Thermal transfer laminate, composite laminate, and production method
By using treated polyester films to reduce oligomer elution, the issue of clouding in resin layers containing hydrogenated modified block copolymers is resolved, enabling efficient and transparent multilayer substrate production.
Patent Information
- Application Number
- JP2023052585
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The use of a resin layer containing a hydrogenated modified block copolymer in thermal transfer laminates results in undesirable clouding and increased haze due to direct contact with untreated polyester films.
Employing a polyester film treated to reduce oligomer elution, either through low oligomerization treatment or with a barrier layer, to prevent clouding in the resin layer during heat transfer.
Suppresses clouding in the resin layer and maintains the benefits of using hydrogenated modified block copolymers while facilitating easy manufacturing of multilayer substrates with high adhesion and transparency.
Smart Images

Figure 2024141114000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermal transfer laminate, a composite laminate, methods for producing them, and a method for producing a multilayer substrate using them. [Background technology]
[0002] 2. Description of the Related Art When forming a multi-layer structure including a glass substrate and a layer other than glass (e.g., a film having an optical function, a protective film, a conductive layer, an inorganic coating, etc.) for the manufacture of optical devices such as display devices and light-emitting devices, it is known to provide a highly adhesive resin layer between these layers in order to increase the adhesion between these layers.
[0003] When forming such a multilayered product, it is convenient for the convenience of production to prepare a multilayered substrate consisting of a glass substrate and a highly adhesive resin layer provided directly on the surface of the glass substrate. For the convenience of production, it is convenient to transfer a resin layer formed separately to the surface of the glass substrate. For such transfer, it is convenient for the convenience of production to prepare a laminate for transfer in advance, which includes a release film and a resin layer provided directly thereon. Transfer using such a transfer laminate can be achieved by superposing the resin layer side of the laminate on a glass substrate, pressing the laminate under heating, and then peeling off the release film. As such a release film, a film made of a polyester film such as PET (polyethylene terephthalate) is usually used. In addition, such a heat transfer laminate can be prepared by using such a release film as a base film, providing a layer of the material of the resin layer on the base film, and forming a resin layer by drying, etc. as necessary.
[0004] Meanwhile, modified hydrogenated block copolymers are known, which are obtained by hydrogenating a block copolymer having a repeating unit derived from an aromatic vinyl compound and a repeating unit derived from a linear conjugated diene compound and further modifying it with a silane compound, etc. Modified hydrogenated block copolymers can be used for various applications, and because they have properties such as ease of handling, high storage stability, and high adhesion to glass, their use as components in laminated glass sheets has been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-78090 A [Patent Document 2] International Publication No. 2013 / 176258 Summary of the Invention [Problem to be solved by the invention]
[0006] By using a resin layer containing a hydrogenated modified block copolymer as the adhesive resin layer to be provided on the multilayer substrate described above, it is expected that a multilayer substrate having the advantageous characteristics can be easily obtained.
[0007] However, the present inventors have found that when a thermal transfer laminate is prepared using a resin layer containing a modified hydrogenated block copolymer as such an adhesive resin layer and transfer is performed, an undesirable phenomenon occurs in the resin layer after transfer, in which the film becomes cloudy and the haze increases.
[0008] Therefore, an object of the present invention is to provide a laminate for thermal transfer comprising a resin layer containing a modified hydrogenated block copolymer, in which clouding of the resin layer upon thermal transfer is suppressed. A further object of the present invention is to provide a multilayer substrate that enjoys the benefits of such a thermal transfer laminate and can be easily manufactured, and materials therefor. [Means for solving the problem]
[0009] In order to solve the above problems, the present inventors conducted a study and found that a phenomenon specific to the use of a resin containing a hydrogenated modified block copolymer as a material for the resin layer is caused by direct contact with a polyester film used as a base film, and discovered that the above problems can be solved by using a polyester film treated to reduce oligomer elution as a base film. The present invention was completed based on this finding. That is, the present invention is as follows.
[0010] <1> A thermal transfer laminate comprising a resin layer containing a modified hydrogenated block copolymer [3] and a polyester film provided in direct contact with the resin layer, The modified hydrogenated block copolymer [3] is a hydrogenated block copolymer in which an alkoxysilyl group is introduced into the hydrogenated block copolymer [2], The hydrogenated block copolymer [2] is a hydrogenated product of the block copolymer [1] in which 90% or more of all unsaturated bonds are hydrogenated, The block copolymer [1] comprises at least two polymer blocks [A] each mainly composed of a repeating unit derived from an aromatic vinyl compound, and at least one polymer block [B] mainly composed of a repeating unit derived from a chain conjugated diene compound, and a ratio (wA:wB) of a weight fraction wA of all the polymer blocks [A] in the entire block copolymer to a weight fraction wB of all the polymer blocks [B] in the entire block copolymer is 30:70 to 60:40; The heat transfer laminate, wherein the polyester film is a polyester film that has been treated to reduce oligomer elution. <2> The polyester film is a film made of a material that has been subjected to a low oligomerization treatment. <1> 2. The thermal transfer laminate according to claim 1 . <3> The polyester film is a film having a barrier layer on a surface thereof for reducing oligomer elution. <1> or <2> 2. The thermal transfer laminate according to claim 1 . <4> A composite laminate comprising an inorganic substrate, a resin layer including a hydrogenated modified block copolymer provided in direct contact with the inorganic substrate, and a polyester film provided in direct contact with the resin layer, the modified hydrogenated block copolymer is a hydrogenated block copolymer in which an alkoxysilyl group has been introduced into the hydrogenated block copolymer [2]; The hydrogenated block copolymer [2] is a hydrogenated product of the block copolymer [1] in which 90% or more of all unsaturated bonds are hydrogenated, The block copolymer [1] comprises at least two polymer blocks [A] each mainly composed of a repeating unit derived from an aromatic vinyl compound, and at least one polymer block [B] mainly composed of a repeating unit derived from a chain conjugated diene compound, and a ratio (wA:wB) of a weight fraction wA of all the polymer blocks [A] in the entire block copolymer to a weight fraction wB of all the polymer blocks [B] in the entire block copolymer is 30:70 to 60:40; A composite laminate, wherein the polyester film is a polyester film that has been treated to reduce oligomer elution. <5> The inorganic substrate is glass, ceramic, or metal; <4> 2. The composite laminate according to claim 1 . <6> <4> or <5> A method for producing the composite laminate according to claim 1, A step (X1) of preparing a thermal transfer laminate comprising the resin layer and a polyester film provided in direct contact with the resin layer; A step (X2) of stacking the thermal transfer laminate and an inorganic substrate so that the resin layer and the inorganic substrate are in direct contact with each other to form a deposit (X2); and and (X3) heat-treating the deposit (X2) to bond the resin layer and the inorganic substrate together to form a composite laminate. <7> <4> or <5> A method for producing the composite laminate according to claim 1, A step (Y1) of preparing a resin sheet containing the modified hydrogenated block copolymer; a step (Y2) of stacking the inorganic substrate, the resin sheet, and the polyester film to form a deposit (Y2); and a step (Y3) of heat-treating the deposit (Y2) to bond the polyester film, the resin sheet and the inorganic substrate together to form a composite laminate. <8> The heating temperature in the heat treatment is 130° C. or higher. <6> or <7> A method for producing the composite laminate described in claim 1. <9> The heat treatment is a heat and pressure treatment. <6> ~ <8> 13. A method for producing the composite laminate according to claim 12. <10> <6> ~ <9> 13. A method for producing a multilayer substrate, comprising: a step (Z) of peeling off the polyester film from the composite laminate obtained by the method for producing a composite laminate according to any one of the above items 1 to 7, thereby obtaining a multilayer substrate comprising the inorganic substrate and the resin layer. Effect of the Invention
[0011] According to the present invention, there is provided a laminate for thermal transfer comprising a resin layer containing a modified hydrogenated block copolymer, in which clouding of the resin layer upon thermal transfer is suppressed; and a multilayer substrate that enjoys the benefits of such a laminate for thermal transfer and can be easily manufactured, and a material therefor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0013] (Thermal transfer laminate) The thermal transfer laminate of the present invention comprises a specific resin layer and a specific polyester film provided in direct contact with the resin layer.
