Stretched porous film, wound body, disposable body warmer, and method for manufacturing stretched porous film
A stretched porous film with controlled composition and stretching achieves uniform air permeability and ventilation, addressing uneven ventilation issues in breathable films.
Patent Information
- Application Number
- JP2023054036
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing breathable films lack control over air permeability and uniformity of ventilation, leading to uneven ventilation.
A stretched porous film composed of polyester, inorganic filler, and petroleum wax, with specific ranges for petroleum wax content, inorganic filler particle size, and stretching ratios, to achieve uniform air permeability and ventilation.
The film exhibits appropriate air permeability and excellent uniformity of ventilation, enhancing thermal control in applications like body warmers.
Smart Images

Figure 2024142061000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretched porous film, a roll, a disposable warmer, and a method for producing a stretched porous film. [Background technology]
[0002] Conventionally, a porous film is known in which a resin composition containing a polyolefin and an inorganic filler is stretched to cause interfacial peeling between the polyolefin and the inorganic filler, forming a large number of voids (micropores). In particular, a stretched porous film made of a resin composition containing a polyolefin and an inorganic filler is used as a breathable film that has high air permeability but suppresses the permeation of liquids and powders because the internal micropores form continuous pores. Such breathable films are used, for example, in the manufacture of disposable warmers.
[0003] For example, Patent Document 1 discloses a porous packaging material characterized by bonding an olefin-based porous film and a breathable substrate via a porous adhesive layer formed by fiberizing an adhesive substance. In this document, it is considered to provide a storage bag for a breathable exothermic composition by bonding an olefin-based porous film and a breathable substrate via a porous adhesive layer formed by fiberizing an adhesive substance to form a porous packaging material, and forming a bag using the porous packaging material.
[0004] Patent Document 2 discloses a disposable warmer including a plurality of heat generating parts containing heat generating powder that generates heat in the presence of air, and a laminated structure in which the plurality of heat generating parts are arranged at intervals inside while ensuring breathability for the plurality of heat generating parts, and in which at least one connecting part is provided inside the laminated structure to connect at least two of the plurality of heat generating parts so that air can flow between them. Here, it is disclosed that the laminated structure includes a breathable sheet, and that the breathable sheet is made of a woven or nonwoven fabric such as polyester, cellulose, cotton, hemp, silk, or wool, instead of a nylon nonwoven fabric. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-131472 [Patent Document 2] JP 2014-68702 A Summary of the Invention [Problem to be solved by the invention]
[0006] As mentioned above, breathable films using various resins and the like have been disclosed, but in Patent Document 1, breathability is improved by forming a porous adhesive layer by fibrillating and increasing the volume of an adhesive substance, and in Patent Document 2, temperature unevenness between cells is suppressed by providing at least one connecting part in a pocket warmer that connects heat generating parts so that air can flow between them. However, the prior art has not considered controlling the air permeability of the resin film itself or suppressing uneven ventilation.
[0007] Therefore, in order to solve such problems of the conventional technology, the present inventors have carried out studies with the aim of providing a stretched porous film having appropriate air permeability and excellent air permeability uniformity. [Means for solving the problem]
[0008] Examples of specific embodiments of the present invention are given below.
[0009] [1] Contains polyester, inorganic fillers and petroleum waxes; A stretched porous film having a petroleum wax content of 20 to 30,000 ppm. [2] The stretched porous film according to [1], having an air permeability of 5,000 to 50,000 sec / 100 ml or more based on a film thickness of 60 μm. [3] The stretched porous film according to [1] or [2], wherein the petroleum wax is paraffin wax. [4] The stretched porous film according to [3], wherein the paraffin wax is normal paraffin. [5] The stretched porous film according to any one of [1] to [4], wherein the inorganic filler has an average particle size of 0.1 to 10 μm. [6] The stretched porous film according to any one of [1] to [5], wherein the inorganic filler is calcium carbonate. [7] The stretched porous film according to any one of [1] to [6], wherein the polyester is polybutylene adipate terephthalate. [8] The stretched porous film according to any one of [1] to [7], which has a thickness of 10 to 150 μm. [9] A roll obtained by rolling up the stretched porous film according to any one of [1] to [8].
[10] A disposable hand warmer having a stretched porous film described in any one of [1] to [8].
[11] A step of mixing a polyester and an inorganic filler coated with a petroleum wax to obtain a resin composition; A step of forming the resin composition into a sheet to obtain a sheet; and stretching the sheet.
[12] The method for producing a stretched porous film according to
[11] , wherein the content of the petroleum wax relative to the total mass of the inorganic filler coated with the petroleum wax is 0.01 mass% or more. Effect of the Invention
[0010] According to the present invention, it is possible to obtain a stretched porous film having an appropriate air permeability and excellent air permeability uniformity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment or a specific example, but the present invention is not limited to such an embodiment. In this specification, when "X to Y" (X and Y are any numbers) is used, it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also means "preferably greater than X" or "preferably less than Y". In the following description, "film" and "sheet" are not clearly distinguished from each other, and when "film" is used, it includes "sheet", and when "sheet" is used, it includes "film".
