Semiconductor element and manufacturing method thereof

The semiconductor device addresses etching damage and electrode breakage by employing a recess structure with angled and terraced side surfaces, enhancing electrode coverage and reducing contact resistance.

JP2024141592AActive Publication Date: 2024-10-10TOYODA GOSEI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023053329
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing semiconductor devices with recess structures face issues such as etching damage, reduced 2DEG concentration, and electrode breakage due to sloped recess sides and precise electrode placement challenges.

Method used

A semiconductor device with a recess structure featuring a first side surface at a specific angle, a terrace, and a second side surface with a smaller angle, formed through dry and wet etching processes, ensuring electrode coverage and preventing breakage.

Benefits of technology

The solution enhances electrode coverage and reduces contact resistance by preventing electrode breakage and maintaining 2DEG concentration, improving the semiconductor device's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141592000001_ABST
    Figure 2024141592000001_ABST
Patent Text Reader

Abstract

To realize a semiconductor element that can achieve good contact with a 2DEG layer.SOLUTION: A semiconductor element, having a substrate 10, a channel layer 12 formed on the substrate 10 and made of a Group III nitride semiconductor, and a barrier layer 13 formed on and in contact with the channel layer 12 and made of a Group III nitride semiconductor having a higher Al composition than the channel layer 12, includes a recess 20 formed in a partial region of the surface of the barrier layer 13 and having a depth reaching the channel layer 12, and an electrode provided so as to cover the recess 20, and the recess has a first side face on which the barrier layer 13 is exposed and which is angled with respect to the main surface of the substrate 10, a terrace which is connected to the first side face and on which the surface of the channel layer 12 is exposed, and a second side face which is connected to the terrace and on which the channel layer 12 is exposed, the second side face inclined with respect to the main surface of the substrate and having an inclination angle smaller than that of the first side face.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a method for manufacturing the same. [Background technology]

[0002] 2. Description of the Related Art Semiconductor devices are known that have a heterojunction structure in which a channel layer made of GaN and a barrier layer made of AlGaN are laminated in this order, and operate using a two-dimensional electron gas (2DEG) layer formed at the heterojunction interface as a channel.

[0003] In such semiconductor elements, a recess structure is sometimes provided so that the electrodes can make good contact with the 2DEG layer (for example, Patent Document 1). The recess structure is a structure in which a groove (recess) is provided in a partial region of the barrier layer surface to a depth that reaches the channel layer, a heterojunction interface is exposed on the side of the groove, and electrodes are provided along the top, side, and bottom surfaces of the recess. With this structure, the electrodes come into contact with the 2DEG layer, thereby reducing the contact resistance.

[0004] Patent Documents 2 and 3 disclose an HFET with a two-stage inclination on the side of a recess, in which the inclination angle of the recess side changes at the position where the barrier layer is exposed, and the inclination of the upper side is gentler than the lower side. Patent Document 4 also discloses a configuration in which the inclination angle of the recess side is changed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5329606 [Patent Document 2] JP 2012-99542 A [Patent Document 3] Patent No. 5625314 [Patent Document 4] Patent No. 7057473 Summary of the Invention [Problem to be solved by the invention]

[0006] However, since the recess is formed by dry etching, etching damage to the recess occurs, and the etching damage cannot be removed.

[0007] In addition, since the side surface of the recess is inclined, the effective thickness of the AlGaN layer becomes thin, and the 2DEG concentration decreases in the vicinity of the recess.

[0008] In addition, when forming an electrode in the recess, it is necessary to precisely fit the recess step so that the electrode does not break or not make contact with the 2DEG layer. Therefore, it is necessary to select sputtering, which has excellent step coverage, as the method for forming the electrode. However, sputtering can damage the semiconductor.

[0009] The present invention has been made in view of the above background, and aims to provide a semiconductor element capable of achieving good contact with the 2DEG layer, and a method for manufacturing the same. [Means for solving the problem]

[0010] One aspect of the present invention is A semiconductor device having a substrate, a channel layer formed on the substrate and made of a Group III nitride semiconductor, and a barrier layer formed on and in contact with the channel layer and made of a Group III nitride semiconductor having a higher Al composition than the channel layer, a recess provided in a portion of a surface of the barrier layer and having a depth reaching the channel layer; an electrode provided so as to cover the recess; The recess is a first side surface on which the barrier layer is exposed and which is angled with respect to a main surface of the substrate; a terrace connected to the first side surface and exposing a surface of the channel layer; The semiconductor element has a second side surface that is connected to the terrace, exposes the channel layer, and is inclined with respect to the main surface of the substrate, with the inclination angle being smaller than that of the first side surface.

