Copper alloy sheet material, method for producing the same, and current-carrying component

A Cu-Fe-P copper alloy with controlled composition and manufacturing processes addresses the trade-off in strength, conductivity, and bendability, enhancing the performance and reducing costs of board-to-board connectors.

JP2024141255APending Publication Date: 2024-10-10DOWA METALTECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052793
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing Cu-Fe-P copper alloys used in board-to-board connectors face a trade-off between strength, conductivity, and bendability, failing to meet the demands of smaller, higher-current connectors.

Method used

A Cu-Fe-P copper alloy with specific compositional ranges (Fe 0.05-1.10%, P 0.02-0.50%, Mg 0-0.50%, Ni 0-0.80%, Sn 0-0.80%, Zn 0-0.80%, and other elements ≤0.10%) and controlled manufacturing processes, including hot rolling, intermediate and final cold rolling, and heat treatments, to achieve a crystallite size ≤30 nm and precipitate particle density of 50 particles/μm², enhancing strength, conductivity, and bendability.

Benefits of technology

The alloy achieves high strength, conductivity, and improved bendability, reducing manufacturing costs and improving the performance of board-to-board connectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a Cu-Fe-P-based copper alloy sheet material which exhibits excellent strength and electrical conductivity and also has a higher level of bending workability.SOLUTION: There is provided a copper alloy sheet material which has a chemical composition containing, in terms of mass%, 0.05 to 1.10% of Fe, 0.02 to 0.50% of P, 0 to 0.50% of Mg, 0 to 0.80% of Ni, 0 to 0.80% of Sn, 0 to 0.80% of Zn, and a total of 0 to 0.10% of elements other than Fe, P, Mg, Ni, Sn, Zn and Cu, with the remainder comprising Cu. The crystallite size, as determined using the Halder-Wagner method on the basis of integrated widths of peaks in an X-ray diffraction pattern using Cu-Kα rays on a surface of the sheet, is 30 nm or less. The 0.2% proof stress in a direction perpendicular to the direction of rolling is 450 N / mm2 or more.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Cu-Fe-P-based copper alloy sheet suitable for a connector for connecting board-to-board (sometimes referred to as "BtoB" or "BTB"), a method for manufacturing the same, and an electrically conductive part using the copper alloy sheet. [Background technology]

[0002] Among the copper alloys used in current-carrying parts such as connectors, there are Cu-Fe-P copper alloys that use relatively inexpensive additive elements and can be strengthened by Fe-P precipitates. Patent Document 1 describes a Cu-Fe-P-based copper alloy material that combines strength, electrical conductivity, and drawability by enhancing the orientation of the {220} plane. It describes that the material is produced by a process in which cold rolling and recrystallization annealing are repeated after hot rolling, and stress relief annealing is performed after the final cold rolling. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5467163 Summary of the Invention [Problem to be solved by the invention]

[0004] In a connector, conduction between paired pins (current-carrying components) is ensured by fitting the bent portions of both pins together. A board-to-board connector is made up of many pins, each of which is subjected to a complex bending process. When inserting and removing a board-to-board connector, some pins may be subjected to a large amount of stress depending on slight misalignment between the boards and the method of insertion and removal (how it is handled). For this reason, it is extremely important that the bent portions of each pin are quality-controlled to be in a sound state without cracks. It is also important that the connector has high strength and high conductivity.

[0005] In recent years, as board-to-board connectors have become smaller, lower profile, and larger current capable, the materials used therein are required to have higher levels of strength, conductivity, and bending workability than ever before. According to the technology of Patent Document 1, it is possible to obtain a Cu-Fe-P-based copper alloy sheet material having excellent strength and electrical conductivity. However, since there is generally a trade-off between strength and bending workability, there is still room for improvement in terms of providing excellent bending workability that can meet the strict requirements of recent board-to-board connectors.

[0006] An object of the present invention is to provide a Cu-Fe-P based copper alloy sheet material that is excellent in strength and electrical conductivity and has an improved level of bending workability. [Means for solving the problem]

[0007] In order to achieve the above object, the present specification discloses the following invention. [1] The chemical composition is, by mass%, 0.05-1.10% Fe, 0.02-0.50% P, 0-0.50% Mg, 0-0.80% Ni, 0-0.80% Sn, 0-0.80% Zn, the sum of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0-0.10%, and the balance is Cu. The crystallite size according to the Halder-Wagner method based on the integral width of the peak in the X-ray diffraction pattern using CuKα radiation on the plate surface is 30 nm or less, and the 0.2% proof stress in the direction perpendicular to the rolling direction is 450 N / mm 2 That is all about the copper alloy sheet material. [2] In the observation plane parallel to the plate surface, the number density of precipitate particles with a major axis of 10 to 100 nm is 50 particles / μm 2 The copper alloy sheet material according to the above-mentioned [1]. [3] The copper alloy sheet material according to [1] or [2] above, having an electrical conductivity of 50% IACS or more. [4] The copper alloy sheet material according to any one of the above [1] to [3], wherein a ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a 90°L bending test with the bending axis parallel to the rolling direction (BW) is 0.7 or less.