[0012] In this specification, the MD direction of the film is the extrusion direction (or take-up direction or flow direction) during film formation and is also called the machine direction, while the TD direction is the direction perpendicular to the MD direction and is also called the transverse direction or width direction.
[0013] (Stretched porous film) The present embodiment relates to a stretched porous film (hereinafter also referred to as the present stretched porous film) containing polyester, an inorganic filler, and a petroleum wax, and the content of the petroleum wax is 20 to 30,000 ppm. The stretched porous film of the present embodiment has a large number of voids (micropores), and these voids are connected in the thickness direction, so that the film can exhibit appropriate air permeability.
[0014] The pore size of the voids (micropores) is preferably 0.05 to 0.5 μm. If the pore size of the voids (micropores) is within the above range, the film can be made liquid-impermeable (waterproof) while allowing water vapor and air to pass through. The pore size can be evaluated as the maximum pore size measured by the bubble point method (JIS K3832:1990 or ASTM F316), and more specifically, the pore size can be measured using a perm porometer.
[0015] The stretched porous film is a uniaxially stretched film. Since the stretched porous film contains an inorganic filler, the resin composition is stretched in the production process to cause interfacial peeling between the polyester and the inorganic filler, thereby forming a film having a large number of voids (micropores) having the above-mentioned pore size.
[0016] In this embodiment, the inorganic filler is preferably coated with petroleum wax, and such an inorganic filler is mixed with polyester and formed into a sheet, so that the film contains 20 to 30,000 ppm of petroleum wax. The petroleum wax may be present on the surface of the inorganic filler (fine particles) or may be present in a state of being detached from the inorganic filler. Since the particle size distribution of the inorganic filler is wide, the size of the voids generated during stretching also varies, and it is presumed that this causes variation in air permeability. In this embodiment, by using an inorganic filler coated with petroleum wax in the manufacturing process of this stretched porous film, the affinity between the polyester having a polar ester bond and the inorganic filler can be appropriately reduced, and as a result, the inorganic filler is loosely aggregated, the particle size distribution becomes narrow, and the variation in the size of the voids generated during stretching is reduced, and it is presumed that the variation coefficient of air permeability is reduced.
[0017] The air permeability of the stretched porous film of this embodiment calculated as a thickness of 60 μm is preferably 5000 sec / 100 ml or more, more preferably 6000 sec / 100 ml or more, even more preferably 7000 sec / 100 ml or more, even more preferably 8000 sec / 100 ml or more, even more preferably 9000 sec / 100 ml or more, and particularly preferably 10000 sec / 100 ml or more. The air permeability of the stretched porous film calculated as a thickness of 60 μm is preferably 50000 sec / 100 ml or less, more preferably 48000 sec / 100 ml or less, and even more preferably 45000 sec / 100 ml or less. By setting the air permeability of the stretched porous film within the above range, for example, when the stretched porous film is used as a component sheet of a heat-retaining product such as a pocket warmer or a cold-weather product, the heat permeability can be appropriately controlled.
[0018] The air permeability of the stretched porous film can be measured using an air permeability measuring device (Oken type air permeability measuring device EGO1-55 type, manufactured by Asahi Seiko Co., Ltd.) in accordance with JIS P8117: 2009. In this embodiment, the air permeability converted into a film thickness of 60 μm can be calculated using the following formula. Air permeability per 60 μm = Air permeability (measured value) × 60 (μm) / sample thickness (μm)
[0019] In this embodiment, the coefficient of variation of air permeability is suppressed to a small value. Here, the coefficient of variation of air permeability is a value calculated by calculating the standard deviation of the air permeability obtained by the above measurement as a whole population and dividing the obtained standard deviation by the average value of the air permeability. Specifically, the coefficient of variation of air permeability is preferably 0.060 or less, more preferably 0.055 or less, even more preferably 0.050 or less, even more preferably 0.045 or less, and particularly preferably 0.040 or less. The lower limit of the coefficient of variation of air permeability is not particularly limited, and may be 0.000. If the coefficient of variation of air permeability is within the above range, it is possible to suppress the occurrence of uneven ventilation, and for example, when the present stretched porous film is used as a constituent sheet of a warming product such as a pocket warmer or a cold protection product, the thermal permeability can be made uniform.
