Nonwoven fabric for supporting solid electrolyte and solid electrolyte sheet
A nonwoven fabric with fibrillated natural cellulose and controlled diameter polyester fibers addresses defects and adhesion issues in solid electrolytes, enhancing lithium ion conductivity and reducing production costs.
Patent Information
- Application Number
- JP2023052618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nonwoven fabrics for supporting solid electrolytes in batteries suffer from issues such as hole defects, cracks, poor adhesion, and high impedance due to the use of polyester fibers, making them unsuitable for continuous coating and increasing production costs.
A nonwoven fabric composed of fibrillated natural cellulose fibers and short synthetic resin fibers, specifically drawn and undrawn polyester fibers with controlled diameters, is used to support a solid electrolyte, with a basis weight and thickness optimized to minimize defects and improve adhesion and conductivity.
The proposed nonwoven fabric reduces hole defects, cracks, and impedance, ensuring effective adhesion and high lithium ion conductivity, facilitating continuous coating and reducing production costs.
Smart Images

Figure 2024141133000001 
Figure 2024141133000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric for supporting a solid electrolyte and a solid electrolyte sheet. Hereinafter, the term "nonwoven fabric for supporting a solid electrolyte" may be abbreviated to "support nonwoven fabric". [Background technology]
[0002] In recent years, there has been an increasing demand for large-capacity, high-performance secondary batteries for use in portable information terminals, portable electronic devices, small home power storage devices, motor-driven motorcycles, electric vehicles, hybrid electric vehicles, etc. As the range of applications expands, there is a demand for further improvements in safety and performance of secondary batteries.
[0003] As a method for ensuring the safety of lithium batteries, which are typical secondary batteries, it is effective to use a solid electrolyte instead of an organic solvent electrolyte. A solid electrolyte is non-flammable and has a higher safety than an organic solvent electrolyte. An all-solid-state lithium battery using a solid electrolyte and having a high safety includes a solid electrolyte layer, a positive electrode active material layer, a negative electrode active material layer, and a current collector bonded to the positive electrode active material layer and the negative electrode active material layer. The solid electrolyte must have lithium ion conductivity, and examples of the solid electrolyte include a sulfide-based solid electrolyte, a hydride-based solid electrolyte, and an oxide-based solid electrolyte.
[0004] For ease of handling, a sheet-type solid electrolyte layer is required. In addition, since the lithium ion conductivity of a solid electrolyte depends on the thickness of the solid electrolyte layer, the sheet-type solid electrolyte layer needs to be thin. However, it is difficult to form a thin single-layer solid electrolyte layer consisting of only a solid electrolyte.
[0005] In response to such problems, Patent Document 1 discloses a solid electrolyte sheet formed by applying a coating liquid containing a solid electrolyte to the surface of a nonwoven fabric placed on a substrate and drying the coating liquid. The document also discloses a solid electrolyte sheet that is a sheet containing a nonwoven fabric and a solid electrolyte on the surface and inside of the nonwoven fabric, the weight of the nonwoven fabric being 8 g or less per square meter, and the thickness of the nonwoven fabric being 10 μm or more and 25 μm or less. The document further discloses that the nonwoven fabric is made of flexible fibers having a fineness in the range of 0.01 to 1 dtex, and that the flexible fibers are polyethylene terephthalate (polyethylene terephthalate) fibers.
[0006] However, the nonwoven fabric disclosed in the cited document 1 has an extremely low tensile strength, making continuous coating difficult. Therefore, a coating liquid is applied to a nonwoven fabric placed on a substrate, which has problems such as low mass productivity and high production costs.
[0007] In addition, compared to a single-layer solid electrolyte layer consisting of only a solid electrolyte, a sheet containing a solid electrolyte on the surface and inside of a nonwoven fabric has a high resistance, so there is a demand for further reduction in basis weight and thickness of the nonwoven fabric. 2 At the basis weight below this level, the number of fibers constituting the nonwoven fabric itself is reduced, and the fibers adhere to the papermaking wire or papermaking blanket and fall off, forming holes. This void defect area poses the problem of being unable to support a solid electrolyte.
[0008] Furthermore, when the solid electrolyte coating solution is applied to the nonwoven fabric and then the nonwoven fabric is subjected to a heat press treatment to increase the density of the solid electrolyte layer, fine cracks due to the fibers that make up the nonwoven fabric are generated in the solid electrolyte sheet, and there is also a problem that poor adhesion occurs at the interface between the fibers that make up the nonwoven fabric and the solid electrolyte, resulting in a decrease in lithium ion conductivity.
[0009] Cited Document 2 discloses a nonwoven fabric for supporting a solid electrolyte, which supports a solid electrolyte on the surface and inside of the nonwoven fabric, comprising fibrillated heat-resistant fibers and synthetic resin staple fibers, the content of the fibrillated heat-resistant fibers being 2% by mass or more and 40% by mass or less of all fiber components contained in the nonwoven fabric for supporting a solid electrolyte, and the synthetic resin staple fibers include core-sheath type composite fibers having a resin with a melting point of 160° C. or more as a core component and a polyethylene resin as a sheath component. Cited Document 3 discloses a nonwoven fabric for supporting a solid electrolyte, which is characterized in that the nonwoven fabric A contains 60% by mass or more and 100% by mass or less of heat-fusible composite fibers having crimping and is heat-fused. As a heat-fusible conjugate fiber having crimping, a core-sheath type heat-fusible conjugate fiber is disclosed in which the core is made of a polypropylene-based polymer and the sheath is made of a polyolefin-based polymer having a lower melting point than the polypropylene-based polymer used in the core. References 2 and 3 do not disclose any means for solving hole defects, cracks caused by fibers, poor adhesion at the interface between fibers and solid electrolytes, etc. in a nonwoven fabric for supporting a solid electrolyte that mainly contains polyester fibers represented by polyethylene terephthalate fibers. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2016-31789 A [Patent Document 2] JP 2020-24860 A [Patent Document 3] International Publication No. 2021 / 200621 Brochure Summary of the Invention [Problem to be solved by the invention]
[0011] The object of the present invention is to provide a nonwoven fabric for supporting a solid electrolyte, which contains polyester fibers and has few hole defects and excellent solid electrolyte supporting ability, and also to provide a solid electrolyte sheet which has low impedance, is less susceptible to cracks caused by the fibers of the nonwoven fabric for supporting a solid electrolyte, and is less susceptible to poor adhesion at the interface between the fibers and the solid electrolyte. [Means for solving the problem]
[0012] As a result of intensive research to solve the above problems, the following invention was discovered.
