Conductive paste
A combination of flexible epoxy resin and reactive diluent with a specific structure addresses high viscosity and conductivity issues in conductive pastes, resulting in a low-viscosity resin composition with high conductivity and impact resistance.
Patent Information
- Application Number
- JP2023053122
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Conductive pastes using flexible epoxy resins face high viscosity issues, and adding diluents to lower viscosity can compromise mechanical strength and conductivity.
A combination of flexible epoxy resin and reactive diluent with a specific structure, along with silver particles, is used to maintain viscosity and conductivity in the cured product.
The solution achieves a low-viscosity resin composition that produces a cured product with high conductivity and impact resistance, maintaining mechanical strength.
Smart Images

Figure 00000014_0000
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive paste. [Background technology]
[0002] Conventionally, it is known that a thermosetting conductive paste containing silver particles is used as an alternative connection method to solder for assembling electronic components and connecting them to a substrate (Patent Document 1). The conductive paste may be used to electrically connect a plurality of components and to form wiring and electrodes in the manufacture of electronic devices such as camera modules and printed wiring boards. In order to form finer connections, wiring and electrodes, it may be required to reduce the viscosity of the conductive paste. For example, a low-viscosity diluent is known as a means for reducing the viscosity of the conductive paste. In addition, when used in electronic devices, printed wiring boards, etc., the cured product of the conductive paste may be required to have impact resistance. For example, an epoxy resin having a flexible structure (flexible epoxy resin) is known as a means for imparting impact resistance to the cured product (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2015-42696 [Patent Document 2] Patent No. 5786418 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a flexible epoxy resin is used in a conductive paste, the viscosity of the conductive paste also becomes high because the viscosity of the flexible epoxy resin is high. In this case, it is possible to use a diluent to reduce the viscosity, but if the amount used is large, the physical properties such as the mechanical strength of the cured product tend to decrease, and if the amount used is limited, the viscosity of the conductive paste may not decrease sufficiently depending on the type of diluent. In addition, depending on the type of diluent, problems such as a decrease in the conductivity of the cured product (high resistance) may occur.
[0005] An object of the present invention is to provide a low viscosity resin composition which uses a flexible epoxy resin and a diluent in combination to give a cured product having high electrical conductivity. [Means for solving the problem]
[0006] The present inventors have discovered that when a flexible epoxy resin is used in combination with a reactive diluent having a specific structure, it is possible to maintain an appropriate viscosity as a paste and also to suppress a decrease in the electrical conductivity of the cured product, and have completed the present invention.
[0007] That is, the present invention includes the following aspects. [1] (A) a flexible epoxy resin containing a linear hydrocarbon structural unit having 4 to 20 carbon atoms and / or a polyalkylene ether structural unit having 3 to 20 ether oxygen atoms, (B) a reactive diluent having a structure (Gly-ORO-Gly) in which two glycidyl ether groups (-O-Gly) are bonded to a divalent aliphatic hydrocarbon group (R) and having a viscosity of 500 mPa s or less at 25°C; (C) an epoxy resin hardener; (D) silver particles; A resin composition comprising: [2] The resin composition according to [1] above, wherein the aliphatic hydrocarbon group (R) is a saturated aliphatic hydrocarbon group. [3] The resin composition according to [1] or [2] above, wherein the aliphatic hydrocarbon group (R) is a non-alicyclic aliphatic hydrocarbon group. [4] The resin composition according to any one of the above [1] to [3], wherein the aliphatic hydrocarbon group (R) has 3 or more and 6 or less carbon atoms. [5] The resin composition according to [4] above, wherein the aliphatic hydrocarbon group (R) has 4 or 5 carbon atoms. [6] The resin composition according to any one of the above [1] to [5], wherein the reactive diluent (B) has a viscosity at 25° C. of 100 mPa·s or less. [7] The resin composition according to any one of the above [1] to [6], wherein the flexible epoxy resin (A) further contains a bisphenol-type structural unit. [8] The resin composition according to any one of the above [1] to [7], wherein the epoxy resin curing agent (C) is at least one selected from the group consisting of a tertiary amino group-containing modified polyamine, a urea bond-containing modified polyamine, and an imidazole-containing modified polyamine. [9] The resin composition according to any one of the above [1] to [8], further comprising (E) an epoxy resin (excluding the flexible epoxy resin (A)).
[10] The resin composition according to any one of the above [1] to [9], comprising 0.1 to 40 mass % of the flexible epoxy resin (A) relative to the total mass of the resin composition.
[11] The resin composition according to any one of the above [1] to
[10] , comprising 0.1 to 30 mass % of the reactive diluent (B) relative to the total mass of the resin composition.