[0020] The tear strength in the MD direction of the stretched porous film of this embodiment is preferably 0.5 N / mm or more, more preferably 0.6 N / mm or more, even more preferably 0.7 N / mm or more, even more preferably 0.8 N / mm or more, and particularly preferably 0.9 N / mm or more. The upper limit of the tear strength in the MD direction of the stretched porous film is not particularly limited, but is preferably, for example, 5 N / mm or less. In this embodiment, the tear strength in the MD direction of the stretched porous film is particularly increased. Usually, when a uniaxially stretched film is produced, stretching is performed in the MD direction (longitudinal direction), so that the tear strength in the MD direction tends to decrease. However, in this embodiment, polyester is used as the resin constituting the stretched porous film, and further, polyester and an inorganic filler coated with petroleum wax are mixed, so that the tear strength in the MD direction, where the tear strength tends to decrease significantly, can be effectively increased.
[0021] In addition, the tear strength in the TD direction of the stretched porous film of this embodiment is preferably 5.0 N / mm or more, more preferably 7.0 N / mm or more, and even more preferably 9.0 N / mm or more. The upper limit of the tear strength in the TD direction of the stretched porous film is not particularly limited, but is preferably, for example, 30 N / mm or less. In this embodiment, polyester and an inorganic filler coated with petroleum wax are mixed, so that the tear strength in the TD direction (transverse direction) is also increased. By increasing the tear strength of the stretched porous film, breakage during film formation or printing can be suppressed, and the strength of the stretched porous film when used as a component of a disposable warmer or the like is sufficient. The tear strength of this stretched porous film is measured in accordance with JIS K7128-1:1998 by cutting a sample to a length of 100 mm and a width of 25 mm in the measurement direction, making a 25 mm cut in the center of the width, and using a tensile tester at 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 25 mm.
[0022] The stretched porous film has a breaking elongation in the TD direction of preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, even more preferably 90% or more, and particularly preferably 100% or more. The stretched porous film has a breaking elongation in the TD direction of preferably 800% or less.
[0023] The MD breaking elongation of the stretched porous film is preferably 30% or more, more preferably 33% or more, and even more preferably 35% or more. The MD breaking elongation of the stretched porous film is preferably 200% or less. The breaking elongation of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measuring direction, and using a tensile tester under the conditions of 23°C, 50% relative humidity, a pulling speed of 200 m / min, and a chuck distance of 20 mm.
[0024] In this embodiment, it is preferable that the breaking elongation in the TD direction is greater than that in the MD direction. In a typical stretched porous film using a polyolefin resin or a polylactic acid resin, the breaking elongation in the MD direction is usually greater than that in the TD direction, but in this embodiment, it is preferable that the breaking elongation in the TD direction is increased and that the breaking elongation in the TD direction is greater than that in the MD direction.
[0025] Here, when the breaking elongation in the TD direction is P and the breaking elongation in the MD direction is Q, the value of P / Q is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, and particularly preferably 1.9 or more. The value of P / Q is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less. By setting the value of P / Q within the above range, the air permeability of the stretched porous film can be more effectively increased.
[0026] The tensile strength in the MD direction of the present stretched porous film is preferably 10.0 MPa or more, more preferably 12.0 MPa or more, and even more preferably 14.0 MPa or more. The tensile strength in the MD direction of the present stretched porous film is preferably 50 MPa or less, more preferably 48 MPa or less, and even more preferably 45 MPa or less.
[0027] The tensile strength of the stretched porous film in the TD direction is preferably 1.0 MPa or more, more preferably 1.2 MPa or more, and even more preferably 1.4 MPa or more. The tensile strength of the stretched porous film in the TD direction is preferably 10 MPa or less, more preferably 8 MPa or less, and even more preferably 7 MPa or less. The tensile strength of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measurement direction, and using a tensile tester under the conditions of 23°C, relative humidity of 50%, a pulling speed of 200 m / min, and a chuck distance of 20 mm.
[0028] The thickness of the present stretched porous film is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the present stretched porous film is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less. By making the thickness of the present stretched porous film within the above range, it is possible to make the film thinner while maintaining a balance between air permeability and mechanical strength.
[0029] The present embodiment may relate to a rolled body obtained by rolling up a stretched porous film. Since the stretched porous film has appropriate strength and flexibility, it can be stored or distributed in the form of a roll.
[0030] (polyester) The stretched porous film contains polyester. Examples of polyester include polyethylene terephthalate, polyethylene terephthalate copolymer, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene adipate terephthalate, polybutylene adipate, polyethylene adipate, polybutylene adipate terephthalate, polyethylene adipate terephthalate, polyethylene succinate, polybutylene succinate, polybutylene succinate carbonate, polybutylene succinate terephthalate, polypropylene succinate, polybutylene succinate adipate, polybutylene succinate terephthalate, polybutylene succinate adipate terephthalate, polybutylene succinate lactate, polybutylene succinate hydroxycaproate, and polybutylene succinate carbonate. polyhydroxyalkanoates such as polyhydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), polyhydroxybutyrate valerate, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyacyl), and polyhydroxyacyl; polylactic acid, polyglycolic acid, lactic acid-glycolic acid copolymer, polycaprolactone, polycaprolactone butylene succinate, polybutylene adipate caprolactone, polypropiolactone, salts and derivatives thereof, and polyester elastomers. Among them, the polyester is preferably at least one selected from the group consisting of polyethylene succinate, polybutylene succinate, polypropylene succinate, polybutylene succinate adipate, and polybutylene adipate terephthalate, and the polyester is particularly preferably polybutylene adipate terephthalate (PBAT).