[0008] The copper alloy sheets [1] to [4] above can be produced by the following method. [5] A hot rolling process in which a slab having a chemical composition, in mass%, of Fe 0.05-1.10%, P: 0.02-0.50%, Mg: 0-0.50%, Ni: 0-0.80%, Sn: 0-0.80%, Zn: 0-0.80%, the sum of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0-0.10%, and the balance being Cu is subjected to rolling at a rolling reduction rate of 70% or more in a temperature range of 950°C to 650°C and then to rolling at a rolling reduction rate of 60% or more in a temperature range of 350°C to 650°C; An intermediate cold rolling process in which cold rolling is performed at a rolling ratio of 30% or more; An intermediate heat treatment step in which the material obtained in the intermediate cold rolling step is subjected to a heat treatment at a temperature of 400°C or more and 700°C or less for one hour or more; A finish cold rolling process in which the material obtained in the intermediate heat treatment process is subjected to cold rolling at a rolling ratio of 80% or more; A finish heat treatment process in which the material obtained in the finish cold rolling process is subjected to a heat treatment in a temperature range of 180 ° C. or more and 500 ° C. or less; A method for producing a copper alloy sheet material, comprising the steps of: [6] The method for producing a copper alloy sheet material according to the above-mentioned [5], wherein in the finish heat treatment step, a material is obtained having a crystallite size of 30 nm or less as determined by the Halder-Wagner method based on the integral width of a peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface.

[0009] The present invention also provides the following: [7] An electrical conductive part using the copper alloy sheet material according to any one of [1] to [4] above.

[0010] In this specification, the notation "n1~n2" indicating a numerical range means "n1 or more and n2 or less". Here, n1 and n2 are numerical values satisfying n1 < n2. "Sheet material" means a sheet-shaped metal material formed by utilizing the malleability of metal. A thin sheet-shaped metal material may also be called "foil", and such "foil" is also included in the "sheet material" referred to herein. A long sheet-shaped metal material wound in a coil shape is also included in the "sheet material". In this specification, the thickness of the sheet-shaped metal material is referred to as "sheet thickness". "Sheet surface" is a surface perpendicular to the sheet thickness direction of the sheet material. "Sheet surface" may also be called "rolling surface". The "major axis" of a particle is defined as the diameter of the smallest circle surrounding the particle. The "number density of precipitate particles with a major axis of 10 to 100 nm" can be obtained as follows.

[0011] [Method for obtaining the number density of precipitate particles] For the observation surface obtained by electrolytic polishing the sheet surface under the following electrolytic polishing conditions and then performing ultrasonic cleaning in ethanol for 20 minutes using an ultrasonic cleaner, observe with a field emission scanning electron microscope (FE-SEM) at an acceleration voltage of 15 kV and a magnification of 100,000 times, and randomly set an observation field in which some or all of the particles with a major axis of 1.0 μm or more are not included in the field of view. For that observation field, count the number of precipitate particles with a major axis of 10 to 100 nm among the particles whose entire contour can be seen. Perform this operation for a plurality of non-overlapping observation fields so that the total observed area is 10 to 100 μm 2 and divide the total count obtained by the above counting in all the observed fields by the total area of the observation fields, and the value obtained is the number density of precipitate particles (particles / μm 2 ). (Electrolytic polishing conditions) · Electrolyte: A mixture of distilled water, phosphoric acid, ethanol, and 2-propanol in a volume ratio of 10:5:5:1 · Liquid temperature: 20°C · Voltage: 15 V · Electrolysis time: 20 seconds

[0012] The rolling rate in a certain process is obtained by the following formula (1). Rolling rate (%) = [(t0 - t1) / t0] × 100 …(1) t0: Plate thickness before rolling in that process (mm) t1: Plate thickness after rolling in that process (mm) Effect of the Invention

[0013] According to the present invention, a sheet material having high levels of strength, electrical conductivity, and bending workability has been realized in a Cu-Fe-P-based copper alloy. This sheet material uses relatively inexpensive additive elements and can be manufactured in a process that does not require solution treatment or repeated cold rolling and recrystallization annealing, so it is advantageous in terms of manufacturing cost compared to high-strength sheet materials of the same type of copper alloy or other copper alloys. The present invention contributes to improving the performance and reducing the cost of board-to-board connectors, which are becoming increasingly smaller in size. [Brief description of the drawings]

