Copper alloy, and, component for electronic / electric equipment

A Cu-Fe-P alloy with controlled precipitate particle morphology addresses conductive anisotropy issues, enhancing longitudinal conductivity and strength for applications like bus bars.

JP2024141454APending Publication Date: 2024-10-10MITSUBISHI MATERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053123
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional Cu-Fe-P alloys do not adequately address conductive anisotropy, particularly in applications where electric current flows in a specific direction, such as bus bars, leading to insufficient electrical conductivity in the longitudinal direction.

Method used

A Cu-Fe-P based copper alloy with controlled precipitate particle morphology, specifically Fe: 1.5% to 2.7% by mass, P: 0.008% to 0.20% by mass, Zn: 0.01% to 0.5% by mass, and Sn: 0.01% to 0.5% by mass, with a conductivity ratio exceeding 100.1% to 105.0% and a particle length ratio of 0.8 or less, enhancing electrical conductivity in the longitudinal direction.

Benefits of technology

The alloy achieves superior electrical conductivity in the longitudinal direction compared to the perpendicular direction, with improved strength and thermal conductivity, suitable for applications requiring high conductivity and resistance to surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141454000004
    Figure 2024141454000004
  • Figure 2024141454000005
    Figure 2024141454000005
  • Figure 2024141454000001
    Figure 2024141454000001
Patent Text Reader

Abstract

To provide a Cu-Fe-P based copper alloy having more excellent electric conductivity in a direction parallel to a longitudinal direction than in a direction perpendicular to the longitudinal direction.SOLUTION: Copper alloy is provided, having a composition containing Fe;1.5 mass% or more and 2.7 mass% or less, P;0.008 mass% or more and 0.20 mass% or less, Zn;0.01 mass% or more and 0.5 mass% or less, and Sn;0.01 mass% or more and 0.5 mass% or less, and the balance composed of Cu with unavoidable impurities. In the copper alloy, a ratio σP / σO between electric conductivity σP measured in a direction parallel to a longitudinal direction and electric conductivity σO measured in a direction perpendicular to the longitudinal direction is more than 100.1% and 105.0% or less, and regarding particles of precipitate having a particle diameter of 150nm or more and less than 1000nm observed on a cross section including a longitudinal direction, an average value of a ratio LO / LP between a particle length LO in a direction perpendicular to a longitudinal direction and a particle length LP in a direction parallel to a longitudinal direction is 0.8 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper alloy suitable for use in home appliances, semiconductor parts such as lead frames, printed wiring boards, heat sinks, switch parts, bus bars, connectors, and other electric and electronic device parts, and to electric and electronic device parts made of this copper alloy. [Background technology]

[0002] Conventionally, copper or copper alloys having excellent electrical conductivity have been used for electronic and electric device parts such as terminals, bus bars, lead frames, and heat dissipation members. As the copper alloy for the above-mentioned various applications, Cu-Fe-P alloys containing Fe and P have been widely used. Cu-Fe-P alloys are precipitation-strengthened alloys in which intermetallic compounds such as Fe or Fe-P are precipitated in the copper matrix, and are widely used in various applications due to their excellent strength, electrical conductivity, and thermal conductivity. In recent years, with the expansion of applications of Cu-Fe-P alloys and the weight reduction, thinning, and miniaturization of electric and electronic devices, Cu-Fe-P alloys are also required to have higher strength, higher electrical conductivity, and better thermal conductivity. For example, Patent Document 1 proposes a Cu-Fe-P alloy in which the crystal grains of the Cu matrix are equiaxed in order to reduce the anisotropy of mechanical properties. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-057116 A Summary of the Invention [Problem to be solved by the invention]

[0004] For example, electrical conductivity in the longitudinal direction is particularly required for applications such as bus bars in electrical and electronic equipment parts where current flows in a specific direction. However, no conventional Cu-Fe-P alloys have been proposed in which the anisotropy of electrical conductivity has been fully examined. Although Patent Document 1 examines the anisotropy of characteristics, the purpose is to reduce the anisotropy of mechanical properties, and no attention is paid to electrical conductivity.

[0005] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a Cu-Fe-P based copper alloy having higher electrical conductivity in a direction parallel to the longitudinal direction than in a direction perpendicular to the longitudinal direction, and an electronic / electrical device part made of this copper alloy. [Means for solving the problem]

[0006] In order to solve the above problems, a copper alloy according to a first aspect of the present invention contains Fe; 1.5% by mass to 2.7% by mass, P; 0.008% by mass to 0.20% by mass, Zn; 0.01% by mass to 0.5% by mass, Sn; 0.01% by mass to 0.5% by mass, and the balance being Cu and unavoidable impurities, and has a conductivity σ measured in a direction parallel to the longitudinal direction. P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O is more than 100.1% and less than 105.0%, and the particle diameter observed on the cross section including the longitudinal direction is 150 nm or more and less than 1000 nm, the particle length L in the direction perpendicular to the longitudinal direction is O and the particle length L parallel to the longitudinal direction P Compared to L O / L P The average value of is 0.8 or less.

[0007] The copper alloy of the first aspect of the present invention contains Fe; 1.5% by mass to 2.7% by mass, P; 0.008% by mass to 0.20% by mass, Zn; 0.01% by mass to 0.5% by mass, Sn; 0.01% by mass to 0.5% by mass, with the balance being Cu and unavoidable impurities. This provides excellent strength and electrical conductivity as well as good thermal conductivity.