[0031] Polybutylene adipate terephthalate is a biodegradable resin, and is preferably a thermoplastic resin. When the stretched porous film contains polybutylene adipate terephthalate as a constituent resin, the stretched porous film has excellent biodegradability. In this specification, biodegradability refers to the property of a film being decomposed by the action of organisms such as microorganisms.
[0032] Polybutylene adipate terephthalate is a copolymer of adipic acid, terephthalic acid, and butanediol. Adipic acid, terephthalic acid, and butanediol may be copolymerized simultaneously or in multiple stages.
[0033] When synthesizing polybutylene adipate terephthalate, in addition to adipic acid, terephthalic acid, and butanediol, a small amount of other copolymerization components may be added. Examples of other copolymerization components include dicarboxylic acids other than terephthalic acid and adipic acid, and modifiers for the purpose of chain extension, terminal blocking, etc. These may be used alone or in combination of two or more. Examples of other dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, etc. These may be used alone or in combination of two or more. Examples of modifiers include polyisocyanate compounds, glycol compounds, etc. Examples of the polyisocyanate compound include diisocyanate compounds, and examples of the diisocyanate compound include hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, 1,5-naphthylene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, carbodiimide-modified MDI, and polymethylene phenyl polyisocyanate. Examples of the glycol compound include diols other than butanediol and polyalkylene glycols. Examples of the other diols include methanediol, ethanediol, propanediol, pentanediol, and hexanediol. Examples of polyalkylene glycols include polymethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol (polytetramethylene glycol), etc. These may be used alone or in combination of two or more kinds.
[0034] In 100 mol % of the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate, the constituent units derived from terephthalic acid are preferably contained at 40 to 60 mol %, and the constituent units derived from adipic acid are preferably contained at 40 to 60 mol %. By setting the ratio of the constituent units derived from terephthalic acid and the constituent units derived from adipic acid among the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate within the above range, a film having a good balance of mechanical strength, biodegradability, and flexibility can be easily obtained.
[0035] The melting point of polybutylene adipate terephthalate is preferably 105°C or higher, more preferably 108°C or higher, and even more preferably 110°C or higher. The melting point of polybutylene adipate terephthalate is preferably 130°C or lower, more preferably 128°C or lower, and even more preferably 125°C or lower. The melting point of polybutylene adipate terephthalate is measured by DSC or the like in accordance with JIS K 7121 (2012). By setting the melting point of polybutylene adipate terephthalate within the above range, a film having a good balance between heat resistance and moldability can be easily obtained.
[0036] Examples of polybutylene adipate terephthalate include biodegradable synthetic polymer compounds listed in the positive list of the Japan Bioplastics Association's GreenPla (biodegradable plastic) classification number A-1. Commercially available products include, for example, F Blend C1200 manufactured by BASF and ECO-A05 manufactured by Taiwan Chang Chun Co., Ltd.
[0037] The weight average molecular weight (Mw) of the polyester is preferably 50,000 or more, more preferably 70,000 or more, and even more preferably 100,000 or more. The weight average molecular weight (Mw) of the polyester is preferably 400,000 or less, more preferably 350,000 or less, and even more preferably 300,000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) or the like. By setting the weight average molecular weight (Mw) of the polyester within the above range, a film having a good balance between extrusion moldability and mechanical strength can be easily obtained.
[0038] The molecular weight distribution (Mw / Mn) of the polyester is preferably 1.5 or more, more preferably 1.7 or more, and even more preferably 1.9 or more. The molecular weight distribution (Mw / Mn) of the polyester is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.0 or less. By setting the molecular weight distribution (Mw / Mn) of the polyester within the above range, a film having a good balance of film formability, film rigidity, and impact resistance can be easily obtained.
[0039] The content of polyester in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of polyester is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of polyester in the stretched porous film within the above range, it becomes easier to control the air permeability of the stretched porous film to an appropriate range, and the uniformity of ventilation can be more effectively improved.