[0014] (Thermal transfer laminate: polyester film) The polyester film included in the thermal transfer laminate is a polyester film that has been treated to reduce oligomer elution. The polyester film is a film containing polyester as a polymer as a main component, and a specific example of such a polymer is PET (polyethylene terephthalate). The polyester film may contain any additive component, but the proportion of polyester as a polymer in the polyester film is preferably 90% by weight or more, more preferably 95% by weight or more.
[0015] Examples of films that have been treated to reduce oligomer elution include the following two types of films. (i) A film made of a low oligomerization processed material. (ii) A film having a barrier layer on its surface that reduces oligomer leaching.
[0016] The low-oligomerization treatment in (i) is a treatment for removing low molecular weight oligomers from a material before forming the material containing a polymer into a film, thereby reducing the proportion of oligomers. The oligomer here may be a cyclic trimer generated during the polymerization of polyester. When the polyester is PET (polyethylene terephthalate), a substance with a molecular weight of less than 600 may be distinguished from a polymer as an oligomer. From the viewpoint of enabling easy preparation, the lower limit of the proportion of oligomer content in the film is preferably 0.3% by weight, more preferably 0.33% by weight, and even more preferably 0.35% by weight. From the viewpoint of achieving the effects of the present invention, the upper limit of the oligomer content is preferably 0.7% by weight, more preferably 0.6% by weight, and even more preferably 0.5% by weight. Examples of PET films made of materials subjected to such treatment include heat-resistant and hydrolysis-resistant grade products (product numbers X10S and A8, etc.) of the product name "Lumirror (registered trademark)" manufactured by Toray Industries, Inc.
[0017] The barrier layer (ii) is a layer that has the property of suppressing oligomers from permeating even when subjected to heat treatment. The barrier layer is preferably a layer containing 50% by weight or more of a resin with a Tg of 90° C. or more. Examples of such resins are amino resins such as melamine, alkyd resins, polystyrene, acrylic resins, etc. The upper limit of the Tg of the resin is preferably 200° C. The lower limit of the thickness of the barrier layer is preferably 0.01 μm, more preferably 0.03 μm, and even more preferably 0.05 μm. If it is less than the above, sufficient barrier effect may not be obtained. The upper limit of the thickness of the barrier layer is preferably 10 μm, more preferably 5 μm, and even more preferably 2 μm. If it exceeds the above, the effect may become saturated. An example of a PET film having such a barrier layer is "FILMBYNA (registered trademark)" manufactured by Fujimori Kogyo Co., Ltd.
[0018] According to the inventor's findings, when the film treated to reduce oligomer elution (i) and (ii) is used as the base film constituting the thermal transfer laminate of the present invention, the clouding of the resin layer after thermal transfer can be effectively suppressed. The reason is presumed to be as follows. That is, a normal PET film product contains a large amount of oligomers with a relatively small molecular weight, and when a PET film is used as a base film and laminated with a resin layer to form a transfer laminate, such oligomers may come into contact with the surface of the resin layer. In many cases, such contact of oligomers does not cause a problem, but when the resin layer is a resin layer containing a modified block copolymer hydrogenated product and the resin layer is thermally transferred, the oligomers in contact with the surface of the resin layer act on the resin layer, causing clouding. Therefore, when the film treated to reduce oligomer elution (i) and (ii) is used as the base film constituting the thermal transfer laminate, it is possible to suppress clouding.
[0019] (Thermal transfer laminate: resin layer) The resin layer of the thermal transfer laminate contains a specific modified hydrogenated block copolymer [3].
[0020] The modified hydrogenated block copolymer [3] is a hydrogenated block copolymer [2] in which alkoxysilyl groups have been introduced, and the hydrogenated block copolymer [2] is a hydrogenated block copolymer [1] in which more than 90% of all unsaturated bonds have been hydrogenated.
[0021] The block copolymer [1] comprises at least two polymer blocks [A] mainly composed of repeating units derived from an aromatic vinyl compound, and at least one polymer block [B] mainly composed of repeating units derived from a linear conjugated diene compound, in which the ratio (wA:wB) of the weight fraction wA of all polymer blocks [A] in the entire block copolymer to the weight fraction wB of all polymer blocks [B] in the entire block copolymer is 30:70 to 60:40. However, in the present invention, each compound such as the modified block copolymer hydrogenated product [3] is not limited by its production method.
[0022] (Block copolymer[1]) The block copolymer [1] contains at least two polymer blocks [A] and at least one polymer block [B].
[0023] The polymer block [A] is mainly composed of structural units derived from aromatic vinyl compounds, and the content of structural units derived from aromatic vinyl compounds in the polymer block [A] is usually 90% by weight or more, preferably 95% by weight or more, and more preferably 99% by weight or more. In addition, components other than the structural units derived from aromatic vinyl compounds in the polymer block [A] may include structural units derived from chain conjugated dienes and / or structural units derived from other vinyl compounds, and the content is usually 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less. If the structural units derived from aromatic vinyl compounds in the polymer block [A] are too few, the heat resistance of the thermal transfer laminate of the present invention may be reduced. The multiple polymer blocks [A] may be the same or different from each other as long as they satisfy the above range.