[0013] (1) A nonwoven fabric for supporting a solid electrolyte, which supports a solid electrolyte on the surface and inside of the nonwoven fabric, comprises fibrillated natural cellulose fibers and synthetic resin staple fibers, the content of fibrillated natural cellulose fibers being 5% by mass or more and 20% by mass or less of all fiber components contained in the nonwoven fabric for supporting a solid electrolyte, the synthetic resin staple fibers including stretched polyester fibers having an average fiber diameter of 2.7 μm or less and unstretched polyester fibers having an average fiber diameter of 4.5 μm or less, and the basis weight of the nonwoven fabric for supporting a solid electrolyte is 3.0 g / m. 2 The nonwoven fabric for supporting a solid electrolyte is characterized in that the thickness of the nonwoven fabric is less than or equal to 100 μm.
[0014] (2) The basis weight of the nonwoven fabric for supporting a solid electrolyte is 2.0 g / m 2 More than 2.9g / m 2 The nonwoven fabric for supporting a solid electrolyte according to (1), wherein the thickness of the nonwoven fabric for supporting a solid electrolyte is 4 μm or more and less than 10 μm.
[0015] (3) A solid electrolyte sheet comprising the nonwoven fabric for supporting a solid electrolyte according to (1) or (2) above, and a solid electrolyte supported on the surface and inside of the nonwoven fabric for supporting a solid electrolyte. Effect of the Invention
[0016] According to the present invention, a nonwoven fabric for supporting a solid electrolyte containing polyester fibers can be provided that has few hole defects and is excellent in supporting the solid electrolyte, and also provides a solid electrolyte sheet that has low impedance, is less susceptible to cracks caused by the fibers of the nonwoven fabric for supporting a solid electrolyte, and is less susceptible to poor adhesion at the interface between the fibers and the solid electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An example of the structure of an all-solid-state lithium battery will be described below. The all-solid-state lithium battery in which the nonwoven fabric for supporting a solid electrolyte and the solid electrolyte sheet of the present invention can be used is not limited to this example.
[0018] An all-solid-state lithium battery is composed of a positive electrode current collecting member, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collecting member.
[0019] The positive electrode current collecting member and the negative electrode current collecting member are not particularly limited as long as they are conductive, and for example, a plate-like or foil-like member made of a metal such as copper, magnesium, titanium, iron, cobalt, nickel, zinc, aluminum, germanium, indium, or lithium, or an alloy containing these metals, can be used.
[0020] The positive electrode active material layer contains a solid electrolyte, a positive electrode active material, a positive electrode layer conductive assistant, and a positive electrode layer binder.
[0021] The solid electrolyte preferably contains at least lithium sulfide as a first component, and one or more compounds selected from the group consisting of silicon sulfide, phosphorus sulfide, and boron sulfide as a second component, and Li2S-P2S5 is particularly preferred. This sulfide-based solid electrolyte is known to have higher lithium ion conductivity than other inorganic compounds. Li2S-P2S5 may further contain sulfides such as SiS2, GeS2, and B2S3. The solid electrolyte may also contain Li3O4, halogens, halogen compounds, and the like, as appropriate.
[0022] The sulfide-based solid electrolyte can be obtained by heating Li2S and P2S5 to a melting temperature or higher, melting and mixing them in a predetermined ratio, holding the mixture for a predetermined time, and then quenching (melt quenching method). The predetermined time for the heat treatment is preferably 0.1 hours or more. Examples of the quenching method include a method in which the mixture is quenched in liquid nitrogen to obtain the desired vitrified solid electrolyte, a method in which the mixture is vacuum sealed in a glass tube, heated and melted, and then quenched with ice water or the like. The sulfide can also be obtained by Li2S-P2S5 mechanical milling method. The sulfide represented by the above Li2S-P2S5 can be a sulfide obtained by mixing Li2S and P2S5 in a molar ratio of preferably 50:50 to 80:20, more preferably 60:40 to 75:25.
[0023] In addition to sulfide-based solid electrolytes, examples of solid electrolytes include those that contain a lithium ion conductor made of an inorganic compound as an inorganic solid electrolyte. Examples of such lithium ion conductors include Li3N, LISICON, and LiPON (Li 3+y PO 4-x N x ), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), and Li2O-Al2O3-TiO2-P2O5 (LATP).
[0024] The solid electrolyte has a structure such as amorphous, glassy, or crystalline (crystallized glass). The solid electrolyte in each of the positive electrode active material layer, the negative electrode active material layer, and the electrolyte layer is composed of, for example, a mixture of an amorphous body and a crystalline body. The amorphous body can be produced by mixing the first component and the second component of the sulfide described above and processing them by a mechanical milling method. The crystalline body can be produced by firing the amorphous body, etc.
[0025] The cathode active material is not particularly limited as long as it can reversibly occlude and release lithium ions. For example, lithium cobaltate (LCO), lithium nickelate, lithium nickel cobaltate, lithium nickel cobalt aluminum oxide (hereinafter sometimes abbreviated as "NCA"), lithium nickel cobalt manganese oxide (hereinafter sometimes abbreviated as "NCM"), lithium manganate, lithium iron phosphate, nickel sulfide, copper sulfide, sulfur, iron oxide, vanadium oxide, etc. may be mentioned. These cathode active materials may be used alone or in combination of two or more.
[0026] As the cathode active material, it is particularly preferably a lithium salt of a transition metal oxide having a layered rock salt structure. Here, "layered" means a thin sheet-like shape, and "rock salt structure" means a sodium chloride-type structure which is a kind of crystal structure, and refers to a structure in which the face-centered cubic lattices formed by cations and anions are shifted from each other by 1 / 2 of the edge of the unit cell. As such a lithium salt of a transition metal oxide having a layered rock salt structure, for example, Li 1.1-x Ni y Co Z Al 1-y-z O2 (NCA) or Li 1.1-x Ni y Co z Mn 1-y-z O2 (NCM) (0 <x <0.6, 0 <y <1, 0 <z <1 and y + z <1), a lithium salt of a ternary transition metal oxide represented by this may be mentioned.
[0027] The cathode layer conductive aid is added to form a conductive network between the cathode active materials and reduce the resistance of the cathode active material layer. The conductive aid may be contained in an appropriate amount in the cathode active material layer. Examples of the cathode layer conductive aid include carbon blacks such as ketjen black and acetylene black, graphite, natural graphite, carbon nanotubes, carbon nanofibers, etc. There is no particular limitation as long as it enhances the conductivity of the cathode layer, and it may be used alone or in combination of a plurality.