[0008] In the copper alloy of the first embodiment of the present invention, the electrical conductivity σ P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O Since the conductivity is set to be more than 100.1% and not more than 105.0%, the material has good electrical conductivity, particularly when used in applications where electric current is passed in the longitudinal direction. In addition, the precipitate particles are an obstacle to the electrons flowing through the matrix, which causes electrical resistance. Therefore, the particle length L O and the particle length L parallel to the longitudinal direction P When these are different, anisotropy occurs in the electrical conductivity. Therefore, the electrical conductivity in the longitudinal direction can be improved by controlling the morphology of the precipitates. O and the particle length L parallel to the longitudinal direction P Compared to L O / L P To obtain small precipitates, coarse precipitates are necessary, and such coarse precipitates may cause surface defects. Small precipitates are often spherical and have small anisotropy.

[0009] Therefore, in the copper alloy of the first embodiment of the present invention, the particle length L in the direction perpendicular to the longitudinal direction of the precipitate particles having an observed particle diameter of 150 nm or more and less than 1000 nm is measured. O and the particle length L parallel to the longitudinal direction P Compared to L O / L P The average value of is 0.8 or less, which makes it possible to improve electrical conductivity in the longitudinal direction and suppress surface defects. In the present invention, the grain size of a precipitate grain is the diameter of a circle having an area equal to the area of ​​the precipitate grain in microstructural observation (equivalent circle diameter), and the lengths of the precipitate grain in the direction parallel to the longitudinal direction and the direction perpendicular to the longitudinal direction are the lengths of the precipitate grain measured in those directions.

[0010] The copper alloy of the second aspect of the present invention is the copper alloy of the first aspect of the present invention, which has an electrical resistance ratio R measured in a direction parallel to the longitudinal direction. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O is more than 100.1% and less than 105.0%.

[0011] According to the copper alloy of the second aspect of the present invention, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O R P / R O is set to exceed 100.1% and be equal to or less than 105.0%, and has excellent longitudinal conductivity even at low temperatures. The electrical resistivity ratio (R) is calculated by measuring the electrical resistivity at 293K (ρ293K) and the electrical resistivity at liquid nitrogen temperature (77K) (ρ77K) as R=ρ293K / ρ77K.

[0012] The copper alloy of the third aspect of the present invention is characterized in that, in the copper alloy of the first or second aspect of the present invention, it further contains one or two of Mg; 0.005% by mass or more and 0.5% by mass or less, and Co; 0.005% by mass or more and 0.5% by mass or less.

[0013] According to the copper alloy of the third embodiment of the present invention, the copper alloy further contains one or two of Mg; 0.005% by mass or more and 0.5% by mass or less, and Co; 0.005% by mass or more and 0.5% by mass or less. Therefore, Mg and Co are dissolved in the matrix and partly in the Fe-based and Fe-P-based precipitates, and the heat resistance and strength can be improved by solid solution strengthening and partly precipitation strengthening.

[0014] The copper alloy of embodiment 4 of the present invention is characterized in that, in the copper alloy of any one of embodiments 1 to 3 of the present invention, it further contains one or more of the following: Ni; 0.005% by mass or more and 0.5% by mass or less; Al; 0.005% by mass or more and 0.5% by mass or less; and Si; 0.005% by mass or more and 0.5% by mass or less.

[0015] According to the copper alloy of the fourth aspect of the present invention, the copper alloy further contains one or more of Ni; 0.005% by mass or more and 0.5% by mass or less, Al; 0.005% by mass or more and 0.5% by mass or less, and Si; 0.005% by mass or more and 0.5% by mass or less, thereby making it possible to further improve the heat resistance and strength.

[0016] A copper alloy according to a fifth aspect of the present invention is characterized in that, in the copper alloy according to any one of the first to fourth aspects of the present invention, the electrical conductivity in a direction parallel to the longitudinal direction is 55% IACS or more. According to the copper alloy of the fifth aspect of the present invention, the electrical conductivity in the direction parallel to the longitudinal direction is 55% IACS or more, and therefore the copper alloy can be used in applications where high electrical conductivity is required.

[0017] The copper alloy of embodiment 6 of the present invention is characterized in that, in the copper alloy of any one of embodiments 1 to 5 of the present invention, the content of C contained as the unavoidable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass.

[0018] According to the copper alloy of the sixth aspect of the present invention, the elements having the effect of promoting liquid phase separation during melting and casting are reduced, so that the generation of coarse Fe-based crystals in the ingot can be suppressed, and the number of generated surface defects can be reduced.

[0019] A seventh aspect of the present invention provides an electronic / electrical device part, which is characterized in that it is made of the copper alloy according to any one of the first to sixth aspects of the present invention. According to the electronic / electrical device part of aspect 7 of the present invention, since it is made of the copper alloy of any one of aspects 1 to 6 of the present invention, it can exhibit excellent properties even in a high-temperature environment. Effect of the Invention

[0020] It is now possible to provide a Cu-Fe-P based copper alloy having better electrical conductivity in a direction parallel to the longitudinal direction than in a direction perpendicular to the longitudinal direction, and electronic / electrical device components made of this copper alloy. [Brief description of the drawings]

[0021] [Figure 1] 1 is an observation photograph showing an example of precipitate particles of the copper alloy according to the present embodiment. [Diagram 2] FIG. 1 is a flow diagram of a method for producing a copper alloy according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, a copper alloy according to one embodiment of the present invention will be described. The copper alloy of this embodiment contains Fe; 1.5% by mass to 2.7% by mass, P; 0.008% by mass to 0.20% by mass, Zn; 0.01% by mass to 0.5% by mass, Sn; 0.01% by mass to 0.5% by mass, with the balance being Cu and unavoidable impurities.