[0014] [Figure 1] This is a laser microscope photograph of the outer surface of the bent portion of a sheet material sample (intermediate product) after finish cold rolling, which is an intermediate stage in the manufacturing process of invention example No. 2, in a 90°L bending test at BW with an R / t of approximately 0.6. [Diagram 2] A laser microscope photograph of the outer surface of the bent portion of a plate sample (finished product) after final heat treatment obtained in Invention Example No. 2, which was subjected to a 90°L bending test at BW with an R / t of approximately 0.6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [Chemical composition] The present invention is directed to a Cu-Fe-P based copper alloy. Hereinafter, "%" regarding the alloy components means "mass %" unless otherwise specified.

[0016] Fe (iron) forms a compound with P and precipitates finely in the matrix (metallic base of copper alloy), thereby contributing to improving strength. To fully exert this effect, the Fe content must be 0.05% or more. Excessive Fe content can lead to a decrease in electrical conductivity, so the Fe content must be in the range of 1.10% or less. It is more preferable that the Fe content be 0.90% or less, and even more preferable that the Fe content be 0.50% or less, and it may be 0.30% or less.

[0017] P (phosphorus) generally serves as a deoxidizer for copper alloys, but in the present invention, it forms fine precipitates of Fe-P compounds or even Mg-P compounds, thereby contributing to improving strength. In order to fully exert this effect, the P content is ensured to be 0.02% or more. It is more preferable that it is 0.03% or more, and even more preferable that it is 0.05% or more. Since hot cracking is more likely to occur when the P content is high, the P content is set to 0.50% or less. It is more preferable that it is 0.30% or less, and it may be controlled to 0.15% or less.

[0018] The Cu-Fe-P based copper alloy may contain one or more of Mg (magnesium), Ni (nickel), Sn (tin) and Zn (zinc) as required. Like Fe, Mg forms a compound with P and contributes to improving strength. When Mg is contained, it is more effective to set the content to 0.03% or more. If the Mg content is high, Mg oxides are likely to be entrapped during hot rolling, so the Mg content is set to a range of 0.50% or less. It is more preferable that the Mg content is 0.30% or less, and even more preferable that the Mg content is 0.20% or less. It is also preferable to set the Mg content so that the total content of Fe and Mg is 1.10% or less. The (Fe+Mg) / P ratio, which represents the mass ratio of the total content of Fe and Mg to the P content, is preferably in the range of 0.4 to 13.0, and more preferably in the range of 0.5 to 12.5.

[0019] Ni, Sn, and Zn are dissolved in the matrix and contribute to improving heat resistance. When one or more of these elements are contained, from the viewpoint of maintaining high electrical conductivity, the content of each of Ni, Sn, and Zn is allowed to be up to 0.80%, and it is more preferable that each of them is in the content range of 0.50% or less, and each of them may be controlled to be in the content range of 0.30% or less. When one or more of Ni, Sn, and Zn are contained, it is effective to set each of the contained elements to 0.001% or more, and it is more effective to set each of them to 0.002% or more.

[0020] The inclusion of other elements is permitted within a range that does not impair the object of the present invention (combining strength, electrical conductivity, and bending workability at a high level). Specifically, the total content of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu (copper) may be controlled to 0.10% or less. For example, depending on the application, one or more of Al (aluminum), B (boron), Co (cobalt), Cr (chromium), Mn (manganese), Pb (lead), S (sulfur), Si (silicon), Te (tellurium), Ti (titanium), and Zr (zirconium) may be contained so that the total content of these elements is 0.10% or less. In addition, when one or more of Al, B, Co, Cr, Mn, Pb, S, Si, Te, Ti, and Zr are contained, the content of each of these elements may be, for example, 0.001% or more.

[0021] An example of an alloy composition in which the total content of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu is 0.10% or less is "a chemical composition consisting of, in mass%, Fe 0.05-1.10%, P: 0.02-0.50%, Mg: 0-0.50%, Ni: 0-0.80%, Sn: 0-0.80%, Zn: 0-0.80%, Al, B, Co, Cr, Mn, Pb, S, Si, Te, Ti, and Zr in total: 0-0.10%, and the balance being Cu and unavoidable impurities." In this case, the unavoidable impurities refer to elements that are inevitably mixed in during manufacturing and are other than the elements listed above.