[0028] Examples of the positive electrode layer binder include styrene-based thermoplastic elastomers such as SBS (styrene butadiene styrene block polymer), SEBS (styrene ethylene butadiene styrene block polymer), and styrene-styrene butadiene-styrene block polymer, SBR (styrene butadiene rubber), BR (butadiene rubber), NR (natural rubber), IR (isoprene rubber), EPDM (ethylene-propylene-diene terpolymer), NBR (nitrile rubber), CR (chloroprene rubber), and their partially hydrogenated or fully hydrogenated products, copolymers of polyacrylic acid esters, PVDF (polyvinylidene fluoride), PDF-HFP (vinylidene fluoride-hexafluoropropylene copolymer), and their carboxylic acid modified products, CM (chlorinated polyethylene), polymethacrylic acid esters, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polyimides, polyamides, polyamideimides, etc. Other examples include polystyrene, polyolefins, polyolefin-based thermoplastic elastomers, polycycloolefins, and silicone resins.
[0029] The ratio of the contents of the solid electrolyte, the positive electrode active material, the positive electrode layer conductive assistant, and the positive electrode layer binder in the positive electrode active material layer is not particularly limited. For example, it is preferable that the solid electrolyte is 3 to 50 mass%, the positive electrode active material is 45 to 95 mass%, the positive electrode layer conductive assistant is 1 to 10 mass%, and the positive electrode layer binder is 0.5 to 4 mass% relative to the total mass of the positive electrode active material layer.
[0030] The solid electrolyte layer is made of the solid electrolyte sheet of the present invention. The solid electrolyte sheet has a nonwoven fabric for supporting a solid electrolyte and a solid electrolyte supported on the surface and inside of the nonwoven fabric for supporting a solid electrolyte. The solid electrolyte may be supported together with an electrolyte binder. The solid electrolyte sheet is preferably self-supporting. Since the solid electrolyte, particularly the sulfide-based solid electrolyte, is highly reactive, the electrolyte binder is preferably a non-polar resin having no polar functional group. As the solid electrolyte, the same solid electrolyte as the above-mentioned positive electrode layer binder can be used. As the electrolyte binder, it is preferable to include the binder exemplified as the above-mentioned positive electrode layer binder.
[0031] In the solid electrolyte layer, the content ratio of the solid electrolyte and the electrolyte binder is not particularly limited. For example, it is preferable that the solid electrolyte is 95 to 99.5 mass % and the electrolyte binder is 0.5 to 5 mass % with respect to the total mass of the solid electrolyte and the electrolyte binder.
[0032] A method for producing the solid electrolyte sheet of the present invention will be described. The solid electrolyte sheet of the present invention can be produced by preparing a coating liquid containing the solid electrolyte by slurried using a medium, applying the coating liquid to a nonwoven support fabric, and drying the coating liquid. The medium is not particularly limited as long as it does not adversely affect the performance of the solid electrolyte. Examples of the medium include nonaqueous solvents. Examples of the nonaqueous solvent include nonaqueous solvents used in electrolytic solutions such as dry heptane, toluene, hexane, tetrahydrofuran (THF), N-methylpyrrolidone, acetonitrile, dimethoxyethane, and dimethyl carbonate. The moisture content of the medium is preferably 100 ppm or less, more preferably 50 ppm or less.
[0033] As an apparatus for applying the coating liquid containing a solid electrolyte to both sides or one side of the supporting nonwoven fabric, various coating apparatuses can be used, such as a gravure coater, a die coater, a lip coater, a blade coater, a curtain coater, an air knife coater, a rod coater, a roll coater, a kiss touch coater, a dip coater, etc.
[0034] After the coating liquid of the solid electrolyte is applied, it is dried to form a coating layer of the solid electrolyte. For drying, a drying device using hot air, a heater, high frequency, or the like can be used. Drying may be performed from both sides of the solid electrolyte sheet, or from one side. At this time, it is preferable to adjust the drying conditions so that the solvent in the slurry is not insufficiently removed. For example, in the case of hot air drying, it is preferable to optimally adjust the temperature and air volume. The dried solid electrolyte sheet can be used as it is, but it can also be further heat-pressed to increase its strength. For the heat press treatment, a sheet press, a roll press, or the like can be used. If the pressure during pressing is low, the thickness of the solid electrolyte layer may become non-uniform. If the pressure is high, cracks may occur in the solid electrolyte or poor adhesion may occur at the interface between the solid electrolyte layer and the constituent fibers. In addition, the supporting nonwoven fabric coated with the solid electrolyte may be damaged.
[0035] The negative electrode active material layer contains a negative electrode active material, a negative electrode layer binder, and a solid electrolyte. As the negative electrode layer binder and the solid electrolyte, the same binder and solid electrolyte as those for the positive electrode layer binder described above can be used.
[0036] Examples of the negative electrode active material include graphite-based active materials such as graphite (e.g., artificial graphite, natural graphite, a mixture of artificial graphite and natural graphite, natural graphite coated with artificial graphite, etc.), metallic lithium, silicon alloys, tin alloys, etc. The graphite powder may be at least partially coated with an inorganic compound or a metal.
[0037] The ratio of the contents of the negative electrode active material, the solid electrolyte, and the negative electrode layer binder is not particularly limited. For example, it is preferable that the negative electrode active material layer contains 0 to 40 mass% of the sulfide-based solid electrolyte, 60 to 99.5 mass% of the negative electrode active material, and 0.5 to 5 mass% of the negative electrode layer binder, relative to the total mass of the negative electrode active material layer.
[0038] Next, the nonwoven fabric for supporting a solid electrolyte of the present invention will be described.
[0039] The nonwoven fabric for supporting a solid electrolyte of the present invention is a nonwoven fabric for supporting a solid electrolyte on the surface and inside of the nonwoven fabric. The nonwoven fabric for supporting a solid electrolyte of the present invention contains fibrillated natural cellulose fibers and synthetic resin staple fibers, the content of the fibrillated natural cellulose fibers being 5% by mass or more and 20% by mass or less of the total fiber components contained in the nonwoven fabric for supporting a solid electrolyte, the synthetic resin staple fibers including stretched polyester fibers having an average fiber diameter of 2.7 μm or less and unstretched polyester fibers having an average fiber diameter of 4.5 μm or less, and the basis weight of the nonwoven fabric for supporting a solid electrolyte of the present invention is 3.0 g / m 2 It is characterized in that it is less than.
[0040] Natural cellulose fibers include wood fibers such as those from conifers and broad-leaved trees; seed hair fibers such as cotton linters, bombax cotton, and kaboku; bamboo fibers, sugarcane fibers, and jute bark fibers such as hemp, paper mulberry, and mitsumata; and leaf fibers such as Manila hemp.