[0023] The copper alloy of this embodiment may further contain one or two of Mg; 0.005% by mass or more and 0.5% by mass or less, and Co; 0.005% by mass or more and 0.5% by mass or less. In addition, the copper alloy of this embodiment may further contain one or more of the following: Ni; 0.005% by mass or more and 0.5% by mass or less; Al; 0.005% by mass or more and 0.5% by mass or less; and Si; 0.005% by mass or more and 0.5% by mass or less.

[0024] Furthermore, in the copper alloy of the present embodiment, it is preferable that the content of C contained as the inevitable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass.

[0025] In the copper alloy of this embodiment, the electrical conductivity σ P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O is set to be greater than 100.1% and less than 105.0%. In the copper alloy according to the present embodiment, as shown in FIG. 1, the particle length L in the direction perpendicular to the longitudinal direction (particle diameter in the direction perpendicular to the longitudinal direction) is calculated for precipitate particles 12 having a particle diameter of 150 nm or more and less than 1000 nm observed in a cross section including the longitudinal direction. O and the particle length in the direction parallel to the longitudinal direction (particle diameter in the longitudinal direction) L P Compared to L O / L P The average value is said to be below 0.8.

[0026] That is, in the copper alloy of this embodiment, as shown in Fig. 1, precipitate particles 12 of Fe, Fe-P, etc. are dispersed in a matrix phase 11, and the particle size of the precipitate particles 12 is specified as described above. Note that the matrix phase 11 refers to a phase other than the precipitate particles 12 of Fe, Fe-P, etc., and is a phase containing Cu as a main component (Cu content exceeds 97 mass%) with some Fe, Zn, P, Sn, etc. in solid solution. Here, small precipitates with a particle diameter of less than 150 nm are often spherical and have little effect on anisotropy, so they were excluded. Also, precipitate particles 12 with a particle diameter of 1000 nm or more were excluded because they can cause surface defects. Note that the particle diameter of the precipitate particles 12 in this embodiment is the diameter of a circle (equivalent circle diameter) having an area equal to the area of ​​the precipitate particles 12 in the structure observation, and is the particle length L in the direction perpendicular to the longitudinal direction. O , and the particle length L parallel to the longitudinal direction P are the lengths of the precipitate grains 12 measured in those directions.

[0027] Here, in the copper alloy of this embodiment, the electrical conductivity is preferably 55% IACS or more. In addition, in the copper alloy of this embodiment, it is preferable that the strength is 480 MPa or more. Furthermore, in the copper alloy of this embodiment, it is preferable that the Vickers hardness is 100 HV or more.

[0028] The reasons for specifying the component composition, various characteristics, and crystal structure of the copper alloy of this embodiment as described above will be explained below.

[0029] (Fe) Fe dissolves in the matrix 11 and generates Fe or Fe-P precipitate particles 12. The Fe or Fe-P precipitate particles 12 are dispersed in the matrix 11, improving strength, hardness, and heat resistance without reducing electrical conductivity. If the Fe content is less than 1.5 mass%, the effect of improving strength is insufficient. On the other hand, if the Fe content exceeds 2.7 mass%, large crystals may be generated, which may impair the cleanliness of the surface. Furthermore, there is a risk of reducing electrical conductivity and workability. Therefore, in this embodiment, the Fe content is set to 1.5 mass % or more and 2.7 mass % or less. In order to ensure the above-mentioned effects, the lower limit of the Fe content is preferably 1.8 mass% or more, more preferably 2.1 mass% or more, and in order to ensure the suppression of the formation of large crystallized particles, the upper limit of the Fe content is preferably 2.6 mass% or less, more preferably 2.4 mass% or less.

[0030] (P) P is an element having a deoxidizing effect. As described above, P forms Fe-P precipitate particles 12 together with Fe, improving strength, hardness, and heat resistance without reducing electrical conductivity. If the P content is less than 0.008% by mass, the effect of improving strength is insufficient. On the other hand, if the P content exceeds 0.20% by mass, electrical conductivity and workability are reduced. Therefore, in this embodiment, the P content is set to 0.008 mass % or more and 0.20 mass % or less. In order to ensure that the above-mentioned effects are achieved, the lower limit of the P content is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more. In order to ensure that the electrical conductivity and workability are prevented from decreasing, the upper limit of the P content is preferably 0.15 mass% or less, and more preferably 0.12 mass% or less.

[0031] (Zn) Zn is an element that has the effect of improving solder wettability and solder weather resistance. If the Zn content is less than 0.01% by mass, the effect of improving the solder wettability and solder weather resistance cannot be fully achieved. On the other hand, if the Zn content exceeds 0.5% by mass, the effect will be saturated. Therefore, in this embodiment, the Zn content is set to 0.01 mass % or more and 0.5 mass % or less. In order to ensure the above-mentioned effects, the lower limit of the Zn content is preferably 0.02% by mass or more, more preferably 0.05% by mass or more, and the upper limit of the Zn content is preferably 0.35% by mass or less, more preferably 0.20% by mass or less.