[0022] [Crystallite size] The inventors have found that by reducing the crystallite size, bending workability can be significantly improved while maintaining high strength and high electrical conductivity. Specifically, it is extremely effective that the crystallite size according to the Halder-Wagner method based on the integral width of the peak in the X-ray diffraction pattern using CuKα radiation on the plate surface is 30 nm or less, and more preferably 25 nm or less. There is no particular lower limit for the crystallite size, but according to previous investigations, it is considered that the crystallite size may be adjusted to, for example, a range of 10 to 30 nm, and may be controlled to a range of 15 to 25 nm.

[0023] The Halder-Wagner method is based on the integral width β of each of the multiple diffraction peaks in the X-ray diffraction pattern, with the horizontal axis being β / (tanθ×sinθ) and the vertical axis being (β / tanθ). 2 Then, an approximation line of the following equation (2) is drawn for the plots, and the crystallite size D is calculated from the slope Kλ / D of the line. (β / tanθ) 2 =(Kλ / D)×[β / (tanθ×sinθ)]+16ε 2 ……(2) Here, β is the integral width of the diffraction peak, θ is the Bragg angle of the diffraction peak, K is the Scherrer constant, λ is the X-ray wavelength (nm), D is the crystallite size (nm), and ε is the lattice distortion. Here, the integral width β of four diffraction peaks resulting from the crystal planes (111), (200), (220), and (311) in the diffraction angle 2θ range of 30 to 150° is measured, and the Halder-Wagner method is applied.

[0024] [Number density of precipitate particles] Precipitate particles with a major axis of 10 to 100 nm contribute to improving the strength of copper alloy sheets. The number density of precipitate particles with a major axis of 10 to 100 nm is 50 particles / μm 2 The upper limit of the number density is not particularly limited, but the number density is usually 200 particles / μm 2 Less than 150 particles / μm 2 It may be managed as follows:

[0025] [0.2% yield strength] In order to meet the needs for smaller and thinner current-carrying components, it is important to maintain a high level of strength. Considering the use of board-to-board connectors, the 0.2% yield strength of copper alloy sheet material in the transverse direction (TD) of rolling is 450N / mm 2 It is preferable that it is more than 500Nmm 2 More preferably, it should be 550N / mm 2 The 0.2% yield strength of the copper alloy sheet material of the present invention is usually 900 N / mm 2 Adjustment within the following range is sufficient: 700N / mm 2 It may be managed as follows:

[0026] [conductivity] Considering the use of current-carrying parts such as connectors, the electrical conductivity of the copper alloy sheet is preferably 50% IACS or more, more preferably 65% ​​IACS or more. It is also possible to adjust it to 70% IACS or more. In the copper alloy sheet having the above-mentioned composition range, the electrical conductivity is usually 90% IACS or less, and may be controlled to 85% IACS or less.

[0027] [Bending workability] Considering the use of board-to-board connectors that undergo complex bending, the ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a 90°L bending test with the bending axis parallel to the rolling direction (BW) of the copper alloy sheet material is preferably 0.7 or less, and more preferably 0.5 or less. According to the manufacturing method described below, it is also possible to adjust the above MBR / t to a level of bending workability that is extremely excellent for a Cu-Fe-P-based copper alloy, such as 0.3 or less.

[0028] [Manufacturing method] The copper alloy sheet material described above can be obtained, for example, by the following manufacturing process. Melting / casting → hot rolling → intermediate cold rolling → intermediate heat treatment → final cold rolling → final heat treatment Although not described in the above steps, facing is performed as necessary after hot rolling, and pickling, polishing, or further degreasing is performed as necessary after each heat treatment. Each step will be described below.

[0029] [Melting and Casting] A copper alloy having the above-mentioned chemical composition is melted to obtain a cast piece. As a casting method, a known method such as a semi-continuous casting method or a continuous casting method can be applied. An ingot (cast piece) obtained by an ingot casting method is also included in the "cast piece" as used in this specification.

[0030] [Hot rolling] After heating the slab, it is subjected to hot rolling. The heating temperature of the slab is preferably 850 to 1000°C. The holding time in the above temperature range is preferably 0.3 hours or more, and more preferably 0.5 to 10 hours. This heating and holding promotes homogenization of the cast structure (mitigation of solidification segregation) and promotes solid solution of coarse Fe-P compounds and Mg-P compounds.

