Magnetic viscous fluid and damping device

A magnetorheological fluid with specific coercive force and redispersibility properties addresses the issue of characteristic changes in existing fluids, maintaining stable viscosity for prolonged use in vibration damping applications.

JP2024142259APending Publication Date: 2024-10-10SEIKO EPSON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054378
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Magnetorheological fluids in existing technologies experience a decrease in dispersoid redispersion and changes in characteristics when a magnetic field is applied and removed, hindering the realization of functions such as vibration damping and braking.

Method used

The magnetorheological fluid is formulated with magnetic metal particles having a coercive force of 796 A/m or less, a fluctuation rate of 10% or less in supernatant layer thickness after acceleration and magnetic field application, and a specific composition including additives and a dispersion medium to ensure stable viscosity changes.

Benefits of technology

The fluid maintains stable viscosity changes and performance over time, even with repeated application and removal of magnetic fields, ensuring high performance in vibration damping devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide magnetic viscous fluid that applies a magnetic field, allows satisfactory re-dispersion of a dispersoid even after removal of the magnetic field after the application, and shows stable characteristics, and a damping device that has such magnetic viscous fluid.SOLUTION: Magnetic viscous fluid has a dispersoid including magnetic metal particles and a liquid dispersion medium. The dispersoid has a coercive force of 796 A / m or less (10 Oe or less). When tA is the thickness of a supernatant layer generated when acceleration is applied to the magnetic viscous fluid so that the product of acceleration and time becomes 690 km / s in a state where the magnetic viscous fluid is stored in a cylindrical container, and tB is the thickness of a supernatant layer generated when a magnetic field is applied and subsequently the acceleration is applied to the magnetic viscous fluid in a state where the magnetic viscous fluid is stored in the cylindrical container, the regulation |tA-tB| / tA is 10% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetorheological fluid and a vibration damping device. [Background technology]

[0002] A magnetorheological fluid is, for example, a fluid in which magnetic metal particles are dispersed in a dispersion medium. When a magnetic field is applied to a magnetorheological fluid, the magnetic metal particles are magnetized and align in the direction of the magnetic field. This causes the formation of chain-like clusters, which changes the viscosity of the fluid. Therefore, the use of magnetorheological fluids in vibration control devices and braking devices, etc., is being considered, taking advantage of the change in viscosity.

[0003] In these devices, for example, the viscosity of the magnetorheological fluid is adjusted by repeatedly applying and removing a magnetic field, thereby achieving various functions such as vibration suppression and braking.

[0004] For example, Patent Document 1 discloses a magnetorheological fluid in which iron carbonyl particles and fumed silica particles are dispersed in a liquid containing poly-alpha-olefin. It also discloses that this magnetorheological fluid has the ability to reversibly change its fluidity under the influence of an applied magnetic field, and is therefore used in, for example, shock absorbers, vibration dampers (vibration dampers), torque transmission devices, and the like. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-032114 Summary of the Invention [Problem to be solved by the invention]

[0006] In the magnetorheological fluid described in Patent Document 1, when a magnetic field is applied and then removed, the redispersion of the magnetic particles, which are the dispersoid, may be reduced. In this case, the properties of the magnetorheological fluid change before and after the application of the magnetic field, which may hinder the realization of various functions such as vibration suppression and braking. [Means for solving the problem]

[0007] The magnetorheological fluid according to the application example of the present invention is A dispersoid containing magnetic metal particles; A liquid dispersion medium; having The coercive force of the dispersoid is 796 [A / m] or less (10 [Oe] or less), The thickness of the supernatant layer that is generated when the material is placed in a cylindrical container and accelerated so that the product of acceleration and time is 690 km / s is tA. When the magnetic field is applied to the sample contained in the cylindrical container and then the acceleration is applied, the thickness of the supernatant layer that is generated is defined as tB. The fluctuation rate |tA-tB| / tA is less than 10%.

[0008] The vibration damping device according to the application example of the present invention comprises: A magnetorheological fluid according to an application example of the present invention; A container for storing the magnetorheological fluid; a magnetic field generating unit that generates a magnetic field acting on the magnetorheological fluid stored in the container; has. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic diagram showing a magnetorheological fluid according to an embodiment; [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic diagram of the magnetic metal particle shown in FIG. [Diagram 3] 1 is a vertical cross-sectional view showing a vibration damping device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The magnetorheological fluid and the vibration damping device of the present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings.

