Material, refractory material, fire-resistant insulating board, and structure
A hydraulic compound-based material with a resin composition layer and crystal water addresses fire resistance and shape retention issues in insulation materials, ensuring long-term performance and thermal insulation.
Patent Information
- Application Number
- JP2023054005
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional fire-resistant insulation materials face issues with fire resistance, shape retention, and performance degradation over time, particularly in organic resin materials, and inorganic materials suffer from high thermal conductivity and poor workability.
A material comprising a cured product of a hydraulic compound with a resin composition layer and crystal water, having a moisture permeability coefficient of 1,000 ng/m²·s·Pa or less, which includes ettringite and gypsum, ensuring excellent fire resistance and shape retention.
The material maintains superior fire resistance and shape retention, even after prolonged storage, with improved thermal insulation properties.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001
Abstract
Description
[Technical field]
[0001] The present invention relates to materials, fire resistant materials, fire resistant insulation boards and structures. [Background technology]
[0002] A variety of insulating and fire-resistant materials are used in buildings, including polyurethane foam, polystyrene foam, and phenol foam, which are resin materials that have high insulating properties, are lightweight, and are easy to work with. In addition, inorganic fiber aggregates such as glass wool and rock wool, which are inexpensive, are also used.
[0003] Since resin materials are organic substances, they burn when a fire occurs and often cause damage by the fire spreading, so measures to prevent this are needed.
[0004] On the other hand, inorganic fiber aggregates such as glass wool and rock wool are mainly composed of non-flammable materials, but they tend to have higher thermal conductivity than resin compositions, making them inferior in terms of insulation, and because they are fibrous, they feel punctured and are difficult to work with.Furthermore, in the past, the fiber aggregate was packed in a plastic bag and inserted between the pillars and exterior walls of the house, but this had issues such as gaps and the bag falling off over time.
[0005] On the other hand, heat insulating materials and fireproof materials that have been given non-combustibility to resin materials are already on the market. For example, there is a non-combustible heat insulating board in which one or both sides of a phenol foam board are laminated with non-combustible materials such as aluminum foil, aluminum hydroxide paper, and gypsum-based boards. However, in the case of a fire, although the surface facing the flames of such a conventional non-combustible heat insulating board does not burn, the heat melts the phenol foam inside, creating a cavity, causing the board itself to fall off and spread the fire. Therefore, the material does not meet the fire-resistant construction specifications stipulated in the Building Standards Act.
[0006] Examples of existing technologies for improving the flame resistance of resin materials include a technology for improving the flame resistance of polyurethane foam that relates to an insulating material in which a foam is formed from an alkali metal carbonate, an isocyanate, water, and a reaction catalyst (Patent Document 1), and a technology for insulating coated granules in which synthetic resin foam particles are surface-treated by forming a coating consisting of sepiolite and an aqueous organic binder mainly composed of a water-soluble resin, and then further coated with a coating material consisting of an inorganic powder and an aqueous inorganic binder containing water glass mainly composed of an alkali metal silicate, and then dried and hardened (Patent Document 2).
[0007] However, in the conventional method of reacting an aqueous solution of 30% or more alkali metal carbonate with isocyanates as in Patent Document 1, a large amount of water is used, leaving a large amount of unreacted water, so it must be dried before it can be used as a heat insulating material, and the foam obtained has large bubbles, so it is considered that the heat insulating properties are not great. In the conventional technology using silicates as in Patent Document 2, the resin foam melts upon combustion, and the binding strength of the filled silicate itself is lost and it is turned into powder, so it is considered that it is difficult to maintain the shape.
[0008] Also known are a composition containing calcium aluminate having a CaO content of 40 mass% or more, gypsum, an inorganic powder having a hollow structure with an average particle size of 20 to 60 μm, and a waste glass foam powder with an average particle size of 20 to 130 μm (Patent Document 3); a fire-resistant coating material consisting of 100 parts by weight of calcium aluminate, 5 to 500 parts by weight of gypsum, and a setting retarder (Patent Document 4); and a fire-resistant coating composition containing ettringite as a main component, an inorganic compound powder or titanium oxide powder that releases a non-flammable gas at 100 to 1000° C. (Patent Document 5).