[0040] (inorganic filler / petroleum wax) The stretched porous film contains an inorganic filler. Examples of inorganic fillers include various carbonates such as calcium carbonate, magnesium carbonate, and barium carbonate, various sulfates such as magnesium sulfate, barium sulfate, and calcium sulfate, various oxides such as zinc oxide, silicon oxide (silica), zirconium oxide, magnesium oxide, calcium oxide, titanium oxide, magnesium oxide, iron oxide, and alumina, and other hydroxides such as aluminum hydroxide, silicate minerals, various composite oxides such as hydroxyapatite, mica, talc, kaolin, clay, montmorillonite, and zeolite, various phosphates such as lithium phosphate, calcium phosphate, and magnesium phosphate, and various salts such as lithium chloride and lithium fluoride. Among these, from the viewpoint of air permeability, strength, and the like, the inorganic filler is preferably at least one selected from the group consisting of calcium carbonate, barium carbonate, barium sulfate, silicon oxide (silica), and titanium oxide, more preferably at least one selected from the group consisting of calcium carbonate and barium sulfate, and particularly preferably calcium carbonate.
[0041] The average particle size of the inorganic filler is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. The average particle size of the inorganic filler is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. By setting the average particle size of the inorganic filler to the above lower limit or more, poor dispersion and secondary aggregation of the inorganic filler are suppressed, and it is preferable that the inorganic filler can be uniformly dispersed in the resin composition constituting the stretched porous film. If the average particle size is the above upper limit or less, it is possible to suppress the generation of large voids when the film is thinned, and the film can have sufficient strength and water resistance.
[0042] The average particle size of the inorganic filler is calculated from the specific surface area measured by the constant pressure transmission method using a Shimadzu powder specific surface area measuring instrument SS-100. The measurement conditions are as follows: sample weight 3.0 g, sample thickness 1.35 cm, cross-sectional area of the sample layer 2 cm 2, air pressure is 50cmH2O, and the viscosity coefficient of air is 181×10 -6 Calculate the average particle size as g / (cm sec).
[0043] The inorganic filler is preferably surface-treated, and is preferably coated with petroleum wax. Petroleum wax is a hydrocarbon that is solid at room temperature and exists in petroleum, and is composed of linear, branched, or cyclic aliphatic saturated hydrocarbons. Examples of petroleum wax include paraffin wax, microcrystalline wax, and petrolatum. These waxes can be used alone or in combination of two or more. Among them, the petroleum wax is preferably paraffin wax, and the paraffin wax is particularly preferably normal paraffin, which is a linear saturated hydrocarbon. In addition to normal paraffin, the petroleum wax may contain other petroleum waxes.
[0044] The average carbon number of normal paraffins is preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more. The average carbon number of normal paraffins is preferably 50 or less, and even more preferably 40 or less.
[0045] The molecular weight of the normal paraffin is preferably 100 or more, more preferably 150 or more, and even more preferably 200 or more. The molecular weight of the normal paraffin is preferably 1000 or less, more preferably 900 or less, and even more preferably 800 or less.
[0046] In this way, the inorganic filler coated with the petroleum wax is mixed with polyester and formed into a sheet, so that the film contains 20 to 30,000 ppm of petroleum wax. The petroleum wax may be present on the surface of the inorganic filler (fine particles) or may be present in a state of being detached from the inorganic filler.
[0047] The petroleum wax coats the surface of the inorganic filler, and therefore may also be called a surface treatment agent or a coating agent. That is, the stretched porous film of the present embodiment preferably contains 20 to 30,000 ppm of the inorganic filler surface treatment agent or a compound derived from the surface treatment agent.
[0048] The content of the petroleum wax is preferably 20 ppm or more, more preferably 30 ppm or more, even more preferably 40 ppm or more, and particularly preferably 50 ppm or more, based on the total mass of the stretched porous film. The content of the petroleum wax is preferably 30000 ppm or less, more preferably 25000 ppm or less, even more preferably 20000 ppm or less, even more preferably 15000 ppm or less, and particularly preferably 10000 ppm or less, based on the total mass of the stretched porous film. By setting the content of the petroleum wax in the stretched porous film within the above range, the inorganic filler is appropriately aggregated, and as a result, the air permeability of the stretched porous film can be easily controlled within an appropriate range, and the uniformity of the air permeability can be more effectively improved.
[0049] The content of the petroleum wax (the proportion of the petroleum wax in the inorganic filler) is preferably 0.01% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.02% by mass or more, based on the total mass of the inorganic filler coated with the petroleum wax. The content of the petroleum wax is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the inorganic filler coated with the petroleum wax. By setting the content of the petroleum wax in the inorganic filler within the above range, the inorganic filler is appropriately aggregated, which makes it easier to control the air permeability of the stretched porous film within an appropriate range, and furthermore effectively improves the uniformity of ventilation.
[0050] The content of the inorganic filler in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of the inorganic filler is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of the inorganic filler in the stretched porous film within the above range, it becomes easier to control the air permeability of the stretched porous film to an appropriate range, and the uniformity of ventilation can be more effectively improved.
[0051] The inorganic filler may be one of the above inorganic fillers, or may be a mixture of two or more different fillers having different materials, average particle sizes, types of surface treatment agents, etc. When the inorganic filler is composed of two or more types, the total amount is preferably within the above range.