[0011] Another aspect of the present invention is A method for manufacturing a semiconductor device having a substrate, a channel layer formed on the substrate and made of a Group III nitride semiconductor, and a barrier layer formed on and in contact with the channel layer and made of a Group III nitride semiconductor having a higher Al composition than the channel layer, comprising: a first recess forming step of dry etching a predetermined region of the barrier layer surface to form a first recess having a side surface inclined with respect to the main surface of the substrate and a bottom surface deeper than the channel layer surface; a second recess forming step of wet-etching a side surface of the first recess with an alkaline solution to form a second recess; and forming an electrode on the barrier layer so as to cover the second recess, The second recess formation process in the method for manufacturing a semiconductor element is a process of wet-etching the barrier layer to form a first side surface that is angled with respect to the main surface of the substrate, exposing a surface of the channel layer to form a terrace, and wet-etching the channel layer to form a second side surface that is inclined with respect to the main surface of the substrate and has a smaller inclination angle than the first side surface. Effect of the Invention

[0012] According to the present invention, the electrode has high coverage over the recess, and step disconnection of the electrode can be prevented, thereby reducing the contact resistance of the electrode. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a cross-sectional view showing the configuration of the semiconductor element in the first embodiment, the cross-section being perpendicular to the main surface of the substrate. [Diagram 2] FIG. 3 is an enlarged cross-sectional view showing a recessed portion of the semiconductor element according to the first embodiment. [Diagram 3] FIG. 2 is a diagram showing a planar pattern of an electrode. [Figure 4] 2A to 2C are diagrams illustrating a manufacturing process of the semiconductor element according to the first embodiment. [Diagram 5] 2A to 2C are diagrams illustrating a manufacturing process of the semiconductor element according to the first embodiment. [Figure 6] 3A to 3C are diagrams illustrating a manufacturing process for a recessed portion of a semiconductor element according to the first embodiment. [Figure 7] Graph comparing contact resistivity. [Figure 8] 1 is a graph showing the distribution of on-resistance of each semiconductor element. [Figure 9] Cross-sectional SEM image of the recess. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The semiconductor element has a substrate, a channel layer made of a Group III nitride semiconductor provided on the substrate, and a barrier layer made of a Group III nitride semiconductor having a higher Al composition than the channel layer and provided in contact with the channel layer, the semiconductor element having a recess provided in a partial region of a surface of the barrier layer to a depth reaching the channel layer, and an electrode provided so as to cover the recess, the recess having a first side surface which is an exposed surface of the barrier layer and angled with respect to a main surface of the substrate, a terrace connected to the first side surface which is an exposed surface of the channel layer, and a second side surface which is connected to the terrace and is an exposed surface of the channel layer, inclined with respect to the main surface of the substrate with an angle smaller than that of the first side surface.

[0015] The width of the terrace may be 100 nm or more, which can improve the electrode coverage and better prevent the electrode from being disconnected.

[0016] The first side surface may be a surface having an angle of 80 degrees or more and 90 degrees or less with respect to the main surface of the substrate. The first side surface may be an m-plane of the barrier layer. This can prevent the 2DEG concentration of the 2DEG layer from decreasing near the side surface of the recess.

[0017] A method for manufacturing a semiconductor device having a substrate, a channel layer formed on the substrate and made of a Group III nitride semiconductor, and a barrier layer formed on and in contact with the channel layer and made of a Group III nitride semiconductor having a higher Al composition than the channel layer, the method includes a first recess formation step of dry-etching a predetermined region on a surface of the barrier layer to form a first recess whose side is inclined with respect to a main surface of the substrate and whose bottom surface is deeper than the surface of the channel layer, a second recess formation step of wet-etching the side of the first recess with an alkaline solution to form a second recess, and an electrode formation step of forming an electrode on the barrier layer so as to cover the second recess, the second recess formation step being a step of wet-etching the barrier layer to form a first side surface that is angled with respect to the main surface of the substrate, exposing a surface of the channel layer to form a terrace, and wet-etching the channel layer to form a second side surface that is inclined with respect to the main surface of the substrate, the inclination angle being smaller than that of the first side surface.