[12] The resin composition according to any one of [1] to
[11] above, comprising 2 to 40 parts by weight of the epoxy resin curing agent (C) relative to 100 parts by weight of the epoxy resin contained in the resin composition.
[13] The resin composition according to any one of [1] to
[12] above, comprising 30 to 95 mass% of the silver particles (D) relative to the total mass of the resin composition.
[14] A cured product of the resin composition according to any one of [1] to
[13] above. Effect of the Invention
[0008] According to the present invention, it is possible to provide a low-viscosity resin composition that uses a flexible epoxy resin and a diluent in combination to give a cured product having high electrical conductivity. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 shows a test sample for contact resistance measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention relates to a resin composition containing (A) a flexible epoxy resin containing a linear hydrocarbon structural unit having from 4 to 20 carbon atoms and / or a polyalkylene ether structural unit having from 3 to 20 ether oxygen atoms, (B) a reactive diluent having a structure (Gly-ORO-Gly) in which two glycidyl ether groups (-O-Gly) are bonded to a divalent aliphatic hydrocarbon group (R) and having a viscosity of 500 mPa s or less at 25°C, (C) an epoxy resin curing agent, and (D) silver particles.
[0011] (A) Flexible epoxy resin The flexible epoxy resin used in the present invention contains linear hydrocarbon structural units having 4 to 20 carbon atoms and / or polyalkylene ether structural units having 3 to 20 ether oxygen atoms.
[0012] The linear hydrocarbon structural unit contained in flexible epoxy resins is -(CH2) x -, where x is 4 or more and 20 or less. x is preferably 4 or more and 10 or less. In place of the hydrogen atom, a substituent such as a hydroxyl group may be present, and further, at least one of the hydrogen atoms may be substituted with a hydrocarbon group, an alkoxyl group, an aryl group, an aryloxy group, or the like. The hydrocarbon or alkoxyl group as the substituent preferably has 4 or less carbon atoms, and the aryl group of the aryl group or aryloxy group is preferably a phenyl group. These substituents can be present within a range that does not impair the flexibility of the structural unit.
[0013] The polyalkylene ether structural unit contained in the flexible epoxy resin has 3 or more and 20 or less ether oxygen atoms, preferably 3 or more and 10 or less. Specific examples include structural units derived from a polymer of one or more alkylene oxides selected from ethylene oxide, propylene oxide, butylene oxide, isobutylene oxide, neopentylene oxide, tetramethylene oxide, etc. In addition, examples include those in which one or more hydrogen atoms of this alkylene oxide are substituted with, for example, a hydroxyl group, an alkoxyl group, an aryl group, an aryloxy group, a hydrocarbon group, etc. The hydrocarbon or alkoxyl group as the substituent preferably has 4 or less carbon atoms, and the aryl group of the aryl group or aryloxy group is preferably a phenyl group. These substituents can be present within a range that does not impair the flexibility of the structural unit.
[0014] The linear hydrocarbon structural unit having 4 to 20 carbon atoms improves the heat resistance of the cured product, and the polyalkylene ether structural unit improves, for example, the adhesion and bonding to metal substrates. By appropriately selecting these structural units, it is possible to accommodate a variety of substrates, manufacturing processes, and required performance.
[0015] The flexible epoxy resin preferably contains a bisphenol-type structural unit in addition to the above-mentioned linear hydrocarbon structural unit and / or polyalkylene ether structural unit. Examples of the bisphenol-type structural unit include structural units derived from bisphenol A, bisphenol F, and bisphenol S. Specifically, the structural units include units obtained by removing the OH groups at the terminals of these structural units and units represented by the following general formula (1), and the rings may be hydrogenated. Furthermore, these rings may have a substituent such as a hydrocarbon group, an alkoxyl group, an aryl group, an aryloxy group, or a hydroxyl group.
[0016] JPEG2024141453000001.jpg37170
[0017] When the flexible epoxy resin contains bisphenol-type structural units, the molar ratio of the linear hydrocarbon structural units and / or polyalkylene ether structural units to the bisphenol-type structural units is preferably 1:10 to 5:1, more preferably 1:5 to 3:1. If the amount of the bisphenol-type structural units is more than this range, the cured product will not have sufficient flexibility. If the amount of the bisphenol-type structural units is less than the above range, the Tg of the cured product will be lowered, and the heat resistance will be reduced.
[0018] Specifically, the flexible epoxy resin containing a bisphenol structural unit preferably has one or more structures shown in the following structural formulas (2-i) to (2-iv). In addition, multiple hydroxyl groups in the structural formulas shown below may undergo a crosslinking reaction, and oxygen atoms of the hydroxyl groups may bond unspecified structures.