[0009] Also, a fire-resistant structure for a wooden building is known which includes a wooden base made of wood material, a first gypsum board attached to the interior side of the wooden base, an aluminum-layered glass fiber sheet attached to the interior side of the first gypsum board, and a second gypsum board attached to the interior side of the aluminum-layered glass fiber sheet, in which the aluminum-layered glass fiber sheet is made of a glass fiber sheet with at least one side covered with aluminum foil (Patent Document 6). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 10-67576 [Patent Document 2] JP 2001-329629 A [Patent Document 3] JP 2017-77994 A [Patent Document 4] Japanese Patent Application Publication No. 7-48153 [Patent Document 5] Japanese Patent Application Publication No. 7-61841 [Patent Document 6] JP 2007-39915 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, when the above-mentioned conventional techniques are used in fire-resistant insulation boards used under normal conditions, there is a demand for improved fire resistance and shape retention. In particular, there is a demand for performance not to deteriorate with age when stored for a long period of time.
[0012] In view of the above, an object of the present invention is to provide a material that has excellent fire resistance and shape retention and can maintain the above-mentioned performance. [Means for solving the problem]
[0013] As a result of intensive research conducted by the present inventors in light of the above-mentioned problems, they found that the above-mentioned problems can be solved by a material in which a substrate contains a cured product of a hydraulic compound, has a resin composition layer defined by a predetermined moisture permeability coefficient, and contains water of crystallization, and thus completed the present invention.
[0014] [1] A material comprising a substrate containing a cured product of a hydraulic compound, the substrate having a resin composition layer having a moisture permeability coefficient of 1,000 ng / m s Pa or less, and the substrate containing water of crystallization. [2] The water content derived from the water of crystallization is 40 kg / m 3 The material described in [1] above. [3] The substrate further contains free water, and the water content derived from the free water is 10 kg / m 3 The material according to the above [1] or [2]. [4] The material according to any one of the above [1] to [3], wherein the hardened body of the hydraulic compound contains ettringite and / or gypsum. [5] The material according to any one of the above [1] to [4], wherein the content of the ettringite is 20 to 95 mass%. [6] The material according to any one of the above [1] to [5], wherein the gypsum content is 20 to 95 mass %. [7] A fire-resistant material comprising any one of the materials described in [1] to [6] above. [8] Density: 200-800 kg / m 3 The fireproof material according to [7] above. [9] A fire-resistant insulation board containing the fire-resistant material described in [7] or [8] above.
[10] A structure comprising a substrate containing a cured product of a hydraulic compound provided on at least a surface of a building that requires fire resistance, the substrate having a resin composition layer having a moisture permeability coefficient of 1,000 ng / m s Pa or less on the side opposite the building, the substrate containing water of crystallization.
[11] The structure according to
[10] above, which is a fire-resistant structure. Effect of the Invention
[0015] According to the present invention, it is possible to provide a material, such as a fire-resistant insulation board, which has excellent fire resistance and shape retention and can maintain the above-mentioned properties. [Brief description of the drawings]
[0016] [Figure 1] 1 is a side view showing a structure of a fireproof material structure according to an embodiment of the present invention. [Diagram 2] 1 is a top view showing a structure of a fireproof material structure according to an embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to this embodiment. In addition, "%" and "parts" in this specification are based on mass unless otherwise specified, and the numerical range in this specification includes the upper and lower limits unless otherwise specified.
[0018] [1. Materials] The material according to the present embodiment is a material including a substrate containing a cured product of a hydraulic compound, the substrate having a resin composition layer with a moisture permeability coefficient of 1,000 ng / m·s·Pa or less, and the substrate containing water of crystallization. The material of the present invention has a substrate containing a cured product of a hydraulic compound, has a resin composition layer defined by a predetermined moisture permeability coefficient, and contains water of crystallization, and thus has excellent fire resistance and shape retention, and can maintain these performances.
[0019] The substrate contains a hardened product of a hydraulic compound. In the present invention, the hydraulic compound refers to a compound that hardens when mixed with water, and the hardened product is called a hardened product. As the hydraulic compound, for example, cement or gypsum can be used.