[0018] The second recess forming step may be a step of forming a terrace so that the terrace has a width of 100 nm or more, which can improve the electrode coverage and better prevent the electrode from being disconnected.

[0019] The second recess forming step may be performed so that the first side surface is at an angle of 80 degrees or more and 90 degrees or less with respect to the main surface of the substrate. The second recess forming step may be performed so that the first side surface is an m-plane. This can prevent the 2DEG concentration of the 2DEG layer from decreasing near the recess side surface. The alkaline solution may be a TMAH aqueous solution.

[0020] (Embodiment 1) 1. Structure of semiconductor elements Fig. 1 is a cross-sectional view showing the configuration of a semiconductor element in embodiment 1, and is a view showing a cross section perpendicular to the main surface of a substrate. The semiconductor element in embodiment 1 is a polarization super junction (PSJ) FET, and as shown in Fig. 1, has a substrate 10, a buffer layer 11, a channel layer 12, a barrier layer 13, an undoped layer 14, a p-layer 15, a gate electrode 16, a source electrode 17, and a drain electrode 18. Fig. 2 is an enlarged cross-sectional view of a recessed portion of the semiconductor element in embodiment 1. Fig. 3 is a top view showing an electrode pattern. The AA cross section in Fig. 3 is Fig. 1.

[0021] The substrate 10 is made of sapphire with the c-plane or a-plane as the principal surface, and has a thickness of, for example, 50 to 500 μm.

[0022] The channel layer 12 is located on the substrate 10 via a buffer layer 11. The channel layer 12 is made of undoped GaN. The buffer layer 11 is, for example, low-temperature grown AlN or GaN. The thickness of the channel layer 12 is, for example, 300 to 5000 nm.

[0023] The barrier layer 13 is located on the channel layer 12. The barrier layer 13 is made of undoped AlGaN. The Al composition is 10 to 50%. The channel layer 12 and the barrier layer 13 form a heterojunction, and a two-dimensional electron gas (2DEG) layer 19 is generated in the channel layer 12 near the interface. The semiconductor device in the first embodiment operates with this 2DEG layer 19 as a channel. The barrier layer 13 has a thickness of, for example, 20 to 150 nm.

[0024] The undoped layer 14 is located in a partial region on the barrier layer 13 (a region excluding the regions where the source electrode 17 and the drain electrode 18 are formed). The undoped layer 14 is undoped GaN. The barrier layer 13 and the undoped layer 14 form a heterojunction, and a two-dimensional hole gas (2DHG) layer 22 is generated in the undoped layer 14 near the interface. This 2DHG layer 22 does not function as a channel, but flattens the electric field distribution and improves the breakdown voltage. The undoped layer 14 has a thickness of, for example, 10 to 1000 nm.

[0025] The p-layer 15 is located in a portion of the undoped layer 14, close to the source electrode 17. The p-layer 15 is made of p-GaN. The Mg concentration is, for example, 1×10 17 cm -3 More than 3×10 20 cm -3 The thickness of p-layer 15 is, for example, 20 to 150 nm. P-layer 15 may be a two-layer structure including a low-concentration p-type layer and a high-concentration p-type layer.

[0026] The gate electrode 16 is located on the p-layer 15. The material of the gate electrode 16 is, for example, Ni / Au.

[0027] The recess 20 is a groove provided in a region of the surface of the barrier layer 13 where the source electrode 17 and the drain electrode 18 are provided, and has a depth reaching the channel layer 12. The recess 20 has a two-stepped side surface, and has a shape including a side surface 20a where the barrier layer 13 is exposed, a terrace 20b that is continuous with the lower end of the side surface 20a and where the surface of the channel layer 12 is exposed, a side surface 20c that is continuous with one end of the terrace 20b and where the channel layer 12 is exposed, and a bottom surface 20d that is continuous with the lower end of the side surface 20c and is a surface where the channel layer 12 is exposed and is located deeper than the surface of the channel layer 12.