[0019] JPEG2024141453000002.jpg103170
[0020] In structural formulas (2-i) to (2-iv), Ar 1 , Ar 2 are bisphenol structural units which may be the same or different, may be hydrogenated, and may have a substituent, and X is a linear hydrocarbon group having 4 to 20 carbon atoms and / or a polyalkylene ether structure having 1 to 18 ether oxygen atoms. When X is a linear hydrocarbon group having 4 to 20 carbon atoms, X is a linear hydrocarbon structural unit, and when X is a polyalkylene ether structure having 1 to 18 ether oxygen atoms, -OXO- is a polyalkylene ether structural unit. In addition, n is the average value of the repeating units and is 1 to 30.
[0021] Examples of flexible epoxy resins containing bisphenol structural units include "EPICLON EXA4816" and "EPICLON EXA4822" (both manufactured by DIC Corporation), "YL7175-500" and "YL7175-1000" (both manufactured by Mitsubishi Chemical Corporation).
[0022] The content of the flexible epoxy resin is preferably 0.1 to 40 mass% of the total mass of the resin composition, more preferably 0.2 to 35 mass%, and even more preferably 0.5 to 30 mass%, and may be, for example, 0.8 to 20 mass%, 1 to 10 mass%, or 1.5 to 6 mass%. If the amount of the flexible epoxy resin is within the above range, the impact resistance and adhesiveness of the cured product can be improved while suppressing an increase in the viscosity of the resin composition.
[0023] (B) Reactive diluent The reactive diluent used in the present invention has a structure (Gly-ORO-Gly) in which two glycidyl ether groups (-O-Gly) are bonded to a divalent aliphatic hydrocarbon group (R), and has a viscosity at 25°C of 500 mPa s or less.
[0024] The aliphatic hydrocarbon group (R) may be unsaturated or saturated, and may be alicyclic or acyclic. From the viewpoint of obtaining a cured product having good impact resistance and electrical conductivity while reducing the viscosity of the resin composition, the aliphatic hydrocarbon group (R) is preferably saturated and preferably acyclic. The number of carbon atoms in the aliphatic hydrocarbon group (R) is preferably 6 or less, more preferably 5 or less, and preferably 3 or more, more preferably 4 or more.
[0025] The reactive diluent has a viscosity of 500 mPa·s or less at 25°C. Since the flexible epoxy resin (A) is usually highly viscous and has a viscosity of more than 500 mPa·s at 25°C (for example, a viscosity of more than 100 Pa·s at 25°C), a diluent having a viscosity of 500 mPa·s or less can reduce the viscosity of a resin composition containing the flexible epoxy resin. The reactive diluent preferably has a viscosity of 100 mPa·s or less at 25°C, more preferably 75 mPa·s or less, even more preferably 50 mPa·s or less, preferably 1 mPa·s or more, more preferably 3 mPa·s or more, and even more preferably 5 mPa·s or more. A low viscosity of 500 mPa·s or less can be measured, for example, by putting 1.2 ml of a sample into an E-type viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.) and measuring the viscosity value after 2 minutes at 25°C, 5 rpm, and a procedure conforming to JIS-K7117-2 using a 1.34°×R24 rotor. A viscosity of more than 1 Pa·s can be measured, for example, by putting 0.22 ml of a sample into an E-type viscometer (RE-80U manufactured by Toki Sangyo Co., Ltd.) and measuring the viscosity value after 2 minutes at 25°C, 20 rpm, and a procedure conforming to JIS-K7117-2 using a 3°×R9.7 rotor.
[0026] Examples of reactive diluents include "ED-523L" and "ED-503G" (both manufactured by ADEKA Corporation), "BD(D)" (manufactured by Yokkaichi Chemical Co., Ltd.), and "ZX-1658GS" (manufactured by Nippon Steel Chemical Co., Ltd.).
[0027] The content of the reactive diluent is preferably 0.1 to 30 mass% of the total mass of the resin composition, more preferably 0.2 to 25 mass%, and even more preferably 0.5 to 20 mass%, and may be, for example, 1 to 15 mass%, 1.5 to 12.5 mass%, or 2 to 10 mass%. When the amount of the reactive diluent is within the above range, it is possible to obtain a cured product having good electrical conductivity while reducing the viscosity of the resin composition.
[0028] (C) Epoxy resin hardener As the epoxy resin curing agent in the present invention, any known epoxy resin curing agent can be used without any particular limitation.
[0029] From the viewpoint of handling of the resin composition, the epoxy resin curing agent is preferably a latent curing agent. In this specification, the latent curing agent is a compound that is blended into the resin composition for the purpose of curing the epoxy resin, and does not react with functional groups such as epoxy groups under the normal storage conditions of the resin composition (room temperature, visible light, etc.), but exhibits reaction activity with functional groups by heat or light, and can cure the resin composition. These may be used alone or in combination of two or more.