[0031] The heated slab is removed from the furnace and hot rolling begins. Hot rolling is performed according to a pass schedule in which rolling at a reduction rate of 70% or more is performed in a temperature range of 950°C or less and 650°C or more, followed by rolling at a reduction rate of 60% or more in a temperature range of 350°C or more and less than 650°C. The rolling temperature in each rolling pass can be monitored by the surface temperature of the material immediately after it leaves the work rolls of the hot rolling mill. "Rolling at a reduction rate of 70% or more in a temperature range of 950°C or less and 650°C or more" means that the rolling reduction rate is 70% or more, expressed as [(h0-h1) / h0] x 100(%), where h0 (mm) is the plate thickness (slab thickness) before the start of the first rolling pass where the rolling temperature is 950°C or less, and h1 (mm) is the plate thickness after the end of the last rolling pass where the rolling temperature is 650°C or more. In addition, "rolling at a reduction ratio of 60% or more in a temperature range of 350°C or more but less than 650°C" means that, when the sheet thickness before the start of the first rolling pass where the rolling temperature is less than 650°C is h1 (mm), and the sheet thickness after the end of the last rolling pass where the rolling temperature is 350°C or more is h2 (mm), the rolling reduction ratio, expressed as [(h1-h2) / h1]×100(%), is 60% or more.

[0032] In the temperature range of 950°C or less and 650°C or more, dynamic recrystallization is likely to occur. In order to obtain a structure consisting of fine and highly uniform crystal grains from a coarse and non-uniform cast structure, it is extremely effective to set the rolling ratio in the temperature range of 950°C or less and 650°C or more to 70% or more, and it is even more effective to set it to 80% or more. In the temperature range of 950°C or less and 650°C or more, the rolling ratio may be adjusted to, for example, 92% or less. On the other hand, in the temperature range of less than 650°C and 350°C or more, Fe-P compounds and Mg-P compounds are likely to precipitate. In order to generate many precipitation nuclei of Fe-P compounds and Mg-P compounds, it is extremely effective to set the rolling ratio in the temperature range of less than 650°C and 350°C or more to 60% or more. In the temperature range of less than 650°C and 350°C or more, the rolling ratio may be set to, for example, 85% or less, or may be set to 75% or less. By leaving the material (hot-rolled sheet) after hot rolling in a structural state in which a large amount of precipitation nuclei of the above compounds or extremely fine precipitates resulting from them are present, it becomes possible to rapidly and sufficiently generate fine precipitates of Fe-P compounds and Mg-P compounds in the intermediate heat treatment step described below, which is performed without going through a solution treatment step. The sheet thickness after hot rolling may be adjusted, for example, in the range of 5 to 20 mm depending on the final target sheet thickness.

[0033] [Intermediate cold rolling] The material after hot rolling is subjected to cold rolling at a rolling reduction of 30% or more, more preferably 35% or more, and even more preferably 55% or more. The upper limit of the cold rolling reduction can be set according to the target plate thickness and the mill power of the cold rolling machine. Usually, the rolling reduction is 95% or less, and may be set in the range of 85% or less. Note that, as long as the structure state containing a large amount of precipitation nuclei of Fe-P-based compounds and Mg-P-based compounds formed by hot rolling or ultrafine precipitates resulting therefrom is maintained, this intermediate cold rolling may be performed on the material that has been subjected to cold rolling and annealing one or more times to reduce the plate thickness, as necessary.

[0034] [Intermediate heat treatment] The material obtained by the above intermediate cold rolling is subjected to a heat treatment in which it is held at a temperature of 400°C to 700°C for 1 hour or more. Since a large amount of precipitation nuclei of Fe-P compounds and Mg-P compounds or extremely fine precipitates resulting therefrom are formed by the above hot rolling, and cold working strain is added by the above intermediate cold rolling, it is possible to rapidly form a large amount of precipitates consisting of Fe-P compounds and Mg-P compounds by heating and holding at a temperature range of 400°C to 700°C. Specifically, the density of precipitates having a particle diameter of 10 to 100 nm is set to 50 precipitates / μm 2 It is possible to adjust the temperature to above 400°C. It is also possible to obtain a fine and highly uniform recrystallized structure. If the maximum temperature of the material exceeds 700°C, the recrystallized grains may become coarse. There is no particular upper limit to the holding time at 400°C to 700°C, but it is usually sufficient to hold the material for no more than 24 hours.

[0035] [Finishing cold rolling] The material obtained by the intermediate cold rolling is subjected to cold rolling at a rolling ratio of 80% or more to adjust the final plate thickness and further improve the strength. By setting the rolling ratio at 80% or more, a large amount of dislocations can be introduced, which is advantageous for obtaining a structure with a small crystallite size in the finishing heat treatment described below. It is more effective to set the rolling ratio at 90% or more, and even more effective to set it at 95% or more. The upper limit of the rolling ratio may be set, for example, in the range of 99% or less depending on the mill power.