[0028] The side surface 20a is a surface perpendicular to the main surface of the barrier layer 13, and is, for example, the m-plane of AlGaN. It may be a surface other than the m-plane, such as the a-plane. It is not necessary for the surface to be perpendicular, as long as the inclination angle with respect to the main surface of the substrate 10 is larger than that of the side surface 20c. However, it is preferable that the surface is as close to perpendicular as possible, and for example, it is preferable that the surface has an angle of 80 degrees or more and 90 degrees or less with respect to the main surface of the substrate 10, and is most preferably perpendicular. The side surface 20a is a surface exposed by wet etching, and is a surface that is not damaged by etching.

[0029] The terrace 20b is the surface of the channel layer 12, which is the c-plane of GaN. The terrace 20b is a surface exposed by wet etching and is free of etching damage. The terrace 20b is perpendicular to and continuous with the side surface 20a.

[0030] The width of the terrace 20b is preferably 100 nm or more. Here, the width of the terrace 20b refers to the width of the terrace 20b in the direction of the shortest straight line connecting the source electrode 17 and the drain electrode 18 in a plan view. In the case where the electrode pattern is as shown in FIG. 2 described later, the width is the width in the direction perpendicular to the stripe. By making the width of the terrace 20b 100 nm or more and making the width of the terrace 20b sufficiently wide, the coverage of the source electrode 17 and the drain electrode 18 to the recess 20 can be further improved, and the source electrode 17 and the drain electrode 18 can be prevented from being cut off by the step of the recess 20. More preferably, the width is 140 nm or more.

[0031] Moreover, the width of the terrace 20b is preferably 1000 nm or less, because the area of ​​the 2DEG layer 19 decreases as the width of the terrace 20b increases.

[0032] The side surface 20c is angled with respect to the main surface of the channel layer 12. The angle is smaller than the angle of the side surface 20a, and is, for example, 40 to 80 degrees with respect to the main surface of the substrate 10. Since the side surface 20c is inclined, the coverage of the recess 20 with the source electrode 17 and the drain electrode 18 can be further improved. The side surface 20c is a surface exposed by wet etching and is free from etching damage. The side surface 20c is connected to the terrace 20b at an angle. The side surface 20c is, for example, an inclined m-plane.

[0033] The bottom surface 20d is a surface parallel to the main surface of the channel layer 12 and is the c-plane of GaN. The bottom surface 20d is a surface located deeper than the surface of the channel layer 12 (on the substrate 10 side) and is a surface exposed by dry etching of the channel layer 12. The bottom surface 20d is connected to the side surface 20c at an angle. The height from the bottom surface 20d to the surface of the channel layer 12 can be any value greater than 0, but is, for example, 10 nm or greater.

[0034] The source electrode 17 and the drain electrode 18 are provided in a predetermined region on the barrier layer 13, spaced apart from each other. The source electrode 17 and the drain electrode 18 are provided so as to cover the recess 20. That is, the source electrode 17 and the drain electrode 18 are provided so as to contact the side surface 20a, the terrace 20b, the side surface 20c, and the bottom surface 20d of the recess 20. Therefore, the source electrode 17 and the drain electrode 18 are in contact with the 2DEG layer 19 near the corner formed by the side surface 20a and the terrace 20b of the recess 20. This reduces the contact resistance of the source electrode 17 and the drain electrode 18. The material of the source electrode 17 and the drain electrode is, for example, Ti / Al / Ti or V / Al / Ti.

[0035] Next, the planar pattern of the recess 20 and the electrodes will be described. The source electrode 17 and the drain electrode 18 are provided at a predetermined interval in a plan view, and are patterned so that the gate electrode 16 is sandwiched between the source electrode 17 and the drain electrode 18.

[0036] 2, the source electrode 17 and the drain electrode 18 have a comb-like planar pattern. That is, they have stripe-like portions in which long, thin linear patterns are arranged in parallel at a predetermined interval, and portions that connect to each of the linear patterns. The stripe portions of the source electrode 17 and the stripe portions of the drain electrode 18 are arranged so as to interdigitate with each other.

