Asphalt composition

The use of a specific slack wax-based asphalt composition with an organic silane compound enhances heat resistance and low-temperature workability, addressing high energy consumption and emissions in asphalt production, facilitating low-temperature mixing and extended construction capabilities.

JP2024141149APending Publication Date: 2024-10-10IDEMITSU KOSAN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052638
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing asphalt compositions require high temperatures for production and mixing, leading to high energy consumption and carbon emissions, and lack optimal heat resistance and low-temperature workability, making them unsuitable for extended construction periods and natural disaster resilience.

Method used

An asphalt composition containing 95% slack wax that meets specific melting endotherm and molecular weight criteria, combined with asphalt in a 1:4 ratio, and optionally including an organic silane compound, allowing low-temperature production and mixing with aggregates.

Benefits of technology

The composition achieves excellent heat resistance, strength, and low-temperature workability, reducing energy consumption and emissions, enabling long-distance transportation and broader construction applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141149000001
    Figure 2024141149000001
  • Figure 2024141149000002
    Figure 2024141149000002
  • Figure 2024141149000003
    Figure 2024141149000003
Patent Text Reader

Abstract

To provide an asphalt composition excellent in heat resistance and strength, capable of being produced at a low temperature, and excellent in low-temperature construction property, and to provide an asphalt mixture.SOLUTION: An asphalt composition is slack-wax which contains wax components (A) and asphalt (B), and in which 95 mass% or more of the wax components (A) satisfies (1)-(5): (1) melting endotherm quantity is 50-170 J / g; (2) in a melting peak in a melting endothermic curve obtained by a differential scanning calorimetry measurement, an area of less than 20°C is 0-20%; (3) in the melting peak, an area of 20°C or more and less than 55°C is 40-70%; (4) in the melting peak, an area of 55°C or more and less than 80°C is 20-50%; and (5) in the melting peak, an area of 80°C or more is 0%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an asphalt composition and an asphalt mix. [Background technology]

[0002] In asphalt paving of roads and parking lots, the mixing and construction of petroleum asphalt and aggregates are carried out at high temperatures. Drying the aggregate also requires energy. Reducing the temperature and energy consumed during the production and application of these asphalt mixtures and during aggregate drying will contribute to a reduction in carbon dioxide emissions and cost savings. It will also make it possible to transport the mixture over long distances from the factory where it is manufactured to the construction site, thereby contributing to an expansion of the range of construction. Therefore, studies are being conducted to improve workability at low temperatures. For example, Patent Document 1 discloses an asphalt paving mixture containing a lubricant that can be mixed at high temperatures and then paved and compacted at temperatures 10 to 55°C lower than that temperature, with the aim of increasing transportation time, working time, and working temperature range. Patent Document 2 discloses a bitumen composition containing petroleum slack wax and Fischer-Tropsch wax for the purpose of imparting excellent properties to bitumen and asphalt mixing processing, and an asphalt composition containing the same. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] US Patent Application Publication No. 2012 / 0213584 [Patent Document 2] Special Publication No. 2019-517607 Summary of the Invention [Problem to be solved by the invention]

[0004] Although Patent Documents 1 and 2 can improve low-temperature workability, in recent years, when further energy reduction and centralization of asphalt mixture production are being promoted, it is still not sufficient. In particular, high temperatures are required for the production of asphalt mixture. Patent Document 2 attempts to improve low-temperature workability by mixing wax, but there is a problem that it is necessary to adjust multiple waxes, making it difficult to find an optimal blend. Therefore, there has been a demand for an asphalt composition that can be produced at low temperatures by blending substantially one type of wax, and that can be applied at low temperatures. In addition, since paved roads become extremely hot in summer, asphalt compositions are required to have high heat resistance, and it is desirable to have both heat resistance and low-temperature workability. Furthermore, paved roads are required to have high strength to withstand long-term vibrations and natural disasters. Therefore, an object of the present disclosure is to provide an asphalt composition and asphalt mixture that have excellent heat resistance and strength, can be produced at low temperatures, and have excellent low-temperature workability. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that an asphalt composition containing a specific slack wax and asphalt can solve the above problems.

[0006] That is, the present disclosure provides the following: <1> ~ <9> Regarding. <1> An asphalt composition comprising a wax component (A) and an asphalt (B), wherein 95 mass % or more of the wax component (A) is a slack wax (A1) that satisfies the following (1) to (5). (1) The heat of fusion (ΔH) is 50 to 170 J / g. (2) The area of ​​the melting peak below 20°C in the melting endothermic curve is 0 to 20%. (3) The area of ​​the melting peak in the melting endothermic curve that is between 20°C and 55°C is 40-70%. (4) The area of ​​the melting peak in the melting endothermic curve between 55°C and 80°C is 20-50%. (5) The area of ​​the melting peak at 80°C or higher in the melting endothermic curve is 0%. (Note that the areas shown in (2) to (5) above are areas obtained by dividing the melting peak in a melting endothermic curve obtained by differential scanning calorimetry at a heating rate of 10° C. / min.) <2> The slack wax (A1) is a slack wax that further satisfies the following (6) and (7). <1> The asphalt composition according to claim 1. (6) The number of butyl branches per 1,000 carbon atoms is 0.1 or more. (7) Weight average molecular weight of 500 to 3,000 <3> The slack wax (A1) has a needle penetration at 23°C of 60 to 120. <1> or <2> The asphalt composition according to claim 1. <4> The combination of the wax component (A) and the asphalt (B) is such that the mixture [(A) / (B)=1 / 4] does not have a glass transition temperature in the range of 0 to 15° C. <1> ~ <3> 13. The asphalt composition according to claim 12, <5> The content of the wax component (A) is 1 to 20 mass %. <1> ~ <4> 13. The asphalt composition according to claim 12, <6> The composition further contains an organic silane compound (C) in an amount of 0.1 to 5% by mass. <1> ~ <5> 13. The asphalt composition according to claim 12, <7> The asphalt composition satisfies the following (8) and (9): <1> ~ <6> 13. The asphalt composition according to claim 12, (8) The heterogeneous component of the complex shear viscosity at 100°C during the cooling process is 0.01 to 20 mPa s (9) Storage modulus at 60°C during heating is 100-5000 Pa <8> The above <1> ~ <7> 10. An asphalt mixture comprising the asphalt composition according to claim 1 and aggregate, the aggregate content being 80 to 99 mass %. <9> The above <1> ~ <7> 13. A method for producing an asphalt mixture, comprising the step of mixing the asphalt composition according to any one of claims 1 to 12 with aggregate at 90 to 140°C. Effect of the Invention

[0007] It is possible to provide an asphalt composition and an asphalt mixture which have excellent heat resistance and strength, can be produced at low temperatures, and have excellent low-temperature workability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Asphalt composition] The asphalt composition of the present disclosure contains a wax component (A) and an asphalt (B), in which 95 mass% or more of the wax component (A) is a slack wax (A1) that satisfies the following (1) to (5). (1) The heat of fusion (ΔH) is 50 to 170 J / g. (2) The area of ​​the melting peak below 20°C in the melting endothermic curve is 0 to 20%. (3) The area of ​​the melting peak in the melting endothermic curve that is between 20°C and 55°C is 40-70%. (4) The area of ​​the melting peak in the melting endothermic curve between 55°C and 80°C is 20-50%. (5) The area of ​​the melting peak at 80°C or higher in the melting endothermic curve is 0%. (Note that the areas shown in (2) to (5) above are areas obtained by dividing the melting peak in a melting endothermic curve obtained by differential scanning calorimetry at a heating rate of 10° C. / min.)