[0011] 1. Magnetorheological fluid First, the magnetorheological fluid according to the embodiment will be described.

[0012] Fig. 1 is a schematic diagram showing a magnetorheological fluid 1 according to an embodiment. The magnetorheological fluid 1 shown in Fig. 1 has a dispersoid 5 and a dispersion medium 4. The dispersoid 5 contains magnetic metal particles 2 and an additive 3, and is dispersed in the liquid dispersion medium 4.

[0013] Such a magnetorheological fluid 1 behaves like a liquid when no magnetic field is applied, and behaves like a semi-solid when a magnetic field is applied. By utilizing this change in viscosity, it is possible to control the stress of the magnetorheological fluid 1. This allows the magnetorheological fluid 1 to be used in various devices that utilize the change in stress to perform various functions.

[0014] 1.1.Characteristics of magnetorheological fluids 1.1.1.Coercive force of dispersoids In the magnetorheological fluid 1 according to this embodiment, the coercive force of the dispersoid 5 is 796 [A / m] or less (10 [Oe] or less). The coercive force refers to the value of an external magnetic field in the opposite direction required to return a magnetized magnetic body to an unmagnetized state. In other words, the coercive force means the resistance force against an external magnetic field. The dispersoid 5 having a coercive force within the above range has a small residual magnetization, so it is hardly magnetized when a magnetic field is not applied, but is magnetized when a magnetic field is applied, so that the magnetization has a high follow-up ability to changes in the magnetic field. Therefore, the magnetorheological fluid 1 having the dispersoid 5 with such a low coercive force is excellent in response to changes in the magnetic field. In addition, the dispersoid 5 with such a low coercive force is not likely to aggregate when a magnetic field is not applied, so it can be uniformly dispersed even if it is contained in a high concentration in the dispersion medium 4. Therefore, the magnetorheological fluid 1 according to this embodiment has a sufficient low viscosity recovery property.

[0015] Furthermore, if the low viscosity recovery is sufficient, it is possible to ensure a sufficient range of viscosity change between when a magnetic field is applied and when the magnetic field is removed. Furthermore, since the hysteresis of the viscosity change can be kept small, the range of viscosity change can be stabilized even when the magnetic field is repeatedly applied and removed. This makes it possible to realize a magnetorheological fluid 1 that exhibits good characteristics over a long period of time. As a result, it is possible to impart high performance and long-term reliability to various devices that use the magnetorheological fluid 1.

[0016] The coercive force of the dispersoid 5 is preferably 398 [A / m] or less (5 [Oe] or less), and more preferably 239 [A / m] or less (3 [Oe] or less).

[0017] On the other hand, the lower limit of the coercivity of the dispersoid 5 does not need to be set in particular, but is set to 8 [A / m] or more (0.1 [Oe] or more) from the viewpoint of sufficiently suppressing the variation in coercivity between production lots.

[0018] The coercive force of the dispersoid 5 is measured, for example, by using a vibrating sample magnetometer (VSM). An example of a vibrating sample magnetometer is TM-VSM1550HGC manufactured by Tamagawa Manufacturing Co., Ltd. The maximum applied magnetic field when measuring the coercive force is, for example, 1194 [kA / m] (15 [kOe]). When separating the dispersoid 5 from the magnetorheological fluid 1, a method is used in which the dispersion medium 4 is removed by using an organic solvent such as normal hexane or acetone.

[0019] 1.1.2.Redispersibility of magnetorheological fluids In addition, the redispersibility of the magnetorheological fluid 1 according to this embodiment after a magnetic field is applied is evaluated while the fluid is contained in a cylindrical container, based on the change in thickness of the supernatant layer before and after a predetermined magnetic field is applied to the cylindrical container.

[0020] Specifically, the magnetorheological fluid 1 is placed in a cylindrical container, and acceleration is applied to the cylindrical container.Then, the thickness of the supernatant layer generated in the magnetorheological fluid 1 after the acceleration is applied is measured.

[0021] Next, a magnetic field is applied to the magnetorheological fluid 1 contained in the cylindrical container. Next, acceleration is again applied to the cylindrical container after the magnetic field has been applied, and the thickness of the supernatant layer generated in the magnetorheological fluid 1 after the acceleration is applied is measured.

[0022] Next, the redispersibility of the magnetorheological fluid 1 is evaluated based on the change (rate of fluctuation) in thickness of the supernatant layer before and after application of a magnetic field.