[0037] The gate electrodes 16 are provided in a ring-shaped pattern surrounding each of the elongated linear patterns of the source electrodes 17 .

[0038] 2, inside each linear pattern of the source electrode 17 and the drain electrode 18, a plurality of recesses 20 are arranged at predetermined intervals along the line. The planar shape of the recesses 20 is, for example, a regular hexagon. This is because the side surface 20a of the recess 20 is an m-plane. Of course, the planar shape of the recess is not limited to a regular hexagon. For example, it may be an equilateral triangle, a square, a rectangle, a circle, or the like.

[0039] The diameter of the recess 20 may be large enough so that it is included in the patterns of the source electrode 17 and the drain electrode 18 in a plan view. In the case of Fig. 2, the diameter may be smaller than the width of the linear patterns of the source electrode 17 and the drain electrode 18. For example, the width of the linear patterns is 20 µm, and the diameter of the recess 20 is 5 µm.

[0040] The planar patterns of the gate electrode 16, the source electrode 17, and the drain electrode 18 are merely examples, and are not limited to the patterns shown in FIG.

[0041] 2. Operation of Semiconductor Devices The semiconductor element in the first embodiment is a normally-on type element in which a current flows from the drain electrode 18 to the source electrode 17 via the 2DEG layer 19 when no voltage is applied to the gate electrode 16. When a voltage (negative voltage) equal to or lower than the threshold voltage is applied to the gate electrode 16, the current from the drain electrode 18 to the source electrode 17 is turned off.

[0042] When a voltage (negative voltage) equal to or lower than the threshold voltage is applied to the gate electrode 16, holes are extracted and disappear from the 2DHG layer 22, and electrons disappear from the 2DEG layer 19 below the undoped layer 14. As a result, the entire lower region of the undoped layer 14 is depleted, and the electric field strength becomes constant. This allows the electric field applied from the drain electrode 18 to the gate electrode 16 to be evenly distributed, and there is no region where the electric field is concentrated. As a result, an extremely high breakdown voltage can be achieved.

[0043] Furthermore, when a voltage higher than the threshold voltage is applied to the gate electrode 16, a current flows from the drain electrode 18 to the source electrode 17, turning the device on. At this time, a current flows from the drain electrode 18 to the 2DEG layer 19 via the surface of the barrier layer 13 and the side surface 20a of the recess 20. Then, a current flows from the 2DEG layer 19 to the source electrode 17 via the surface of the barrier layer 13 and the side surface 20a of the recess 20.

[0044] 2, the source electrode 17 and the drain electrode 18 can make good contact with the 2DEG layer 19. The details are as follows.

[0045] Since the side surface 20a of the recess 20 is perpendicular to the main surface of the substrate 10, there is no substantial reduction in the thickness of the barrier layer 13. If the side surface 20a has an inclination, the strain is relaxed and the substantial thickness of the barrier layer 13 is reduced. Since there is no substantial reduction in the thickness of the barrier layer 13, it is possible to prevent a reduction in the 2DEG concentration of the 2DEG layer 19 in the vicinity of the side surface of the recess 20. As a result, the source electrode 17 and the drain electrode 18 can make good contact with the 2DEG layer 19.

[0046] The side of the recess 20 has a side 20a perpendicular to the main surface of the substrate 10, a terrace 20b which is the surface of the channel layer 12, and a side 20c inclined with respect to the main surface of the substrate 10, forming two steps. This step structure can improve the coverage of the recess 20 with the source electrode 17 and the drain electrode 18, and can prevent the source electrode 17 and the drain electrode 18 from being cut off by the steps. As a result, the source electrode 17 and the drain electrode 18 can be reliably adhered to the corner formed by the terrace 20b and the side 20c, and can make good contact with the 2DEG layer 19 near the corner.

[0047] The side surface 20a, the terrace 20b, and the side surface 20c of the recess 20 are exposed by wet etching after dry etching, as will be described in detail in the manufacturing method section. Therefore, these surfaces are free from etching damage. The source electrode 17 and the drain electrode 18 are in contact with these surfaces free from etching damage, so that the contact resistance can be reduced.