[0032] (Sn) Sn is an element that improves heat resistance and strength by dissolving in the matrix 11. If the Sn content is less than 0.01% by mass, the above-mentioned effects cannot be fully achieved. On the other hand, if the Sn content exceeds 0.5% by mass, the electrical conductivity is significantly reduced. Therefore, in this embodiment, the Sn content is set to 0.01 mass % or more and 0.5 mass % or less. In order to ensure the above-mentioned effects, the lower limit of the Sn content is preferably 0.02 mass% or more, more preferably 0.03 mass% or more, and in order to further suppress the decrease in electrical conductivity, the upper limit of the Sn content is preferably 0.3 mass% or less, more preferably 0.2 mass% or less.

[0033] (Mg,Co) Mg and Co have the effect of improving heat resistance and strength by dissolving in the parent phase 11 and solid solution strengthening. Therefore, they may be added appropriately depending on the required characteristics. Here, if the Mg content is less than 0.005 mass% or the Co content is less than 0.005 mass%, the above-mentioned effect cannot be fully achieved. On the other hand, if the Mg content exceeds 0.5 mass% or the Co content exceeds 0.5 mass%, the electrical conductivity will be significantly reduced. Therefore, in this embodiment, when Mg and Co are added, it is preferable that the Mg content be 0.005 mass % or more and 0.5 mass % or less, and the Co content be 0.005 mass % or more and 0.5 mass % or less.

[0034] When Mg and Co are added, the lower limit of the Mg content is preferably 0.01% by mass or more, and the lower limit of the Co content is preferably 0.01% by mass or more. Furthermore, the lower limit of the Mg content is preferably 0.02% by mass or more, and the lower limit of the Co content is preferably 0.02% by mass or more. Furthermore, the upper limit of the Mg content is preferably 0.2% by mass or less, and the upper limit of the Co content is preferably 0.2% by mass or less. When Mg and Co are contained as impurities, they may be contained in amounts less than the above-mentioned lower limit values.

[0035] (Ni, Al, Si) Ni, Al, and Si have the effect of further improving heat resistance and strength. Therefore, they may be added appropriately depending on the required characteristics. Here, when the Ni content is less than 0.005 mass%, when the Al content is less than 0.005 mass%, or when the Si content is less than 0.005 mass%, the above-mentioned effects cannot be fully achieved. On the other hand, when the Ni content exceeds 0.5 mass%, when the Al content exceeds 0.5 mass%, or when the Si content exceeds 0.5 mass%, the electrical conductivity is significantly reduced. Therefore, when Ni, Al, and Si are added in this embodiment, it is preferable that the Ni content be 0.005 mass% or more and 0.5 mass% or less, the Al content be 0.005 mass% or more and 0.5 mass% or less, and the Si content be 0.005 mass% or more and 0.5 mass% or less.

[0036] When Ni, Al, and Si are added, the lower limit of the Ni content is preferably 0.01% by mass or more, the lower limit of the Al content is preferably 0.01% by mass or more, and the lower limit of the Si content is preferably 0.01% by mass or more. Furthermore, the upper limit of the Ni content is preferably 0.1% by mass or less, the upper limit of the Al content is preferably 0.1% by mass or less, and the upper limit of the Si content is preferably 0.1% by mass or less. When Ni, Al, and Si are contained as impurities, they may be contained in amounts less than the above-mentioned lower limit values.

[0037] (Inevitable impurities: C, Cr, Mo, W, V, Nb) C, Cr, Mo, W, V, and Nb are contained in the above-mentioned copper alloy as inevitable impurities. Here, when the contents of C, Cr, Mo, W, V, and Nb are high, the surface defects of the copper alloy sheet are significantly increased. These surface defects are caused by iron alloy particles containing at least one of Cr, Mo, W, V, and Nb, as well as Fe and C.

[0038] Usually, when the above-mentioned copper alloy is melted and cast, the Fe element exists in a dissolved state in a liquid phase mainly composed of Cu. However, when a certain amount or more of C, Cr, Mo, W, V, and Nb are present, the copper alloy melt is separated into a liquid phase mainly composed of Cu and a liquid phase mainly composed of Fe and containing at least one of C and Cr, Mo, W, V, and Nb, and as a result, coarse crystallized products containing at least one of Cr, Mo, W, V, and Nb, Fe, and C are present in the ingot. Then, by rolling the ingot, the iron alloy particles are exposed on the surface of the copper alloy thin plate, which is considered to cause the above-mentioned surface defects. In addition, the iron alloy particles cause shape defects when pressing, etching, or silver plating is performed.

[0039] From the above, it is possible to suppress surface defects and defective product shapes caused by iron alloy particles by reducing the amounts of C, Cr, Mo, W, V, and Nb. Therefore, in this embodiment, in order to suppress the generation of coarse crystals, it is preferable to limit the content of C, which is an inevitable impurity, to less than 5 ppm by mass, the content of Cr to less than 7 ppm by mass, the content of Mo to less than 5 ppm by mass, the content of W to less than 1 ppm by mass, the content of V to 1 ppm by mass, and the content of Nb to less than 1 ppm by mass.