[0024] The polymer block [B] is mainly composed of a structural unit derived from a chain conjugated diene compound, and the content of the structural unit derived from the chain conjugated diene compound in the polymer block [B] is usually 90% by weight or more, preferably 95% by weight or more, and more preferably 99% by weight or more. When the structural unit derived from the chain conjugated diene compound is in the above range, the thermal shock resistance and adhesion at low temperature of the thermal transfer laminate of the present invention are excellent. In addition, as a component other than the structural unit derived from the chain conjugated diene compound in the polymer block [B], a structural unit derived from an aromatic vinyl compound and / or a structural unit derived from another vinyl compound may be included, and the content thereof is usually 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less. When the content of the structural unit derived from an aromatic vinyl compound in the polymer block [B] increases, the flexibility of the adhesive resin layer at low temperatures may decrease, and the mechanical strength of the resin layer may decrease. When there are a plurality of polymer blocks [B], the polymer blocks [B] may be the same or different from each other as long as the above range is satisfied.
[0025] Specific examples of aromatic vinyl compounds include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, and 5-t-butyl-2-methylstyrene. Styrene is particularly preferred because of its industrial availability.
[0026] Specific examples of the chain conjugated diene compound include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. From the viewpoints of industrial availability and ease of control of the polymerization reaction, 1,3-butadiene and isoprene are particularly preferred.
[0027] Other vinyl compounds include linear vinyl compounds and cyclic vinyl compounds. Specifically, linear olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-eicosene, 4-methyl-1-pentene, and 4,6-dimethyl-1-heptene; and cyclic olefins such as vinylcyclohexane, which do not contain polar groups, are preferred in terms of hygroscopicity, linear olefins are more preferred, and ethylene and propylene are particularly preferred.
[0028] The number of polymer blocks [A] in the block copolymer [1] is usually 4 or less, preferably 3 or less, more preferably 2. When a plurality of polymer blocks [A] and / or polymer blocks [B] are present, when the weight average molecular weights of the polymer blocks [A] having the maximum and minimum weight average molecular weights are Mw(A1) and Mw(A2), respectively, and the weight average molecular weights of the polymer blocks [B] having the maximum and minimum weight average molecular weights are Mw(B1) and Mw(B2), respectively, the ratio of Mw(A1) to Mw(A2) (Mw(A1) / Mw(A2)) and the ratio of Mw(B1) to Mw(B2) (Mw(B1) / Mw(B2)) are each 2.0 or less, preferably 1.5 or less, more preferably 1.2 or less.
[0029] The block form of the block copolymer [1] may be either a chain block or a radial block, but a chain block is preferable because it has excellent mechanical strength. The most preferred forms of the block copolymer [1] are a triblock copolymer in which a polymer block [A] is bonded to both ends of a polymer block [B], and a pentablock copolymer in which a polymer block [B] is bonded to both ends of a polymer block [A], and further, a polymer block [A] is bonded to the other ends of each of the polymer blocks [B].
[0030] When the weight fraction of all polymer blocks [A] in the block copolymer [1] in the entire block copolymer is wA and the weight fraction of all polymer blocks [B] in the entire block copolymer is wB, the ratio of wA to wB (wA:wB) is 30:70 to 60:40, preferably 30:70 to 55:45, and more preferably 40:60 to 50:50. If wA is too high, the heat resistance of the hydrogenated modified block copolymer [3] used in the present invention will be high, but the flexibility will be low and the mechanical strength of the resin layer may be reduced, while if wA is too low, the heat resistance will be poor.
[0031] The molecular weight of the block copolymer [1] is, in terms of polystyrene, a weight average molecular weight (Mw) measured by GPC using tetrahydrofuran (THF) as a solvent, usually 30,000 to 200,000, preferably 40,000 to 150,000, more preferably 50,000 to 100,000. The molecular weight distribution (Mw / Mn) of the block copolymer [1] is preferably 3 or less, more preferably 2 or less, particularly preferably 1.5 or less.
[0032] The block copolymer [1] can be produced, for example, by alternately polymerizing a monomer mixture (a) containing an aromatic vinyl compound as a main component and a monomer mixture (b) containing a linear conjugated diene compound as a main component by a method such as living anionic polymerization; or by sequentially polymerizing a monomer mixture (a) containing an aromatic vinyl compound as a main component and a monomer mixture (b) containing a linear conjugated diene compound as a main component, and then coupling the ends of the polymer block [B] together using a coupling agent.
[0033] (Hydrogenated block copolymer[2]) The hydrogenated block copolymer [2] is obtained by hydrogenating the carbon-carbon unsaturated bonds derived from the conjugated diene of the block copolymer [1], and the hydrogenation rate is usually 90% or more, preferably 95% or more, and more preferably 98% or more. The hydrogenation rate of the carbon-carbon unsaturated bonds of the aromatic ring derived from the aromatic vinyl compound is preferably 20% or less, more preferably 10% or less, and particularly preferably 5% or less.
[0034] The higher the hydrogenation rate of the carbon-carbon unsaturated bonds derived from the conjugated diene, the better the weather resistance and heat degradation resistance. In addition, by suppressing the hydrogenation of the carbon-carbon unsaturated bonds of the aromatic rings derived from the aromatic vinyl compounds, the creep deformation resistance and heat degradation resistance can be maintained. The hydrogenation rate of the hydrogenated block copolymer [2] is 1 It can be determined by H-NMR measurement.
[0035] The method and reaction form for selectively hydrogenating only the carbon-carbon unsaturated bonds derived from the conjugated diene are not particularly limited, and may be carried out according to a known method, but a hydrogenation method that can increase the hydrogenation rate and cause less polymer chain scission reaction is preferred. Specific examples of such hydrogenation methods include those described in JP-A-59-133203, JP-A-1-275605, JP-A-5-222115, and JP-A-7-90017.
[0036] The hydrogenated block copolymer [2] obtained by the above-mentioned method is recovered from the reaction solution containing the hydrogenated block copolymer [2] after removing the hydrogenation catalyst and / or polymerization catalyst from the reaction solution. The form of the recovered hydrogenated block copolymer [2] is not limited, but it is usually preferable to make it into a pellet shape so that it can be easily subjected to the subsequent silylation modification reaction.
[0037] The molecular weight of the hydrogenated block copolymer [2] is the weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent, and is usually 30,000 to 300,000, preferably 40,000 to 200,000, and more preferably 50,000 to 150,000. The molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer [2] is preferably 3 or less, more preferably 2 or less, and particularly preferably 1.5 or less. When Mw and Mw / Mn are within the above ranges, the mechanical strength and heat resistance of the resin layer as an adhesive are improved.
[0038] (Modified hydrogenated block copolymer [3]) The modified hydrogenated block copolymer [3] is obtained by reacting the hydrogenated block copolymer [2] with an ethylenically unsaturated silane compound in the presence of an organic peroxide to introduce an alkoxysilyl group. The alkoxysilyl group may be bonded to the hydrogenated block copolymer [2] via a divalent organic group such as an alkylene group or an alkyleneoxycarbonylalkylene group.
