast furnace slag powder is used in combination with cement. The higher the basicity of blast furnace slag powder, the greater its reactivity. Basicity is the ratio of the (CaO+MgO+Al) content of blast furnace slag powder. 2 O 3 ) / SiO 2 From the viewpoint of high reactivity, the blast furnace slag powder used in the present invention preferably has a basicity of 1.60 or more, more preferably 1.68 or more.

[0024] The cement-based solidification material of the present invention is particularly suitable for use in the solidification of organic soil or volcanic ash clay soil in a water-containing state. In particular, the cement-based solidification material of the present invention is used in the solidification of organic soil or volcanic ash clay soil with a water content of preferably 50% to 200%, more preferably 50% to 150%, and even more preferably 50% to 70%. By using the cement-based solidification material of the present invention for soil with such a water content, it is possible to achieve high strength even in soil that has previously been difficult to achieve strength. In this specification, the term "wet state" refers to a state in which the moisture content is greater than 0%. The moisture content is the ratio of the mass of water in the soil to the dry mass of the soil, expressed as a percentage. The moisture content can be measured in accordance with JIS A1203:2009.

[0025] The organic soil or volcanic ash clayey soil preferably has a wet density of 1.250 g / cm 3 More preferably, 1.400 g / cm 3 More preferably, 1.500 / cm 3 By using the cement-based solidification material of the present invention for soil having such a wet density, it is possible to make the soil develop high strength, even though it has been difficult to develop strength in the past. There is no particular upper limit for the wet density, but it is preferable to use a material with a wet density of 2,300 g / cm3 or less. 3 The wet density can be measured in accordance with JIS A1225:2020.

[0026] In this specification, "organic soil" refers to soil classified as "organic soil" in the book "Methods and Commentary on Soil Material Testing" (published November 2009 by the Geotechnical Society, pages 53-79). Specifically, organic soil includes organic soil classified as O (O), such as organic clay and organic volcanic ash soil, and highly organic soil classified as Pt, such as peat and black mud. These soils contain organic matter. Organic soil has an organic matter content of less than 20% by mass, and highly organic soil has an organic matter content of 20% by mass or more. The organic matter content can be the value of the loss on ignition, which will be described later. In this specification, unless otherwise specified, "organic soil" is a general term for these soils.

[0027] The organic soil to which the cement-based solidification material of the present invention is applied may contain humic substances in a water-containing state. Humic substances are components that constitute the organic matter contained in organic soil, and examples of such components include humic acidic components such as humic acid and fulvic acid, humin, and bitumen. The cement-based solidification material of the present invention is particularly effective in the solidification treatment of organic soil having a humus content of 5% by mass or more, and is even more effective in the solidification treatment of organic soil having a humus content of 7% by mass or more. The humus content is the ratio to the mass of the organic soil in a water-containing state. When the cement-based solidification material of the present invention is used for organic soil containing such a proportion of humus, the solidification reaction is less likely to be inhibited by the humus, making it possible to efficiently promote the solidification reaction in organic soil that was previously difficult to develop strength in, and allowing the soil to develop high strength after solidification treatment.

[0028] In particular, the cement-based solidification material of the present invention is preferably used for the solidification treatment of organic soil containing at least one selected from humic acid and fulvic acid among humic substances. In particular, the cement-based solidification material of the present invention is particularly effective in the solidification treatment of organic soil in which the ratio of the total amount of humic acid and fulvic acid is 5% by mass or more, and is even more effective in the solidification treatment of organic soil in which the ratio of the total amount of humic acid and fulvic acid is 7% by mass or more. The content of humic acid and fulvic acid is the ratio to the mass of the organic soil in a water-containing state. By solidifying such organic soil with the cement-based solidification material of the present invention, the reaction between the solidification material and components such as humic acid and fulvic acid is suppressed, so that the solidification reaction is less likely to be inhibited. As a result, it is possible to efficiently proceed with the solidification reaction for organic soil that has been difficult to develop strength in the past, and the soil after solidification treatment can develop high strength.