[0009] <Wax component (A) and slack wax (A1)> The wax component (A) contained in the asphalt composition of the present disclosure is 95 mass % or more of slack wax (A1) that satisfies the following (1) to (5). (1) The heat of fusion (ΔH) is 50 to 170 J / g. (2) The area of ​​the melting peak below 20°C in the melting endothermic curve is 0 to 20%. (3) The area of ​​the melting peak in the melting endothermic curve that is between 20°C and 55°C is 40-70%. (4) The area of ​​the melting peak in the melting endothermic curve between 55°C and 80°C is 20-50%. (5) The area of ​​the melting peak at 80°C or higher in the melting endothermic curve is 0%. (Note that the areas shown in (2) to (5) above are areas obtained by dividing the melting peak in a melting endothermic curve obtained by differential scanning calorimetry at a heating rate of 10° C. / min.)

[0010] The content of the wax component (A) contained in the asphalt composition of the present disclosure is preferably 1 to 20 mass%, more preferably 3 mass% or more, even more preferably 5 mass% or more, and even more preferably 7 mass% or more. Also, it is more preferably 18 mass% or less, even more preferably 15 mass% or less, and even more preferably 13 mass% or less. By having the content of the wax component (A) within the above range, the obtained asphalt composition can achieve low-temperature workability while maintaining sufficient durability and heat resistance.

[0011] The content of the slack wax (A1) in the wax component (A) is 95% by mass or more, preferably 97% by mass or more, more preferably 98% by mass or more, even more preferably 99% by mass or more, and even more preferably 100% by mass. The wax component (A) may consist of only the slack wax (A1), and the upper limit of the content of the slack wax (A1) in the wax component (A) is 100% by mass or less.

[0012] The wax other than the slack wax (A1) contained in the wax component (A) is preferably at least one selected from the group consisting of mineral waxes, synthetic waxes and microcrystalline waxes, and more preferably a synthetic wax. Examples of mineral waxes include montan wax. Examples of synthetic waxes include polyolefin waxes such as polyethylene wax and polypropylene wax, and Fischer-Tropsch wax. The content of waxes other than the slack wax (A1) in the wax component (A) is 5% by mass or less, preferably 3% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, and even more preferably 0% by mass. It is even more preferable that the wax component (A) does not contain any wax other than the slack wax (A1).

[0013] Slack wax (A1) is a waxy substance obtained as a by-product during the refining of petroleum and the production of lubricating oils, etc., and this includes wax that has been further refined, bleached, and hydrogenated.

[0014] The slack wax (A1) satisfies the above (1) to (5). The above (1) to (5) can be obtained by differential scanning calorimetry at a temperature rise rate of 10° C. / min. A specific method for measuring the melting endotherm (ΔH) (above (1)) is to use a differential scanning calorimeter to hold a sample of slack wax (A1) at -10°C for 5 minutes under a nitrogen atmosphere, and then heat the sample to 140°C at a rate of 10°C / min, thereby obtaining the melting endotherm (ΔH) from the total area of ​​the melting peak in the melting endotherm curve obtained. The total area of ​​the melting peak refers to the area enclosed by the melting endotherm curve and the baseline, which is a line connecting a point on the low-temperature side where there is no change in heat quantity and a point on the high-temperature side where there is no change in heat quantity. More specifically, the melting endotherm (ΔH) can be obtained by the method shown in the examples.

[0015] The area of ​​each temperature range of the melting peak in the melting endothermic curve is the area obtained by dividing the melting peak in the melting endothermic curve obtained by differential scanning calorimetry at a heating rate of 10°C / min. Specifically, the proportion of the area of ​​each temperature range of the melting peak in the melting endothermic curve (above (2) to (5)) is calculated as follows. In the same manner as in the measurement method of the melting endotherm (ΔH), a differential scanning calorimeter is used to hold a sample of the slack wax (A1) at -10°C for 5 minutes under a nitrogen atmosphere, and then the temperature is raised to 140°C at 10°C / min to obtain a melting endotherm curve. Next, a line perpendicular to the horizontal axis (temperature axis) is drawn from a predetermined temperature (20°C, 55°C, 80°C) of the melting endotherm curve to the baseline. The area surrounded by the lines corresponding to the melting endotherm curve, the baseline, and each temperature is defined as the area of ​​each temperature range. The ratio of the area of ​​each temperature range to the total area of ​​the melting peak is the ratio of the area of ​​each temperature range of the melting peak in the melting endotherm curve. Specifically, the "area below 20°C" is the area surrounded by the melting endothermic curve, the baseline, and the line corresponding to 20°C. The "area from 20°C to less than 55°C" is the area surrounded by the melting endothermic curve, the baseline, the line corresponding to 20°C, and the line corresponding to 55°C. The "area from 55°C to less than 80°C" is the area surrounded by the melting endothermic curve, the baseline, the line corresponding to 55°C, and the line corresponding to 80°C. The "area above 80°C" is the area surrounded by the melting endothermic curve, the baseline, and the line corresponding to 80°C. When the melting peak does not include the above-mentioned temperature range, the area of ​​that temperature range is not considered to exist, and the area of ​​that temperature range is considered to be zero. More specifically, the area of ​​each temperature range of the melting peak in the melting endothermic curve can be determined by the method shown in the Examples.

[0016] The fusion endotherm (ΔH) of the slack wax (A1) is 50 to 170 J / g, preferably 100 to 150 J / g, more preferably 105 to 130 J / g, and further preferably 105 to 120 J / g. When the melting endotherm (ΔH) of the slack wax (A1) is within the above range, the resulting asphalt composition has excellent low-temperature workability.

[0017] The area of ​​the melting peak in the melting endothermic curve of the slack wax (A1) below 20° C. is 0 to 20%, preferably 0 to 15%, more preferably 1 to 12%, and further preferably 2 to 9%. The area of ​​the melting peak from 20° C. to less than 55° C. in the melting endothermic curve of the slack wax (A1) is 40 to 70%, preferably 40 to 60%, more preferably 40 to 55%, and even more preferably 40 to 50%. The area of ​​the melting peak at 55° C. or higher and lower than 80° C. in the melting endothermic curve of the slack wax (A1) is 20 to 50%, preferably 25 to 50%, more preferably 30 to 50%, and further preferably 35 to 50%. The area of ​​the melting peak at or above 80° C. in the melting endothermic curve of the slack wax (A1) is 0%. When the ratio of the area of ​​each temperature range of the melting peak in the melting endothermic curve of the slack wax (A1) is within the above range, the obtained asphalt composition has excellent low-temperature workability. Also, when the ratio of the area of ​​each temperature range of the melting peak in the melting endothermic curve of the slack wax (A1) is within the above range, the obtained asphalt composition has excellent heat resistance even when applied in summer.

[0018] The slack wax (A1) is preferably a slack wax which further satisfies the following (6) and (7). (6) The number of butyl branches per 1,000 carbon atoms is 0.1 or more. (7) Weight average molecular weight of 500 to 3,000

[0019] The number of butyl branches per 1000 carbon atoms indicates the degree of branching of the slack wax (A1): the higher the number of butyl branches, the higher the degree of branching. The number of butyl branches per 1,000 carbon atoms of the slack wax (A1) is, from the viewpoints of reducing crystallinity, enabling the production of the resulting asphalt composition at low temperatures, and improving low-temperature workability, preferably 0.1 or more, more preferably 0.5 or more, even more preferably 1.0 or more, still more preferably 2.0 or more, and even more preferably 3.0 or more, and from the viewpoints of durability and heat resistance, more preferably 10.0 or less, even more preferably 5.0 or less, and even more preferably 4.0 or less. Here, the number of butyl branches per 1000 carbon atoms is: 13 The ratio of the number of alkyl branches per carbon can be calculated from the ratio of integrated intensities of peaks derived from each alkyl branch in a C-NMR spectrum, using the following formula: (Butyl branches per 1000 carbon atoms) = (branching ratio of butyl branches) / (total ratio of alkyl branches) x 1000 Specifically, it is determined by the method in the Examples.