[0020] The cement is not particularly limited, and examples thereof include various cements such as normal, early strength, super early strength, low heat and medium heat, various mixed cements obtained by mixing these cements with blast furnace slag, fly ash, silica fume, etc., environmentally friendly cements (eco-cements) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials, commercially available fine particle cements, etc. It is also possible to use various cements and various mixed cements in a fine powder form. Also, cements adjusted by increasing or decreasing the amount of components used in normal cements can be used.
[0021] As gypsum, any of anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum can be used, and there is no particular limitation. Anhydrous gypsum is calcium sulfate anhydrite, CaSO 4 Hemihydrate gypsum is a general term for compounds with the molecular formula CaSO 4 1 / 2H 2 It is a general term for compounds with the molecular formula CaSO 4 2H 2 It is a general term for compounds with the molecular formula O.
[0022] The hardened body of the hydraulic compound preferably contains ettringite and / or gypsum. Ettringite is produced by a hydration reaction between cement, calcium aluminate, etc. and gypsum, etc. As the gypsum, the above-mentioned anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum can be used, and it is preferable to contain anhydrous gypsum and / or dihydrate gypsum.
[0023] The calcium aluminate is a mixture of CaO and Al obtained by mixing calcia raw materials and alumina raw materials, firing them in a kiln or melting them in an electric furnace, and then cooling them. 2 O 3It is a general term for a substance having hydration activity and mainly composed of calcium aluminate. Although there is no particular limitation on calcium aluminate, amorphous calcium aluminate that is melted and then quenched is preferred from the viewpoint of initial strength development after hardening. From the viewpoint of reaction activity, the CaO content of calcium aluminate is preferably 30 mass% or more, more preferably 34 mass% or more, and most preferably 40 mass% or more. Although there is no particular upper limit, 50 mass% is preferred.
[0024] Calcium aluminate includes calcium aluminate CaO and Al 2 O 3 Compounds in which a part of the above is replaced with an alkali metal oxide, an alkaline earth metal oxide, silicon oxide, titanium oxide, iron oxide, an alkali metal halide, an alkaline earth metal halide, an alkali metal sulfate, an alkaline earth metal sulfate, or the like, can also be used. Alternatively, CaO and Al 2 O 3 Compounds containing small amounts of these as solid solutions in which the above are the main components can also be used.
[0025] The vitrification rate of calcium aluminate is preferably 8% or more, more preferably 50% or more, and even more preferably 90% or more. The vitrification rate of calcium aluminate can be calculated by the following method. For a sample before heating, the main peak area S of the crystalline mineral is measured in advance by powder X-ray diffraction method, and then the sample is heated at 1,000°C for 2 hours and slowly cooled at a cooling rate of 1 to 10°C / min, and the main peak area S of the crystalline mineral after heating by powder X-ray diffraction method is measured. 0 Furthermore, these S 0 Using the values of and S, the vitrification rate χ is calculated using the following formula. Vitrification rate χ(%)=100×(1-S / S 0 )
[0026] The particle size of calcium aluminate is 3,000 cm2 in terms of early strength development. 2 / g or more is preferable, and 5,000 cm 2 / g or more is more preferable, and the particle size is 3,000 cm 2 / g or more, the early strength development is likely to be improved. Here, the Blaine specific surface area value is a value measured in accordance with the method specified in JIS R 5201:2015 "Physical test methods for cement."
[0027] The particle size of the gypsum is preferably an average particle size of 1 to 30 μm, more preferably 5 to 25 μm, in terms of obtaining non-combustibility, early strength development, and an appropriate working time. Here, the average particle size is a value measured using a laser-based particle size distribution analyzer in a dispersed state using an ultrasonic device. Also, in terms of obtaining non-combustibility, early strength development, and an appropriate working time, a gypsum having a Blaine specific surface area value of 3,000 cm is preferable. 2 / g or more is preferable, and 4,000 cm 2 / g or more is more preferable.
[0028] The pH of gypsum when immersed in water is preferably a value ranging from weakly alkaline to acidic, and more preferably 8 or less. A pH of 8 or less is preferable because the solubility of the gypsum component is low, and non-combustibility and early strength development are improved. The pH here is the pH of a diluted slurry at 20°C with gypsum / ion-exchanged water = 1g / 100g, measured using an ion-exchange electrode or the like.