[0041] Among these natural cellulose fibers, pulp-derived natural cellulose fibers such as wood fibers and seed hair fibers are preferred because they can be easily adjusted to an appropriate fiber diameter by fibrillation.The natural cellulose fibers are preferably high-purity natural cellulose fibers with low lignin and hemicellulose content and an α-cellulose content of 98 to 100% by mass.
[0042] In the present invention, the average fiber diameter of the fibrillated natural cellulose fibers is preferably 0.15 to 5 μm, more preferably 0.20 to 3 μm, even more preferably 0.25 to 2 μm, and particularly preferably 0.25 to 1 μm. The average fiber diameter of the fibrillated natural cellulose fibers is determined by measuring the diameters of 50 fibers randomly selected from the fibers constituting the nonwoven fabric through scanning electron microscope observation of the surface or cross section of the nonwoven fabric for supporting a solid electrolyte, and averaging the diameters of 50 fibers.
[0043] The length-weighted average fiber length of the fibrillated natural cellulose fibers is preferably 0.2 mm or more and 3.0 mm or less, more preferably 0.2 mm or more and 2.0 mm or less, and even more preferably 0.2 mm or more and 1.6 mm or less. By having a length-weighted average fiber length of 0.2 mm or more, it is possible to prevent an increase in the rate at which the fibers fall off the papermaking net during wet papermaking and are lost in wastewater. In addition, since the fibrillated natural cellulose fibers form a dense network with the synthetic resin short fibers, the wet paper strength is increased, and fiber loss to the papermaking net or papermaking blanket is prevented, and the occurrence of hole defects can be prevented. In addition, by having a length-weighted average fiber length of 3.0 mm or less, it is possible to prevent the fibers from becoming tangled and clumping. As a result, the solid electrolyte can be uniformly applied, making it easier to maintain a low impedance.
[0044] The length-weighted average fiber length of the fibrillated natural cellulose fibers of the present invention is a value measured using a fiber quality analyzer (FQA-360) manufactured by OpTest Equipment Inc. based on "JIS P 8226-2:2011, Pulp - Fiber length measurement method by optical automatic analysis method, Part 2: Non-polarized method". The fiber quality analyzer (FQA-360) can measure the true length (L) of the entire bent fiber and the shortest length (l) of both ends of the bent fiber for each fiber passing through the detection section. The "length-weighted average fiber length" is the length-weighted average fiber length calculated from the projected fiber length measured for the shortest length (l) of both ends of the bent fiber.
[0045] The effects of being fibrillated (beaten) include an effect that the fibrillated natural cellulose fibers form a fine structure inside the nonwoven fabric for supporting a solid electrolyte, thereby improving the retention performance of the solid electrolyte slurry and improving the supportability of the solid electrolyte. In addition, an effect that the pore size becomes smaller, making it difficult for the solid electrolyte to fall off, can be mentioned.
[0046] In the present invention, the method for producing fibrillated native cellulose fibers involves dispersing the raw material, native cellulose fibers, in a medium to prepare a dispersion. Examples of the medium include water and organic solvents, with water being preferred in terms of productivity and cost. Dispersion is performed using a Homo Disper, Three-One Motor (registered trademark), or the like. The concentration of the dispersion is preferably 0.01 to 5 mass%, more preferably 0.1 to 3 mass%. For example, a pressure difference of 20 to 200 MPa is applied to the dispersion to pass through a small-diameter orifice at a high speed, and the dispersion is then collided with a wall surface to rapidly decelerate, and the process is repeated 5 to 100 times using a high-pressure homogenizer that applies a shearing force or cutting force to the native cellulose fibers, thereby obtaining fibrillated native cellulose fibers.
[0047] In the present invention, the fibrillated natural cellulose fibers may be produced by fibrillation using only a high-pressure homogenizer, but they can also be produced by combining a high-pressure homogenizer with other devices, such as a refiner, a beater, or a grinding device.
[0048] The content of fibrillated natural cellulose fibers is 5% by mass or more and 20% by mass or less with respect to the total fiber components contained in the nonwoven fabric for supporting a solid electrolyte. It is more preferably 7% by mass or more, and even more preferably 10% by mass or more. It is more preferably 18% by mass or less, and even more preferably 15% by mass or less. If the content of fibrillated natural cellulose fibers is less than 5% by mass, the dense network with synthetic resin short fibers is insufficient, the wet paper strength is reduced, and the constituent fibers may fall off the papermaking net or papermaking blanket, causing hole defects in the supporting nonwoven fabric. On the other hand, if the content of fibrillated natural cellulose fibers exceeds 20% by mass, if the basis weight of the nonwoven fabric for supporting a solid electrolyte is low, the strength of the supporting nonwoven fabric may be insufficient, and wrinkles or tears may occur when the supporting nonwoven fabric is coated with a solid electrolyte. In addition, excessive bonding between the fibrillated natural cellulose fibers may reduce the voids in the supporting nonwoven fabric, creating areas where the solid electrolyte cannot be applied, inhibiting the conductivity of lithium ions and resulting in a deterioration in impedance.
[0049] The solid electrolyte-supporting nonwoven fabric of the present invention contains, as the synthetic resin short fibers, stretched polyester fibers having an average fiber diameter of 2.7 μm or less and unstretched polyester fibers having an average fiber diameter of 4.5 μm or less.
[0050] The content of stretched polyester fibers having an average fiber diameter of 2.7 μm or less relative to the total fiber components of the nonwoven fabric for supporting a solid electrolyte is preferably 40% by mass to 60% by mass, more preferably 45% by mass to 58% by mass, and even more preferably 50% by mass to 55% by mass. If the content of stretched polyester fibers having an average fiber diameter of 2.7 μm or less is less than 40% by mass, the amount of voids in the nonwoven fabric for supporting a solid electrolyte is reduced, and the supportability of the solid electrolyte is reduced, which may result in a reduction in the conductivity of lithium ions. On the other hand, if it exceeds 60% by mass, the content of unstretched polyester fibers is reduced, which may result in a reduction in the strength of the nonwoven fabric for supporting a solid electrolyte, which may make it difficult to apply the solid electrolyte.
[0051] The content of unstretched polyester fibers having an average fiber diameter of 4.5 μm or less relative to the total fiber components of the nonwoven fabric for supporting a solid electrolyte is preferably 35% by mass or more and 45% by mass or less, more preferably 35% by mass or more and 42% by mass or less, and even more preferably 35% by mass or more and 40% by mass or less. If the content of unstretched polyester fibers having an average fiber diameter of 4.5 μm or less is less than 35% by mass, the strength of the nonwoven fabric for supporting a solid electrolyte may decrease, making it difficult to apply the solid electrolyte. On the other hand, if the content of unstretched polyester fibers having an average fiber diameter of 4.5 μm or less exceeds 45% by mass, the supportability of the solid electrolyte may decrease, resulting in a decrease in the conductivity of lithium ions, or when the solid electrolyte sheet is subjected to a heat press treatment, fine cracks may occur inside the sheet, or poor adhesion may occur at the interface between the solid electrolyte and the fibers.