[0020] The weight average molecular weight (Mw) of the slack wax (A1) is preferably 500 to 3000. From the viewpoint of mechanical strength and durability, the weight average molecular weight (Mw) of the slack wax (A1) is preferably 500 or more, more preferably 700 or more, even more preferably 800 or more, and even more preferably 850 or more. From the viewpoint of mixability with asphalt and low-temperature workability, the weight average molecular weight (Mw) of the slack wax (A1) is preferably 3000 or less, more preferably 2000 or less, even more preferably 1200 or less, and even more preferably 1000 or less. In the present disclosure, the weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples.

[0021] The penetration of the slack wax (A1) at 23° C. is preferably 60 to 120. The penetration of the slack wax (A1) at 23° C. is preferably 40 or more, and from the viewpoint of mixability with asphalt and low-temperature workability, it is more preferably 60 or more, and even more preferably 80 or more, and from the viewpoint of heat resistance, it is even more preferably 90 or more. From the viewpoint of mechanical strength and durability, the penetration of the slack wax (A1) at 23° C. is preferably 120 or less, more preferably 110 or less, and from the viewpoint of achieving both heat resistance and low-temperature workability, it is even more preferably 100 or less, and even more preferably 90 or less. In the present disclosure, the penetration at 23° C. is measured in accordance with JIS K 2235:2022. Specifically, it is measured by the method described in the examples.

[0022] <Asphalt (B)> The asphalt composition of the present disclosure contains the wax component (A) and asphalt (B). Asphalt (B) is used as an asphalt base oil. Examples of the asphalt (B) include straight asphalt, solvent deasphalt, blown asphalt, and semi-blown asphalt. The asphalt (B) is preferably at least one selected from the group consisting of straight asphalt, solvent deasphalt, blown asphalt, and semi-blown asphalt. The asphalt (B) may be used alone or in combination of two or more kinds. Among the above, the asphalt (B) is more preferably at least one selected from the group consisting of straight asphalt, solvent deasphalted asphalt, and blown asphalt, and even more preferably at least one selected from the group consisting of straight asphalt and solvent deasphalted asphalt, and even more preferably the asphalt (B) is straight asphalt. When two or more types are used in combination, it is preferable to use straight asphalt. The content of straight asphalt in asphalt (B) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more in asphalt (B), and asphalt (B) may consist of only straight asphalt. By having the straight asphalt content within the above range, the obtained asphalt composition can suppress an increase in viscosity even in low-temperature paving, and can have sufficient durability, high strength, and heat resistance while having low-temperature workability.

[0023] The straight asphalt may be asphalt or a mixture thereof as specified in JIS K 2207: 2006. It is preferable to use the straight asphalt having a penetration grade of 40-60 or 200-300. Solvent deasphalted asphalt corresponds to the residue obtained by extracting solvent deasphalted oil (high viscosity lubricating oil fraction) from vacuum distillation residual oil (see "New Petroleum Dictionary," edited by the Japan Petroleum Institute, 1982, p. 308). It is called propane deasphalted asphalt when propane or propane and butane are used as the solvent. Propane deasphalted asphalt is preferred as solvent deasphalted asphalt. Blown asphalt is, for example, asphalt defined in JIS K 2207:2006. Semi-blown asphalt is, for example, the semi-blown asphalt defined in "Asphalt Pavement Guidelines," published by the Japan Road Association, January 13, 1997, p. 51, Table 3.3.4.

[0024] The content of asphalt (B) contained in the asphalt composition of the present disclosure is preferably 80 to 99 mass%, more preferably 82 mass% or more, even more preferably 85 mass% or more, and even more preferably 87 mass% or more. Also, it is more preferably 97 mass% or less, even more preferably 95 mass% or less, and even more preferably 93 mass% or less. By having the content of asphalt (B) in the above range, the obtained asphalt composition can have sufficient durability, high strength, and heat resistance while having low-temperature workability. In addition, the mass ratio of the wax component (A) content to the asphalt (B) content in the asphalt composition of the present disclosure [(A) / (B)] is preferably 1 / 99 to 20 / 80, more preferably 3 / 97 to 18 / 82, even more preferably 5 / 95 to 15 / 85, and even more preferably 7 / 93 to 13 / 87. By having the mass ratio of the wax component (A) content to the asphalt (B) content within the above range, the obtained asphalt composition can achieve low-temperature workability while maintaining sufficient durability and heat resistance. Furthermore, the mass ratio of the content of the slack wax (A1) to the content of the asphalt (B) in the asphalt composition of the present disclosure [(A1) / (B)] is preferably 1 / 99 to 20 / 80, more preferably 3 / 97 to 18 / 82, even more preferably 5 / 95 to 15 / 85, and even more preferably 7 / 93 to 13 / 87. By having the mass ratio of the content of the slack wax (A1) to the content of the asphalt (B) within the above range, the obtained asphalt composition can achieve low-temperature workability while maintaining sufficient durability and heat resistance.

[0025] <Organosilane Compound (C)> The asphalt composition of the present disclosure may further contain an organosilane compound (C), and the content thereof is preferably 0.1 to 5 mass%. That is, the asphalt composition of the present disclosure further contains 0.1 to 5 mass% of the organosilane compound (C). By including the organic silane compound (C), the water resistance of the asphalt mixture obtained using the asphalt composition of the present disclosure can be improved. In particular, sufficient water resistance can be imparted to the asphalt mixture without drying the aggregate. This further reduces the energy consumption, reduces carbon dioxide emissions, and contributes to cost reduction.

[0026] The content of the organosilane compound (C) contained in the asphalt composition of the present disclosure is preferably 0.1 to 5 mass%, more preferably 0.2 mass% or more, and even more preferably 0.5 mass% or more. Also, it is more preferably 4 mass% or less, even more preferably 3 mass% or less, and even more preferably 2 mass% or less. By having the content of the organosilane compound (C) in the above range, the water resistance of the asphalt mixture containing the obtained asphalt composition can be improved.

[0027] The organic silane compound (C) is preferably at least one selected from the group consisting of a copolymer of a trialkoxyvinylsilane and a component having a polymerizable unsaturated bond, a hydrogenated product thereof, and a silane-modified petroleum resin. The trialkoxyvinylsilane is preferably at least one selected from the group consisting of vinyltrimethoxysilane, vinyltriethoxysilane, and 3-(trimethoxysilyl)propyl methacrylate. The component having a polymerizable unsaturated bond is preferably at least one selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, ethylindene, cyclopentadiene, dicyclopentadiene, isoprene, piperylene, and indene.

[0028] The organosilane compound (C) is more preferably a silane-modified petroleum resin (hereinafter referred to as "silane-modified petroleum resin"). The silane-modified petroleum resin preferably contains 0.1 to 10 mass %, more preferably 0.3 to 8 mass %, and even more preferably 0.5 to 2 mass % of silicon element calculated as silicon atom based on the silane-modified petroleum resin. The silicon content in silane-modified petroleum resin can be measured by ICP atomic emission spectrometry such as JPI-5S-38-03 Lubricants - Testing Method for Added Elements - Inductively Coupled Plasma Atomic Emission Spectroscopy. Specifically, 0.1 g of silane-modified petroleum resin is heated in an electric furnace at 550°C for 12 hours, and the measurement solution is prepared by alkali fusion of the ash, and then ICP atomic emission spectrometry is performed (ICP atomic emission spectrometer: 720-ES, manufactured by Agilent Technologies, Inc.) to determine the silicon content. The silane-modified petroleum resin is preferably a silane-modified hydrogenated petroleum resin having an organosilane structure, and more preferably a silane-modified hydrogenated petroleum resin in which an alkoxysilyl group is bonded to the main chain of the hydrogenated petroleum resin via a bond.