[0040] In order to further suppress the generation of coarse crystals, the content of C, which is an unavoidable impurity, is more preferably less than 4 ppm by mass, even more preferably 3 ppm by mass or less, and even more preferably 2 ppm by mass or less. Moreover, the content of Mo, which is an unavoidable impurity, is more preferably less than 1 ppm by mass, and even more preferably less than 0.6 ppm by mass. In addition, it is preferable that the content of unavoidable impurities, Cr, W, V, and Nb, be less than 5 ppm by mass, 0.6 ppm by mass, and 0.6 ppm by mass, respectively.

[0041] In addition, examples of inevitable impurities other than the above-mentioned elements and C, Cr, Mo, W, V, and Nb include Ca, Sr, Ba, rare earth elements, Zr, Be, Ti, H, Li, B, N, O, F, Na, S, Cl, K, Mn, Ga, Ge, As, Se, Br, Rb, Tc, Ru, Rh, Pd, Ag, Cd, In, Sb, Te, I, Cs, Hf, Ta, Re, Os, Ir, Pt, Au, Hg, Tl, Pb, Bi, etc. These inevitable impurities may be contained to the extent that they do not affect the characteristics. Since these unavoidable impurities may reduce electrical conductivity, the total amount is preferably 0.1 mass % or less, more preferably 0.05 mass % or less, even more preferably 0.03 mass % or less, and even more preferably 0.01 mass % or less.

[0042] (ratio of particle length of precipitate particles) The precipitate particles 12 act as an obstacle to the electrons flowing through the matrix 11. Therefore, the particle length L O and the particle length L parallel to the longitudinal direction P On the other hand, the particle length L in the direction perpendicular to the longitudinal direction O and the particle length L parallel to the longitudinal direction P Ratio of L O / L P To obtain small precipitates, coarse precipitates are necessary, and such coarse precipitates may cause surface defects. Small precipitates are often spherical and have small anisotropy. Therefore, in this embodiment, the particle length L of the precipitate particle 12 in the direction perpendicular to the longitudinal direction is calculated for the precipitate particle 12 having a particle diameter of 150 nm or more and less than 1000 nm observed in a cross section including the longitudinal direction. O and the particle length L parallel to the longitudinal direction P Ratio of L O / L P The average value is set to 0.8 or less. In order to obtain the above-mentioned effects, the particle length ratio L of the precipitate particles 12 is O / L PThe average value of is preferably 0.75 or less, and more preferably 0.7 or less.

[0043] (conductivity) In the copper alloy of this embodiment, when the electrical conductivity is 55% IACS or more, it is particularly suitable as a material for electrical and electronic equipment parts such as bus bars, etc. The electrical conductivity of the copper alloy of this embodiment is preferably 57% IACS or more, and more preferably 60% IACS or more. In the copper alloy of this embodiment, the electrical conductivity σ P is the electrical conductivity σ measured perpendicular to the longitudinal direction O When the electrical conductivity is higher than 100%, it is particularly suitable for use in electrical and electronic equipment components that pass current in a specific direction, such as bus bars. In other words, the electrical conductivity σ measured in a direction parallel to the longitudinal direction is P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O It is preferable that the electrical conductivity measured in the direction parallel to the longitudinal direction is more than 100.1%. P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O In order to increase the aspect ratio, precipitates with a high aspect ratio are necessary, but such precipitates are coarse and may cause surface defects.

[0044] Therefore, in the copper alloy of this embodiment, the electrical conductivity σ P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O is set to be greater than 100.1% and less than 105.0%. The conductivity σ measured in the direction parallel to the longitudinal direction P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ OThe lower limit of is preferably 100.2% or more, more preferably 100.3% or more. The electrical conductivity σ measured in a direction parallel to the longitudinal direction is P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O The upper limit is preferably 103.0% or less, and more preferably 102.0% or less.

[0045] (Electrical resistance ratio (R)) In the copper alloy of this embodiment, when the electrical resistance ratio (R), which is an index of electrical conductivity at low temperatures, measured in a direction parallel to the longitudinal direction is higher than the value measured in a direction perpendicular to the longitudinal direction, the copper alloy is particularly suitable as a material for electrical and electronic equipment parts that pass current in a specific direction, such as bus bars, even at low temperatures. That is, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O It is preferable that the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is more than 100.1%. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O In order to increase the aspect ratio, precipitates with a high aspect ratio are necessary, but such precipitates are coarse and may cause surface defects.

[0046] Therefore, the electrical resistance ratio R measured parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O It is preferable that the ratio is more than 100.1% and not more than 105.0%. The electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R OThe lower limit of the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is preferably 100.2% or more, and more preferably 100.3% or more. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O The upper limit is preferably 103.0% or less, and more preferably 102.0% or less.

[0047] (Tensile strength) In the copper alloy of this embodiment, when the tensile strength is 400 MPa or more, the copper alloy is excellent in strength and is particularly suitable as a material for electric / electronic device parts such as bus bars, etc. In this embodiment, the tensile strength is set to 400 MPa or more when a tensile test is performed in a direction parallel to the rolling direction. The tensile strength of the copper alloy of this embodiment is more preferably 415 MPa or more, and even more preferably 430 MPa or more.

[0048] (Vickers hardness) In the copper alloy of this embodiment, when the Vickers hardness is 100 HV or more, it does not easily deform and is particularly suitable as a material for parts for electric and electronic devices such as bus bars. The Vickers hardness of the copper alloy of this embodiment is preferably 110 HV or more, and more preferably 120 HV or more.

[0049] Next, an example of a method for producing the copper alloy according to this embodiment will be described with reference to the flow chart shown in FIG.