[0052] The average fiber diameter of the stretched polyester fibers is 2.7 μm or less, more preferably 2.0 μm or less, and even more preferably 1.5 μm or less. On the other hand, although there is no lower limit for the average fiber diameter of the stretched polyester fibers, it is preferably 0.7 μm or more in terms of productivity and price of the fibers and dispersibility of the fibers during the production of the supporting nonwoven fabric.
[0053] The average fiber diameter of the unstretched polyester fibers is 4.5 μm or less, more preferably 3.7 μm or less, and even more preferably 3.5 μm or less. On the other hand, although there is no lower limit for the average fiber diameter of the unstretched polyester fibers, it is preferably 3.1 μm or more in terms of fiber productivity and binder ability.
[0054] The average fiber diameter of the stretched polyester fiber and the unstretched polyester fiber is the average value of the fiber diameters of 50 fibers selected from the fibers forming the nonwoven fabric for support, whose cross sections are perpendicular or nearly perpendicular to the length direction of the fibers, from a scanning electron microscope photograph of the cross section of the nonwoven fabric for support. The synthetic resin short fibers may melt or deform due to heat or pressure. In such cases, the cross-sectional area is measured to calculate the fiber diameter in terms of a perfect circle.
[0055] The fiber length of the synthetic resin short fibers is preferably 1 to 15 mm, more preferably 2 to 10 mm, and even more preferably 3 to 5 mm. If the fiber length of the synthetic resin short fibers is shorter than 1 mm, the synthetic resin short fibers may fall off from the supporting nonwoven fabric, or the strength of the supporting nonwoven fabric may decrease, making it difficult to apply the solid electrolyte. If the fiber length of the synthetic resin short fibers is longer than 15 mm, the fibers may become tangled and clumped, and the solid electrolyte may not be pressed into the inside or surface of the supporting nonwoven fabric, or when the solid electrolyte sheet is subjected to a heat press treatment, cracks may occur inside the sheet, poor adhesion may occur at the interface between the solid electrolyte and the fibers, or the thickness may not be adjusted to a predetermined value.
[0056] In the present invention, examples of polyester include polyesters such as polyethylene terephthalate, polyethylene isophthalate, polytrimethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate. Since polyester fibers can be thinned, the basis weight of the nonwoven fabric for supporting a solid electrolyte can be reduced, and the thickness can be made thin. In addition, polyester fibers have the advantage that they are easy to form into a wet paper. The polyester fibers may be made of one type or two or more types of polyester.
[0057] The basis weight of the nonwoven fabric for carrying the solid electrolyte is 3.0 g / m 2 Less than 2.0 g / m 2 More than 2.9g / m 2 Less than 2.3 g / m is preferred. 2 More than 2.8g / m 2 Less than 2.5 g / m is more preferable. 2 ~2.7g / m 2 More preferably, the basis weight of the supporting nonwoven fabric is 2.0 g / m 2 If the basis weight is less than 3.0 g / m, the strength of the nonwoven fabric for support may decrease, which may result in poor workability when supporting the solid electrolyte, or holes may easily occur in the nonwoven fabric for support. 2 If the thickness is more than this, depending on the average fiber diameter of the constituent fibers, cracks may occur in the solid electrolyte or the lithium ion conductivity may decrease during a hot press treatment performed to improve the density of the solid electrolyte layer.
[0058] The thickness of the nonwoven fabric for supporting a solid electrolyte is preferably less than 10 μm, more preferably 9 μm or less, and even more preferably 8 μm or less. The thickness of the nonwoven fabric for supporting a solid electrolyte is preferably 4 μm or more, more preferably 5 μm or more, and even more preferably 6 μm or more. When the thickness of the nonwoven fabric for supporting a solid electrolyte is within the above range, the nonwoven fabric for supporting a solid electrolyte of the present invention can maintain the strength required for coating the slurried solid electrolyte, so that the workability in each process, including the wet papermaking process of the nonwoven fabric for supporting a solid electrolyte, is not impaired. If the thickness of the nonwoven fabric for supporting a solid electrolyte exceeds 10 μm, the lithium ion conductivity of the nonwoven fabric for supporting a solid electrolyte may decrease. In addition, the all-solid-state lithium battery may not be able to have a high capacity. If the thickness of the nonwoven fabric for supporting a solid electrolyte is less than 4 μm, the tensile strength of the nonwoven fabric for supporting a solid electrolyte may be too weak, and the nonwoven fabric for supporting a solid electrolyte may be damaged when handling the nonwoven fabric for supporting a solid electrolyte or when coating the slurried solid electrolyte, and the workability of coating may be deteriorated.
[0059] The density of the nonwoven fabric for carrying the solid electrolyte is 0.25 g / cm 3 More than 0.50g / cm 3 Less than 0.28 g / cm is preferred. 3 More than 0.46g / cm 3Less than 0.30 g / cm is more preferable. 3 More than 0.40g / cm 3 More preferably, the density of the nonwoven fabric for supporting a solid electrolyte is 0.25 g / cm 3 If the density of the nonwoven fabric for supporting a solid electrolyte is less than 0.50 g / cm, the strength of the nonwoven fabric for supporting the solid electrolyte becomes too weak, and the nonwoven fabric for supporting the solid electrolyte may be damaged during handling or coating. 3 If the thickness exceeds this range, the supporting nonwoven fabric becomes too dense, and the supporting ability of the solid electrolyte deteriorates, which may result in deterioration of the lithium ion conductivity of the solid electrolyte sheet.
[0060] The nonwoven fabric for supporting a solid electrolyte of the present invention is preferably a wet nonwoven fabric produced by a wet papermaking method. In the wet papermaking method, a papermaking slurry in which fibers are dispersed in water is made by a papermaking machine to produce a wet nonwoven fabric. Examples of the papermaking machine include a cylinder papermaking machine, a Fourdrinier papermaking machine, an inclined papermaking machine, an inclined short wire papermaking machine, and a combination of these. In the process of producing the wet nonwoven fabric, a hydroentanglement treatment may be performed as necessary. As a processing treatment of the wet nonwoven fabric, a heat treatment, a calendaring treatment, a heat calendaring treatment, etc. may be performed. EXAMPLES
[0061] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. In the examples, percentages (%) and parts are all based on mass unless otherwise specified. Furthermore, the coating amount is a dry coating amount.