[0023] Before applying the magnetic field, the magnetorheological fluid 1 may be stirred under certain conditions while still contained in the cylindrical container. By stirring in this manner, the dispersion state of the magnetorheological fluid 1 becomes constant when the magnetic field is applied, so that the magnetic field applied to the magnetic metal particles 2 can be made uniform, thereby improving the accuracy of the evaluation.

[0024] Furthermore, before the application of the acceleration, the magnetorheological fluid 1 may be stirred under certain conditions while still contained in the cylindrical container. By stirring in this manner, the dispersion state of the magnetorheological fluid 1 before the application of the acceleration can be made uniform. This improves the accuracy of the evaluation when evaluating the redispersibility of the magnetorheological fluid by comparing the thickness of the supernatant layer before and after the application of a magnetic field.

[0025] As a result of calculating the rate of change in this manner, the magnetorheological fluid 1 according to this embodiment has a rate of change of 10% or less, preferably 7% or less, and more preferably 5% or less.

[0026] A magnetorheological fluid 1 that satisfies such a rate of change exhibits stable redispersibility, with little aggregation occurring even when a magnetic field is applied after an acceleration that promotes aggregation has been applied. Therefore, even when used in applications where the application and removal of a magnetic field is repeated, the range of change in viscosity is unlikely to decrease, and stable characteristics based on stress changes can be maintained. As a result, various devices that exhibit high performance over a long period of time can be realized.

[0027] If the rate of change exceeds the upper limit, the redispersibility of the magnetorheological fluid 1 after the application and subsequent removal of a magnetic field is insufficient, and in this case, the range of change in the viscosity of the magnetorheological fluid 1 cannot be sufficiently ensured in applications where the application and removal of a magnetic field are repeated.

[0028] More specifically, the above fluctuation range is measured by the following procedure. First, 1 mL of magnetorheological fluid 1 is placed in a 1.5 mL centrifuge tube (cylindrical solution). The temperature during measurement is 25°C and the relative humidity is 50±5%. Note that magnetorheological fluid 1 is left in this temperature and humidity environment for at least 24 hours in advance.

[0029] Next, the centrifuge tube is set in a stirrer to stir the magnetorheological fluid 1. For example, a microtube stirrer E-36 manufactured by Taitec is used for stirring. The stirring conditions include a horizontal eccentric shaking method, a shaking speed of 2500 r / min, and a shaking time of 10 minutes.

[0030] Next, acceleration is applied to the centrifuge tube so that the product of acceleration and time becomes 690 km / s. This applies energy to the magnetorheological fluid 1 to promote aggregation. Examples of acceleration include centrifugal acceleration and gravitational acceleration. Of these, the method of applying centrifugal acceleration is preferably used from the viewpoint of being able to perform the work in a short time.

[0031] Immediately after the application of acceleration is terminated, the thickness of the supernatant layer formed by the application of acceleration is measured. The measurement result is called "thickness tA."

[0032] The centrifugal acceleration can be applied, for example, by using a centrifuge. An example of a centrifuge is a microcentrifuge Model 3300 manufactured by Kubota Manufacturing Co., Ltd. One example of a method for applying centrifugal acceleration is to apply a centrifugal acceleration of 293 G for 4 minutes. The centrifugal acceleration of 293 G is a relative value of the acceleration of gravity (relative centrifugal acceleration), and when the unit is converted, it is expressed as 293 × 9.81 = 2874 [m / s 2 ]. This acceleration is 2874 [m / s 2The product of this and a time of 240 seconds is 690 km / s.

[0033] On the other hand, as an example of a method for applying gravitational acceleration, the gravitational acceleration can be applied by leaving the centrifuge tube containing the magnetorheological fluid 1 stationary for 19.54 hours. In other words, the gravitational acceleration of 9.81 [m / s 2 ] and the time 70,344 seconds (= 3,600 x 19.54) is 690 [km / s].

[0034] Next, the centrifuge tube is set in the stirrer again, and the magnetorheological fluid 1 is stirred. For example, a microtube stirrer E-36 manufactured by Taitec is used for stirring. The stirring conditions include a horizontal eccentric shaking method, a shaking speed of 2500 r / min, and a shaking time of 10 minutes.

[0035] Next, a magnetic field is applied to the centrifuge tube by contacting the side and bottom of the centrifuge tube with a magnet having a surface magnetic flux density of 0.25 T for 20 minutes. A neodymium magnet is preferably used as the magnet.