[0050] (Melting and casting process S01) First, the above-mentioned elements are added to the molten copper obtained by melting the copper raw material to adjust the composition, and a molten copper alloy is produced. In addition, a single element or a master alloy can be used to add various elements. In addition, a raw material containing the above-mentioned elements may be melted together with the copper raw material. In addition, recycled materials and scrap materials of this alloy may be used. Here, the molten copper is preferably so-called 4NCu, which has a purity of 99.99 mass% or more, or so-called 5NCu, which has a purity of 99.999 mass% or more. Then, the molten copper alloy with the adjusted composition is poured into a mold to produce an ingot. In addition, when considering mass production, it is preferable to use a continuous casting method or a semi-continuous casting method.

[0051] (Homogenization step S02) Next, the obtained ingot is subjected to a heat treatment for homogenization. The ingot is preferably held at 850°C to 1050°C for 1 hour or more. There is no upper limit to the holding time in the homogenization step S02, but it is preferably 24 hours or less in consideration of costs and manufacturing efficiency. There is also no particular limit to the cooling rate in the homogenization step S02, and air cooling or water cooling may be performed.

[0052] (Hot processing process S03) Next, hot working is performed. This hot working step may also serve as the homogenization step S02. After holding at 850°C to 1050°C for 1 hour or more, hot working is performed at 850°C to 1050°C, and then water cooling is performed. In addition, in this hot working step S03, the processing method is not particularly limited, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be adopted. In this embodiment, rolling processing is performed.

[0053] (Rough machining process S04) After the hot working step S03, rough processing is performed in the cold state. In this processing, the hot-worked material is immersed in liquid nitrogen for 1 minute or more, and processing is performed while cooling the processing tool with liquid nitrogen. The processing rate is preferably in the range of 10% to 95%. As a result, heat generated by processing is removed, and processing at an extremely low temperature suppresses recovery and recrystallization caused by processing heat, so that the precipitate can be processed at a low temperature, and the particle length ratio of the precipitate particles 12 can be reduced. In addition, in this rough processing step S04, the processing method is not particularly limited, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be adopted. In this embodiment, rolling processing is performed.

[0054] (First precipitation heat treatment step S05) Next, a heat treatment is performed at 450°C to 600°C for more than 1 hour and not more than 24 hours. It is preferable to shorten the holding time when the heat treatment is performed at a high temperature, and to lengthen the holding time when the heat treatment is performed at a low temperature. This first precipitation heat treatment step S05 improves the electrical conductivity. The temperature increase rate and temperature decrease rate in the first precipitation heat treatment step S05 may be set appropriately, but the temperature increase rate is preferably 1° C. / min or more, and the temperature decrease rate up to 300° C. is preferably 0.1° C. / min or more.

[0055] (First cold working process S06) After the first precipitation heat treatment step S05, the first cold working is performed. In this processing, the first precipitation heat treatment material is immersed in liquid nitrogen for 1 minute or more, and processing is performed while cooling the processing tool with liquid nitrogen. The processing rate is preferably in the range of 10% to 95%. Furthermore, the processing rate is preferably in the range of 20% to 95%, more preferably in the range of 30% to 95%, and more preferably in the range of 40% to 95%. By removing heat generated by processing and processing at an extremely low temperature, recovery and recrystallization due to processing heat are suppressed, and the precipitate can be processed at a low temperature, so that the average particle length ratio of the precipitate particles 12 can be set to 0.8 or less. In addition, in the first cold working step S06, the processing method is not particularly limited, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be adopted. In this embodiment, rolling processing is performed.

[0056] (Second precipitation heat treatment step S07) Next, a heat treatment is performed at 450°C to 600°C for more than 1 hour and not more than 24 hours. It is preferable to shorten the holding time when performing heat treatment at a high temperature, and to lengthen the holding time when performing heat treatment at a low temperature. This second precipitation heat treatment step S07 further improves the electrical conductivity. It is preferable to set the electrical conductivity of the final product to 55% IACS or more, taking into account the conditions of the subsequent steps. The temperature increase rate and temperature decrease rate in the second precipitation heat treatment step S07 may be set appropriately, but the temperature increase rate is preferably 1° C. / min or more, and the temperature decrease rate up to 300° C. is preferably 0.1° C. / min or more.

[0057] (Finishing process S08) After the second precipitation heat treatment step S07, a finish processing is performed, and the processing rate at this time is preferably within a range of 10% to 95%. In addition, in this finishing process S08, the processing method is not particularly limited, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be adopted. In this embodiment, rolling is performed.

[0058] (Distortion removal heat treatment process S09) Next, as necessary, a distortion removal heat treatment is performed in which the material is held at 200° C. or higher and lower than 700° C. for 1 second or longer and less than 24 hours in order to remove residual distortion generated in the finishing process S08. When the heat treatment is performed at a high temperature, it is preferable to shorten the holding time, and when the heat treatment is performed at a low temperature, it is preferable to lengthen the holding time.

[0059] The copper alloy of this embodiment is manufactured by the above-mentioned steps. In this embodiment, since rolling is performed as the processing method in the finish processing step S08, a copper alloy plate strip material having a predetermined plate thickness is manufactured.

[0060] The copper alloy of this embodiment having the above-described configuration contains Fe; 1.5% by mass to 2.7% by mass, P; 0.008% by mass to 0.20% by mass, Zn; 0.01% by mass to 0.5% by mass, Sn; 0.01% by mass to 0.5% by mass, with the balance being Cu and unavoidable impurities, and therefore has excellent strength and electrical conductivity as well as good thermal conductivity.