[0029] The "petroleum resin" referred to here is a resin obtained by polymerizing or copolymerizing one or more unsaturated compounds selected from aliphatic olefins and aliphatic diolefins having 4 to 10 carbon atoms, which are obtained as by-products during the production of olefins such as ethylene by thermal decomposition of petroleum such as naphtha, or aromatic compounds having 8 or more carbon atoms and having an olefinically unsaturated bond. Petroleum resins can be roughly classified into, for example, "aliphatic petroleum resins" obtained by polymerizing aliphatic olefins or aliphatic diolefins, "aromatic petroleum resins" obtained by polymerizing aromatic compounds having olefinic unsaturated bonds, and "aliphatic-aromatic copolymer petroleum resins" obtained by copolymerizing aliphatic olefins or aliphatic diolefins with aromatic compounds having olefinic unsaturated bonds.

[0030] Examples of aliphatic olefins having 4 to 10 carbon atoms include butene, pentene, hexene, and heptene. Examples of aliphatic diolefins having 4 to 10 carbon atoms include butadiene, pentadiene, isoprene, piperylene, cyclopentadiene, dicyclopentadiene, and methylpentadiene. Examples of aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, and ethylindene. Furthermore, the raw material compounds for the petroleum resin do not all need to be by-products in the production of olefins by thermal decomposition of petroleum such as naphtha, and chemically synthesized unsaturated compounds may also be used.

[0031] Preferable examples of petroleum resins include dicyclopentadiene-based petroleum resins obtained by polymerization of cyclopentadiene or dicyclopentadiene, dicyclopentadiene-styrene-based petroleum resins obtained by copolymerizing these cyclopentadiene or dicyclopentadiene with styrene, C5-based petroleum resins obtained by polymerization of isoprene or piperylene, and C9-based petroleum resins obtained by polymerization of C9 monomers such as indene or vinyltoluene.

[0032] The term "hydrogenated petroleum resin" as used herein refers to a petroleum resin obtained by adding hydrogen atoms to the above-mentioned petroleum resin. Hydrogenated petroleum resins include fully hydrogenated petroleum resins in which substantially no unsaturated bonds remain and partially hydrogenated petroleum resins in which unsaturated bonds remain, and fully hydrogenated petroleum resins are preferred. As the hydrogenated petroleum resin, hydrogenated aliphatic-aromatic copolymer petroleum resin is preferred.

[0033] Furthermore, the phrase "the alkoxysilyl group is bonded to the main chain of the hydrogenated petroleum resin via a bonding part" means that, for example, a bonding part is bonded directly to a carbon atom contained in a hydrogenated polymer (hydrogenated petroleum resin) obtained by polymerizing aliphatic olefins, aliphatic diolefins, and an aromatic compound having an olefinically unsaturated bond as described above and adding hydrogen atoms, and further an alkoxysilyl group is bonded to the carbon atom. The alkoxysilyl group is preferably a trialkoxysilyl group having an alkoxy group having 1 to 20 carbon atoms, which may be linear or branched, and more preferably a trialkoxysilyl group having an alkoxy group having 1 to 10 carbon atoms, which may be linear or branched. Specific examples include a trimethoxysilyl group, a triethoxysilyl group, and a tripropoxysilyl group, and the like, with the trimethoxysilyl group and the triethoxysilyl group being preferred. The bonding portion may be any divalent or higher organic group that can bond to a carbon atom in the main chain of the hydrogenated petroleum resin and to which an alkoxysilyl group can be bonded, and is preferably an alkylene group, more preferably an alkylene group having 2 to 3 carbon atoms.

[0034] <Other ingredients> The asphalt composition of the present disclosure may contain aromatic heavy mineral oil, a reinforcing material, and any additives as components other than the wax component (A), the asphalt (B), and the silane compound (C).

[0035] (Aromatic heavy mineral oil) In the asphalt composition, the aromatic heavy mineral oil may be a solvent-extracted oil, that is, an extract, obtained by subjecting a solvent-deasphalted oil obtained by deasphalting a vacuum distillation residual oil of crude oil with propane or the like, to solvent extraction using a polar solvent such as furfural to obtain bright stock (heavy lubricating oil). In particular, in the asphalt composition which is one embodiment of the present invention, it is preferable to add an extract as the aromatic heavy mineral oil.

[0036] In the asphalt composition, the role of the extract is to increase the solubility of the thermoplastic elastomer in asphalt and prevent separation during storage stability, and the amount of extract required to be added increases as the amount of thermoplastic elastomer added increases. In addition, the extract also has the property of softening hardened asphalt components when using paving materials that utilize asphalt mixtures made from recycled aggregates or recycled asphalt. In addition, if more extract than necessary is added relative to the amount of thermoplastic elastomer added, the elastic modulus of the asphalt composition decreases.

[0037] The content of the extract relative to the entire asphalt composition is determined taking into consideration the penetration, softening point, storage stability, complex modulus indicating strength, dynamic stability (DS) in a wheel tracking test, and bending work and bending stiffness indicating low-temperature properties. In the range considered in this embodiment, the content of the extract relative to the entire asphalt composition is preferably 2.0 mass% or more and 8.0 mass% or less, but it is not particularly essential that the extract is contained, and it is not necessary that it is contained.

[0038] (Reinforcement) The asphalt composition may further contain a thermoplastic elastomer as a reinforcing material. As the thermoplastic elastomer, SBS (styrene-butadiene-styrene copolymer) is preferred. The performance of SBS can be estimated mainly from its molecular weight and styrene content, which is the mass % of styrene contained in the SBS.

[0039] The weight average molecular weight of SBS is preferably from 120,000 to 250,000. The styrene content of SBS is from 25.0 to 35.0% by mass, preferably from 27.0 to 33.0% by mass, of the total SBS.

[0040] In addition to the above, SBS with different molecular weights and styrene contents are available, and the molecular weight of these SBS is between 80,000 and 90,000. Furthermore, the styrene content is between 25.0% and 50.0% by mass of the total SBS.

[0041] In the asphalt composition, it is not essential that SBS is contained, and it is not necessary that SBS is contained, but from the viewpoint of improving the water resistance of the asphalt pavement, it is preferable that the content of SBS in the entire asphalt composition is 7.0 mass% or less. By making the content of SBS 7.0 mass% or less, it is possible to maintain the asphalt continuous phase, and it is possible to improve the water resistance of the dense-graded mixture with excellent water impermeability while solving the above-mentioned problems. On the other hand, when it is desired to produce an asphalt mixture with high drainage or water permeability by intentionally providing voids inside the pavement, it is possible to produce an asphalt composition with high drainage or water permeability by causing a phase transition of SBS while solving the above-mentioned problems by making the content of SBS in the entire asphalt composition of this embodiment more than 7.0 mass%.

[0042] In the asphalt composition, only one type of SBS may be mixed, or two or more types of SBS having specific molecular structures may be selected and mixed. Mixing only one type of SBS is preferable because it eliminates the complication of selecting and mixing two or more types of SBS and enables a reduction in manufacturing labor.

[0043] (Optional Additives) The asphalt composition of the present disclosure may contain any additive as long as it does not impair the effects of the present disclosure.