[0030] From the viewpoints of the viscosity of the resin composition and the electrical conductivity and adhesion of the cured product, the epoxy resin curing agent is preferably one or more selected from the group consisting of a tertiary amino group-containing modified polyamine, a urea bond-containing modified polyamine, and an imidazole-containing modified polyamine, and from the viewpoint of adhesion, it is more preferable to use a urea bond-containing modified polyamine and an imidazole-containing modified polyamine in combination.
[0031] In this specification, the tertiary amino group-containing modified polyamine is a compound that has a polymer structure containing an aliphatic tertiary amine other than imidazole, in which the active amine forms a stabilized structure with an epoxy resin and / or a phenolic resin and can be used as a latent curing agent. Examples of the tertiary amino group-containing modified polyamine include EH4380S, EH3616S, EH5001P, and EH4357S manufactured by ADEKA CORPORATION.
[0032] The imidazole group-containing modified polyamine is a compound that has a polymer structure containing imidazole, in which an active amine forms a stabilized structure with an epoxy resin and / or a phenolic resin and can be used as a latent curing agent. Examples of the imidazole group-containing modified polyamine include PN-23, PN-H, and PN-40 manufactured by Ajinomoto Fine-Techno Co., Ltd., EH4346S manufactured by ADEKA Co., Ltd., FXR-1121 manufactured by T&K TOKA Co., Ltd., and Sanmide LH210 manufactured by Air Products Japan Co., Ltd.
[0033] The urea bond-containing modified polyamine is a compound in which an active amine has a stabilized structure due to the urea bond formed with an isocyanate resin, and can be used as a latent curing agent. Examples of the urea bond-containing modified polyamine include FXR-1020 and FXR-1081 manufactured by T&K TOKA Corporation.
[0034] The epoxy resin curing agent is preferably 1 to 50 parts by weight relative to 100 parts by weight of the epoxy resin contained in the resin composition. In consideration of the curing speed of the epoxy resin, sufficient crosslinking formation, viscosity of the resin composition, and coatability, the amount is more preferably 2 to 40 parts by weight, and further preferably 5 to 35 parts by weight, and may be, for example, 10 to 30 parts by weight, 15 to 28 parts by weight, or 20 to 27 parts by weight relative to 100 parts by weight of the epoxy resin contained in the resin composition.
[0035] (D) Silver particles The resin composition of the present invention contains silver particles to impart electrical conductivity. The shape of the silver particles used in the present invention is not particularly limited, and known shapes such as spherical, flake, and needle shapes can be used, but flake shapes are preferred from the viewpoint of obtaining good electrical conductivity in the cured product. The flake shape is a plate-like shape (see JIS Z2500:2000), and is also called scale-like because it is a thin plate-like shape like a scale.
[0036] The average particle size of the silver particles used in the present invention is preferably 1 to 15 μm. Considering the ease of handling of the resin composition (adequate viscosity) or the occurrence of nozzle clogging when applying with a dispenser, 1.5 to 12.5 μm is more preferable, and 2 to 10 μm is even more preferable. In this specification, the average particle size is measured using a laser diffraction particle size distribution meter as the particle size (median size) at which the relative particle amount is 50% (50% of the total particle amount, the particle size at the midpoint of the particle amount when the total particle amount and particle size are graphed).
[0037] When using flake-shaped silver particles, the specific surface area must be 0.1 to 1.5 m 2 From the viewpoint of the electrical conductivity of the cured product or the dispensability of the resin composition (in this specification, dispensability means application performance such as ease of application when the resin composition is filled in a syringe and applied with a dispenser), it is preferable that the viscosity is 0.15 to 1.0 m / g. 2 / g is more preferable, and 0.2 to 0.9 m 2 The specific surface area is measured by a BET (a method for measuring specific surface area based on a multilayer adsorption model expanded by Brunauer, Emmett and Teller, named after the initials of the three persons) single point method using a specific surface area measuring device.
[0038] The content of the silver particles is preferably 30 to 95 mass% of the total mass of the resin composition, and from the viewpoints of the electrical conductivity of the cured product and the viscosity of the resin composition, is more preferably 40 to 80 mass%, and may be, for example, 50 to 80 mass%, or 60 to 75 mass%.