[0061] And the conductivity measured in the direction parallel to the longitudinal direction is σ P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O Since the conductivity is set to be more than 100.1% and not more than 105.0%, the material has good electrical conductivity, particularly when used in applications where electric current is passed in the longitudinal direction. In addition, for precipitate particles with an observed particle diameter of 150 nm or more and less than 1000 nm, the particle length L O and the particle length L parallel to the longitudinal direction P Compared to L O / L P Since the average value of is 0.8 or less, it is possible to improve the electrical conductivity in the longitudinal direction.

[0062] Furthermore, in the copper alloy of this embodiment, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O R P / R O When the ratio is more than 100.1% and not more than 105.0%, the material has excellent electrical conductivity in the longitudinal direction even at low temperatures, and is therefore particularly suitable as a material for electronic and electrical equipment parts used in low-temperature environments.

[0063] In addition, in the copper alloy of the present embodiment, when one or two of Mg; 0.005 mass% or more and 0.5 mass% or less and Co; 0.005 mass% or more and 0.5 mass% or less are further contained, it becomes possible to improve the heat resistance and strength by solid solution strengthening.

[0064] In addition, in the copper alloy of this embodiment, when the copper alloy further contains one or more of Ni; 0.005 mass% or more and 0.5 mass% or less, Al; 0.005 mass% or more and 0.5 mass% or less, and Si; 0.005 mass% or more and 0.5 mass% or less, it is possible to further improve the heat resistance and strength.

[0065] Furthermore, in the copper alloy of this embodiment, when the content of C contained as unavoidable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass, elements having the effect of promoting liquid phase separation in the melting and casting step S01 are reduced, and the generation of coarse Fe-based crystals in the ingot can be suppressed, and the number of surface defects that occur can be reduced.

[0066] Furthermore, in the copper alloy of this embodiment, when the electrical conductivity is set to 55% IACS or more, it can also be used in applications where high electrical conductivity is required. Furthermore, in the copper alloy of this embodiment, when the tensile strength is 400 MPa or more, it can be applied to applications requiring high strength. Furthermore, in the copper alloy of this embodiment, when the Vickers hardness is set to be 100 HV or more, it does not easily deform and is particularly suitable for use as parts for electric and electronic equipment.

[0067] Although the copper alloy according to the embodiment of the present invention has been described above, the present invention is not limited thereto, and can be appropriately modified within the scope of the technical idea of ​​the invention. In the above embodiment, an example of a method for producing a copper alloy has been described, but the method for producing a copper alloy is not limited to the one described in the embodiment, and an existing method may be appropriately selected to produce the copper alloy.

[0068] For example, in the present embodiment, rolling is performed as a processing method to obtain a copper alloy plate strip material made of the copper alloy of the present invention, but when wire drawing, extrusion, groove rolling, or the like is performed as a processing method, a copper alloy wire rod material made of the copper alloy of the present invention can be obtained, and when forging, pressing, or the like is performed as a processing method, copper alloy members of various shapes made of the copper alloy of the present invention can be obtained. EXAMPLES

[0069] First, in the melting and casting process, a copper raw material made of oxygen-free copper (ASTM B152 C10100) with a purity of 99.99% by mass or more was prepared, and this was placed in an alumina crucible and melted in a high-frequency melting furnace with an Ar gas atmosphere. Fe, P, Zn, Sn, Mg, Al, Si, Co, and Ni were added to the obtained molten copper. These elements were added using a Cu master alloy. In this way, a molten copper alloy with the composition shown in Table 1 was melted and poured into a carbon mold to produce an ingot. The size of the ingot was about 25 mm thick x about 70 mm wide x about 100 mm long.

[0070] Next, in the hot rolling process, the obtained ingot was heat-treated for 4 hours at the hot rolling temperature shown in Table 2, and then hot-worked at 900°C until the thickness became 12 mm. Note that reheating was performed appropriately as necessary. After the hot rolling, water cooling was performed. In order to remove the oxide film formed on the surface after the hot rolling, facing was performed. Next, as a rough rolling step, the material was immersed in liquid nitrogen for 10 minutes or more, and then cold-rolled to a thickness of 2 mm while cooling the rolling roll surface with liquid nitrogen.

[0071] Next, in the first precipitation heat treatment step, the sample was held for a predetermined time between 1 hour and 24 hours at the heat treatment temperature shown in Table 2 using an electric furnace, and then air-cooled, furnace-cooled, or water-cooled. Then, polishing was performed to remove the oxide film formed on the surface after the heat treatment. Next, in the first cold rolling step, the sample was immersed in liquid nitrogen for 10 minutes or more, and then cold rolling was performed until the thickness reached 0.7 mm while cooling the rolling roll surface with liquid nitrogen. Next, in the second precipitation heat treatment step, an electric furnace was used to hold the material for a predetermined time between 1 hour and 24 hours at the heat treatment temperature shown in Table 2. After the heat treatment, the material was furnace-cooled to 300° C., and then air-cooled or water-cooled.

[0072] Then, in the finish rolling step, cold rolling was performed until the thickness reached 0.5 mm in Inventive Examples 1 to 11 and Comparative Examples 1 and 2, and until the thickness reached 0.2 mm in Inventive Examples 12 to 22, to prepare samples for evaluation and measurement. Thereafter, as shown in Table 2, some of the samples were subjected to a distortion removal heat treatment for 1 minute at the temperature shown in the table using a salt bath furnace, and were used as samples for evaluation and measurement.