[0044] Optional additives include petroleum resins and hydrogenated petroleum resins obtained by adding hydrogen atoms to petroleum resins. Petroleum resins are resins obtained by polymerizing or copolymerizing one or more unsaturated compounds selected from aliphatic olefins and aliphatic diolefins having 4 to 10 carbon atoms, which are obtained as by-products during the production of olefins such as ethylene by thermal decomposition of petroleum such as naphtha, or aromatic compounds having 8 or more carbon atoms and having an olefinically unsaturated bond. Petroleum resins can be roughly classified into, for example, "aliphatic petroleum resins" obtained by polymerizing aliphatic olefins or aliphatic diolefins, "aromatic petroleum resins" obtained by polymerizing aromatic compounds having olefinic unsaturated bonds, and "aliphatic-aromatic copolymer petroleum resins" obtained by copolymerizing aliphatic olefins or aliphatic diolefins with aromatic compounds having olefinic unsaturated bonds. Examples of the aliphatic olefins having 4 to 10 carbon atoms include butene, pentene, hexene, and heptene. Examples of the aliphatic diolefins having 4 to 10 carbon atoms include butadiene, pentadiene, isoprene, piperylene, cyclopentadiene, dicyclopentadiene, and methylpentadiene. Examples of aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, and ethylindene. Furthermore, the raw material compounds for the petroleum resin do not all need to be by-products in the production of olefins by thermal decomposition of petroleum such as naphtha, and chemically synthesized unsaturated compounds may also be used. Suitable examples of petroleum resins include dicyclopentadiene-based petroleum resins obtained by polymerization of cyclopentadiene or dicyclopentadiene, dicyclopentadiene-styrene-based petroleum resins obtained by copolymerizing these cyclopentadiene or dicyclopentadiene with styrene, C5-based petroleum resins obtained by polymerization of isoprene or piperylene, and C9-based petroleum resins obtained by polymerization of C9 monomers such as indene or vinyltoluene. Hydrogenated petroleum resins are petroleum resins obtained by adding hydrogen atoms to the above-mentioned petroleum resins, and include fully hydrogenated petroleum resins in which substantially no unsaturated bonds remain and partially hydrogenated petroleum resins in which unsaturated bonds remain, with partially hydrogenated petroleum resins being preferred.

[0045] In addition, as an optional additive, a polyethylene-based polyolefin can be used, specifically, Hi-Zex 1300J, Neo-Zex 20201J, Ult-Zex 15150J (manufactured by Prime Polymer Co., Ltd.), Affinity GA1950, Affinity GA1900H (manufactured by DOW), etc.

[0046] Other optional additives include antioxidants. An antioxidant may be added to enhance thermal stability. As the antioxidant, known antioxidants can be used. As the antioxidant, it is preferable to use a phenol-based antioxidant. Examples of the phenol-based antioxidant include triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 3,5-di-tert- Examples of such compounds include butyl-4-hydroxybenzylphosphonate-diethyl ester, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamamide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane. Commercially available antioxidants that can be used include pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (BASF Ltd., IRGANOX1010) and 1,3,5-tris-(3',5'-di-tert-butyl-4'-hydroxybenzyl)isocyanuric acid (ADEKA Corporation, Adeka STAB AO-20).

[0047] <Characteristics of asphalt composition> The asphalt composition of the present disclosure preferably has the following properties:

[0048] The combination of wax component (A) and asphalt (B) used in the asphalt composition of the present disclosure is a combination in which the mixture [(A) / (B)=1 / 4] does not have a glass transition temperature in the range of 0 to 15°C. If the compatibility between the wax component (A) and the asphalt (B) is low, the low-temperature paving properties will be impaired if the aggregate and asphalt are heated and mixed at the asphalt mixture manufacturing plant, transported to the paving site, and separated before construction. On the other hand, high compatibility allows for a wider range of construction and results in good low-temperature paving properties. Asphalt (B) usually has a glass transition temperature of 0 to 15°C, but this glass transition temperature disappears or shifts when mixed with a wax component (A) that has good compatibility. By using such a combination of wax component (A) and asphalt (B), the mixture using the asphalt composition of the present disclosure can expand the range of application and has good low-temperature paving properties. The mixture used is obtained by mixing the wax component (A) and the asphalt (B) in a mass ratio of 1:4. The presence or absence of a glass transition temperature is evaluated by using a differential scanning calorimeter to determine whether or not an inflection point appears in the range of 0 to 15° C. in the melting endothermic curve obtained by holding a sample of the mixture at −10° C. for 5 minutes under a nitrogen atmosphere and then heating the sample at a rate of 10° C. / min to 140° C. If no inflection point appears, the mixture can be determined to have no glass transition temperature in the range of 0 to 15° C.

[0049] The asphalt composition of the present disclosure preferably satisfies the following (8) and (9). (8) The heterogeneous component of the complex shear viscosity at 100°C during the cooling process is 0.01 to 20 mPa s (9) Storage modulus at 60°C during heating is 100-5000 Pa

[0050] The hetero-phase component of the complex shear viscosity of the asphalt composition of the present disclosure at 100° C. during the cooling process is preferably 0.01 to 20 mPa·s. The asphalt composition of the present disclosure has a heterogeneous phase component with a complex shear viscosity in the above range, particularly at a low temperature of 100° C., so that the asphalt composition can be produced at low temperatures and has excellent low-temperature workability.

[0051] In JP 2018-035625 A, it is shown that the workability of an asphalt mixture can be predicted by the heterophase components of the complex shear viscosity of the asphalt composition. This is explained below. The asphalt composition behaves like a "liquid" in a temperature range of about 100°C to 140°C, which is the temperature range in which the asphalt composition is mixed with aggregate and compacted. Since the heterogeneous component of the complex shear viscosity only indicates the elastic properties of the asphalt composition, it is possible to confirm the extent to which the asphalt composition, which behaves like a liquid, contains "solid" components by measuring the heterogeneous component of the complex shear viscosity of the asphalt composition. Specifically, the heterogeneous component of the complex shear viscosity is highly correlated with the mix density, and for example, when the heterogeneous component of the complex shear viscosity is large, it is possible to predict the tendency for the mix density to decrease and the workability of the asphalt mix to deteriorate. In particular, by measuring the heterophase components of the complex shear viscosity during the temperature drop process, it is possible to perform accurate measurements by measuring the wax components and additives in a state where they are sufficiently dispersed in the asphalt composition after heating. This is because the temperature of the asphalt mixture drops over time at actual road paving construction sites (JP Patent Publication No. 2018-035625).

[0052] The heterogeneous component of the complex shear viscosity at 100°C during the temperature drop is preferably 0.01 mPa·s or more, more preferably 0.02 mPa·s or more, and even more preferably 0.03 mPa·s or more. Also, it is preferably 10 mPa·s or less, more preferably 7 mPa·s or less, even more preferably 1.0 mPa·s or less, and even more preferably 0.10 mPa·s or less. The heterogeneous phase component of the complex shear viscosity at 100°C during the temperature drop was measured in accordance with JIS K 7244-10: 2005. More specifically, it can be determined by the method described in the examples.

[0053] The storage modulus of the asphalt composition of the present disclosure at 60° C. during the heating process is preferably 100 to 5,000 Pa. When the storage modulus is within the above range, the asphalt composition has excellent durability at high temperatures. The storage modulus at 60°C is an index of heat resistance on paved roads in summer and also an index of strength of paved roads. The storage modulus at 60° C. during the temperature rise process is preferably 100 Pa or more, more preferably 110 Pa or more, and even more preferably 150 Pa or more, from the viewpoint of durability and heat resistance at high temperatures. Also, from the viewpoint of strength, it is preferably 5000 Pa or less, more preferably 1000 Pa or less, even more preferably 500 Pa or less, and even more preferably 200 Pa or less. The storage modulus at 60° C. during the temperature rise process can be measured using a viscoelasticity measuring device, with an angular frequency of 6.3 rad / sec, while raising the temperature from 20° C. to 160° C. at a rate of 5° C. / min and changing the strain linearly from 1% to 5%. More specifically, it can be determined by the method described in the Examples.

[0054] [Asphalt mixture] The asphalt mixture of the present disclosure contains the asphalt composition and aggregate, and the aggregate content is preferably 80 to 99 mass %.