[0039] (E) Epoxy resin (excluding flexible epoxy resin (A)) The resin composition of the present invention may optionally contain an epoxy resin different from the flexible epoxy resin (A) in order to impart high adhesion. The epoxy resin (E) may be solid or liquid at 25°C, and in the case of a liquid, the viscosity at 25°C is preferably greater than 500 mPa·s. The viscosity at 25°C is preferably 750 mPa·s or more, more preferably 1000 mPa·s or more, preferably 20000 mPa·s or less, more preferably 10000 mPa·s or less, and may be, for example, 5000 mPa·s or less, or 4000 mPa·s or less. The viscosity at 25°C of the epoxy resin (E) can be measured, for example, by putting a 0.22 ml sample into an E-type viscometer (RE-80U manufactured by Toki Sangyo Co., Ltd.) and measuring the value after 2 minutes at 25°C, 20 rpm, according to a procedure in accordance with JIS-K7117-2, using a rotor of 3°×R9.7.
[0040] The epoxy resin (E) is not particularly limited, but is preferably one having an average of two or more epoxy groups per molecule. For example, bisphenol A type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, bisphenol F type epoxy resins, phosphorus-containing epoxy resins, bisphenol S type epoxy resins, aromatic glycidylamine type epoxy resins (e.g., tetraglycidyldiaminodiphenylmethane, triglycidyl-p-aminophenol, diglycidyl toluidine, diglycidyl aniline, etc.), alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, epoxy resins having a butadiene structure, epoxy resins having a dicyclopentadiene structure, diglycidyl ethers of bisphenols, diglycidyl ethers of naphthalene diols, glycidyl ethers of phenols, and diglycidyl ethers of alcohols, as well as alkyl-substituted, halogenated and hydrogenated versions of these epoxy resins, etc. These may be used alone or in combination. Among these, it is preferable to use a bisphenol type epoxy resin, which has low viscosity and good stability, and it is more preferable to use a bisphenol A type epoxy resin or a bisphenol F type resin, and it is preferable to use a mixture of a bisphenol A type epoxy resin and a bisphenol F type resin.
[0041] Available bisphenol type epoxy resins include, for example, RE-310S, RE-304S, and RE-404S manufactured by Nippon Kayaku Co., Ltd., and YD-115, YD-115G, YD-115CA, YD-118P, YD-127, YD-128, YD-128G, YD-128S, YD-128CA, YD-134, and YD-134 manufactured by Nippon Steel Chemical Co., Ltd. N, YD-011, YD-012, YD-013, YD-014, YD-017, YD-019, YD-020, YD-8125, YD-7011R, YD-7014R , YD-7017, YD-7019, YD-7020, YD-900, YD-901, YD-902, YD-903, YD-904, YD-907, YD-909, YD- 927H, ZX-1059, YDF-8170, YDF-170, YDF-175S, YDF-2001, YDF-2004, Epicron series 840, 840S, 850, 850S, 850CRP, 855, 857, D-515, 860, 900-IM, 1050, 1055, 2055, 3050, 40 manufactured by Dainippon Ink and Chemicals, Ltd. 50, 4055, 7050, 9055, 830, 830S, 830LVP, 835, 835LV, EXA-1514, EXA-4004, 828, 828EL, 827, 806, 807, YL980, YL983 manufactured by Mitsubishi Chemical Corporation, and EP-4100, EP-4500, and EP-4901 of the Adeka Resin series manufactured by ADEKA Corporation.
[0042] The epoxy resin (E) can be blended in the resin composition of the present invention in an amount of preferably 0.5% by mass to 50% by mass, more preferably 1% by mass to 40% by mass, for example, 5% by mass to 30% by mass, or 10 to 20% by mass.
[0043] <(F) Metal powder other than silver particles (D)> The resin composition of the present invention may contain a metal powder other than the silver particles (D) in order to suppress an increase in the contact resistance value of the cured product under high temperature and high humidity. As the metal powder other than the silver particles (D), preferably, tin powder, zinc powder, and aluminum powder can be mentioned. The shape of the metal powder (F) is not particularly limited, and known ones such as spherical, flake, and needle-shaped can be used, but spherical is preferable from the viewpoint of the viscosity of the resin composition.
[0044] The particle size of the metal powder (F) is preferably from 1 to 15 μm, and more preferably from 1 to 10 μm, taking into consideration the handleability of the resin composition and the occurrence of nozzle clogging when applying with a dispenser.
[0045] The specific surface area of the metal powder (F) is preferably 0.1 to 1.5 m from the viewpoints of the electrical conductivity of the cured product, the dispensability of the resin composition, etc. 2 / g, more preferably 0.1 to 1.0 m 2 / g.
[0046] The content of the metal powder (F) is preferably 3% by mass or more, more preferably 5% by mass or more, and preferably 20% by mass or less, and more preferably 15% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition, from the viewpoint of suppressing the contact resistance of the cured product under high temperature and high humidity conditions. In one embodiment of the present invention, the content of the metal powder (F) is preferably 3% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 15% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition.