[0029] The organic soil to be treated with the cement-based solidification material of the present invention has an ignition loss of preferably 20% by mass or more and 90% by mass or less, more preferably 25% by mass or more and 70% by mass or less. The ignition loss of the organic soil can be measured, for example, in accordance with JIS A1226:2009.

[0030] The solidifying material of the present invention can be manufactured, for example, by mixing each material with a known mixer. The method for manufacturing the solidifying material of the present invention is a method for manufacturing a solidifying material in which the blending ratio of high-early-strength Portland cement is 40 mass% or more and 85 mass% or less, and the blending ratio of gypsum powder is SO 3 The mixing ratio of the thiosulfate is 0.1% by mass to 7.5% by mass, and the mixing ratio of the blast furnace slag powder is 5% by mass to 60% by mass. There is no particular limitation on the type of mixer, and for example, a ball mill can be used to mix and grind the materials to produce the solidification material.

[0031] According to the present invention, there is also provided a soil solidification method in which a cement-based solidification material is mixed with the soil to be treated to solidify the soil. In the mixing method in this method, the cement-based solidification material is added to the soil to be treated and mixed. The cement-based solidification material may be used as it is in a powder form, or may be dispersed in a dispersion medium such as water to form a slurry and mixed with the soil.

[0032] The amount of cement-based solidification material added can be changed as appropriate depending on the type and properties of the soil to be treated. Generally, the amount of cement-based solidification material added is about 1 m 3 The volume is preferably 20 kg or more and 1000 kg or less, more preferably 40 kg or more and 900 kg or less, and even more preferably 50 kg or more and 800 kg or less. By mixing the cement-based solidification material and the soil in such a range, ettringite can be efficiently generated in the soil, and the strength of the soil after the solidification treatment can be increased. In addition, with the improvement in strength, the elution of heavy metals such as hexavalent chromium can be reduced. The above volume of the soil to be treated is the value before the solidification treatment.

[0033] There is no particular limitation on the means for mixing the cement-based solidification material with the soil to be treated. For example, a backhoe, a backhoe equipped with a mixing bucket, a stabilizer, a self-propelled soil improvement machine, a stationary mixer, a Hobart mixer, a trencher type agitation mixer, a deep layer mixer, a power blender, a plant mixer, or other device or method commonly used in the relevant technical field can be used. EXAMPLES

[0034] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0035] [Examples 1 to 36 and Comparative Examples 1 to 7] (1) Manufacturing of cement-based solidification materials High early strength Portland cement, anhydrous gypsum powder, sodium thiosulfate and blast furnace slag powder were mixed in the ratios shown in Tables 1 to 3 below to obtain a cement-based solidification material. The details of each material are as follows. -High-early-strength Portland cement (manufactured by UBE Mitsubishi Cement) Anhydrous gypsum powder (manufactured by Kokusai Shoji Co., Ltd., Blaine specific surface area value: 4010 cm 2 / g) Sodium thiosulfate pentahydrate (Kanto Pharmaceutical Co., Ltd., crushed in a mortar and processed into powder with an average particle size of about 15 μm) Blast furnace slag powder (ASTM C989 Grade 80 product, Blaine specific surface area value: 3850 cm 2 / g, however, the blast furnace slag powder used in Comparative Examples 6 and 7 had an activity index of less than 75 at an age of 28 days, and did not meet any of the grades of ASTM C989.

[0036] (2) Soil to be solidified Organic soil A (type: sludge, humic acid content: 36.3%, wet density: 1.295g / cm 3 , water content ratio: 197.3%)

[0037] (3) Method of preparing specimens of solidified treated soil Powdered cement-based solidification material is added to organic soil A1m 3 The two were mixed for 360 seconds using a Hobart mixer at 20°C and 35°C. After that, the mixture was left to stand for 7 days in a moist state at the specified temperature.

[0038] (4) Evaluation Mortar specimens were prepared using parts of the cement-based solidification materials of the examples and the comparative examples, and the unconfined compressive strength was measured. The preparation of the specimens and the measurement of the compressive strength were performed in accordance with ASTM C109. In addition, the unconfined compressive strength of the solidified soil specimens was measured in accordance with JIS A 1216:2020. Furthermore, the amount of hexavalent chromium eluted from the specimens of the solidified treated soil was measured in accordance with Notification No. 46 of the Environment Agency.