[0036] [Finishing heat treatment] The material obtained by the above-mentioned finish cold rolling is subjected to a heat treatment in which the material is heated to a temperature range of 180°C to 500°C. Since cold working strain is introduced by the above-mentioned finish cold rolling, even if the time for which the material is held in the temperature range of 180°C to 500°C is short, for example, about a few seconds, the crystallite size can be reduced by rearrangement of dislocations. As specific heat treatment conditions, the optimum conditions for obtaining a material having a crystallite size of 30 nm or less may be applied depending on the heat treatment furnace. However, the maximum temperature is set to a range of 180°C to 500°C. Either a continuous heat treatment furnace or a batch heat treatment furnace may be used as the heat treatment furnace. In the case of a continuous heat treatment furnace, the time for which the material temperature is 180°C to 500°C (hereinafter referred to as "heat treatment time") can be easily set in the range of, for example, 3 to 120 seconds. In the case of a batch heat treatment furnace, the heat treatment time can be easily set in the range of, for example, 10 minutes or more. The upper limit of the heat treatment time is not particularly specified, but it can be set in the range of, for example, 5 hours or less.

[0037] The mechanism by which this final heat treatment can produce a structure with small crystallite sizes has not been fully elucidated, but the intermediate heat treatment reduces the number of precipitates with particle sizes of 10 to 100 nm to 50 / μm. 2 It is presumed that the pinning effect of the finely dispersed precipitates is exerted when the material is heated to a temperature range of 180 to 500 ° C., and that the rearrangement of dislocations occurs in a form favorable for miniaturization of crystallite size. If the heating temperature is 180 ° C. or higher, it is believed that the rearrangement of dislocations can be caused, and as a result, the crystallite size can be miniaturized. It is believed that the dislocations introduced by the finish cold rolling can be sufficiently retained by controlling the maximum temperature of the material to 500 ° C. or lower, and as a result, softening can be prevented.

[0038] In this manner, a Cu-Fe-P-based copper alloy sheet having excellent strength, electrical conductivity, and bending workability can be obtained. The thickness of the sheet can be, for example, 0.02 to 2.0 mm, preferably 0.04 to 0.8 mm. This Cu-Fe-P-based copper alloy sheet can be used as a material to manufacture conductive parts such as connectors by, for example, punching or bending. EXAMPLES

[0039] A copper alloy having the chemical composition shown in Table 1 was melted and cast pieces having a thickness of 215 mm, a width of approximately 500 mm, and a length of approximately 5,500 mm were obtained. Samples taken from the cast pieces were quantitatively analyzed using the method described below. As a result, it was found that all of the examples met the requirement of "total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10 mass%."

[0040] (Elemental analysis method) O (oxygen) and N (nitrogen) were quantified using an oxygen / nitrogen / hydrogen analyzer (LECO, ONH-836), H (hydrogen) was quantified using a hydrogen analyzer (HORIBA, EMGA-921), C (carbon) and S (sulfur) were quantified using a carbon-sulfur analyzer (LECO, CS844), elements from the second to sixth periods (excluding C, N, O, group 17 elements, group 18 elements, Tc (technetium), Po (polonium), and Pm (promethium)) were quantified using an ICP-MS (Agilent, 7900), and F (fluorine), Cl (chlorine), and Br (bromine) were quantified using a combustion-ion chromatography apparatus (Thermo Scientific, DIONEX ICS-1600). These measurements allow the quantification of virtually all elements that may be contained in copper alloys.

[0041] The obtained slab was held at 950°C for 4 hours, removed from the furnace, and then subjected to hot rolling. The rolling temperature in each rolling pass was recorded by monitoring the material surface temperature at the work roll exit side of the hot rolling mill. Except for some examples (Comparative Examples No. 33 and 39), the pass schedule was set so that the rolling reduction ratio at rolling temperatures of 950°C or less and 650°C or more was 87%, and the rolling reduction ratio at rolling temperatures of 650°C or less and 350°C or more was 63 to 68%. In No. 39, the pass schedule was set so that the rolling reduction ratio at rolling temperatures of 950°C or less and 650°C or more was 87%, and the rolling reduction ratio at rolling temperatures of 650°C or less and 350°C or more was 50%. The total rolling reduction ratio was 95.1 to 95.8%, and the rolling temperature of the final pass was 350°C or more in all examples. In this way, hot-rolled sheets with a thickness of 9.5 to 11.0 mm were obtained. In No. 33, cracks occurred in the material during hot rolling, so further processing was discontinued.