[0052] (Other resins) The present stretched porous film may contain other resins in addition to polyester. Examples of the other resins include polyolefin resins, polystyrene resins, acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, ethylene-vinyl alcohol copolymers, ethylene-vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyarylate resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, fluorine-based resins, and polyacetal resins. As the other resin, for example, biodegradable resins such as polyvinyl alcohol, polyamide, polyethylene glycol, etc. These other resins may be used alone or in combination of two or more.
[0053] When the present stretched porous film contains other resins in addition to polyester, the content of the other resins is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less, based on the total mass of the stretched porous film.
[0054] (optional ingredient) The stretched porous film may contain various additives as optional components. Examples of additives include plasticizers, lubricants, compatibilizers, processing aids, antioxidants, heat stabilizers, light stabilizers, UV absorbers, antiblocking agents, antifogging agents, matting agents, antibacterial agents, deodorants, antistatic agents, flame retardants, colorants, and pigments. Examples of plasticizers that can be used include low molecular weight polymers (oligomers) such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, metal soaps, higher alcohols, petrolatum, paraffin wax, glycerin fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, castor oil, hydrogenated castor oil, hardened castor oil, dehydrated castor oil, aromatic esters, aromatic amides, polyesters, and the like. The content of additives is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the stretched porous film. In this embodiment, the amount of plasticizer added may be 1% by mass or less, 0.1% by mass or less, or substantially no plasticizer may be included. In particular, when polybutylene adipate terephthalate is used as the polyester, the stretched porous film can exhibit high flexibility even without the inclusion of a plasticizer.
[0055] (Method of manufacturing the stretched porous film) The method for producing the stretched porous film preferably includes, for example, a step of mixing a polyester with an inorganic filler coated with a petroleum wax to obtain a resin composition, a step of forming the resin composition into a sheet to obtain a sheet, and a step of stretching the sheet. The step of stretching the sheet preferably includes a step of stretching the sheet in at least one axial direction.
[0056] The stretched porous film may be either planar or tubular, but is preferably planar from the viewpoints of productivity (several pieces can be produced in the width direction of the raw sheet) and printing on the inner surface. The method for producing a planar film preferably includes, for example, a step of melting a resin composition using an extruder, extruding the resin composition into a film shape from a die, and cooling and solidifying the film with a cooling roll, air cooling, or water cooling to obtain an unstretched film, and a step of stretching the unstretched film in at least one axial direction to obtain a stretched porous film.
[0057] The step of obtaining the resin composition preferably includes a step of mixing the polyester and the inorganic filler coated with the petroleum wax, followed by melt-kneading. Specifically, it is preferable to mix the mixture for an appropriate time using a mixer such as a tumbler mixer, a mixing roll, a Banbury mixer, a ribbon blender, or a super mixer, and then uniformly disperse the resin composition using an extruder such as a counter-rotating twin-screw extruder or a co-rotating twin-screw extruder.
[0058] The content of the petroleum wax (the proportion of the petroleum wax in the inorganic filler) is preferably 0.01% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.02% by mass or more, based on the total mass of the inorganic filler coated with the petroleum wax. The content of the petroleum wax is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the inorganic filler coated with the petroleum wax. By setting the content of the petroleum wax within the above range in the inorganic filler mixed in the step of obtaining the resin composition, the inorganic filler is appropriately aggregated, and as a result, the air permeability of the stretched porous film can be easily controlled within an appropriate range, and the uniformity of the air permeability can be more effectively improved.
[0059] In the process of obtaining a sheet (unstretched sheet), it is preferable to connect a die such as a T-die or a round die to the tip of an extruder and form the obtained resin composition into a film. Alternatively, a strand die may be connected to the tip of a kneader, and the resin composition may be pelletized by a method such as strand cutting or die cutting. The pellets obtained (along with an additional composition in some cases) may then be introduced into a single-screw extruder or the like, and a die such as a T-die or a round die may be connected to the tip of the extruder to form the resin into a film. When forming the resin into a film, it is preferable to employ a film forming method such as inflation molding, tubular molding, or T-die molding.
[0060] In the process of stretching the sheet, the unstretched film is stretched at least uniaxially. For example, the resin is melted using an extruder, extruded from a T-die or a round die, cooled and solidified with a cooling roll, and stretched at least uniaxially by roll stretching in the MD direction (longitudinal direction) or tenter stretching in the transverse direction (perpendicular to the flow direction of the film, TD). Among them, the process of obtaining a stretched porous film preferably includes a process of uniaxially stretching in the MD direction (longitudinal direction), and the stretched porous film is preferably a uniaxially stretched porous film. The process of uniaxially stretching in the MD direction (longitudinal direction) may include a process of stretching two or more times in the same direction. The stretching ratio is preferably 2.5 to 6.0 times, and more preferably 3.0 to 5.5 times. By setting the stretching ratio to be equal to or more than the lower limit above, a stretched porous film having appropriate air permeability and excellent appearance due to being uniformly stretched can be obtained. Moreover, by setting the stretching ratio to be equal to or less than the above upper limit, the breaking elongation of the film can be increased.