[0047] (G) Core-shell polymer The resin composition of the present invention can be blended with a core-shell polymer in order to improve adhesion and impart stress relaxation properties. The core-shell polymer is a polymer having a core and a shell, and is obtained by polymerizing a relatively hard shell layer prepared from a (meth)acrylic acid ester, aromatic vinyl, vinyl cyanide, epoxy alkyl vinyl ether, unsaturated acid derivative, (meth)acrylamide derivative, and / or maleimide derivative, etc., on a relatively soft core prepared from a rubber elastomer, a polysiloxane rubber elastomer, or a mixture thereof, etc., prepared from a diene monomer, a (meth)acrylic acid ester monomer, and / or a vinyl monomer, etc. Available core-shell polymers include MX-120, MX-125, MX-130, MX-135, MX-960, and MX-965 from Kaneka Corporation, RKB-3040 and RKB-1133 from Resinous Chemicals, JF-001 and JF-003 from Mitsubishi Rayon Co., Ltd., and F351G from Ganz Chemicals. The core-shell polymer may be a known one in the form of a single powder or one dispersed in an epoxy resin. These may be used alone or in combination of a powder and one dispersed in an epoxy resin. The content of the core-shell polymer is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, and may be, for example, 0.5 to 5% by mass, or 1 to 3% by mass, of the total mass of the resin composition.
[0048] The resin composition of the present invention is a liquid resin composition having fluidity at 25°C, and considering the use of penetrating into the gaps of an adherend for adhesion, the viscosity at 25°C is preferably less than 20 Pa·s, more preferably 10 Pa·s or less, preferably 1 Pa·s or more, and more preferably 5 Pa·s or more. In one embodiment of the present invention, the viscosity of the resin composition at 25°C is preferably 1 Pa·s or more and less than 20 Pa·s, more preferably 5 Pa·s or more and less than 15 Pa·s, and even more preferably 5 Pa·s or more and 10 Pa·s or less. In the present invention, the viscosity of the resin composition at 25°C can be measured, for example, by putting 0.22 ml of a sample into an E-type viscometer (RE-80U manufactured by Toki Sangyo Co., Ltd.) and measuring the value after 2 minutes at 25°C, 20 rpm, and using a rotor of 3°×R9.7 according to a procedure in accordance with JIS-K7117-2.
[0049] As other additives, a silane coupling agent may be added to the resin composition of the present invention from the viewpoint of improving the adhesion of the resin composition to the substrate, a corrosion inhibitor such as benzimidazole may be added from the viewpoint of protecting the connection terminals, and a thixotropic agent such as a boric acid ester or aerosil may also be appropriately added.
[0050] The resin composition of the present invention is produced by mixing the above-mentioned components in a conventional manner and dispersing them uniformly using a planetary mixer, a roll mill or the like to form a paste.
[0051] The present invention further relates to a cured product of the resin composition. The resin composition of the present invention, which uses a flexible epoxy resin in combination with a reactive diluent having a specific structure, can provide a cured product with excellent impact resistance and electrical conductivity. The cured product of the present invention also exhibits good electrical conductivity (contact resistance value) and adhesive strength even under high temperature and high humidity conditions. Heating is preferred as a curing method, and the heating conditions can be appropriately adjusted. For example, the resin composition may be cured by maintaining the temperature at 60 to 100°C, preferably 70°C to 90°C, for example, for 20 minutes to 3 hours, preferably 40 minutes to 2 hours.