[0048] As described above, in the semiconductor element of embodiment 1, the recess 20 has a shape having the side surface 20a, the terrace 20b, the side surface 20c, and the bottom surface 20d as shown in FIG. 2 , so that the coverage of the source electrode 17 and the drain electrode 18 is high, discontinuity of the source electrode 17 and the drain electrode 18 can be prevented, and the contact resistance of the source electrode 17 and the drain electrode 18 can be reduced.

[0049] 3. Manufacturing method of semiconductor device Next, a method for manufacturing the semiconductor device according to the first embodiment will be described with reference to the drawings.

[0050] First, a channel layer 12, a barrier layer 13, an undoped layer 14, and a p-layer 15 are sequentially stacked on a substrate 10 via a buffer layer 11 by MOCVD (see FIG. 4). For example, TMG (trimethylgallium) is used as a Ga source gas, TMA (trimethyl) is used as an Al source gas, and ammonia is used as a nitrogen source gas. Hydrogen or nitrogen is used as a carrier gas.

[0051] Next, a predetermined region on the surface of the p-layer 15 is dry etched to expose the undoped layer 14. Furthermore, of the exposed undoped layer 14, a region in which the source electrode 17 and the drain electrode 18 are to be formed is dry etched to expose the barrier layer 13 (see FIG. 5).

[0052] Next, a predetermined region of the barrier layer 13 is dry-etched to form the recess 21 (see FIG. 6(a)). Here, the etching conditions are set so that the side surface of the recess 21 is inclined. The inclination angle of the side surface of the recess 21 is, for example, 30 to 70 degrees with respect to the main surface of the substrate 10. Moreover, the recess 21 is formed deeper than the surface of the channel layer 12. This dry etching causes etching damage to the side surface and bottom surface of the recess 21.

[0053] Next, the side surface of the recess 21 is wet-etched with a TMAH aqueous solution. The concentration of the TMAH aqueous solution is, for example, 15 to 25 wt %. The temperature of the TMAH aqueous solution is, for example, 60 to 90° C. If the concentration and temperature are within these ranges, the difference in etching rate between the barrier layer 13 and the channel layer 12 becomes appropriate, and the recess 20 can be easily formed.

[0054] The etching time is, for example, 10 to 30 minutes. If the etching time is shorter than 10 minutes, the width of the terrace 20b does not expand sufficiently, and there is a possibility that the coverage of the source electrode 17 and the drain electrode 18 may decrease or the step may be broken. If the etching time is longer than 30 minutes, the etching of the channel layer 12 progresses, the m-plane is exposed, the side surface 20c becomes vertical, and there is a possibility that the coverage of the source electrode 17 and the drain electrode 18 may decrease or the step may be broken.

[0055] In wet etching of a group III nitride semiconductor using a TMAH aqueous solution, the side surface of the recess 20 is etched because it is a surface other than the c-plane, but the surface of the barrier layer 13, the surface of the channel layer 12, and the bottom surface of the recess 20 are not etched because they are c-planes. Also, the higher the Al composition, the faster the etching rate. Also, as the etching progresses, the m-plane is exposed, and the etching progresses while maintaining the m-plane.

[0056] Therefore, the recess 20 having the side surface 20a, the terrace 20b, the side surface 20c, and the bottom surface 20d is formed by wet etching the recess 21 (see FIG. 6(b)).

[0057] The region of the side of the recess 21 where the barrier layer 13 is exposed is etched quickly in the lateral direction, while the region of the side of the recess 21 where the barrier layer 13 is exposed is etched slower. This is because the barrier layer 13 has a higher Al composition than the channel layer 12. This etching exposes the surface of the channel layer 12. This exposed surface of the channel layer 12 is not etched because it is the c-plane. This forms the terrace 20b of the recess 20. The terrace 20b is a surface that was not exposed when the recess 21 was formed, and is therefore free from etching damage.

[0058] As the etching of the barrier layer 13 progresses, the m-plane of the barrier layer 13 is exposed, and a side surface 20a of the recess 20 perpendicular to the main surface of the barrier layer 13 is formed. Furthermore, etching damage to the side surface 20a is removed by etching the barrier layer 13.