[0055] In the asphalt mixture, the content of the aggregate is preferably 80 to 99 mass %, more preferably 90 to 97 mass %, based on the total mass of the asphalt mixture. The aggregate may be crushed stone, gravel, recycled aggregate, sand, etc., and is preferably dried by heating before mixing with the asphalt composition, but may be used without drying. In particular, when the asphalt composition of the present disclosure contains an organic silane compound (C), the adhesion between the asphalt and the aggregate is excellent, so that an asphalt mixture with the desired physical properties can be obtained without drying the aggregate. In the asphalt mixture, the content of the asphalt composition is preferably 1 to 20 mass %, and more preferably 3 to 10 mass %, based on the total mass of the asphalt mixture. Since the asphalt mixture of the present disclosure contains the asphalt composition described above, it can be produced at low temperatures and has excellent low-temperature workability.

[0056] <Method of producing asphalt composition and method of producing asphalt mixture> The asphalt composition of the present disclosure is not limited in its production method, so long as it contains a wax component (A) and asphalt (B), and 95 mass% or more of the wax component (A) is slack wax (A1) that satisfies the above (1) to (5). Furthermore, the asphalt mixture of the present disclosure contains the asphalt composition and aggregate, and there is no limitation on the manufacturing method as long as the aggregate content is preferably 80 to 99 mass%, but since it can be manufactured at low temperatures, it is preferable to obtain it by a manufacturing method having a step of mixing the asphalt composition and aggregate at 90 to 140° C. Manufacturing at low temperatures reduces energy consumption, contributes to reducing carbon dioxide emissions and costs, and further enables long-distance transportation from the factory where the mixture is manufactured to the construction site, thereby contributing to expanding the scope of construction.

[0057] As long as the asphalt mixture ultimately contains the asphalt composition and aggregate, it is also possible to mix a part of the components constituting the asphalt composition with the aggregate, and then mix the remaining components in. Specifically, there is a method in which the asphalt (B) and the aggregate are mixed in advance, and then the wax component (A) is mixed. The following describes a method for producing an asphalt composition and then an asphalt mix.

[0058] In the method of producing an asphalt composition and then producing an asphalt mixture, a production method including, in this order, a wax component mixing step, a first storage step (asphalt composition storage step), an aggregate mixing step, and a second storage step (asphalt mixture storage step) is preferred.

[0059] (Wax component mixing process) The wax component mixing step is preferably a step of heating and mixing asphalt (B), wax component (A), and any other optional components (organosilane compound (C), aromatic heavy mineral oil, reinforcing material, additives, etc.). When aromatic heavy mineral oil or the like is used, the aromatic heavy mineral oil or the like may be mixed with the asphalt (B) and stirred and mixed in a mixing vessel equipped with a stirring device at, for example, 140°C or higher to prepare an asphalt base oil in advance. In this process, a reinforcing material may be added at the same time. When a reinforcing material is added, it is preferable to set the temperature at 180°C or higher. In a mixing vessel, the wax component (A), the organosilane compound (C), and any other additives are added to the asphalt base oil. Then, the mixture is stirred and mixed for a predetermined time in a stirring device under conditions of, for example, 140° C. or higher and a rotation speed of 2,000 rpm to 4,000 rpm. By this process, an asphalt composition can be obtained.

[0060] (First storage step (asphalt composition storage step)) Next, the asphalt composition obtained in the wax component mixing step is transferred to a first product container for temporary storage and preservation. At this time, the temperature in the product container may be controlled so as to maintain a predetermined temperature.

[0061] (Aggregate mixing process) In the aggregate mixing step, after the asphalt composition is obtained or stored, aggregate is added to the asphalt composition as necessary, and the mixture is heated and mixed at a predetermined rotation speed to produce an asphalt mixture having desired properties. The aggregate is preferably dried by heating before mixing with the asphalt composition, but can be used without drying. In particular, when the asphalt composition of the present disclosure contains an organic silane compound (C), the adhesion between the asphalt and the aggregate is excellent, so that an asphalt mixture with the desired physical properties can be obtained without drying the aggregate. When producing an asphalt mixture, it is usually heated to 145°C or higher. However, since the asphalt composition of the present disclosure can be produced at low temperatures, an asphalt mixture having the desired properties can be obtained by mixing the asphalt composition and aggregate at 90 to 140°C. When selling or shipping the asphalt composition, this step is not necessary, and the product may be shipped immediately after the wax component mixing step, or may be stored for a certain period of time in the first storage step and then shipped as necessary.

[0062] (Second storage process (asphalt mixture storage process)) In the second storage step, the asphalt mixture obtained in the aggregate mixing step is transferred to a second product container for temporary storage and safekeeping. At this time, the temperature in the product container may be controlled to maintain a predetermined temperature. EXAMPLES

[0063] Next, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to these examples in any way.

[0064] [Analysis of Slack Wax (A1)] [1. Heat of fusion (ΔH)] Using a differential scanning calorimeter (Perkin-Elmer, "DSC-7"), 10 mg of the sample was held at -10°C for 5 minutes under a nitrogen atmosphere, and then heated to 140°C at 10°C / min to obtain a melting endothermic curve. The melting endothermic amount (ΔH) was calculated from the total area of ​​the melting peak in the obtained melting endothermic curve. The melting endotherm (ΔH) was calculated by determining the total area enclosed by the line including the peak of the melting endotherm obtained by DSC measurement using a differential scanning calorimeter (Perkin-Elmer, "DSC-7"), with a line connecting a point on the low temperature side where there is no change in heat quantity and a point on the high temperature side where there is no change in heat quantity as the baseline.

[0065] [2. Area of ​​each temperature range of the melting peak in the melting endothermic curve] The melting endothermic curve was obtained in the same manner as in [1. Melting endothermic amount (ΔH)]. Next, lines perpendicular to the horizontal axis (temperature axis) were drawn from the predetermined temperatures (20°C, 55°C, 80°C) of the melting endothermic curve to the baseline, and the areas enclosed by the lines corresponding to the melting endothermic curve, the baseline, and each temperature were defined as the areas of each temperature range. The ratio of the area of ​​each temperature range to the total area of ​​the melting peak was calculated, and defined as the ratio of the area of ​​each temperature range to the area of ​​the melting peak in the melting endothermic curve. Specifically, the "area below 20°C" was defined as the area surrounded by the melting endothermic curve, the baseline, and the line corresponding to 20°C; the "area from 20°C to below 55°C" was defined as the area surrounded by the melting endothermic curve, the baseline, the line corresponding to 20°C, and the line corresponding to 55°C; the "area from 55°C to below 80°C" was defined as the area surrounded by the melting endothermic curve, the baseline, the line corresponding to 55°C, and the line corresponding to 80°C; and the "area above 80°C" was defined as the area surrounded by the melting endothermic curve, the baseline, and the line corresponding to 80°C. When the melting peak does not include the above-mentioned temperature range, the area of ​​that temperature range was not included and the area of ​​that temperature range was set to zero.

[0066] 3. Number of butyl branches per 1000 carbon atoms Using the following equipment and conditions: 13 The C-NMR spectrum was measured. 13 The method for calculating the number of butyl branches per 1,000 carbon atoms from the results of C-NMR spectrum is also shown below. Equipment: JEOL Ltd., "JNM-EX400 NMR equipment" Method: Proton complete decoupling method Concentration: 220mg / mL Solvent: 90:10 (volume ratio) mixture of 1,2,4-trichlorobenzene and heavy benzene Temperature: 130℃ Pulse width: 45° Pulse repetition time: 4 seconds Accumulation: 10,000 times

[0067] <Calculation method> (Peak attribution: units are ppm, chemical shift) Methyl branch origin: 20.0, 33.3 From the ethyl branch: 11.2, 26.8, 39.7 Butyl branched: 23.4, 36.0, 38.0-38.2 Isobutyl branched: 23.4, 44.9, 36.0 Amyl branch origin: 32.7, 36.0, 38.0-38.2 Long chain (hexyl or more) branch origin: 36.0, 38.0-38.2

[0068] (How to calculate the branch ratio) The ratio of the number of alkyl branches is calculated from the ratio of the integrated intensities of the peaks originating from each branch. For peaks originating from multiple branches, the integrated intensities of the peaks whose attribution is clear were subtracted to calculate the integrated intensities originating from each alkyl branch. For peaks originating from multiple carbon atoms, the integrated intensity per carbon was calculated by dividing the peak by the number of carbon atoms.