[0061] If necessary, a heat treatment or relaxation treatment may be performed after the stretching. When the stretching is performed by roll stretching, the stretched film can be brought into contact with a heated roll (anneal roll) between the stretching step and the winding step to perform a heat treatment. Alternatively, while heating with the anneal roll, the speed of the next roll to be contacted can be made slower than the anneal roll speed to perform a relaxation treatment. Note that these heat treatments and relaxation treatments can also be performed in a separate step after stretching the unstretched film and winding up the stretched porous film.
[0062] The method for producing the present stretched porous film may, if necessary, include a step of performing a surface treatment or surface processing such as slitting, corona treatment, printing, application of an adhesive, coating, deposition, etc. The present stretched porous film may, for example, be printed, or may be a film having a printed layer.
[0063] (Application) The present stretched porous film can be suitably used in a wide range of applications, particularly in disposable applications, such as packaging materials for liquids, powders, and solids, such as various foods, medicines, and daily consumables, agricultural materials, and building materials. Specific applications include, for example, agricultural mulch films, tunnel films, greenhouse films, sunshades, weed control sheets, ridge sheets, germination sheets, forestry fumigation sheets, binding tapes containing flat yarns, back sheets for diapers and sanitary products, packaging sheets, hand warmer sheets, shopping bags, plastic bags, garbage bags, draining bags, compost bags, etc. Among these, the present stretched porous film is preferably used for disposable hand warmers, since it has moderate air permeability.
[0064] The present embodiment may relate to a disposable warmer including the above-mentioned stretched porous film. EXAMPLES
[0065] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0066] <Thickness> The thickness of the film was measured using a stand-type constant pressure thickness measuring instrument in accordance with JIS K7130:1999, and the average of 36 measured values was calculated.
[0067] <Breaking elongation / tensile strength> In accordance with JIS K7127:1999, samples were cut to a length of 100 mm and a width of 10 mm in the measurement direction, and the breaking elongation and tensile strength were measured using a tensile tester under conditions of 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 20 mm, and the average of the measured values for three samples was calculated.
[0068] <Tear strength> In accordance with JIS K7128-1:1998, a sample was cut to a length of 100 mm and a width of 25 mm in the measurement direction, a 25 mm notch was made in the center of the width, and the tear strength was measured using a tensile tester under conditions of 23°C, relative humidity 50%, a tensile speed of 200 m / min, and a chuck distance of 25 mm, and the average of the measured values for three samples was calculated.
[0069] <Air permeability (60μm equivalent)> The air permeability was measured using an air permeability measuring device (Oken type air permeability measuring device EGO1-55 type, manufactured by Asahi Seiko Co., Ltd.) in accordance with JIS P8117: 2009. After calculating the average of the measured values of the five sheets, the air permeability per 60 μm was calculated using the following formula. Air permeability per 60 μm = Air permeability (measured value) × 60 (μm) / sample thickness (μm)
[0070] <Coefficient of variation of air permeability> The coefficient of variation of the air permeability was calculated by calculating the standard deviation of the air permeability obtained in the above measurement for the entire population and dividing the obtained standard deviation by the average value of the air permeability.
[0071] <Quantification of the Concentration of the Surface Treatment Agent in the Inorganic Filler> 5 mL of THF was added to 300 mg of the inorganic filler, and after stirring for 2 hours, centrifugation was performed. The extract obtained by drying the supernatant was dissolved in chloroform. Subsequently, qualitative analysis was performed using a gas chromatograph-mass spectrometer (GC / MS) under the following conditions. Thereafter, palmitic acid, stearic acid, and methyl stearate selected as standard substances were dissolved in chloroform and subjected to gas chromatographic analysis (GC measurement), and the peak areas of the extract of the inorganic filler were compared. <<GC / MS Measurement Conditions>> · Apparatus: GC / MS-QP2020 (manufactured by Shimadzu Corporation) · Column: UA1(MS / HT)-30M-0.1F · Carrier gas: Helium · Flow rate: 1 mL / min · Injection volume: 1 μL · Injection temperature: 320 °C · Column temperature: Held at 70 °C for 1 minute → Heated to 320 °C at 25 °C / min → Held at 320 °C for 5 minutes · Interface temperature: 320 °C · Ion source temperature: 250 °C · Ionization method: EI (70 eV) · Detection range: 35 - 800 m / z <<GC Measurement Conditions>> · Apparatus: GC-2010Plus (manufactured by Shimadzu Corporation) · Column: UA1(MS / HT)-30M-0.1F · Carrier gas: Helium · Flow rate: 1 mL / min · Injection volume: 1 μL · Injection temperature: 320 °C · Column temperature: Held at 70 °C for 1 minute → Heated to 320 °C at 25 °C / min → Held at 320 °C for 5 minutes · Detector: FID
[0072] <Quantitative determination of surface treatment agent concentration in film> For the obtained stretched porous film, 1.8 g of the sample was dissolved in chloroform, the resin was precipitated with methanol, and the filtrate was dried and the extract obtained was dissolved in chloroform. Then, a qualitative analysis was performed under the following conditions using a gas chromatograph mass spectrometer (GC / MS). Then, palmitic acid, stearic acid, and methyl stearate selected as standard substances were dissolved in chloroform and gas chromatographic analysis (GC measurement) was performed, and the peak areas of the inorganic filler extracts were compared.