[0062] Example 1 <Preparation of positive electrode structure> A LiNiCoAlO2 ternary powder as the positive electrode active material, an amorphous powder of Li2S-P2S5 (80:20 mol %) as the sulfide-based solid electrolyte, and a conductive additive consisting of carbon fiber as the positive electrode active material layer conductive material (conductive additive) were weighed out to a mass ratio of 60 / 35 / 5 and mixed using a planetary centrifugal mixer.
[0063] A dehydrated xylene solution in which SBR was dissolved as a binder was added to this mixed powder so that the SBR was 5.0% of the total mass of the mixed powder to prepare a primary mixed liquid. Furthermore, a suitable amount of dehydrated xylene was added to this primary mixed liquid to adjust the viscosity to prepare a secondary mixed liquid. Furthermore, to improve the dispersibility of the mixed powder, zirconia balls with a diameter of 5 mm were put into the secondary mixed liquid so that the space, mixed powder, and zirconia balls each occupied 1 / 3 of the total volume of the kneading container. The resulting tertiary mixed liquid was put into a planetary centrifugal mixer and stirred at 3000 rpm for 3 minutes to prepare a positive electrode coating liquid.
[0064] An aluminum foil collector with a thickness of 15 μm was prepared as a positive electrode collector, and the positive electrode collector was placed on a glass plate. The positive electrode coating liquid was applied to the aluminum foil collector using an applicator with a gap adjusted to 150 μm. The positive electrode coating liquid-applied collector was then dried on a hot plate at 60° C. for 30 minutes, and then vacuum-dried at 80° C. for 12 hours. This formed a positive electrode active material layer on the positive electrode collector. The total thickness of the positive electrode collector and the positive electrode active material layer after drying was about 165 μm. The coating amount of the positive electrode active material layer was 150 g / m 2 It was.
[0065] The positive electrode current collector coated with the positive electrode active material layer was rolled using a roll press with a roll gap of 10 μm to produce a positive electrode structure. The thickness of the positive electrode structure was about 120 μm.
[0066] <Preparation of negative electrode structure> Graphite powder (vacuum dried at 80°C for 24 hours) as the negative electrode active material and polyvinylidene fluoride (PVdF) as the binder were weighed out in a mass ratio of 95.0:5.0. These materials and an appropriate amount of N-methyl-2-pyrrolidone (NMP) were then placed in a planetary centrifugal mixer, stirred at 3000 rpm for 3 minutes, and then degassed for 1 minute to prepare a negative electrode coating solution.
[0067] A copper foil current collector having a thickness of 16 μm was prepared as the negative electrode current collector, and the negative electrode current collector was placed on a glass plate. The negative electrode coating liquid was applied to the copper foil current collector using an applicator with a gap adjusted to 150 μm. The sheet coated with the negative electrode coating liquid was stored in a dryer heated to 80° C. and dried for 15 minutes. The dried current collector was further vacuum-dried at 80° C. for 24 hours. The negative electrode current collector coated with the negative electrode active material was rolled using a roll press with a roll gap of 10 μm to prepare a negative electrode structure. The thickness of the negative electrode structure was about 140 μm. The coating amount of the negative electrode active material layer was 150 g / m 2 It was.
[0068] <Preparation of slurried solid electrolyte> A first mixture was prepared by adding a xylene solution of SBR (electrolyte layer binder) to Li2S-P2S5 (80:20 mol%) amorphous powder so that SBR was 1% relative to the amorphous powder. A second mixture was prepared by adding a xylene solution of NBR (electrolyte layer binder) to this first mixture so that NBR was 0.5% relative to the amorphous powder. A third mixture was prepared by adding an appropriate amount of dehydrated xylene to this second mixture to adjust the viscosity. In addition, in order to improve the dispersibility of the powder, the third mixture and zirconia balls with a diameter of 5 mm were put into the kneading vessel so that the space, the mixture, and the zirconia balls each occupied 1 / 3 of the total volume of the kneading vessel. The fourth mixture prepared in this way was put into a planetary centrifugal mixer and stirred at 3000 rpm for 3 minutes to prepare a slurried solid electrolyte.
[0069] <Preparation of supporting nonwoven fabric> Cotton linter pulp was dispersed in water to a concentration of 2%, and the dispersion was repeatedly processed 10 times using a double disc refiner while gradually narrowing the clearance. It was then repeatedly processed 20 times using a high-pressure homogenizer under conditions of 49 MPa, yielding fibrillated natural cellulose fibers with an average fiber diameter of 0.3 μm and a length-weighted average fiber length of 0.22 mm.
[0070] 50 parts of stretched polyester staple fibers with an average fiber diameter of 2.7 μm, 40 parts of unstretched polyester staple fibers with an average fiber diameter of 4.5 μm, and 10 parts of fibrillated natural cellulose fibers were dispersed in water using a pulper to prepare a uniform papermaking slurry with a concentration of 0.5%. The papermaking slurry was made by using a cylinder-type papermaking machine to obtain a wet paper web. The wet paper web was dried by a cylinder dryer with a surface temperature of 135°C to obtain a sheet. The sheet was subjected to a thermal calendaring treatment using a thermal calendaring device with one roll being a chrome-plated steel roll and the other being a resin roll with a Shore hardness of D92, and the surface temperature of the steel roll was 200°C, resulting in a basis weight of 2.9 g / m. 2 A nonwoven fabric for supporting a solid electrolyte having a thickness of 9.4 μm was prepared.
[0071] <Preparation of solid electrolyte sheet> The nonwoven fabric for supporting a solid electrolyte of Example 1 is continuously guided from above through a guide roller into a coating tank containing the above-mentioned slurried solid electrolyte. In the coating tank, the nonwoven fabric is immersed in the slurried solid electrolyte, and in order to impregnate the inside of the nonwoven fabric for supporting with the solid electrolyte, the nonwoven fabric is nipped by a roll press in the coating tank and pulled up through a guide roller. Thereafter, both sides of the nonwoven fabric for supporting are smoothed by applying a plastic blade, and excess slurry is scraped off. The nonwoven fabric for supporting impregnated with the solid electrolyte is guided to a hot air dryer and dried from both sides to produce a solid electrolyte sheet having a thickness of 180 μm.