[0039] The amount of alkoxysilyl groups introduced is usually 0.1 to 10 parts by weight, preferably 0.2 to 5 parts by weight, and more preferably 0.3 to 3 parts by weight, per 100 parts by weight of the hydrogenated block copolymer [2]. If the amount of alkoxysilyl groups introduced is too large, crosslinking between alkoxysilyl groups decomposed by a small amount of moisture or the like proceeds before melt molding into the desired shape, causing problems such as gel generation and reduced fluidity during melting, resulting in reduced moldability. If the amount of alkoxysilyl groups introduced is too small, it is not preferable because it causes problems such as insufficient adhesive strength with glass. The introduction of alkoxysilyl groups can be confirmed by IR spectroscopy, and the amount introduced is 1 It can be calculated using H-NMR spectrum (increase the number of accumulations when the amount introduced is small).
[0040] The ethylenically unsaturated silane compound is not particularly limited as long as it is capable of graft polymerization with the hydrogenated block copolymer [2] and introducing an alkoxysilyl group into the hydrogenated block copolymer [2]. For example, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, and the like are preferably used.
[0041] These ethylenically unsaturated silane compounds may be used alone or in combination of two or more. The amount of the ethylenically unsaturated silane compound used is usually 0.1 to 10 parts by weight, preferably 0.2 to 5 parts by weight, more preferably 0.3 to 3 parts by weight, based on 100 parts by weight of the hydrogenated block copolymer [2].
[0042] The peroxide to be used preferably has a one-minute half-life temperature of 170 to 190°C. For example, t-butylcumyl peroxide, dicumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide, di-(2-t-butylperoxyisopropyl)benzene, etc. are suitably used.
[0043] These peroxides may be used alone or in combination of two or more. The amount of the peroxide used is usually 0.05 to 2 parts by weight, preferably 0.1 to 1 part by weight, and more preferably 0.2 to 0.5 parts by weight, based on 100 parts by weight of the hydrogenated block copolymer [2].
[0044] The method of reacting the hydrogenated block copolymer [2] with the ethylenically unsaturated silane compound in the presence of a peroxide is not particularly limited, but for example, an alkoxysilyl group can be introduced by kneading in a twin-screw kneader at a desired temperature for a desired time. In the hydrogenated block copolymer [2] of the present invention, the temperature is usually 180 to 220°C, preferably 185 to 210°C, and more preferably 190 to 200°C. The heating and kneading time is usually about 0.1 to 10 minutes, preferably 0.2 to 5 minutes, and more preferably about 0.3 to 2 minutes. Continuous kneading and extrusion may be performed so that the temperature and residence time are within the above ranges.
[0045] The molecular weight of the modified hydrogenated block copolymer [3] according to the present invention is substantially the same as that of the hydrogenated block copolymer [2] used as the raw material because the amount of alkoxysilyl groups introduced is small. However, since the modified hydrogenated block copolymer [3] is reacted with an ethylenically unsaturated silane compound in the presence of a peroxide, crosslinking and cleavage reactions of the polymer also occur simultaneously, resulting in a large molecular weight distribution. The weight average molecular weight (Mw) in terms of polystyrene, measured by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent, is usually 30,000 to 300,000, preferably 40,000 to 200,000, and more preferably 50,000 to 150,000. The molecular weight distribution (Mw / Mn) is preferably 3.5 or less, more preferably 2.5 or less, and particularly preferably 2.0 or less. When Mw and Mw / Mn are within the above ranges, the mechanical strength and heat resistance of the adhesive of the thermal transfer laminate of the present invention are maintained.
[0046] The modified hydrogenated block copolymer [3] has high transparency and excellent adhesion to various materials such as glass, resin films, metals, etc., and can be usefully used as a material for layers for adhering these materials. In particular, since it can achieve both high adhesion performance and transparency, it can be particularly preferably used in optical devices such as display devices and light-emitting devices. On the other hand, as mentioned above, the hydrogenated modified block copolymer [3] has the disadvantage that it is prone to becoming cloudy when in direct contact with the polyester film used as the base film. However, by forming the thermal transfer laminate of the present invention, such a disadvantage can be reduced, and therefore the hydrogenated modified block copolymer [3] can be particularly preferably used.
[0047] (Other components of the resin layer) The resin layer constituting the thermal transfer laminate of the present invention may contain optional components in addition to the modified hydrogenated block copolymer [3]. The optional components include a light stabilizer for improving the weather resistance and heat resistance of the ultraviolet absorber, an antioxidant, a polymer other than the modified hydrogenated block copolymer [3] for improving the resin properties, and an antiblocking agent for preventing blocking of the pellets and improving the handling and workability during molding, and may be used alone or in combination of two or more kinds.
[0048] (UV absorber) In order to improve the light resistance of the modified hydrogenated block copolymer [3], an ultraviolet absorber such as a benzophenone-based ultraviolet absorber, a salicylic acid-based ultraviolet absorber, or a benzotriazole-based ultraviolet absorber may be blended into the resin layer.
[0049] Examples of the ultraviolet absorber include benzophenone-based ultraviolet absorbers such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid trihydrate, 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethyoxybenzophenone. 2-(2-hydroxybenzophenone, etc.); salicylic acid-based UV absorbers include phenyl salicylate, 4-t-butylphenyl-2-hydroxybenzoate, phenyl-2-hydroxybenzoate, 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate, hexadecyl-3,5-di-t-butyl-4-hydroxybenzoate, etc.; benzotriazole-based UV absorbers include 2-(2-hydroxy-5-methylphenyl)2H-benzotriazole, 2-(3-t-butyl 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3,5-dicumyl-2-hydroxyphenyl)-2H-benzotriazole, 5-chloro-2-(3,5-di-t-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3,5-di-t-amino 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole, 2-(2-hydroxy-4-octylphenyl)-2H-benzotriazole, 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-[(2H-benzotriazol-2-yl)phenol]];Examples of triazine-based ultraviolet absorbers include 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, and the like. Among these, 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole and 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole are preferred in terms of excellent light resistance.
[0050] The amount of the ultraviolet absorber is usually 0.05 to 2 parts by weight, preferably 0.1 to 1.5 parts by weight, and more preferably 0.2 to 1.0 parts by weight, based on 100 parts by weight of the modified hydrogenated block copolymer [3]. If the amount of the ultraviolet absorber is less than this, the effect of improving the weather resistance of the resin layer is not significant, and if it is more than this, the adhesive strength to glass and metal is likely to decrease, which is not preferable.