[0036] Next, the centrifuge tube is set in the stirrer again, and the magnetorheological fluid 1 is stirred. For example, a microtube stirrer E-36 manufactured by Taitec is used for stirring. The stirring conditions include a horizontal eccentric shaking method, a shaking speed of 2500 r / min, and a shaking time of 10 minutes.

[0037] Next, an acceleration is applied to the centrifuge tube again so that the product of acceleration and time is 690 km / s. Examples of the acceleration include centrifugal acceleration, gravitational acceleration, etc. Among these, the method of applying centrifugal acceleration is preferably used from the viewpoint of being able to perform the operation in a short time.

[0038] Immediately after the application of acceleration is terminated, the thickness of the supernatant layer formed by the application of acceleration is measured again. The measurement result is designated as "thickness tB." Next, the aforementioned rate of change |tA-tB| / tA is calculated from the thicknesses tA and tB.

[0039] Moreover, it is preferable that the magnetorheological fluid 1 maintains good dispersibility even if the product of the acceleration and time is reduced, that is, even if the energy that promotes aggregation is reduced.

[0040] Specifically, even when acceleration is applied such that the product of acceleration and time is 340 km / s, the above fluctuation rate is preferably 10% or less, more preferably 7% or less, and even more preferably 5% or less, as in the case of 690 km / s. By satisfying such a fluctuation rate, the magnetorheological fluid 1 has particularly stable redispersibility.

[0041] Furthermore, even when the product of acceleration and time is reduced to 520 km / s, the above fluctuation rate is preferably 10% or less, more preferably 7% or less, and even more preferably 5% or less for the magnetorheological fluid 1. By satisfying such a fluctuation rate, the magnetorheological fluid 1 has particularly stable redispersibility.

[0042] Furthermore, even when the product of acceleration and time is reduced to 600 km / s, the above fluctuation rate is preferably 10% or less, more preferably 7% or less, and even more preferably 5% or less for the magnetorheological fluid 1. By satisfying such a fluctuation rate, the magnetorheological fluid 1 has particularly stable redispersibility.

[0043] 1.2. Composition of magnetorheological fluid As described above, the magnetorheological fluid 1 includes magnetic metal particles 2 , an additive 3 and a dispersion medium 4 .

[0044] 1.2.1. Composition of magnetic metal particles FIG. 2 is a cross-sectional view that illustrates the magnetic metal particle 2 shown in FIG.

[0045] 2 has a particle body 21, an oxide film 22 provided on the surface of the particle body 21, and a surface modification film 23 provided on the surface of the particle body 21. Note that the oxide film 22 and the surface modification film 23 may be provided as necessary, and either one or both may be omitted.

[0046] 1.2.1.1. Particle body Examples of the constituent material of the particle body 21 include Fe-based metal materials, Ni-based metal materials, Co-based metal materials, etc., and a composite material of one or more of these is used. Also, a composite material of these metal-based magnetic materials and oxide-based magnetic materials may be used. Of these, Fe-based metal materials are preferably used as the constituent material of the particle body 21 from the viewpoint of high saturation magnetization.

[0047] The Fe-based metal material is a metal material whose main component is Fe. The term "main component" means that the Fe content in the Fe-based metal material is 50% or more in terms of atomic ratio. Such Fe-based metal materials have higher saturation magnetization, toughness, and strength than ferrite and the like. For this reason, the Fe-based metal material is useful as a constituent material for the particle body 21.

[0048] The Fe-based metallic material may contain, in addition to Fe, an element that exhibits ferromagnetism by itself, such as Ni or Co, and may contain at least one selected from the group consisting of Cr, Nb, Cu, Al, Mn, Mo, Si, Sn, B, C, P, Ti, and Zr, depending on the target characteristics. The Fe-based metallic material may also contain unavoidable impurities to the extent that the effects of the embodiment are not impaired.

[0049] Inevitable impurities are impurities that are unintentionally mixed into raw materials or during manufacturing. Examples of unavoidable impurities include O, N, S, Na, Mg, and K.

[0050] Such Fe-based metal materials are not particularly limited, but examples thereof include pure iron, carbonyl iron, Fe-Si-Al-based alloys such as sendust, and Fe-Ni-based, Fe-Co-based, Fe-Ni-Co-based, Fe-Si-B-based, Fe-Si-Cr-B-based, Fe-Si-BC-based, Fe-Si-B-Cr-C-based, Fe-Si-Cr-based, Fe-B-based, Fe-PC-based, Fe-Co-Si-B-based, Fe-Si-B-Nb-based, Fe-Si-B-Nb-Cu-based, Fe-Zr-B-based, Fe-Cr-based, and Fe-Cr-Al-based Fe-based alloy materials.