[0072] Example 2 A 2.7 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 60 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 35 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 5 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 8.0 μm was then produced. Next, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0073] Example 3 A 2.5 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 40 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 20 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 7.8 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0074] Example 4 A 2.3 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 50 parts of oriented polyester staple fibers having an average fiber diameter of 2.2 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 3.7 μm, and 10 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 5.6 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0075] Example 5 A 2.0 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 50 parts of oriented polyester staple fibers having an average fiber diameter of 1.0 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 3.7 μm, and 10 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 4.4 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0076] Example 6 In the same manner as in Example 4, a basis weight of 1.9 g / m 2 A solid electrolyte supporting nonwoven fabric having a thickness of 5.1 μm was then produced. Next, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0077] Example 7 In the same manner as in Example 1, a basis weight of 2.8 g / m 2 A solid electrolyte supporting nonwoven fabric having a thickness of 12.5 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0078] Example 8 In the same manner as in Example 1, a basis weight of 2.5 g / m 2A solid electrolyte supporting nonwoven fabric having a thickness of 3.8 μm was then produced. Next, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0079] Comparative Example 1 A 2.8 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 56 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 4 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.3 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0080] Comparative Example 2 A 2.7 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 38 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 22 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.2 μm was then produced. Next, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0081] Comparative Example 3 A 2.7 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 50 parts of oriented polyester staple fibers having an average fiber diameter of 3.2 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 10 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.5 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0082] Comparative Example 4 A 2.9 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 50 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 5.5 μm, and 10 parts of fibrillated natural cellulose fibers were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.8 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0083] Comparative Example 5 In the same manner as in Example 1, a basis weight of 3.2 g / m 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.5 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0084] Comparative Example 6 A fiber having a basis weight of 2.8 g / m was prepared in the same manner as in Example 1, except that 50 parts of stretched polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unstretched polyester staple fibers having an average fiber diameter of 4.5 μm, and 10 parts of fibrillated solvent-spun cellulose fibers having a fiber length of 4 mm and a fiber diameter of 1.25 dtex (average fiber diameter 9.5 μm) were used, and the fibers were beaten in a refiner until the maximum fiber diameter of the stem portion became 5.2 μm. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.8 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0085] Comparative Example 7 A 2.7 g / m2 spunbonded woven fabric was prepared in the same manner as in Example 1, except that 50 parts of oriented polyester staple fibers having an average fiber diameter of 2.7 μm, 40 parts of unoriented polyester staple fibers having an average fiber diameter of 4.5 μm, and 10 parts of a pulp-like material of para-based wholly aromatic polyamide fibers (Twaron (registered trademark) 1094 manufactured by Teijin Limited) were used. 2 A solid electrolyte supporting nonwoven fabric having a thickness of 9.5 μm was then produced. Then, a solid electrolyte sheet was produced in the same manner as in Example 1.
[0086] The solid electrolyte-supporting nonwoven fabrics and solid electrolyte sheets of the Examples and Comparative Examples were measured and evaluated for the following physical properties. The results are shown in Tables 1 and 2.
[0087] <Nonwoven fabric basis weight> The basis weight of the supporting nonwoven fabric was measured in accordance with JIS P8124:2011.
[0088] <Thickness of nonwoven fabric> The thickness was measured under a load of 5N using an outside micrometer specified in JIS B7502:2016.
[0089] <Presence or absence of holes in nonwoven fabric for supporting solid electrolyte> The nonwoven fabrics for supporting a solid electrolyte obtained in the examples and comparative examples were inspected for the presence or absence of holes over a distance of 50 m using a transmission type flaw detector. If the nonwoven fabric has a hole, the solid electrolyte at the hole falls off, causing a hole, which can cause a short circuit in the all-solid-state lithium battery. Therefore, it is necessary to remove the hole from the nonwoven fabric for supporting a solid electrolyte, which significantly reduces the productivity of the nonwoven fabric for supporting a solid electrolyte.
[0090] <Solid electrolyte support> In producing a solid electrolyte sheet, the nonwoven fabric for supporting a solid electrolyte was continuously immersed in a slurried solid electrolyte, nipped with a press roll, and dried. The nonwoven fabric for supporting the solid electrolyte was visually observed for shrinkage in the width direction and wrinkles during running due to inability to withstand the tension, and evaluated according to the following criteria.
[0091] ◯: The supporting nonwoven fabric did not shrink in width, wrinkle, or break during transportation, and the solid electrolyte was supported inside and on the surface of the supporting nonwoven fabric. Δ: The supporting nonwoven fabric may shrink slightly in width or wrinkle during transportation, but the solid electrolyte is supported inside or on the surface of the supporting nonwoven fabric. ×: The supporting nonwoven fabric may shrink in width, wrinkle, or break during transportation, or the solid electrolyte may not be supported sufficiently inside the supporting nonwoven fabric.
[0092] <Preparation of all-solid-state lithium batteries> The above-mentioned negative electrode structure was punched out to 88 mm x 58 mm, the positive electrode structure to 87 mm x 57 mm, and the solid electrolyte sheet to 92 mm x 62 mm with a Thomson blade. After laminating the negative electrode structure / solid electrolyte sheet / positive electrode structure, they were bonded together by a dry lamination method using a hot roll press with a roll gap of 50 μm to produce a single cell (single battery) of an all-solid-state lithium battery.
[0093] <Cracks and poor adhesion in the solid electrolyte layer> The cross section of the fabricated all-solid-state lithium battery was observed using a scanning electron microscope to evaluate whether there were cracks in the solid electrolyte layer or poor adhesion between the fibers constituting the supporting nonwoven fabric and the solid electrolyte, using the following criteria: If there are even small spaces in the solid electrolyte layer due to cracks or poor adhesion with the fibers, this can cause a decrease in the conductivity of lithium ions.
[0094] ◯: The solid electrolyte layer has no cracks or poor adhesion to the fibers. Δ: Cracks in the solid electrolyte layer or slight poor adhesion to the fibers are observed. ×: Cracks or poor adhesion to the fibers are observed in the solid electrolyte layer.
[0095] <Impedance of all-solid-state lithium batteries> The single cell of the all-solid-state lithium battery thus produced was placed in an aluminum laminate film with terminals attached, evacuated with a vacuum machine, heat sealed, and packed. The obtained test cell was subjected to a current of 0.1 mA / cm under an environment of 25°C. 2 The battery was charged to 4.0 V at a current density of (0.1 C), and the impedance was measured at an AC frequency of 0.1 Hz to 1 MHz using an LCZ meter (manufactured by Yokogawa Hewlett-Packard Co.). When the impedance of an all-solid-state lithium battery is high, it indicates that the conductivity of lithium ions is low.