[0051] (Light stabilizer) In order to improve the light resistance of the modified hydrogenated block copolymer [3], a light stabilizer may be added to the resin layer. As the light stabilizer, a hindered amine light stabilizer is preferable, and examples of the light stabilizer include compounds having a 3,5-di-t-butyl-4-hydroxyphenyl group, a 2,2,6,6-tetramethylpiperidyl group, or a 1,2,2,6,6-pentamethyl-4-piperidyl group in the structure.
[0052] Among these, the following are recommended in terms of excellent weather resistance: reaction products of formaldehyde polycondensates and {2,4,6-trichloro-1,3,5-triazine·[N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexane-1,6-diyldiamine]·morpholine polymer} with formic acid, N,N'-bis(2,2,6,6-tetramethyl-4-N-methylpiperidyl)-N,N'-diformyl-alkylenediamines, and N,N'-bis(2,2,6,6-tetramethyl-4-N-methylpiperidyl)-N,N'-diformyl-alkylenediamines. N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-N,N'-diformylalkylenediamines, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-N,N'-bisalkylene fatty acid amides, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], and the like are preferred.
[0053] The amount of the hindered amine-based light resistance stabilizer is usually 0.01 to 1 part by weight, preferably 0.02 to 0.5 parts by weight, and more preferably 0.04 to 0.3 parts by weight, based on 100 parts by weight of the modified hydrogenated block copolymer [3]. If the amount of the hindered amine-based light resistance stabilizer is less than this amount, the effect of improving the weather resistance of the adhesive layer of the thermal transfer laminate is not significant, and if it is more than this amount, the adhesive strength with glass and metal is likely to decrease, which is not preferable.
[0054] (Antioxidants) In order to further improve the thermal stability of the modified hydrogenated block copolymer [3], an antioxidant may be added to the resin layer, such as a phosphorus-based antioxidant, a phenol-based antioxidant, or a sulfur-based antioxidant.
[0055] Specific examples of the antioxidant include phosphorus-based antioxidants such as monophosphite compounds such as triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl)phosphite, tris(dinonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, and 10-(3,5-di-t-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide; -tridecyl phosphite), 4,4'-isopropylidene-bis(phenyl-di-alkyl (C12-C15) phosphite), and other diphosphite compounds; 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetrakis-t-butyldibenzo[d,f][1.3.2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetrakis-t-butyldibenzo[d,f][1.3.2]dioxaphosphepine, and other compounds.
[0056] Examples of phenolic antioxidants include pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene.
[0057] Examples of sulfur-based antioxidants include compounds such as dilauryl-3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, laurylstearyl-3,3'-thiodipropionate, pentaerythritol-tetrakis-(β-lauryl-thio-propionate), 3,9-bis(2-dodecylthioethyl)-2,4,8,10-tetraoxaspiro[5,5]undecane, and the like.
[0058] The amount of the antioxidant is usually 0.02 to 1 part by weight, preferably 0.05 to 0.5 parts by weight, and more preferably 0.1 to 0.3 parts by weight, based on 100 parts by weight of the hydrogenated modified block copolymer [3]. If the amount of the antioxidant is less than this range, the effect of suppressing thermal degradation during melt molding of the hydrogenated modified block copolymer [3] is not significant, while if the amount is more than this range, the molded product becomes more hazy and the adhesive strength to glass and metals tends to decrease, which is not preferable.
[0059] (Polymers other than hydrogenated modified block copolymers [3]) The resin layer may contain polymers other than the modified hydrogenated block copolymer [3]. Examples include hydrogenated block copolymer [2], which is a precursor of the modified hydrogenated block copolymer [3] for adjusting flexibility and softening temperature; polyisobutene, hydrogenated polyisobutene, hydrogenated polyisoprene, hydrogenated 1,3-pentadiene-based petroleum resin, hydrogenated cyclopentadiene-based petroleum resin, hydrogenated styrene-indene-based petroleum resin, etc. for lowering fluidity and adhesion temperature. The amount of these polymers is usually 40 parts by weight or less per 100 parts by weight of the modified hydrogenated block copolymer [3], and the amount is appropriately selected according to the purpose of improving the resin properties.
[0060] Examples of methods for uniformly dispersing the above-mentioned optional components in the modified hydrogenated block copolymer [3] include a method in which the optional components are dissolved in a suitable solvent and added to a solution of the hydrogenated block copolymer [2], which is a precursor of the modified hydrogenated block copolymer [3], and then the solvent is removed to recover the hydrogenated block copolymer containing the optional components, which is then reacted with an ethylenically unsaturated silane compound in the presence of a peroxide; a method in which the modified hydrogenated block copolymer [3] is melted and kneaded with the optional components using a twin-screw kneader, roll, Brabender, extruder, or the like; and a method in which the above-mentioned optional components are uniformly dispersed in the hydrogenated block copolymer [2] and pelletized and the modified hydrogenated block copolymer [3] are mixed and melt-mixed to form a molded product.
[0061] (Thickness of resin layer, etc.) The thickness of the resin layer in the thermal transfer laminate of the present invention is not particularly limited and can be appropriately set to suit the desired resin layer thickness in the final product. The thickness of the resin layer is, for example, preferably 10 μm or more, more preferably 10 μm or more, and preferably 1 mm or less, more preferably 500 μm or less.
[0062] (Method of manufacturing a thermal transfer laminate) The method for producing the thermal transfer laminate of the present invention is not particularly limited, and various known production methods can be appropriately selected and used. For example, the above-mentioned resin layer material is dissolved in a solvent to prepare a resin solution, and the resin solution is applied to the surface of a polyester film as a substrate to form a coating layer of the resin solution, and the coating layer is further dried to produce the thermal transfer laminate. As such a solvent, a soluble solvent such as cyclohexane, methylcyclohexane, toluene, xylene, or tetrahydrofuran is used. The concentration of the solution is usually 5 to 40% by weight, preferably 10 to 30% by weight, from the viewpoint of the balance between productivity and adhesiveness. Alternatively, for example, the material for the resin layer described above may be formed into a sheet by melt extrusion molding or the like, and this may be laminated with a polyester film, thereby producing a thermal transfer laminate.
[0063] (Composite laminate and manufacturing method) The composite laminate of the present invention comprises an inorganic substrate, a resin layer containing a modified hydrogenated block copolymer provided in direct contact with the inorganic substrate, and a polyester film provided in direct contact with the resin layer.
[0064] Examples of inorganic substrates include glass, ceramic, or metal plate-shaped moldings.Specific examples of glass include blue plate glass, white plate glass, aluminosilicate glass, aluminoborosilicate glass, uranium glass, potash glass, silicate glass, crystallized glass, germanium glass, quartz glass, soda glass, lead glass, barium borosilicate glass, borosilicate glass, and heat-reflecting glass coated with an extremely thin metal film on its surface.
[0065] As the resin layer and the polyester film in the composite laminate of the present invention, the same materials as those described above as the components of the heat transfer laminate of the present invention can be used.