[0052] The resin composition of the present invention can be used as a conductive adhesive for use in assembling electronic components and the like, in connecting them to substrates, and in mounting chip components on substrates. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0054] A resin composition was prepared according to the composition shown in Table 1. The components other than components (E) and (F) were mixed for 30 minutes in a planetary mixer (5DMV-01-r, manufactured by Dalton Co., Ltd.). Then, components (E) and (F) were added and mixed for 20 minutes, and then the mixture was degassed and mixed for 30 minutes in the planetary mixer to prepare the resin composition. The materials used are as follows:
[0055] EXA-4816: DIC Corporation, modified epoxy resin (flexible and tough), 100 Pa·s or more ZX-1059: Nippon Steel Chemical Co., Ltd., 1:1 mixture of bisphenol A resin and bisphenol F resin, viscosity 2500 mPa s YDF-8170: Nippon Steel Chemical Co., Ltd., bisphenol F resin, viscosity 1300 mPa·s RKB-3040: Resinous Chemical Co., Ltd., product name: Resinous Bond, epoxy resin containing core-shell polymer, 30% by weight of core-shell polymer, 70% by weight of bisphenol A resin and bisphenol F resin (viscosity measurement of epoxy resin component is not possible because it is a mixture) ED-523L: ADEKA Corporation, neopentyl glycol diglycidyl ether, viscosity 8 mPa·s BD(D): Yokkaichi Chemical Co., Ltd., product name "Epogosei", 1,4-butanediol diglycidyl ether, 8 mPa·s ED-503G: ADEKA Corporation, 1,6-Hexanediol diglycidyl ether, viscosity 24 mPa s ZX-1658GS: Nippon Steel Chemical Co., Ltd., 1,4-cyclohexanedimethanol diglycidyl ether, viscosity 32 mPa s EX-201: Nagase ChemteX Corporation, resorcinol diglycidyl ether, viscosity 350 mPa·s Epolite 200P(N): Kyoeisha Chemical Co., Ltd., tripropylene glycol diglycidyl ether, viscosity 30 mPa·s EX-830: Nagase ChemteX Corporation, polyethylene glycol diglycidyl ether, viscosity 70 mPa·s EX-841: Nagase ChemteX Corporation, polyethylene glycol diglycidyl ether, viscosity 110 mPa·s ZX-1542: Nippon Steel Chemical Co., Ltd., trimethylolpropane triglycidyl ether, viscosity 61 mPa·s PN-H: Ajinomoto Fine-Techno Co., Ltd., product name "Amicure", imidazole group-containing modified polyamine FXR-1081: T&K TOKA, product name "Fujicure", urea bond-containing modified polyamine Silver particles: manufactured by Metallo, trade name EA-0101, average particle diameter 6.8μm, specific surface area 0.28m 2 / g, flake Zinc particles: manufactured by Hakusui Tech Co., Ltd., product name Zinc Powder R powder, average particle size 5.2 μm, specific surface area 0.25 m 2 / g, spherical JF-003: Mitsubishi Rayon Co., Ltd., product name: pregelling agent, core-shell polymer
[0056] The viscosity of the resin compositions of the examples and comparative examples, and the resistivity, tensile shear adhesive strength, and increase in contact resistance under high temperature and high humidity of the cured products were measured by the following methods. The results are shown in Table 1.
[0057] (1) Viscosity measurement (25℃) 0.22 ml of the resin composition was added, and the viscosity was measured using an E-type viscometer (RE-80U manufactured by Toki Sangyo Co., Ltd.) according to a procedure in accordance with JIS-K7117-2, using a 3°×R9.7 rotor at 20 rpm for 2 minutes.
[0058] (2) Measurement of electrical conductivity (resistivity) A 120 mm line with a width of 2 mm and a thickness of about 80 um was bar-coated on an FR-4 substrate with the resin compositions of the Examples and Comparative Examples, and cured at 80°C for 60 minutes in a heat circulation oven (DF-610, manufactured by Yamato Scientific Co., Ltd.) to prepare a test sample for resistivity measurement. The resistance of the cured product was measured in four-terminal mode at a distance of 100 mm using a digital multimeter (R6552, manufactured by Advantest Corporation), and the resistivity was calculated.
[0059] (3) Measurement of tensile shear adhesive strength Adhesive test pieces were prepared from nickel-plated stainless steel (100 mm x 25 mm x 1.5 mm) according to the procedure of JIS-K6850 and cured at 80°C for 60 minutes. The tensile shear adhesive strength was measured according to the procedure of JIS-K6850 using a universal tensile testing machine (TSE AC-50kN).
[0060] (4) Increase in contact resistance under high temperature and humidity As shown in FIG. 1, a conductor 2 was fixed on a nickel-plated stainless steel 4 measuring 100 mm×25 mm×1.5 mm. A resin composition 3 was applied to the conductor 2 so that the resin composition 3 was in contact with the nickel surface at a diameter of 1 mm, and cured in a heat circulation oven at 80° C. for 60 minutes to prepare a test sample for measuring contact resistance. The resistance value between the conductor 2 and the nickel-plated surface was measured using a digital multimeter 1 (R6552 manufactured by Advantest Corporation), and this was taken as the contact resistance value between the resin composition 3 and nickel. The time until the contact resistance exceeded 10 times the initial value after exposure to conditions of a temperature of 85° C. and a humidity of 85% was taken as the reliability retention time.
[0061] The resin compositions or cured products of the Examples and Comparative Examples were evaluated for viscosity, resistivity, adhesion, and reliability under high temperature and high humidity conditions according to the following criteria.