[0096] [Table 1]
[0097] [Table 2]
[0098] As shown in Table 1, the nonwoven fabrics for supporting a solid electrolyte produced in Examples 1 to 8 contained fibrillated natural cellulose fibers and synthetic resin staple fibers, the content of fibrillated natural cellulose fibers was 5% by mass or more and 20% by mass or less of the total fiber components contained in the nonwoven fabric for supporting a solid electrolyte, the synthetic resin staple fibers included stretched polyester fibers having an average fiber diameter of 2.7 μm or less and unstretched polyester fibers having an average fiber diameter of 4.5 μm or less, and the basis weight of the nonwoven fabric for supporting a solid electrolyte was 3.0 g / m. 2 The solid electrolyte-supporting nonwoven fabrics of Examples 1 to 5 have a density of less than 3.0 g / m 2 Although the nonwoven fabric had a basis weight of less than 1000 g, the supporting nonwoven fabric had no holes or cracks, the solid electrolyte had low impedance, and the lithium ion conductivity was excellent.
[0099] The supporting nonwoven fabric of Example 6 has a basis weight of 2 g / m 2 The strength of the supporting nonwoven fabric was reduced, and the supporting ability of the solid electrolyte was reduced compared to the supporting nonwoven fabrics of Examples 1 to 5.
[0100] The nonwoven support fabric of Example 7 had a thickness of 10 μm or more, had no hole defects, and had no cracks in the solid electrolyte. However, due to a decrease in the strength of the nonwoven support fabric, the supportability of the solid electrolyte was decreased compared to the nonwoven support fabrics of Examples 1 to 5.
[0101] The supporting nonwoven fabric of Example 8 had a thickness of less than 4 μm, and had no hole defects and no cracks in the solid electrolyte. However, the fusion of the unstretched polyester fibers progressed and the voids inside the supporting nonwoven fabric decreased, so that the supporting ability of the solid electrolyte was reduced compared to the supporting nonwoven fabrics of Examples 1 to 5, and the impedance of the all-solid-state lithium battery was increased and the lithium ion conductivity was reduced.
[0102] Hole defects were generated in the support nonwoven fabric of Comparative Example 1, in which the content of fibrillated natural cellulose fibers was less than 5% by mass. When a solid electrolyte was applied to the support nonwoven fabric in which holes were generated, hole defects were also generated in the solid electrolyte sheet. When a solid electrolyte sheet with holes was used, the behavior of the battery performance of the all-solid-state lithium battery was abnormal in some cases, and short circuits were observed.
[0103] The supporting nonwoven fabric of Comparative Example 2, in which the content of fibrillated natural cellulose fibers exceeded 20 mass %, had a reduced strength and therefore a reduced ability to support the solid electrolyte.
[0104] The support nonwoven fabric of Comparative Example 3, which used stretched polyester staple fibers with an average fiber diameter exceeding 2.7 μm, was prone to hole defects in the support nonwoven fabric, had fine cracks in the solid electrolyte layer, and slight adhesion failure was observed at the interface between the fibers and the solid electrolyte.
[0105] The nonwoven support fabric of Comparative Example 4, which used unstretched polyester staple fibers with an average fiber diameter exceeding 4.5 μm, was prone to hole defects, and the strength of the nonwoven support fabric was reduced, resulting in a decrease in the ability to support the solid electrolyte. Furthermore, fine cracks were found in the solid electrolyte layer, and poor adhesion was observed at the interface between the fibers and the solid electrolyte.
[0106] Basis weight 3.0g / m 2 The support nonwoven fabric of Comparative Example 5, which exceeded 100%, had fine cracks in the solid electrolyte layer and slight adhesion failure was observed at the interface between the fiber and the solid electrolyte, and an increase in the impedance of the all-solid-state lithium battery was observed compared to the support nonwoven fabric of Example 1.
[0107] 10 parts by weight of fibrillated solvent-spun cellulose fiber was used, with a basis weight of 3.0 g / m 2In the nonwoven support fabric of Comparative Example 6, which had a diameter of less than 1.0 g, holes were generated. In addition, even after beating using a refiner, the stem portion with a maximum fiber diameter of 5.2 μm remained in the fibrillated solvent-spun cellulose fiber, so that cracks were generated in the solid electrolyte layer, poor adhesion was observed at the interface between the fiber and the solid electrolyte, and an increase in impedance of the all-solid-state lithium battery was observed compared to the nonwoven support fabric of Example 1.
[0108] 10 parts by mass of para-based fully aromatic polyamide fiber pulp is used, and the basis weight is 3.0 g / m 2 In the nonwoven support fabric of Comparative Example 7, which had a thickness of less than 100 μm, holes were generated. In addition, fine cracks were observed in the solid electrolyte layer, and slight adhesion defects were observed at the interface between the fiber and the solid electrolyte. Compared with the nonwoven support fabric of Example 1, an increase in impedance of the all-solid-state lithium battery was observed. [Industrial Applicability]
[0109] The nonwoven fabric for supporting a solid electrolyte and the solid electrolyte sheet of the present invention can be suitably used in an all-solid-state lithium battery.
Claims
1. A nonwoven fabric for supporting a solid electrolyte, which supports a solid electrolyte on the surface and inside of the nonwoven fabric, comprises fibrillated natural cellulose fibers and synthetic resin staple fibers, the content of the fibrillated natural cellulose fibers being 5% by mass or more and 20% by mass or less of all fiber components contained in the nonwoven fabric for supporting a solid electrolyte, the synthetic resin staple fibers include stretched polyester fibers having an average fiber diameter of 2.7 μm or less and unstretched polyester fibers having an average fiber diameter of 4.5 μm or less, and the basis weight of the nonwoven fabric for supporting a solid electrolyte is 3.0 g / m. 2 The nonwoven fabric for supporting a solid electrolyte is characterized in that the thickness of the nonwoven fabric is less than or equal to 100 μm.
2. The basis weight of the nonwoven fabric for supporting a solid electrolyte is 2.0 g / m 2 2.9g / m or more 2 2. The nonwoven fabric for supporting a solid electrolyte according to claim 1, wherein the thickness of said nonwoven fabric for supporting a solid electrolyte is 4 μm or more and less than 10 μm.
3. 3. A solid electrolyte sheet comprising the nonwoven fabric for supporting a solid electrolyte according to claim 1 or 2, and a solid electrolyte supported on the surface and inside of the nonwoven fabric for supporting a solid electrolyte.
Citation Information
Patent Citations
Solid electrolyte sheet and all-solid type secondary battery
JP2016031789A
Solid electrolyte carrying nonwoven fabric and solid electrolyte sheet
JP2020024860A
Non-woven fabric for supporting solid electrolyte, and solid electrolyte sheet
WO2021200621A1