[0066] Examples of the method for producing the composite laminate include the following production method (X) or the following production method (Y).
[0067] Manufacturing method (X): A step (X1) of preparing a thermal transfer laminate comprising a resin layer and a polyester film provided in direct contact with the resin layer; A step (X2) of laminating the thermal transfer laminate and the inorganic substrate so that the resin layer and the inorganic substrate are in direct contact with each other to form a deposit (X2); and and (X3) heat-treating the deposit (X2) to bond the resin layer and the inorganic substrate to form a composite laminate.
[0068] Manufacturing method (Y): A step (Y1) of preparing a resin sheet containing a modified hydrogenated block copolymer; A step (Y2) of stacking an inorganic substrate, a resin sheet, and a polyester film to form a deposit (Y2); The production method includes a step (Y3) of heat-treating the deposit (Y2) to bond the polyester film, the resin sheet and the inorganic substrate to form a composite laminate.
[0069] The step (X1) in the manufacturing method (X) can be carried out in the same manner as the manufacturing method of the thermal transfer laminate described above. The heat treatment of the deposit (X2) in the step (X3) can be carried out at a temperature of preferably 110°C or higher, more preferably 130°C or higher. In addition, it is preferable to carry out a pressure treatment at the same time as the heat treatment to bond the resin layer and the inorganic substrate to each other. More specifically, it is preferable to carry out vacuum pressure bonding using a vacuum laminator.
[0070] The step (Y1) in the manufacturing method (Y) can be carried out in the same manner as the method for forming the sheet of the resin layer in the manufacturing method of the thermal transfer laminate described above. The heat treatment of the deposit (Y2) in the step (Y3) can be carried out at a temperature of preferably 110°C or higher, more preferably 130°C or higher, similar to the heat treatment of the deposit (X2) in the step (X3). In addition, it is preferable to carry out a pressure treatment at the same time as the heat treatment, so that the polyester film, the resin layer, and the inorganic substrate are closely attached to each other. More specifically, it is preferable to carry out vacuum pressure bonding using a vacuum laminator.
[0071] (Manufacturing method for multi-layered board) The method for producing a multilayer substrate of the present invention includes a step (Z) of peeling off the polyester film from the composite laminate obtained by the production method (X) or (Y) to obtain a multilayer substrate having an inorganic substrate and a resin layer. The multilayer substrate thus obtained can be further bonded to other layers via a resin layer and used as a component of an optical device such as a display device or a light-emitting device. Since the multilayer substrate of the present invention is obtained via the composite laminate of the present invention, it can be easily produced, can enjoy the free properties of the resin layer containing the modified block copolymer hydrogenated product (ease of handling, high storage stability, high adhesion to glass, etc.), and can be used as a multilayer substrate having a resin layer with low haze and high transparency in which the generation of cloudiness in the resin layer is suppressed. EXAMPLES
[0072] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and may be modified and practiced as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out under normal temperature and pressure conditions unless otherwise specified.
[0073] [Evaluation method] (1) Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) The molecular weights of the block copolymer and the hydrogenated block copolymer were measured as standard polystyrene equivalent values by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent at 38° C. The measuring device used was a Tosoh HLC8020GPC.
[0074] (2) Hydrogenation rate The hydrogenation rates of the main chain, side chain and aromatic ring of the hydrogenated block copolymer are 1 The H-NMR spectrum was measured and calculated.
[0075] (3) Haze Haze was measured using a Nippon Denshoku Haze Material NDH7000.
[0076] [Production Example 1] (P1-1. Preparation of block copolymers) 550 parts of dehydrated cyclohexane, 25.0 parts of dehydrated styrene, and 0.475 parts of n-dibutyl ether were placed in a reactor equipped with a stirrer and fully purged with nitrogen, and 0.68 parts of a 15% cyclohexane solution of n-butyllithium was added with stirring at 60°C to initiate polymerization. The reaction was carried out for 60 minutes at 60°C with stirring. The polymerization conversion at this point was measured by gas chromatography to be 99.5%.
[0077] Next, 50.0 parts of dehydrated isoprene was added and stirring was continued for 30 minutes. At this point, the polymerization conversion rate was 99%. Then, 25.0 parts of dehydrated styrene was further added and stirring was continued for 60 minutes. At this point, the polymerization conversion rate was almost 100%. Then, 0.096 parts of isopropyl alcohol was added to stop the reaction, and a polymer solution containing a block copolymer was obtained. The weight average molecular weight (Mw) of the obtained block copolymer was 61,600, and the molecular weight distribution (Mw / Mn) was 1.05.
[0078] (P1-2. Preparation of hydrogenated block copolymers) The polymer solution obtained in (P1-1) was transferred to a pressure-resistant reactor equipped with a stirrer. A hydrogenation catalyst solution (a solution obtained by mixing 0.042 parts of bis(cyclopentadienyl)titanium dichloride and 0.122 parts of diethylaluminum chloride in 1.0 part of toluene) was added to the polymer solution and mixed. The inside of the reactor was replaced with hydrogen gas, and hydrogen was further supplied while stirring the solution, and a hydrogenation reaction was carried out for 5 hours at a temperature of 90°C and a pressure of 1.0 MPa to obtain a hydrogenation solution containing a hydrogenated block copolymer. The weight average molecular weight (Mw) of the hydrogenated block copolymer was 62,900, and the molecular weight distribution (Mw / Mn) was 1.06.
[0079] 0.10 parts of water was added to the obtained hydride solution, and the mixture was stirred at 60°C for 60 minutes, and then cooled to 30°C or less. 1.5 parts of activated clay (product name "Galeon Earth (registered trademark)", Mizusawa Chemical Industry Co., Ltd.) and 1.5 parts of talc (product name "Microace (registered trademark)", Nippon Talc Co., Ltd.) were added to the cooled hydride solution, and insoluble matters were removed by filtration. 1.0 part of an antioxidant solution (a solution obtained by dissolving 0.1 part of a phenol-based antioxidant pentaerythrityl tetrakis [3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate] (product name "Songnox1010", Koyo Chemical Laboratory Co., Ltd.) in 0.9 parts of xylene) was added to the filtered hydride solution and dissolved. Next, the solution was filtered through a metal fiber filter (pore size 0.4 μm, manufactured by Nichidai Co., Ltd.) to remove minute solids, and then the solvent cyclohexane, xylene, and other volatile components were removed from the solution using a cylindrical concentrating dryer (product name "CONTROL", manufactured by Hitachi, Ltd.) at a temperature of 260° C. and a pressure of 0.001 MPa or less, and the solution was extruded in a molten state in the form of strands from a die directly connected to the concentrating dryer, cooled, and cut with a pelletizer to obtain 92 parts of pellets of a hydrogenated block copolymer. About 100 ppm of fine powder of ethylene bisstearic acid amide was added to the pellets as an anti-blocking agent. The weight average molecular weight (Mw) of the hydrogenated block copolymer obtained was 62,300, and the molecular weight distribution (Mw / Mn) was 1.11. The hydrogenation rate of the double bonds derived from the conjugated diene was 99%, the hydrogenation rate of the double bonds derived from the aromatic ring was less than 5%, and wA:wB=50:50.