[0069] (How to calculate the number of butyl branches per 1000 carbon atoms) As described below, the number of butyl branches obtained as described above was divided by the total number of all alkyl branches, and then multiplied by 1000 to obtain the number of butyl branches per 1000 carbon atoms. (Number of butyl branches per 1000 carbon atoms) = (Ratio of the number of butyl branches) / (Sum of the ratios of the number of alkyl branches) × 1000

[0070] [4. Weight-average molecular weight (Mw)] The weight-average molecular weight (Mw) was determined by gel permeation chromatography (GPC). For the measurement, the following apparatus and conditions were used to obtain the weight-average molecular weight in terms of polystyrene. [GPC measuring apparatus] Column: "TOSO GMHHR-H(S)HT" manufactured by Tosoh Corporation Detector: RI detector for liquid chromatogram "WATERS 150C" manufactured by Waters Corporation [Measurement conditions] Solvent: 1,2,4-trichlorobenzene Measurement temperature: 145 °C Flow rate: 1.0 mL / min Sample concentration: 2.2 mg / mL Injection volume: 160 μL Calibration curve: Universal Calibration Analysis program: HT-GPC (Ver. 1.0)

[0071] [Penetration at 23 °C] The penetration at 23 °C was measured by the following method in accordance with JIS K 2235:2022. The heated and melted sample was taken into a container, and after allowing it to cool until the temperature of the sample reached 23 °C, the depth at which the needle penetrated was measured to 0.1 mm at 23 °C using the following automatic penetration tester, and the value obtained by multiplying by 10 was taken as the penetration. Automatic penetration tester: Manufactured by RPM-101 Co., Ltd. Needle: Type 804 (for wax) Weight: Brass-made 50 ± 0.05 g Plunger: 47.5 ± 0.05 g of holding tool

[0072] [Wax components (wax component (A) and other wax components)] The wax components used in the asphalt compositions of the Examples and Comparative Examples are shown in Table 1.

[0073] [Table 1]

[0074] [Organosilane Compound (C)] Production Example 1 (Production of petroleum resin) 180 g of xylene was added to a 1-liter autoclave and the temperature was raised to 260° C. Then, a mixture of 100 g of dicyclopentadiene and 100 g of styrene was added over 3 hours. The temperature was maintained for an additional 75 minutes to carry out a polymerization reaction, and a polymer mixture was obtained. Thereafter, xylene was recovered from the resulting polymer mixture, and then the mixture was maintained at 20 mmHg for 2 hours to distill off low boiling points, yielding a petroleum resin having a softening point of 63.0°C and a bromine number of 58.

[0075] Production Example 2 (Production of hydrogenated petroleum resin) 180g of the petroleum resin obtained in Production Example 1, 180g of ethylcyclohexane, and 4g of a nickel-based catalyst (N110 series) manufactured by JGC Catalysts and Chemicals Co., Ltd. were charged into a 1-liter autoclave. Hydrogen was charged to 5MPa, and the temperature was raised from room temperature to 230°C. Thereafter, while maintaining the hydrogen pressure at 5MPa, a hydrogenation reaction was carried out for 8 hours to obtain a hydrogenated petroleum resin. The softening point of the obtained hydrogenated petroleum resin was 100°C, and the bromine number was 2.5.

[0076] Production Example 3 (Production of silane-modified hydrogenated petroleum resin) Into a 500 mL separable flask equipped with a nitrogen inlet tube and a stirring blade was placed 110 g of the hydrogenated petroleum resin obtained in Production Example 2, and the mixture was heated to 140° C. in an oil bath under a nitrogen stream. Once the hydrogenated petroleum resin had dissolved, 12 g of vinyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) was added with stirring, and the mixture was stirred until it became uniform. Next, 0.5 g of an organic peroxide (2,5-dimethyl-2,5-di(t-butylperoxy)hexane, trade name "Perhexa (registered trademark) 25B", manufactured by NOF Corporation) was added dropwise. After the addition, the mixture was stirred at an internal temperature (reaction mixture temperature) of 145° C. for 1 hour to react. After the reaction was completed, the contents of the flask were removed onto a stainless steel tray and dried under vacuum at 150°C for 1 hour to obtain 102 g of silane-modified hydrogenated petroleum resin. The bromine number of the obtained silane-modified hydrogenated petroleum resin was 2.3 g / 100 g, the silicon content was 0.8%, the weight average molecular weight was 1120, and the softening point was 92.5°C.

[0077] [Production of asphalt composition] Example 1 Into a 100 mL stainless steel cylindrical container, 36 g of straight asphalt (penetration 72, manufactured by Idemitsu Kosan Co., Ltd.) as asphalt (B) and 4 g of slack wax A (content in the asphalt composition: 10% by mass) as slack wax (A1) were placed, then heated using a mantle heater and stirred at 160°C for 15 minutes to obtain an asphalt composition.

[0078] Examples 2 to 6 and Comparative Examples 1 to 2, 4 to 5 An asphalt composition was obtained in the same manner as in Example 1, except that the wax components shown in Table 2 were used in place of the slack wax A in an amount shown in Table 2.

[0079] Example 7 An asphalt composition was obtained in the same manner as in Example 1, except that 36 g of propane deasphalted asphalt (B) (penetration 20, manufactured by Idemitsu Kosan Co., Ltd.) was used instead of 36 g of straight asphalt (penetration 72, manufactured by Idemitsu Kosan Co., Ltd.) and 4 g of slack wax C was used instead of 4 g of slack wax A.

[0080] Example 8 A 100 mL stainless steel cylindrical container was charged with 35.8 g of straight asphalt (penetration 72, manufactured by Idemitsu Kosan Co., Ltd.) as asphalt (B), 4 g of slack wax C (content in the asphalt composition: 10% by mass) as slack wax (A1), and 0.2 g of the silane-modified hydrogenated petroleum resin obtained in Production Example 3 (content in the asphalt composition: 0.5% by mass) as organosilane compound (C), and then heated using a mantle heater and stirred at 160°C for 15 minutes to obtain an asphalt composition.

[0081] Comparative Example 3 An asphalt composition was obtained in the same manner as in Example 1, except that slack wax A was not used and the amount of straight asphalt was 40 g.

[0082] [Evaluation of asphalt composition] The asphalt compositions obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Tables 2 and 3.