[0029] The content of ettringite in the hardened body of the hydraulic compound is preferably 20 to 95 mass%, more preferably 30 to 80 mass%, and further preferably 45 to 75 mass%. By having the content of ettringite within the above range, the fire resistance can be made more excellent.
[0030] The content of gypsum in the hardened body of the hydraulic compound is preferably 20 to 95 mass%, more preferably 30 to 80 mass%, and even more preferably 45 to 75 mass%. By having the content of gypsum within the above range, it is possible to achieve more excellent fire resistance.
[0031] The hardened body of the hydraulic compound may have a total content of ettringite and gypsum of 100 mass%, and may contain calcium hydroxide, monosulfate hydrate (AFm), and residues of the above-mentioned cement, calcium aluminate, and the like used as raw materials as components other than ettringite and gypsum.
[0032] The hardened hydraulic compound according to this embodiment is produced by, for example, mixing cement, calcium aluminate, or the like with gypsum to prepare a composition, and hardening a slurry containing the composition and water to produce a hardened hydraulic compound. The amount of water used to prepare the slurry is preferably 70 to 250 parts by mass, more preferably 100 to 200 parts by mass, per 100 parts by mass of the composition. When calcium aluminate and gypsum are used in combination, the amount of gypsum used is preferably 70 to 250 parts by mass, more preferably 100 to 200 parts by mass, per 100 parts by mass of calcium aluminate.
[0033] The substrate has a resin composition layer having a moisture permeability coefficient of 1,000ng / m·s·Pa or less. If it exceeds 1,000ng / m·s·Pa, the fire resistance and shape retention may be poor. The moisture permeability coefficient of the resin composition layer is preferably 800ng / m·s·Pa or less, more preferably 750ng / m·s·Pa or less, and even more preferably 600ng / m·s·Pa or less. There is no particular lower limit, but it may be 100ng / m·s·Pa or more. If it is within the above range, the fire resistance and shape retention can be made more excellent. In the present invention, the moisture permeability coefficient can be measured in accordance with the method specified in JIS A 1324:1995 "Method for measuring moisture permeability of building materials".
[0034] From the viewpoint of fire resistance and shape retention, the material preferably has a resin composition on the surface of the hardened hydraulic compound facing the flame, more preferably has a resin composition on the back side, and even more preferably has a resin composition on the entire surface. The form of the fireproof material may include, for example, a board shape, as well as a form having a resin composition layer on the surface of a wall or pillar made of a hardened hydraulic compound, and a form in which a resin composition layer is provided on the surface of a hardened hydraulic compound that has been sprayed and hardened.
[0035] The thickness of the substrate is preferably 10 mm or more, more preferably 30 mm or more, and even more preferably 40 mm or more. By being within the above range, fire resistance and shape retention can be improved.
[0036] The thickness of the resin composition layer is preferably 40 to 1,000 μm, more preferably 50 to 800 μm, and further preferably 55 to 500 μm. The form of the resin composition layer is not particularly limited, but is preferably a coating layer having a thickness that satisfies the above range.
[0037] The resin composition layer preferably contains a (meth)acrylic resin. As the (meth)acrylic resin, a hydrophobic resin capable of forming an emulsion using water as a dispersion medium is preferable. For example, vinyl polymers such as (meth)acrylic copolymer, styrene-(meth)acrylic copolymer, ethylene-vinyl alcohol copolymer, ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer can be used, and one or more of the above may be used in combination.
[0038] The resin composition layer preferably further contains an inorganic material. The inorganic material preferably contains silicate, and more preferably has swelling properties that absorb water and swell by drawing water molecules into the crystal layer. For example, synthetic smectites, synthetic bentonites, synthetic micas, etc. can be used, and one or more of the above may be used in combination.
[0039] The substrate contains water of crystallization. The water content due to water of crystallization is 40 kg / m 3 It is preferable that the content is 50 kg / m or more. 3 More preferably, it contains 70 kg / m or more. 3 It is more preferable that the content is 400 kg / m or more. There is no particular upper limit, but 3 It is preferable that the content is less than 300 kg / m 3 It is more preferable that the content be within the above range. By setting the content within the above range, fire resistance and shape retention can be improved.