[0080] (P1-3. Preparation of hydrogenated modified block copolymers) 2.0 parts of vinyltrimethoxysilane and 0.2 parts of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (product name "Perhexa (registered trademark) 25B", NOF Corp.) were added to 100 parts of pellets of the hydrogenated block copolymer obtained in (P1-2) to obtain a mixture. This mixture was kneaded using a twin-screw extruder (product name "TEM37B", Toshiba Machine Co., Ltd.) at a resin temperature of 200°C and a residence time of 60 to 70 seconds, extruded into a strand shape, air-cooled, and then cut with a pelletizer to obtain 97 parts of pellets of a modified hydrogenated block copolymer having an alkoxysilyl group. Approximately 100 ppm of an antiblocking agent was added to the pellets.
[0081] 10 parts of the resulting hydrogenated modified block copolymer pellets were dissolved in 100 parts of cyclohexane and then poured into 400 parts of dehydrated methanol to solidify the hydrogenated modified block copolymer, which was then filtered and vacuum dried at 25°C to isolate 9.0 parts of hydrogenated modified block copolymer crumbs. In the FT-IR spectrum, -1 Si-OCH3 group, 825cm -1 and 739 cm -1 A new absorption band due to the Si-CH2 group was observed at 1075 cm -1 , 808cm -1 , and 766 cm -1 It was observed in a different position. 1 In the H-NMR spectrum (in deuterated chloroform), an absorption band due to the protons of the methoxy group was observed at 3.6 ppm, and the peak area ratio confirmed that 1.8 parts of vinyltrimethoxysilane were bonded to 100 parts of the hydrogenated block copolymer [2]-1.
[0082] [Example 1] To 100 parts by weight of the pellets of the hydrogenated modified block copolymer obtained in Production Example 1, 0.6 parts of an ultraviolet absorber, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinuvin (registered trademark) 329, manufactured by BASF Japan Ltd.), was added and dissolved in 300 parts by weight of cyclohexane to obtain a resin solution.
[0083] A long polyethylene terephthalate (PET) film ("FILMBYNA (registered trademark) 38E-0010GCOB" manufactured by Fujimori Kogyo Co., Ltd., thickness 38 μm) was prepared as the substrate film. This film is a PET film that has an oligomer barrier layer on the surface on which the resin solution is applied, which prevents the elution of PET oligomers during heat fusion, and further has an easy-adhesion layer on the oligomer barrier layer.
[0084] A resin solution was applied to one side of the substrate film using a die coater to form a coating layer. The thickness of the coating layer was adjusted so that a resin layer having a thickness of 25 μm was obtained. The coating layer was then heated and dried at 100° C. for 10 minutes to form a resin layer having a thickness of 25 μm, and a long laminate [1-1] having a width of 600 mm and including the substrate film and the resin layer was obtained. In the laminate, the resin film was directly in contact with one side of the substrate film. The resin layer side of the obtained laminate [1] was overlapped with a glass substrate (Corning Eagle XG, thickness 0.7 mm) to form a deposit. Using a vacuum laminator (product name "PVL0202S", Nisshinbo Mechatronics), the deposit was degassed in vacuum for 5 minutes at a temperature of 130°C, and then vacuum pressure bonded for 10 minutes to obtain a laminate [1-2] having a layer structure of (glass substrate) / (resin layer) / (PET film). Furthermore, the PET film of the laminate [1-2] was peeled off to obtain a laminate [1-3] having a layer structure of (glass substrate) / (resin layer). The haze of the laminate [1-3] was measured and found to be 0.5%.
[0085] [Example 2] Except for the following changes, the same operations as in Example 1 were carried out to obtain and evaluate laminates [2-1] to [2-3] corresponding to the laminates [1-1] to [1-3]. A long polyethylene terephthalate (PET) film (Toray Industries, Inc.'s [Lumirror (registered trademark) #50-AP8], thickness 50 μm) was used as the base film instead of Fujimori Kogyo Co., Ltd.'s "FILMBYNA (registered trademark) 38E-0010GCOB". This film is a film that has a layer of polyethylene terephthalate that has been treated with low oligomers and an easy-adhesion layer provided on the surface, and the elution of oligomers from the film during heat fusion is reduced.
[0086] [Example 3] Except for the following changes, the same operations as in Example 1 were carried out to obtain and evaluate laminates [3-1] to [3-3] corresponding to the laminates [1-1] to [1-3]. Prior to the process of applying the resin solution to the base film, the surface of the base film to be coated was subjected to corona treatment. The temperature for vacuum degassing and pressure bonding was changed from 130℃ to 180℃.
[0087] [Example 4] To 100 parts by weight of the pellets of the hydrogenated modified block copolymer obtained in Production Example 1, 0.6 parts of 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinuvin (registered trademark) 329, manufactured by BASF Japan Ltd.) as an ultraviolet absorber was added and mixed evenly to obtain a mixture. This mixture was extrusion molded using a T-die type film molding machine (T-die width 600 mm) having a resin melt extruder equipped with a 40 mmφ screw under molding conditions of molten resin temperature 190 ° C., T-die temperature 190 ° C., and roll temperature 50 ° C. to obtain a sheet [4-1] having a thickness of 400 μm and a width of 450 mm. The sheet [4-1], a polyethylene terephthalate (PET) film ("FILMBYNA (registered trademark) 38E-0010GCOB" manufactured by Fujimori Kogyo Co., Ltd., thickness 38 μm), and a glass substrate ("Eagle XG" manufactured by Corning, thickness 0.7 mm) were stacked in this order to form a deposit. Using a vacuum laminator (product name "PVL0202S" manufactured by Nisshinbo Mechatronics Inc.), the deposit was degassed in vacuum for 5 minutes at a temperature of 130°C, and then vacuum pressure bonded for 10 minutes to obtain a laminate [4-2] having a layer structure of (glass) / (sheet [4-1]) / (PET film). Furthermore, the PET film of the laminate [4-2] was peeled off to obtain a laminate [4-3] having a layer structure of (glass) / (sheet [4-1]). The haze of the laminate [4-3] was measured and found to be 0.5%.