[0073] The copper alloys of Inventive Examples 1 to 22 and Comparative Examples 1 and 2 obtained as described above were evaluated as follows.

[0074] (Observation of precipitate particles) Observation of precipitate particles was carried out by the following method. The rolled surface of the evaluation and measurement sample, i.e., the ND surface, was mechanically polished to a mirror finish, and then the surface was subjected to ion milling processing using Ar ions at an accelerating voltage of 4.0 kV using an IM-5000 manufactured by Hitachi High-Technologies Corporation, and then observation was carried out using a field emission scanning electron microscope (SU7000 manufactured by Hitachi High-Technologies Corporation). The observation magnification was 5000 times (approximately 450 μm 2) SEM photographs were processed to add contrast only to the precipitates. From the images with added contrast, the image analysis software "Win ROOF" was used to calculate the circle equivalent diameter from the precipitate area, and for precipitate particles with a particle diameter of 150 nm or more and less than 1000 nm, the precipitate particle length ratio was calculated from the precipitate particle diameter in the direction perpendicular to the longitudinal direction and the direction parallel to the longitudinal direction. Observations were made in three or more fields of view.

[0075] (conductivity) Test pieces measuring 10 mm wide and 350 mm long were taken from the samples for evaluation and measurement, and the electrical resistance was determined by the four-terminal method. The dimensions of the test pieces were also measured using a micrometer, and the volume of the test pieces was calculated. The electrical conductivity was then measured from the measured electrical resistivity and calculated volume. The test pieces were taken so that their longitudinal direction was parallel and perpendicular to the rolling direction. The measurement results are shown in Table 3.

[0076] (Electrical resistance ratio (R)) Test pieces measuring 5 mm wide x 200 mm long were taken from the samples for evaluation and measurement, and the electrical resistivity at 293 K (ρ293 K) and at liquid nitrogen temperature (77 K) (ρ77 K) were measured using the four-terminal method, and R = ρ293 K / ρ77 K was calculated. The test pieces were taken so that their longitudinal direction was parallel and perpendicular to the rolling direction. The evaluation results are shown in Table 3.

[0077] (Tensile strength) According to JIS Z 2241, No. 13B test pieces were taken from the samples and the tensile strength was measured. The test pieces were taken so that the tensile direction was parallel to the rolling direction. The evaluation results are shown in Table 3.

[0078] (Vickers hardness) The Vickers hardness was measured with a test load of 0.98 N in accordance with the micro Vickers hardness test method specified in JIS Z 2244. The evaluation results are shown in Table 3.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

[0082] In Comparative Example 1, the first cold rolling step was performed at room temperature, so that the average grain length ratio was large at 0.86, and the anisotropy was also small. In Comparative Example 2, the rough rolling step was carried out at room temperature, so that the average grain length ratio was large at 0.88, and the anisotropy was also small.

[0083] In contrast, in the examples of the present invention, it was confirmed that the electrical conductivity in the direction parallel to the longitudinal direction was superior to that in the direction perpendicular to the longitudinal direction. The tensile strength, electrical conductivity, and Vickers hardness were also superior. From the above, it was confirmed that the examples of the present invention can provide a Cu-Fe-P-based copper alloy having electrical conductivity superior to that in the direction perpendicular to the longitudinal direction.

Claims

1. The composition is Fe; 1.5 mass% or more and 2.7 mass% or less, P; 0.008 mass% or more and 0.20 mass% or less, Zn; 0.01 mass% or more and 0.5 mass% or less, Sn; 0.01 mass% or more and 0.5 mass% or less, and the balance is Cu and unavoidable impurities, Conductivity σ measured parallel to the longitudinal direction P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O is more than 100.1% and is 105.0% or less, For precipitate particles having a particle diameter of 150 nm or more and less than 1000 nm observed in a cross section including the longitudinal direction, the particle length L in the direction perpendicular to the longitudinal direction is O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P The copper alloy is characterized in that the average value of is 0.8 or less.

2. Electrical resistance ratio R measured parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O The copper alloy according to claim 1, characterized in that it has a C content of more than 100.1% and not more than 105.0%.

3. The copper alloy according to claim 1, further comprising one or two of Mg; 0.005% by mass or more and 0.5% by mass or less; and Co; 0.005% by mass or more and 0.5% by mass or less.

4. The copper alloy according to claim 1, further comprising one or more of the following: Ni; 0.005% by mass or more and 0.5% by mass or less; Al; 0.005% by mass or more and 0.5% by mass or less; and Si; 0.005% by mass or more and 0.5% by mass or less.

5. 2. The copper alloy according to claim 1, characterized in that the electrical conductivity parallel to the longitudinal direction is 55% IACS or more.

6. The copper alloy according to claim 1, characterized in that the C content contained as the inevitable impurities is less than 5 ppm by mass, the Cr content is less than 7 ppm by mass, the Mo content is less than 5 ppm by mass, the W content is less than 1 ppm by mass, the V content is less than 1 ppm by mass, and the Nb content is less than 1 ppm by mass.

7. A part for electronic or electric equipment, comprising the copper alloy according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Copper alloy for electric and electronic part and method for producing the same

    JP2013057116A