[0059] Furthermore, the region of the side of the recess 21 where the channel layer 12 is exposed is made of GaN having a lower Al composition than the barrier layer 13 (Al composition is 0), and therefore the etching rate is slower than that of the barrier layer 13. As a result, the etching does not progress to the point where the side becomes vertical, and the side has an inclination. This inclined side of the channel layer 12 becomes the side 20c of the recess 20. The inclination angle of the side 20c is equal to or greater than the inclination angle of the side of the recess 21. This etching of the channel layer 12 removes etching damage to the side 20c.

[0060] The bottom surface of the recess 21 is not etched because it is the c-plane, and remains as it is as the bottom surface 20d of the recess 20. In this manner, the recess 20 having the side surface 20a, the terrace 20b, the side surface 20c, and the bottom surface 20d is formed.

[0061] In addition to TMAH, the wet etching solution can be an alkaline solution such as KOH or NaOH, and the solvent is not limited to water.

[0062] Next, the source electrode 17 and the drain electrode 18 are formed in predetermined regions on the barrier layer 13. The source electrode 17 and the drain electrode 18 are formed so as to cover the recess 20. When the source electrode 17 and the drain electrode 18 are made of the same material, they can be formed at the same time.

[0063] Here, the recess 20 has a terrace 20b where the surface of the channel layer 12 is exposed, and a side surface 20c has an inclination. Therefore, the source electrode 17 and the drain electrode 18 can be formed with good coverage along the step of the recess 20, and step disconnection can be prevented. In particular, the source electrode 17 and the drain electrode 18 can be reliably adhered to the 2DEG layer 19 exposed near the corner formed by the terrace 20b and the side surface 20c.

[0064] The source electrode 17 and the drain electrode 18 can be formed by deposition, sputtering, or the like. In particular, it is preferable to use deposition such as EB deposition. Conventionally, sputtering, which is a forming method with good coverage, has been used to cover the recesses without causing the source electrode 17 and the drain electrode 18 to break up, but sputtering can cause damage to the semiconductor layer. In contrast, the recess 20 in the first embodiment has good coverage of the source electrode 17 and the drain electrode 18 due to its shape, so that breaks can be prevented even if the source electrode 17 and the drain electrode 18 are formed by deposition.

[0065] Furthermore, since the source electrode 17 and the drain electrode 18 are in contact with the side surface 20a, the terrace 20b, and the side surface 20c of the recess 20 that are not damaged by etching, the contact resistance can be reduced.

[0066] Next, a heat treatment is performed to reduce the contact resistance of the source electrode 17 and the drain electrode 18. The heat treatment conditions are, for example, a nitrogen atmosphere, 500 to 700° C., and 60 to 600 seconds.

[0067] Next, the gate electrode 16 is formed by deposition or the like on the p-layer 15. The gate electrode 16 may be formed first, and then the recess 20, the source electrode 17, and the drain electrode 18 are formed. In this manner, the semiconductor element of the first embodiment is manufactured.

[0068] 4. Experimental Results As sample A, a semiconductor device according to embodiment 1 in which a recess 20 was formed in the following manner was fabricated. First, a recess 21 was formed by dry etching to a depth reaching the channel layer 12, and then wet etching was performed at 50°C for 20 minutes using a TMAH aqueous solution with a concentration of 2.3 wt%. This resulted in the formation of a recess 20 with a terrace 20b having a width of 40 nm. Then, electrodes were formed on the top, side, and bottom surfaces of the recess 20. The electrodes were Ti / Al / Ti, and the alloy temperature was 600°C.

[0069] On the other hand, for sample B, the wet etching after the formation of the recess 21 was changed as follows to form the recess 20. The rest was the same as for sample A. The wet etching was performed at 85° C. for 20 minutes using a TMAH aqueous solution with a concentration of 22 wt %. As a result, the recess 20 with a terrace 20b width of 140 nm was formed.

[0070] Figure 7 is a graph showing the results of measuring and comparing the contact resistance by TLM patterns for samples A and B. As shown in Figure 7, both the average and median values ​​of contact resistivity were lower for sample B than for sample A.

[0071] In addition, a plurality of semiconductor elements according to the first embodiment having the recesses 20 of samples A and B were fabricated, and the on-resistance of each element was measured. Fig. 8 is a graph showing the distribution of the on-resistance of each element. As shown in Fig. 8, it was found that the median on-resistance of sample B was one order of magnitude lower than that of sample A.