[0040] The substrate preferably further contains free water, and the water content derived from the free water is 10 kg / m 3 It is preferable that the content is 20 kg / m or more. 3 More preferably, it contains 30 kg / m or more. 3 It is more preferable that the content be within the above range. By setting the content within the above range, fire resistance and shape retention can be made more excellent.
[0041] The substrate preferably further contains fibers. As the fibers, inorganic fibers are preferable, for example, alkali-resistant glass fibers, basalt fibers, ceramic fibers, etc. Basalt fibers are fibers obtained by crushing high-density basalt, melting it at a high temperature of 1,500°C or more, and spinning it. Ceramic fibers are a general term for artificial mineral fibers whose main components are alumina and / or silica. Ceramic fibers are classified into amorphous alumina-silica fibers (RCF: Refractory Ceramic Fibers) and crystalline fibers (AF: Alumina Fibers) made of alumina and silica with an alumina content of 60% or more, and either type can be used.
[0042] The form of use of the fibers is not particularly limited, but the fibers are preferably processed by cross-knitting a bundle of fibers, cut into lengths of about 1 to 50 mm or 1 to 30 mm and processed into short fibers, or mixed with an organic solvent and processed into a sheet having a thickness of about 0.1 to 3 mm by a papermaking method. Such inorganic fibers are preferably applied to a part or the whole of the substrate to reinforce it. They may also be included inside.
[0043] The amount of the fibers used is preferably 0.1 to 20 parts by mass, more preferably 3 to 15 parts by mass, based on 100 parts by mass of the above-mentioned composition. When the amount of the fibers used is within the above range, sufficient effects are easily obtained and it is economical.
[0044] The material according to the present embodiment can use any of various additives within a range that does not affect performance, and the type of additive is not particularly limited. For example, surfactants, air entraining agents, carbonization promoters such as sugars, phosphorus compounds, bromine compounds, boron compounds, nitrogen compounds, magnesium hydroxide, flame retardant agents such as sodium hydrogen carbonate, fire spread inhibitors such as thermally expanded graphite, inorganic substances such as talc and zeolite, hydration promoters such as slaked lime and various carbonates, setting retarders such as oxycarboxylates and tartaric acid, conventional rust inhibitors, antifreeze agents, shrinkage reducing agents, inorganic hollow aggregates such as tumblers, clay minerals such as bentonite and sepiolite, anion exchangers such as hydrotalcite, resin particles such as polystyrene beads, etc. can be used, and one or more of the above may be used in combination.
[0045] The amount of each additive used in the hardened product of the hydraulic compound is preferably 0.1 to 150 parts by mass, more preferably 5 to 100 parts by mass, and even more preferably 85 to 90 parts by mass, based on 100 parts by mass of the above-mentioned composition.
[0046] [2. Fireproof material] The fireproof material according to the present embodiment contains the material of the present invention. By containing the material of the present invention, the fireproof material has excellent fire resistance and shape retention, and can maintain these properties.
[0047] The density of the refractory material is 200-800 kg / m 3 is preferably 250 to 750 kg / m 3 More preferably, it is 300 to 600 kg / m 3 When it is within the above range, sufficient fire resistance and heat insulation are easily ensured.
[0048] [3. Fireproof insulation board] The fireproof and insulating board according to the present embodiment contains the fireproof material of the present invention. As a method for producing the fireproof and insulating board, for example, a plurality of the fireproof materials of the present invention are arranged and combined to form a single fireproof and insulating board.
[0049] The shape of the fireproof and insulating boat is not particularly limited, but is preferably in the range of 500 to 1,500 mm in length, 1,000 to 2,500 mm in width, and 10 to 100 mm in thickness. If the size is within this range, it is not too heavy and the workability during installation is good.
[0050] [4.Structure] The structure according to the present embodiment is a structure in which a base material containing a hardened hydraulic compound is provided on at least the surface of a building that requires fire resistance, and the base material has a resin composition layer having a moisture permeability coefficient of 1,000 ng / m·s·Pa or less on the opposite side of the building, and the base material contains crystal water. By installing the structure on a building, it becomes possible to impart fire resistance to the building. The hardened hydraulic compound, the base material, and the resin composition layer can be those already described. In one embodiment, the structure is preferably a fire-resistant material structure.