[0051] The material constituting the particle body 21 may be an amorphous metal material, a crystalline metal material, or a microcrystalline (nanocrystalline) metal material. Among these, amorphous metal materials or microcrystalline metal materials are preferably used. The microcrystalline metal material refers to a metal material in which microcrystals (nanocrystals) having a crystal grain size of 100 nm or less exist. These materials contribute to sufficiently lowering the coercive force of the dispersoid 5 and optimizing the aforementioned fluctuation rate. In addition, these materials have higher toughness and strength than, for example, metal oxides, and therefore can effectively suppress wear and breakage of the particle body 21. As a result, a magnetorheological fluid 1 with a particularly stable viscosity change range can be realized.

[0052] Examples of amorphous metal materials include binary or multi-component Fe-based amorphous alloys such as Fe-Si-B, Fe-Si-Cr-B, Fe-Si-BC, Fe-Si-B-Cr-C, Fe-Si-Cr, Fe-B, Fe-BC, Fe-PC, Fe-Co-Si-B, Fe-Si-B-Nb, and Fe-Zr-B systems; Ni-based amorphous alloys such as Ni-Si-B and Ni-PB systems; and Co-based amorphous alloys such as Co-Si-B systems.

[0053] Examples of microcrystalline metal materials include Fe-based nanocrystalline alloys such as Fe-Si-B-Nb-Cu, Fe-Zr-B, Fe-Hf-B, Fe-Nb-B, Fe-Zr-B-Co, Fe-Hf-B-Co, Fe-Nb-B-Co, and Fe-Si-BP-Cu.

[0054] Particularly preferred Fe-based metal materials are alloy materials mainly composed of Fe and containing at least one selected from the group consisting of Si, Cr, B, C, Ni, Mn and Cu. Such Fe-based metal materials have high saturation magnetization and high corrosion resistance. Therefore, by using such Fe-based alloy materials, magnetic metal particles 2 that can be used to produce magnetorheological fluid 1 with high corrosion resistance and high excitation shear stress can be obtained.

[0055] The Si (silicon) content in the Fe-based metal material is preferably 1.0 atomic % or more and 20.0 atomic % or less, more preferably 1.5 atomic % or more and 13.0 atomic % or less, and even more preferably 2.0 atomic % or more and 11.0 atomic % or less. Such alloys have high magnetic permeability and tend to have high saturation magnetization. This allows the magnetic metal particles 2 to be obtained that can produce a magnetorheological fluid 1 that has particularly high excitation shear stress and magnetic field response.

[0056] The content of B (boron) in the Fe-based metal material is preferably 5.0 atomic % or more and 16.0 atomic % or less, and more preferably 9.0 atomic % or more and 14.0 atomic % or less. B is an element that promotes amorphization, and contributes to the formation of a stable amorphous structure or microcrystalline structure in the magnetic metal particles 2.

[0057] The C (carbon) content in the Fe-based metal material is preferably 0.5 atomic % or more and 5.0 atomic % or less, and more preferably 1.0 atomic % or more and 3.0 atomic % or less. C is an element that promotes amorphization, and contributes to the formation of a stable amorphous structure or microcrystalline structure in the magnetic metal particles 2.

[0058] The Cr (chromium) content in the Fe-based metal material is preferably 1.0 atomic % or more and 20.0 atomic % or less, and more preferably 1.5 atomic % or more and 5.0 atomic % or less. By keeping the Cr content within this range, the corrosion resistance of the magnetic metal particles 2 can be improved.

[0059] The total content of impurities is preferably 1.0 atomic % or less, so that the effect of the magnetic metal particles 2 is not impaired even if impurities are contained.

[0060] The constituent elements and composition of the particle body 21 can be identified by ICP emission spectrometry as specified in JIS G 1258:2014, spark emission spectrometry as specified in JIS G 1253:2002, or the like. If the particle body 21 is covered with a coating film or the like, it can be removed by a chemical or physical method and then measured by the above method. The magnetic metal particle 2 may be cut and the core part of the particle body 21 may be analyzed by an analyzer such as an EPMA (Electron Probe Micro Analyzer) or EDX (Energy Dispersive X-ray spectroscopy).