[0042] With the exception of some examples (Comparative Example No. 35), the surface oxide film of the obtained hot-rolled sheet was removed by mechanical polishing (face grinding), and then cold rolling was performed at a rolling ratio of about 67 to 98% (intermediate cold rolling process). Since No. 35 had a large amount of Mg oxide inclusions in the hot-rolled sheet, it was not allowed to proceed to the process after hot rolling. The material after the above cold rolling was subjected to a heat treatment in a batch-type heat treatment furnace at a holding temperature set in the range of 500 to 600° C. for 5 to 9 hours (intermediate heat treatment step). Next, except for some examples (Comparative Example No. 41), cold rolling was performed at a rolling reduction rate of about 87 to 98% to a sheet thickness of 0.06 to 0.08 mm (finish cold rolling process). In No. 41, cold rolling was performed at a rolling reduction rate of about 60% to a sheet thickness of 0.10 mm. Next, except for some examples (Comparative Example No. 40), heat treatment was performed in a continuous heat treatment furnace or a batch heat treatment furnace under the conditions of a maximum temperature of 200 to 430°C and a time (heat treatment time) for the material temperature to be 180°C or higher but lower than the maximum temperature of 13 seconds to 30 minutes (final heat treatment step). This heat treatment was omitted in No. 40. In this way, test pieces with a final thickness of 0.06 to 0.10 mm were obtained. The manufacturing conditions are shown in Table 2. The obtained test pieces were subjected to the following investigations.

[0043] (Number density of precipitate particles) According to the above-mentioned "How to calculate the number density of precipitate particles", the number density (particles / μm 2 The electrolytic polishing apparatus used was a BUEHLER ElectroMet4, the ultrasonic cleaner was a BRANSONIC M2800-J, and the FE-SEM was a JEOL JSM-7200F.

[0044] (Crystallite size) The X-ray diffraction pattern of the plate surface of the test material was measured using an X-ray diffractometer (Rigaku, RINT-2000) under the conditions of 2θ / θ method, CuKα radiation (λ=0.1542 nm), tube voltage 40 kV, and tube current 40 mA. Using analysis software (Rigaku, PDXL2), the Kα1 radiation and Kα2 radiation were analyzed without separating them, and the integral width β was measured for the four diffraction peaks due to the crystal planes (111), (200), (220), and (311) in the 2θ range of 30 to 150°. The horizontal axis is β / (tanθ×sinθ) and the vertical axis is (β / tanθ). 2 The function (Halder-Wagner formula) expressed by the above formula (2) was obtained by fitting each plot with a straight line, and the crystallite size D (nm) was calculated from the slope of the function Kλ / D (K: Scherrer constant, λ: X-ray wavelength, D: crystallite size). Here, 0.94 was adopted as the value of the Scherrer constant K.

[0045] (0.2% yield strength) Tensile test pieces (JIS No. 5) were taken from each test material in the transverse direction (TD) and a tensile test was conducted in accordance with JIS Z2241 to measure the 0.2% yield strength. The 0.2% yield strength was 450N / mm 2 Those that met the above criteria were judged to be acceptable.

[0046] (conductivity) The electrical conductivity was determined in accordance with JIS H0505. A sample with a conductivity of 50% IACS or higher was judged to be acceptable.

[0047] (Bending workability) A 0.3 mm wide test piece with its longitudinal direction perpendicular to the rolling direction was cut out from the test material, and a 90°L bending test was performed with the bending axis parallel to the rolling direction (BW). The ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the plate thickness t was calculated. A specimen with an MBR / t of 0.7 or less was judged to pass. The above results are shown in Table 3.

[0048] [Table 1]

[0049] [Table 2]

[0050] [Table 3]

[0051] All of the Cu-Fe-P based copper alloy sheets of the present invention had a structure with a high number density of precipitate particles and small crystallite size, and had excellent strength, electrical conductivity, and bending workability.

[0052] In contrast, the comparative examples gave the following results: No. 31 had poor electrical conductivity because the Fe content was too high. No. 32 had low strength because the Fe content was too low. No. 33 had too high a P content, which caused cracks during hot rolling. No. 34 had a low P content, which resulted in an insufficient density of precipitate particles, resulting in poor strength and electrical conductivity. The dislocation density was low, so the crystallite size could not be reduced even after finishing heat treatment. However, the material was soft, so bending workability was good. In No. 35, the Mg content was too high, resulting in a hot-rolled sheet with a large amount of Mg oxide inclusions, and the subsequent process was discontinued. No. 36 had poor conductivity because the Ni content was too high. No. 37 had poor conductivity because the Sn content was too high. No. 38 had poor conductivity because the Zn content was too high. In No. 39, the rolling ratio in the temperature range of less than 650°C and more than 350°C was low during hot rolling, so the number density of precipitate particles was insufficient, resulting in poor strength and electrical conductivity. Since the dislocation density was low, the crystallite size could not be reduced even after finishing heat treatment. In addition, because it was soft, bending workability was good. In No. 40, the finish heat treatment was omitted, so the crystallite size could not be reduced, and the bending workability was poor. In No. 41, the reduction ratio in the finish cold rolling was low, so although the crystallite size was small, the introduction of dislocations was insufficient and the strength level was low.