[0051] For example, the fireproof material structure, in terms of the layer structure from the exterior wall side, is composed of layers in the order of siding board, moisture-permeable waterproof sheet, resin composition layer, substrate, and structural plywood, with a space of about 100 mm (space for insulating material such as glass wool) provided between the structural plywood and the substrate by partitions. The substrate may further have a resin composition layer on the structural plywood side. The fireproof material structure may have a substrate having the resin composition layer so as to sandwich the structural plywood. Also, a furring strip may be provided between the siding board and the moisture-permeable waterproof sheet.
[0052] When constructing a fireproof structure, a plurality of substrates each having a resin composition layer may be laminated according to the required fireproof specifications, or a substrate each having a resin composition layer may be provided so as to sandwich a structural plywood. In addition, the fireproof structure may be used in combination with a reinforced gypsum board, a calcium silicate board, or the like. EXAMPLES
[0053] The present invention will be described in more detail below using examples and comparative examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.
[0054] [Experimental Example 1] <Fireproofing material manufacturing> A slurry using the raw materials described below was poured into a specified formwork (size: length 20 cm x width 20 cm x thickness 6 cm), and furthermore, alkali-resistant glass fiber and polyester nonwoven fabric were layered on the top and bottom of the substrate to reinforce the substrate, and the substrate was produced. The produced substrate was cured at room temperature for 3 days, and then a resin material was applied to the entire surface to produce a material in which a resin composition layer was provided on the substrate, and the material was cured for another 3 days to produce a fireproof material. The produced fireproof material was measured for water content (crystal water, free water), fire resistance, shape retention, shape retention rate, and thermal conductivity by the method described below. The results are shown in Table 1 below.
[0055] <Raw materials used> Calcium aluminate 1 (CA1): CaO 43% by mass, Al 2 O 3Amorphous calcium aluminate melted and quenched in an electric furnace to give a calcium aluminate content of 53 mass%, with a Blaine specific surface area of 6,100 cm 2 / g, vitrification rate 98%. Calcium aluminate 2 (CA2): Denka Alumina Cement No. 1, CaO: 36%, vitrification rate: 15%, Blaine specific surface area: 4,570 cm 2 / g. Gypsum 1 (CS1): Type II anhydrous gypsum (manufactured by Noritake Company: D-101A) purity 95%, average particle size 20 μm, pH 8 or less. Gypsum 2 (CS2): Special grade calcined gypsum manufactured by Yoshino Gypsum Co., Ltd., average particle size 20 μm. Inorganic fiber: Silica fiber (BELCOTEX: manufactured by Imae Kogyo Co., Ltd.). Polystyrene beads: Commercially available, particle size 1mm to 5mm. Inorganic hollow aggregate: Shirasu balloon (Marunaka Hakudo Co., Ltd.: Marllite BA-20). Sepiolite: Commercially available product (TOLSA: PANGEL AD). Resin material A: Acrylic resin emulsion (Toagosei Co., Ltd.: Acricept JK). Resin material B: Styrene-acrylic wax composite emulsion (Seiko PMC: XP8829). Resin material C: A composite emulsion prepared by mixing 100 parts by mass of EVA emulsion (NS Slab Fine manufactured by Nippon Kasei Co., Ltd.) with 15 parts by mass of synthetic mica (ME300B-4T manufactured by Katakura Co-op Agri Co., Ltd.). Resin material D: EVA-based emulsion (NS Slab Fine, manufactured by Nippon Kasei Chemical Industry Co., Ltd.).