[0062] (1) Viscosity ○: Viscosity (Pa s) less than 10 ×: Viscosity (Pa s) is 10 or more
[0063] (2) Specific resistance ◎:4.0×10 -3 Less than Ω cm ○:4.0×10 -3 Ω cm or more, 5.0×10 -3 Less than Ω cm △:5.0×10 -3 Ω cm or more, 7.0×10 -3 Less than Ω cm ×:7.0×10 -3 Ω cm or more
[0064] (3) Adhesiveness ○: Tensile shear adhesive strength (N / mm 2 ) is 8 or more △: Tensile shear adhesive strength (N / mm 2 ) is 6 or more and less than 8 ×: Tensile shear adhesive strength (N / mm 2 ) is less than 6
[0065] (4) Reliability retention time under high temperature and high humidity conditions ◎: Retention time is 300 hours or more ○: Retention time is 200 hours or more and less than 300 hours ×: Retention time is less than 200 hours
[0066] [Table 1]
[0067] When a diluent containing an aromatic ring (Comparative Example 2) or a diluent having three glycidyl ether groups (Comparative Example 6) was used, the viscosity of the resin composition was not sufficiently reduced compared to when no diluent was used (Comparative Example 1). Furthermore, when a diluent having an aromatic ring (Comparative Example 2) or a polyether structure (Comparative Examples 3 to 5) was used, even if the diluent had a low viscosity and had two glycidyl ether groups, the resistivity increased significantly compared to when no diluent was used (Comparative Example 1).
[0068] On the other hand, in Examples 1 to 4 in which the reactive diluent of the present invention was used, both low viscosity of the resin composition and high electrical conductivity of the cured product were achieved, and the adhesiveness and reliability under high temperature and high humidity were also good. Among them, Examples 1 to 3 in which a diluent having a non-alicyclic aliphatic hydrocarbon group as the aliphatic hydrocarbon group (R) was used had higher electrical conductivity, and further, Examples 1 and 2 in which a diluent having an aliphatic hydrocarbon group (R) with 4 or 5 carbon atoms was used exhibited high reliability under high temperature and high humidity.
Claims
1. (A) a flexible epoxy resin containing a linear hydrocarbon structural unit having from 4 to 20 carbon atoms and / or a polyalkylene ether structural unit having from 3 to 20 ether oxygen atoms; (B) a reactive diluent having a structure (Gly-O-R-O-Gly) in which two glycidyl ether groups (-O-Gly) are bonded to a divalent aliphatic hydrocarbon group (R) and having a viscosity of 500 mPa s or less at 25°C; (C) an epoxy resin curing agent; and (D) silver particles; A resin composition comprising:
2. The resin composition according to claim 1 , wherein the aliphatic hydrocarbon group (R) is a saturated aliphatic hydrocarbon group.
3. The resin composition according to claim 1 , wherein the aliphatic hydrocarbon group (R) is a non-alicyclic aliphatic hydrocarbon group.
4. The resin composition according to claim 1 , wherein the aliphatic hydrocarbon group (R) has 3 or more and 6 or less carbon atoms.
5. The resin composition according to claim 4, wherein the aliphatic hydrocarbon group (R) has 4 or 5 carbon atoms.
6. The resin composition according to claim 1, wherein the reactive diluent (B) has a viscosity at 25°C of 100 mPa·s or less.
7. The resin composition according to claim 1 , wherein the flexible epoxy resin (A) further contains a bisphenol-type structural unit.
8. The resin composition according to claim 1, wherein the epoxy resin curing agent (C) is at least one selected from the group consisting of a tertiary amino group-containing modified polyamine, a urea bond-containing modified polyamine, and an imidazole-containing modified polyamine.
9. The resin composition according to claim 1, further comprising an epoxy resin (E) other than the flexible epoxy resin (A).
10. The resin composition according to claim 1, comprising 0.1 to 40% by mass of the flexible epoxy resin (A) based on the total mass of the resin composition.
11. The resin composition according to claim 1, comprising 0.1 to 30 mass% of the reactive diluent (B) based on the total mass of the resin composition.
12. The resin composition according to claim 1, comprising 2 to 40 parts by weight of the epoxy resin curing agent (C) relative to 100 parts by weight of the epoxy resin contained in the resin composition.
13. The resin composition according to claim 1, comprising 30 to 95 mass% of the silver particles (D) relative to the total mass of the resin composition.
14. A cured product of the resin composition according to any one of claims 1 to 13.
Citation Information
Patent Citations
Conductive silver adhesive and preparation method thereof
CN105602504A
Silver salt doped silver conductive adhesive, as well as preparation method and application thereof
CN106085276A
Conductive silver glue, preparation method and application thereof
CN106753133A
Conductive silver adhesive and preparation method and application thereof
CN112778948A
Epoxy resin conductive adhesive based on organic silicon modification and preparation method thereof
CN113322023A