[0088] [Comparative Example 1] Except for the following changes, the same operations as in Example 1 were carried out to obtain and evaluate laminates [C1-1] to [C1-3] corresponding to the laminates [1-1] to [1-3]. Instead of Fujimori Kogyo's "FILMBYNA (registered trademark) 38E-0010GCOB," a polyethylene terephthalate (PET) film (Toyobo's "A4300," thickness 50 μm) was used as the base film. This film was a polyethylene terephthalate film that had not been treated with low oligomers, and had an easy-adhesion layer on one side. The resin solution was applied to the surface of the base film that had the easy-adhesion layer.
[0089] [Comparative Example 2] Except for the following changes, the same operations as in Example 1 were carried out to obtain and evaluate laminates [C2-1] to [C2-3] corresponding to the laminates [1-1] to [1-3]. Instead of Fujimori Kogyo's "FILMBYNA (registered trademark) 38E-0010GCOB," a polyethylene terephthalate (PET) film (Toyobo's "A4300," thickness 50 μm) was used as the base film. The resin solution was applied to the layer of the base film where the polyethylene terephthalate was exposed. The temperature for vacuum degassing and pressure bonding was changed from 130℃ to 180℃.
[0090] [Comparative Example 3] Except for the following changes, the same operations as in Example 1 were carried out to obtain laminates [C3-1] to [C3-3] corresponding to the laminates [1-1] to [1-3]. However, the resin layer and the glass substrate did not bond by pressure bonding, and the laminate [C3-2] could not be obtained.
[0091] The outline and results of the examples and comparative examples are shown in Table 1.
[0092] [Table 1]
[0093] The results of the Examples and Comparative Examples show the following. When a normal PET film (Toyobo Co., Ltd. "A4300", thickness 50 μm) is used as the base film, PET oligomers dissolve during heat and pressure bonding, the resin surface becomes cloudy, and the haze becomes 1% or more (Comparative Example 1). When the pressure bonding temperature is raised to 180°C, more PET oligomers dissolve and the haze also worsens (Comparative Example 2). Furthermore, when the pressure bonding temperature is lowered to 100°C, the resin does not melt and does not adhere to the glass (Comparative Example 3). Therefore, by using a PET film with an oligomer barrier layer on ordinary PET ("FILMBYNA (registered trademark) 38E-0010GCOB" manufactured by Fujimori Kogyo Co., Ltd., thickness 38 μm), it was possible to prevent the elution of PET oligomers during pressure bonding, and the haze was reduced to 1% or less (Example 1). Furthermore, with this PET film, the haze was 1% or less even when the pressure bonding temperature was increased to 180°C (Example 3). Furthermore, even when a PET film with reduced oligomer content was used (Toray Industries, Inc. [Lumirror (registered trademark) #50-AP8], thickness 50 μm), the elution of PET oligomers due to lamination could be avoided, and the haze was also reduced to 1% or less (Example 2). As for the manufacturing method of the laminate, the haze was 1% or less in both cases where a laminate in which a resin layer was applied to a PET base material was pressure-bonded to a glass substrate (Example 1), and where an extruded film was superimposed on a PET film and a glass substrate and pressure-bonded (Example 4).
Claims
1. A thermal transfer laminate comprising a resin layer containing a modified hydrogenated block copolymer [3] and a polyester film provided in direct contact with the resin layer, The modified hydrogenated block copolymer [3] is a hydrogenated block copolymer in which an alkoxysilyl group is introduced into the hydrogenated block copolymer [2], The hydrogenated block copolymer [2] is a hydrogenated product of the block copolymer [1] in which 90% or more of all unsaturated bonds are hydrogenated, the block copolymer [1] comprises at least two polymer blocks [A] each mainly composed of a repeating unit derived from an aromatic vinyl compound, and at least one polymer block [B] mainly composed of a repeating unit derived from a chain conjugated diene compound, wherein the ratio (wA:wB) of the weight fraction wA of all the polymer blocks [A] in the entire block copolymer to the weight fraction wB of all the polymer blocks [B] in the entire block copolymer is 30:70 to 60:40; The heat transfer laminate, wherein the polyester film is a polyester film that has been treated to reduce oligomer elution.
2. 2. The heat transfer laminate according to claim 1, wherein the polyester film is a film made of a material that has been subjected to a low oligomerization treatment.
3. 2. The heat transfer laminate according to claim 1, wherein the polyester film is a film having a barrier layer on a surface thereof for reducing elution of oligomers.
4. A composite laminate comprising an inorganic substrate, a resin layer including a hydrogenated modified block copolymer provided in direct contact with the inorganic substrate, and a polyester film provided in direct contact with the resin layer, the modified hydrogenated block copolymer is a hydrogenated block copolymer [2] in which an alkoxysilyl group has been introduced, The hydrogenated block copolymer [2] is a hydrogenated product of the block copolymer [1] in which 90% or more of all unsaturated bonds are hydrogenated, the block copolymer [1] comprises at least two polymer blocks [A] each mainly composed of a repeating unit derived from an aromatic vinyl compound, and at least one polymer block [B] mainly composed of a repeating unit derived from a chain conjugated diene compound, wherein the ratio (wA:wB) of the weight fraction wA of all the polymer blocks [A] in the entire block copolymer to the weight fraction wB of all the polymer blocks [B] in the entire block copolymer is 30:70 to 60:40; A composite laminate, wherein the polyester film is a polyester film that has been treated to reduce oligomer elution.
5. The composite laminate of claim 4 , wherein the inorganic substrate is glass, ceramic, or metal.
6. A method for producing the composite laminate according to claim 4, comprising the steps of: A step (X1) of preparing a thermal transfer laminate comprising the resin layer and a polyester film provided in direct contact with the resin layer; A step (X2) of stacking the thermal transfer laminate and an inorganic substrate so that the resin layer and the inorganic substrate are in direct contact with each other to form a deposit (X2); and and (X3) heat-treating the deposit (X2) to bond the resin layer and the inorganic substrate to form a composite laminate.
7. A method for producing the composite laminate according to claim 4, comprising the steps of: A step (Y1) of preparing a resin sheet containing the modified block copolymer hydrogenated product; a step (Y2) of stacking the inorganic substrate, the resin sheet, and the polyester film to form a deposit (Y2); and a step (Y3) of heat-treating the deposit (Y2) to bond the polyester film, the resin sheet and the inorganic substrate together to form a composite laminate.
8. The method for producing a composite laminate according to claim 6 or 7, wherein the heating temperature in the heat treatment is 130°C or higher.
9. The method for producing a composite laminate according to claim 6 or 7, wherein the heat treatment is a heat and pressure treatment.
10. A method for producing a multilayer substrate, comprising: a step (Z) of peeling off the polyester film from the composite laminate obtained by the method for producing a composite laminate according to claim 6 or 7, to obtain a multilayer substrate comprising the inorganic substrate and the resin layer.
Citation Information
Patent Citations
Glass laminate
JP2015078090A
Glass laminate, and method for using block copolymer hydrogenation product as binder for glass laminate
WO2013176258A1