[0056] <Slurry preparation and substrate fabrication> <Formulation 1> A mixture was prepared by adding 120 parts by mass of gypsum 1 (CS1) to 100 parts by mass of calcium aluminate 1 (CA1), and 120 parts by mass of water, 10 parts by mass of inorganic fiber, and 2 parts by mass of polystyrene beads were added to 100 parts by mass of the above mixture, and the mixture was stirred for 5 minutes to prepare a slurry. The prepared slurry was directly poured into a mold to prepare a substrate. <Formulation 2> A mixture was prepared by adding 120 parts by mass of gypsum 1 (CS1) and 80 parts by mass of inorganic hollow aggregate to 100 parts by mass of calcium aluminate 1 (CA1), and 100 parts by mass of water was added to the above mixture and stirred for 5 minutes to prepare a slurry. The prepared slurry was directly poured into a formwork to prepare a base material. <Formulation 3> 100 parts by mass of calcium aluminate 2 (CA2) was mixed with 120 parts by mass of water and 10 parts by mass of sepiolite, and the mixture was stirred for 5 minutes to prepare a slurry. The prepared slurry was directly poured into a mold to prepare a substrate. <Formulation 4> 100 parts by mass of gypsum 2 (CS2) was mixed with 100 parts by mass of water and stirred for 5 minutes to prepare a slurry. The prepared slurry was directly poured into a mold to prepare a substrate. <Formulation 5> A mixture was prepared by adding 120 parts by mass of gypsum 1 (CS1) to 100 parts by mass of calcium aluminate 1 (CA1), and 120 parts by mass of water was added to 100 parts by mass of the above mixture, and the mixture was stirred for 5 minutes to prepare a slurry. The prepared slurry was directly poured into a mold to prepare a substrate. <Formulation 6> A substrate prepared in the same manner as in Formulation 2 was cured in a drying oven at 200° C. for 2 hours to obtain a substrate.
[0057] <Water content (crystalline water / free water)> A 20 g sample was taken from the fireproof material, and the free water and the resin composition layer were dissolved in acetone. After filtration, the residue was thoroughly washed with acetone and vacuum dried in a desiccator for 48 hours in an environment of 25°C. The amount of crystallization water was calculated by measuring the mass loss in the range of 50 to 200°C using a thermal analyzer (heating rate: 10°C / min, in air) for the dried cured product. The crystallization water referred to here refers to chemically or physically bound water contained in the fireproof material, excluding free water that can be removed by drying with acetone or the like. In addition, 20 g of the fireproof material was sampled so as not to include the resin composition layer, and was dried by heating in a drying oven at 40° C. for 72 hours. The amount of mass loss before and after drying was measured to calculate the amount of free water.
[0058] <Fire resistance> Using a small gas burner and a thermocouple, a test piece measuring 10cm long x 10cm wide x 5cm thick was used, the distance of the gas burner was adjusted so that the surface temperature of the test piece was 900°C, the temperature of the back side was measured with a thermocouple, and the time it took to reach 200°C was measured. In other words, the longer it takes to reach 200°C, the better the fire resistance.
[0059] <Shape retention> If the test specimen had no cracks, breaks, collapse or defects after the fire resistance test, it was rated as "Good", and if any cracks, breaks, collapse or defects were found, it was rated as "NG".
[0060] <Shape retention rate> The test specimen was placed in an electric furnace and heated to 900°C. The volume of the test specimen after one hour was measured and compared with the volume of the test specimen before heating to calculate the shape retention rate.
[0061] <Thermal conductivity> The thermal conductivity of the specimens obtained from the fireproof materials, measuring 10 cm in length, 5 cm in width and 5 cm in thickness, was measured using a rapid thermal conductivity meter (box probe method).
[0062] [Table 1]
[0063] It has been confirmed that the fire-resistant material of the present invention has a resin composition layer with a moisture permeability coefficient of 1,000 ng / m·s·Pa or less and contains water of crystallization, thereby exhibiting excellent fire resistance and shape retention.
[0064] [Experimental Example 2] The fireproof materials manufactured in the same manner as in Experimental Example 1 were dried under the drying conditions described in "4.1.1 Fireproof Performance Test" in the "Fireproof Performance Testing and Evaluation Procedure Manual" (Construction Materials Testing Center, 2021) until the mass change rate per day was less than 0.5%, and tests for fire resistance, shape retention, shape retention rate, and thermal conductivity were performed in the same manner as in Experimental Example 1. The results are shown in Table 2 below.
[0065] [Table 2]
[0066] It was confirmed that the fireproof material of the present invention can maintain its fire resistance and shape retention even when dried. In other words, it was confirmed that the fireproof material of the present invention can exhibit excellent fire resistance and shape retention even when used after being stored for a certain period of time.