[0039] [Examples 37 to 45 and Comparative Examples 8 and 9] Except for changing the soil to be solidified to the following organic soil B, the manufacture of the cement-based solidification material, preparation of test specimens, and evaluation were performed in the same manner as in Examples 1 to 36 and Comparative Examples 1 to 5. The preparation of test specimens was performed in environments at 20°C, 35°C, and 40°C. Organic soil B (soil quality: sludge, humic acid content: 28.1%, wet density: 1.318g / cm 3 , water content ratio: 146.2%) The results are shown in Tables 1 to 4.

[0040] [Table 1]

[0041] [Table 2]

[0042] [Table 3]

[0043] [Table 4]

[0044] From the results shown in Tables 1 to 4, it was confirmed that the strength (psi) of the mortar specimens prepared using the cement-based solidification material was sufficiently high in both the Examples and the Comparative Examples. It was also found that the solidification treatment using the cement-based solidification material of each Example achieved both improved strength of the solidified soil and suppressed the elution of hexavalent chromium, compared to the solidification treatment using the cement-based solidification material of the Comparative Examples. Therefore, it was found that the present invention can solidify organic soft ground or volcanic ash ground to develop sufficient strength and suppress the elution of heavy metals and the like from the solidified ground. Furthermore, from the results shown in Tables 1 to 3, it was confirmed that even when the specimens were prepared and cured at 35°C, the strength could be achieved at the same level as when they were prepared at 20°C. Furthermore, from the results shown in Table 4, it was confirmed that the cement-based solidification materials of each embodiment were able to suppress the decrease in strength development for organic soil B, which is more difficult to develop strength than organic soil A, even when the test specimens were prepared and cured at a maximum temperature of 40°C.

Claims

1. A cement-based solidification material comprising high-early-strength Portland cement, gypsum powder, thiosulfate, and blast furnace slag powder satisfying any one of Grade 80, Grade 100, and Grade 120 of the ASTM C989 standard, The blending ratio of the high-early-strength Portland cement is 40% by mass or more and 85% by mass or less, The mixing ratio of the gypsum powder is SO 3 In terms of mass ratio, the content is 2% by mass or more and 10% by mass or less, The blending ratio of the thiosulfate is 0.1% by mass or more and 7.5% by mass or less, A cement-based solidification material in which the blending ratio of the blast furnace slag powder is 5% by mass or more and 60% by mass or less.

2. 2. The cement-based solidification material according to claim 1, which is used for solidifying organic soil or volcanic ash clayey soil.

3. A method for producing a cement-based solidification material comprising high-early-strength Portland cement, gypsum powder, thiosulfate, and blast furnace slag powder satisfying any one of Grade 80, Grade 100, and Grade 120 of the ASTM C989 standard, The blending ratio of the high-early-strength Portland cement is 40% by mass or more and 85% by mass or less, The mixing ratio of the gypsum powder is SO 3 In terms of mass ratio, the content is 2% by mass or more and 10% by mass or less, The blending ratio of the thiosulfate is 0.1% by mass or more and 7.5% by mass or less, A method for producing a cement-based solidification material, comprising a step of mixing the blast furnace slag powder so that the blending ratio of the blast furnace slag powder is 5 mass% or more and 60 mass% or less.

4. A method for solidifying soil, comprising mixing the cement-based solidification material according to claim 1 or 2 with soil to solidify the soil.

Citation Information

Patent Citations

  • Foundation improver, improved soil and production method of improved soil

    JP2019178274A

  • Ground improvement material, cement milk, and ground improvement method

    JP2020158710A

  • Cement solidification material for organic soil, organic soil solidifying method, and method for producing cement solidification material

    JP2022055749A

  • Ground improvement method

    JP2023012126A

  • Solidification material and soil solidification treatment method

    JP7185794B1

Cited By

  • Composite soil stabilizer for water-rich low-temperature condition

    CN121362020A