[0072] Figure 9 shows cross-sectional SEM images of the recess cross sections of samples A and B. As shown in Figure 9(a), sample A showed a step discontinuity. On the other hand, as shown in Figure 9(b), sample B showed no step discontinuity in the electrode.

[0073] 7 to 9, it is found that the coverage of the electrode to the recess 20 is improved and step disconnection can be prevented by sufficiently increasing the width of the terrace 20b in the recess 20. It is also found that the improved coverage and prevention of step disconnection can reduce the contact resistivity of the electrode and reduce the on-resistance.

[0074] 4. Various Transformations The present invention is not limited to the semiconductor device shown in the first embodiment, but can be applied to any semiconductor device having a channel layer made of a group III nitride semiconductor, a barrier layer made of a group III nitride semiconductor having a higher Al composition than the channel layer, and an electrode in contact with the 2DEG layer through a recess. For example, the present invention can be applied to an HFET or the like. [Explanation of symbols]

[0075] 10: Substrate 11: Buffer layer 12: Channel layer 13: Barrier layer 14: Undoped layer 15:p layer 16: Gate electrode 17: Source electrode 18: Drain electrode 19:2DEG layer 20: Recess

Claims

1. A semiconductor device having a substrate, a channel layer formed on the substrate and made of a Group III nitride semiconductor, and a barrier layer formed on and in contact with the channel layer and made of a Group III nitride semiconductor having a higher Al composition than the channel layer, a recess provided in a portion of a surface of the barrier layer and having a depth reaching the channel layer; an electrode provided so as to cover the recess; The recess is a first side surface on which the barrier layer is exposed and which is angled with respect to a main surface of the substrate; a terrace connected to the first side surface and exposing a surface of the channel layer; a second side surface connected to the terrace, exposing the channel layer, inclined with respect to the main surface of the substrate, the inclination angle of the second side surface being smaller than that of the first side surface.

2. The semiconductor device according to claim 1 , wherein the terrace has a width of 100 nm or more.

3. 3. The semiconductor element according to claim 1, wherein the first side surface is a surface that has an angle of 80 degrees or more and 90 degrees or less with respect to a main surface of the substrate.

4. The semiconductor device according to claim 1 , wherein the first side surface is an m-plane of the barrier layer.

5. A method for manufacturing a semiconductor device having a substrate, a channel layer formed on the substrate and made of a Group III nitride semiconductor, and a barrier layer formed on and in contact with the channel layer and made of a Group III nitride semiconductor having a higher Al composition than the channel layer, comprising: a first recess forming step of dry etching a predetermined region of the barrier layer surface to form a first recess having a side surface inclined with respect to the main surface of the substrate and a bottom surface deeper than the channel layer surface; a second recess forming step of wet-etching a side surface of the first recess with an alkaline solution to form a second recess; and forming an electrode on the barrier layer so as to cover the second recess, a second recess forming step of wet-etching the barrier layer to form a first side surface that is angled with respect to a main surface of the substrate, exposing a surface of the channel layer to form a terrace, and wet-etching the channel layer to form a second side surface that is inclined with respect to the main surface of the substrate and has a smaller inclination angle than the first side surface.

6. The method of claim 5 , wherein the second recess forming step forms the terrace so that the terrace has a width of 100 nm or more.

7. 7. The method for manufacturing a semiconductor element according to claim 5, wherein the second recess forming step forms the first side surface at an angle of 80 degrees or more and 90 degrees or less with respect to the main surface of the substrate.

8. 7. The method for manufacturing a semiconductor device according to claim 5, wherein the second recess forming step forms the first side surface to be an m-plane.

9. 7. The method for manufacturing a semiconductor device according to claim 5, wherein the alkaline solution is an aqueous TMAH solution.

Citation Information

Patent Citations

  • Hetero-structure field effect transistor using nitride semiconductor

    JP2008004720A

  • Semiconductor device made of gallium-nitride compound semiconductor and manufacturing method thereof

    JP2009239144A

  • Semiconductor device and method of manufacturing the same

    JP2011091200A

  • Schottky diode and manufacturing method of the same

    JP2018195819A

  • Semiconductor device and production method for semiconductor device

    WO2021246227A1