[0053] (Test to confirm the effectiveness of finishing heat treatment) The plate material sample (intermediate product with a plate thickness of 0.08 mm) at the time of completing the finish cold rolling of the above No. 2, which is an example of the present invention, and the plate material sample (finished product with a plate thickness of 0.08 mm) that was then subjected to a finish heat treatment at a maximum temperature of 430°C, with a time of 13 seconds for the material temperature to be between 180°C and the maximum temperature, were measured for crystallite size and 0.2% yield strength using the above-mentioned method, and a 90°L bending test was performed with a bending radius of R = 0.05 mm, plate thickness t = 0.08 mm, and BW of R / t = 0.05 / 0.08 ≒ 0.6, and a test example in which the properties of both were compared is shown below. The results are shown in Table 4. For reference, laser microscope photographs of the outer surface of the bent part after the 90°L bending test at R / t ≒ 0.6 for the sheet material samples after finish cold rolling and finish heat treatment, respectively, are shown in Figures 1 and 2. The width of these photographs corresponds to approximately 0.26 mm.

[0054] [Table 4]

[0055] No difference was observed in electrical conductivity before and after the final heat treatment, but the strength and bending workability were improved by the final heat treatment. Although it has been generally believed that there is a trade-off between strength and bending workability, the fact that the final heat treatment was able to improve both properties at the same time is presumably due to the effect of the rearrangement of dislocations caused by the final heat treatment progressing and the crystallite size becoming smaller under the conditions in which the precipitates are finely dispersed by the manufacturing process according to the present invention.

Claims

1. The steel sheet has a chemical composition, in mass%, of 0.05 to 1.10% Fe, 0.02 to 0.50% P, 0 to 0.50% Mg, 0 to 0.80% Ni, 0 to 0.80% Sn, 0 to 0.80% Zn, a total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10%, and the balance being Cu. The crystallite size measured by the Halder-Wagner method based on the integral width of a peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface is 30 nm or less, and the 0.2% proof stress in the direction perpendicular to the rolling direction is 450 N / mm 2 That is all about the copper alloy sheet material.

2. In the observation plane parallel to the plate surface, the number density of precipitate particles with a major axis of 10 to 100 nm is 50 particles / μm 2 The copper alloy sheet material according to claim 1 .

3. 2. The copper alloy sheet according to claim 1, having an electrical conductivity of 50% IACS or more.

4. 2. The copper alloy sheet material according to claim 1, wherein a ratio (MBR / t) of a minimum bending radius (MBR) at which cracks do not occur and a sheet thickness (t) in a 90°L bending test with a bending axis parallel to the rolling direction (B.W.) is 0.7 or less.

5. a hot rolling process in which a slab having a chemical composition, by mass%, of 0.05 to 1.10% Fe, 0.02 to 0.50% P, 0 to 0.50% Mg, 0 to 0.80% Ni, 0 to 0.80% Sn, 0 to 0.80% Zn, a total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10%, and the balance being Cu is rolled at a rolling reduction rate of 70% or more in a temperature range of 950°C or lower and 650°C or higher, and then rolled at a rolling reduction rate of 60% or more in a temperature range of lower than 650°C and 350°C or higher; an intermediate cold rolling process in which cold rolling is performed at a rolling ratio of 30% or more; An intermediate heat treatment step in which the material obtained in the intermediate cold rolling step is subjected to a heat treatment at a temperature of 400° C. or more and 700° C. or less for 1 hour or more; A finish cold rolling process in which the material obtained in the intermediate heat treatment process is subjected to cold rolling at a rolling ratio of 80% or more; A finish heat treatment process in which the material obtained in the finish cold rolling process is subjected to a heat treatment in a temperature range of 180 ° C. or more and 500 ° C. or less; A method for producing a copper alloy sheet material, comprising the steps of:

6. 6. The method for producing a copper alloy sheet according to claim 5, wherein in the finish heat treatment step, a material having a crystallite size of 30 nm or less as determined by the Halder-Wagner method based on the integral width of a peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface is obtained.

7. A current-carrying part using the copper alloy sheet material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Gear device for equipments

    JP1979067163A