[0067] [Experimental Example 3] <Manufacture of fireproof insulation boards> Fireproof insulation boards were manufactured using three sheets of each of the fireproof materials manufactured in the same manner as in Experimental Example 1, and each test was carried out in the same manner as in Experimental Example 1. The results are shown in Table 3 below.
[0068] [Table 3]
[0069] It was confirmed that the fireproof insulation board using the fireproof material of the present invention has excellent fire resistance and shape retention. Note that the fireproof insulation board of the comparative example had significant cracking at the joints between the fireproof materials, whereas the fireproof insulation board of the example did not have any cracking even at the joints and maintained its shape.
[0070] [Experimental Example 4] <Manufacture of fireproof structure> As shown in Figures 1 and 2, a fireproof material structure (1) was produced using fireproof insulation boards (2) and (3) produced in the same manner as in Experimental Example 3. In Figure 2, the fireproof insulation boards (2) and (3) are laminates of a resin composition layer and a substrate. The size of the fireproof material structure (1) was 1,200 mm long x 2,200 mm wide. The material and thickness of the fireproof insulation boards (2) and (3) were changed in the test, and the burning state of the fireproof material structure (1) after the test was confirmed. When the thickness was changed, the number of sheets installed was changed. The results are shown in Table 4 below.
[0071] <Fire resistance test method> The fireproof structure (1) was placed in a fireproof furnace, and heating was performed on the side of the ceramic siding board (4) simulating the exterior wall, and the fireproof structure (1) was heated for one hour using a gas burner (total of five) and a standard heating curve conforming to ISO 834. After that, the heating was stopped and the structure was kept in the fireproof furnace for three hours. The fireproof structure (1) was removed from the fireproof furnace, and the fireproof insulation board (3) placed on the outside of the furnace was peeled off to check the burning state of the pillars. The results are shown in Table 4 below.
[0072] (Materials used) Ceramic siding board: Moen siding, made by Nichia, 16mm thick. Breathable waterproof sheet: Super Airtex KD, manufactured by Fukubi Chemical Co., Ltd. Structural plywood: polyethylene type, JAS standard product, special class, thickness 9mm. Posts (studs): Wood (cedar), length 15mm. Furring strip: wood (cedar), length 105mm.
[0073] [Table 4] [Industrial Applicability]
[0074] The material of the present invention, when made into a fireproof material, for example, has excellent fire resistance and shape retention, and can maintain these properties, so that it can be suitably used in buildings, vehicles, aircraft, ships, refrigeration and freezing equipment, etc. [Explanation of symbols]
[0075] (1) Fireproof material structure (2) and (3) Fireproof insulation board (4) Ceramic siding board (5) Fuselage (6) Breathable waterproof sheet (7) Structural plywood (8) Pillars (studs)
Claims
1. A material including a substrate containing a hardened hydraulic compound, The substrate has a resin composition layer having a moisture permeability coefficient of 1,000 ng / m s Pa or less, The material, wherein the substrate contains water of crystallization.
2. The water content derived from the water of crystallization is 40 kg / m 3 The material according to claim 1 .
3. The substrate further contains free water, and the water content derived from the free water is 10 kg / m 3 The material according to claim 1 or 2.
4. The material according to claim 1 or 2, wherein the set hydraulic compound comprises ettringite and / or gypsum.
5. The material according to claim 4, wherein the content of ettringite is 20 to 95% by mass.
6. The material according to claim 4, wherein the gypsum content is 20 to 95% by weight.
7. 3. A fire-resistant material comprising the material according to claim 1 or 2.
8. Density: 200-800 kg / m 3 The fireproof material according to claim 7,
9. A fire-resistant insulation board comprising the fire-resistant material of claim 8.
10. A structure comprising a substrate containing a cured product of a hydraulic compound provided on at least a surface of a building that requires fire resistance, the substrate having a resin composition layer having a moisture permeability coefficient of 1,000 ng / m s Pa or less on an opposite side to the building, The structure, wherein the substrate contains water of crystallization.
11. 11. The structure of claim 10 which is a fireproof structure.
Citation Information
Patent Citations
Fire-resistant coating material
JP1995048153A
Composition for fire-resistant coating
JP1995061841A
Heat insulating material, its production and execution using the same
JP1998067576A
Heat-insulating coating granule
JP2001329629A
Fireproof structure of wooden building
JP2007039915A