[0073] <Polybutylene adipate terephthalate (A)> A-1: BASF "F Blend C1200" (density 1.270g / cm 3 , MFR 3.8g / 10min, melting point: 116°C, structural units derived from terephthalic acid in 100 mol% of structural units derived from dicarboxylic acid: 48.1 mol%, structural units derived from adipic acid: 51.9 mol%, weight average molecular weight: 150,000, Mw / Mn: 2.4)
[0074] <Inorganic filler (B)> B-1: Calcium carbonate "Suncut-160" manufactured by Kalfin Co., Ltd. (average particle size 1.5 μm, wax surface treatment product, normal paraffin concentration 0.7% by mass) B-2: Bihoku Powder Industry Co., Ltd., calcium carbonate "Lighton BS-0" (average particle size 1.0 μm, fatty acid surface treatment product) B-3: Calcium carbonate "CSK-5" manufactured by Kalfin Co., Ltd. (average particle size 1.5 μm, fatty acid surface treatment product) B-4: Calcium carbonate "Softon 1000" (average particle size 2.2 μm, surface untreated), manufactured by Bihoku Powder Industry Co., Ltd.
[0075] <Example 1> After weighing the raw materials in the composition ratio shown in Table 1, they were put into a Henschel mixer and mixed and dispersed for 5 minutes. Next, the materials were melt-kneaded at a set temperature of 200°C using a co-rotating twin-screw extruder. The resin composition was extruded through a T-die connected to the tip of the co-rotating twin-screw extruder, taken up by a casting roll set at 35°C, and cooled and solidified to obtain an unstretched film with a thickness of 62 μm. The unstretched film obtained was then stretched 3.5 times in the machine direction at a temperature of 63°C using a roll-type stretching machine to obtain a stretched porous film.
[0076] <Comparative Example 1> An unstretched film having a thickness of 59 μm was obtained in the same manner as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 3.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.
[0077] <Comparative Example 2> An unstretched film having a thickness of 55 μm was obtained in the same manner as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 3.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.
[0078] <Comparative Example 3> The raw materials were changed to have the composition ratio shown in Table 1, and an unstretched film having a thickness of 65 μm was obtained in the same manner as in Example 1.
[0079] [Table 1]
[0080] In the examples, appropriate air permeability was achieved compared to the comparative examples. In addition, the stretched porous films obtained in the examples had small variations in air permeability, and were excellent in air permeability uniformity.
Claims
1. Contains polyester, inorganic filler and petroleum wax, The content of the petroleum wax is 20 to 30,000 ppm.
2. 2. The stretched porous film according to claim 1, having an air permeability of 5,000 to 50,000 sec / 100 ml or more in terms of a film thickness of 60 μm.
3. 2. The stretched porous film of claim 1, wherein the petroleum wax is paraffin wax.
4. The stretched porous film according to claim 3 , wherein the paraffin wax is normal paraffin.
5. The stretched porous film according to claim 1, wherein the inorganic filler has an average particle size of 0.1 to 10 μm.
6. 2. The stretched porous film according to claim 1, wherein the inorganic filler is calcium carbonate.
7. 2. The stretched porous film of claim 1, wherein the polyester is polybutylene adipate terephthalate.
8. 2. The stretched porous film according to claim 1, having a thickness of 10 to 150 μm.
9. A roll obtained by rolling up the stretched porous film according to any one of claims 1 to 8.
10. A disposable warmer comprising the stretched porous film according to any one of claims 1 to 8.
11. A step of mixing a polyester with an inorganic filler coated with a petroleum wax to obtain a resin composition; forming the resin composition into a sheet to obtain a sheet; and stretching the sheet.
12. The method for producing a stretched porous film according to claim 11, wherein the content of the petroleum wax relative to the total mass of the inorganic filler coated with the petroleum wax is 0.01 mass% or more.
Citation Information
Patent Citations
Perforated packaging material and its housing bag
JP1996131472A
Disposable body warmer
JP2014068702A