[0083] [1. Heterogeneous components of complex shear viscosity at 100℃ during cooling process (evaluation of low-temperature workability)] The heterogeneous phase components of the complex shear viscosity at 100°C during the cooling process were measured in accordance with JIS K 7244-10:2005. The results are shown in Table 2. The smaller the value of the heterogeneous component of the complex shear viscosity at 100°C during the temperature drop process, the better the low-temperature workability. The heterogeneous component of the complex shear viscosity at 100°C during the temperature drop process is an indicator of the mix density and workability of the asphalt mix. If the value of the heterogeneous component of the complex shear viscosity at 100°C during the temperature drop process exceeds 20 mPa·s and becomes too large, the low-temperature workability will be poor. Also, if the value of the heterogeneous component of the complex shear viscosity at 100°C during the temperature drop process becomes less than 0.01 mPa·s and becomes too small, the asphalt composition will not harden easily, resulting in poor workability. The specific measuring instruments and measurement conditions are shown below. Rheometer body: MCR302 (manufactured by Anton Paar) Temperature controller: P-PTD200 and H-PTD200 Fixture used: Parallel plate PP25 Measurement conditions (when temperature drops): Temperature: 160℃ to 20℃ at 5℃ / min Distortion: Linear change from 5% to 1% Angular frequency: 10rad / sec Measurement conditions (when heating): Temperature: 20℃ to 160℃ at 5℃ / min Distortion: Linear change from 1% to 5% Angular frequency: 10rad / sec

[0084] [2. Storage modulus at 60℃ during heating process (evaluation of heat resistance and strength)] The viscoelasticity was measured under the following conditions using a viscoelasticity measuring device (MCR302, manufactured by PerkinElmer) to obtain the storage modulus at 60°C during the heating process. The results are shown in Table 2. The larger the storage modulus at 60°C during the heating process, the better the heat resistance. The storage modulus at 60°C is an index of heat resistance on paved roads in summer. If the storage modulus at 60°C during the heating process is less than 100 Pa and is too small, the heat resistance will be poor. If the storage modulus at 60°C during the heating process is too large, exceeding 5000 Pa, the asphalt composition will become brittle and will have poor strength. Jig: 25mm parallel Temperature and strain: The temperature was lowered from 160°C to 20°C at a rate of 5°C / min. Then, the strain was held at 1% for 30 minutes. Next, the temperature was raised from 20°C to 160°C at a rate of 5°C / min, while the strain was changed linearly from 1% to 5%. Angular frequency: 6.3rad / sec

[0085] [3. Whether or not the mixture has a glass transition temperature (evaluation of compatibility)] The wax and straight asphalt used in the examples and comparative examples were mixed in a mass ratio of wax / straight asphalt = 1 / 4 to obtain a mixture. Next, a differential scanning calorimeter (Perkin-Elmer, "DSC-7") was used to obtain a melting endothermic curve by holding 10 mg of the mixture at -10°C for 5 minutes under a nitrogen atmosphere, and then heating it at 10°C / min to 140°C. If an inflection point appeared in the range of 0 to 15°C in the melting endothermic curve, the mixture was deemed to have a glass transition temperature, and if no inflection point appeared in the range of 0 to 15°C in the melting endothermic curve, the mixture was deemed not to have a glass transition temperature. When the wax does not have a glass transition temperature, the compatibility between the wax component and the asphalt is excellent, separation is unlikely, and the storage stability of the asphalt composition is also excellent.

[0086] [4. Boiling water peeling test (evaluation of water resistance and peeling resistance)] The asphalt composition and hard sandstone aggregate with a size of 9.5 mm to 13.2 mm were mixed according to the procedure shown below to obtain test specimens. 5.5 g ± 0.5 g of each asphalt composition that had been heated at 180°C for 1 hour was added to 100 g ± 0.5 g of hard sandstone aggregate that had been washed with water and dried, and the mixture was stirred for about 1 minute to prepare the test specimens. Ten specimens were selected from the above test pieces, and the selected specimens were placed in 100 mL of 1.0 mol / L aqueous sodium carbonate solution. The aqueous solution and the specimen in the aqueous solution were then heated on a hot plate, and heated for 1 minute after reaching 90°C. The specimen was then removed from the aqueous sodium carbonate solution and placed in ice water to cool. The specimen was dried, and the peeling area ratio of the specimen was measured. The peeling area ratio of the upper surface of the specimen was measured, and the peeling resistance was judged. When the peeled area ratio was less than 40%, the peel resistance was evaluated as “◯ (good)”, and when the peeled area ratio was 40% or more, the peel resistance was evaluated as “× (bad).” The results are shown in Table 3.

[0087] [Table 2]

[0088] [Table 3]

[0089] The results in Table 2 show that the asphalt composition of the present disclosure has a small, and not too small, value of the heterogeneous component of the complex shear viscosity at 100°C during the cooling process, and therefore the asphalt composition can be produced at low temperatures and the resulting asphalt mixture has excellent low-temperature workability. Manufacturing and construction at low temperatures reduces energy consumption, contributes to reducing carbon dioxide emissions and costs, and also makes it possible to transport the mixture over long distances from the factory where it is manufactured to the construction site, thereby contributing to the expansion of the range of construction possible. Furthermore, the asphalt composition of the present disclosure has a large, but not too large, storage modulus at 60°C during the heating process, resulting in excellent heat resistance and strength, and the resulting asphalt mixture has excellent heat resistance and high strength even when used on paved roads in the summer. In addition, from the results of Table 3, the asphalt composition of the present disclosure containing an organic silane compound has good results in the boiling water stripping test, and is excellent in water resistance and stripping resistance. This not only improves the performance of the resulting asphalt mixture, but also eliminates the need to heat and dry the aggregate, reducing energy consumption, reducing carbon dioxide emissions, and contributing to cost reduction.

Claims

1. Contains a wax component (A) and asphalt (B), An asphalt composition, wherein 95% by mass or more of the wax component (A) is a slack wax (A1) that satisfies the following (1) to (5). (1) Heat of fusion (ΔH) is 50 to 170 J / g (2) The area of ​​the melting peak in the melting endothermic curve below 20°C is 0 to 20%. (3) The area of ​​the melting peak in the melting endothermic curve that is 20°C or higher and less than 55°C is 40 to 70%. (4) The area of ​​the melting peak in the melting endothermic curve that is 55°C or higher and less than 80°C is 20 to 50%. (5) The area of ​​the melting peak at 80° C. or higher in the melting endothermic curve is 0%. (Note that the areas shown in (2) to (5) above are areas obtained by dividing the melting peak in a melting endothermic curve obtained by differential scanning calorimetry at a heating rate of 10° C. / min.)

2. The asphalt composition according to claim 1, wherein the slack wax (A1) is a slack wax that further satisfies the following (6) and (7). (6) The number of butyl branches per 1,000 carbon atoms is 0.1 or more. (7) Weight average molecular weight of 500 to 3,000

3. The asphalt composition according to claim 1, wherein the slack wax (A1) has a penetration at 23°C of 60 to 120.

4. The asphalt composition according to claim 1, wherein the combination of the wax component (A) and the asphalt (B) is such that the mixture [(A) / (B)=1 / 4] does not have a glass transition temperature within the range of 0 to 15°C.

5. The asphalt composition according to claim 1, wherein the content of the wax component (A) is 1 to 20 mass%.

6. The asphalt composition according to claim 1, further comprising 0.1 to 5 mass% of an organic silane compound (C).

7. The asphalt composition according to claim 1, wherein the asphalt composition satisfies the following (8) and (9). (8) The heterogeneous phase component of the complex shear viscosity at 100°C during the cooling process is 0.01 to 20 mPa·s (9) Storage modulus at 60°C during heating is 100 to 5000 Pa

8. An asphalt mixture comprising the asphalt composition according to any one of claims 1 to 7 and aggregate, wherein the aggregate content is 80 to 99 mass%.

9. A method for producing an asphalt mixture, comprising a step of mixing the asphalt composition according to any one of claims 1 to 7 with aggregate at 90 to 140 ° C.

Citation Information

Patent Citations

  • A method to produce a foamed bitumen and a wax dispersion therefor

    EP3992253A1

  • Molecular weight fraction from solid wax

    JP1992145103A

  • Bitumen composition containing a wax mixture consisting of petroleum slack wax and Fischer-Tropsch wax, use of the wax mixture in a bitumen composition, use of the bitumen composition in an asphalt composition, asphalt composition containing the bitumen composition, and method for producing asphalt road pavements therefrom

    JP2019517607A

  • Compositions and methods for restoration of a low-sloped roof

    US20230092077A1

  • Asphalt composition, asphalt composition manufacturing apparatus, asphalt composition manufacturing system, asphalt mixture, asphalt composition manufacturing method and asphalt mixture manufacturing method