[0061] The particle body 21 may be a particle manufactured by any method. Examples of the manufacturing method include various atomizing methods such as water atomizing, gas atomizing, and rotary water flow atomizing, as well as a pulverizing method and a carbonyl method. Among these, the atomizing method can obtain a particle body 21 having a particle shape closer to a perfect sphere. Such a particle body 21 is less likely to aggregate.

[0062] 1.2.1.2.Oxide Film The oxide film 22 is a film provided on the surface of the particle body 21. The oxide film 22 is interposed between the particle body 21 and a surface modification film 23 described later, and enhances the adhesion of the surface modification film 23 to the particle body 21. Further, the oxide film 22 can protect the particle body 21 and suppress aggregation, and can enhance the moisture absorption resistance and rust prevention property of the particle body 21. Note that the oxide film 22 preferably covers the entire surface of the particle body 21, but may be provided only on a part of the surface.

[0063] Examples of the constituent material of the oxide film 22 include silicon oxide, aluminum oxide, titanium oxide, vanadium oxide, niobium oxide, chromium oxide, manganese oxide, tin oxide, zinc oxide, etc., and one or a mixture or composite of two or more of these may be mentioned.

[0064] Among these, silicon oxide is preferably used. Silicon oxide is an oxide represented by the compositional formula SiO x (0 < x ≦ 2), but is preferably SiO 2 .

[0065] The average thickness of the oxide film 22 is preferably 1 nm or more and 500 nm or less, more preferably 3 nm or more and 300 nm or less, and even more preferably 20 nm or more and 100 nm or less. If the average thickness of the oxide film 22 is within the above range, while ensuring the functions of the oxide film 22 described above, it is possible to avoid the oxide film 22 becoming thicker than necessary. Thereby, while suppressing the aggregation and deterioration of the magnetic metal particles 2, it is possible to suppress a decrease in the magnetic properties of the magnetic metal particles 2 due to the ratio of the oxide film 22 becoming too high.

[0066] The average thickness of the oxide film 22 is a value obtained by observing the cross section of the particles of the magnetic metal particles 2 with an electron microscope and averaging the film thicknesses of the oxide film 22 at 10 or more locations.

[0067] The method for forming the oxide film 22 is not particularly limited, but examples thereof include wet film formation methods such as sol-gel methods including the Stober method, and vapor phase film formation methods such as ALD (Atomic Layer Deposition), CVD (Chemical Vapor Deposition), and ion plating. Among these, the sol-gel method, particularly the Stober method, is useful because it allows the oxide film 22 to be formed evenly at low cost.

[0068] The Stöber method is a method for forming an oxide film 22 by hydrolysis of silicon alkoxide. Examples of silicon alkoxide include TEOS (tetraethoxysilane, Si(OC 2 H 5 ) 4 ) is preferably used.

[0069] 1.2.1.3.Surface modified membrane The surface modification film 23 covers the surface of the particle body 21 via the oxide film 22. This can improve the dispersibility of the magnetic metal particles 2 in the dispersion medium 4. Note that the surface modification film 23 preferably covers the entire surface of the oxide film 22 or the particle body 21, but may be provided only on a portion of the surface.

[0070] The constituent materials of the surface modification film 23 include a coupling agent, a surfactant, or an organic compound derived from a polymerized film. The coupling agent is a compound having a functional group and a hydrolyzable group. By using a coupling agent, a functional group can be introduced to the surface of the oxide film 22 (the surface of the magnetic metal particles 2). This can suppress the aggregation of the magnetic metal particles 2 and further increase the dispersibility in the dispersion medium 4. This can realize magnetic metal particles 2 that are excellent in following the change in the magnetic field and can be uniformly dispersed in the dispersion medium 4 even at high concentrations.

[0071] The surface modification film 23 also contributes to improving the moisture resistance, rust prevention, etc. of the magnetic metal particles 2. By improving the moisture resistance and rust prevention, deterioration of the magnetic metal particles 2 due to moisture absorption and rust generation can be suppressed.

[0072] Examples of the functional group possessed by the coupling agent include those containing an aliphatic hydrocarbon group, a cyclic structure-containing group, a fluoroalkyl group, a fluoroaryl group, a nitro group, an acyl group, a cyano group, etc., and in particular, an aliphatic hydrocarbon group or a cyclic structure-containing group is preferably used.

[0073] The aliphatic hydrocarbon group may be a branched or unbranched alkyl group. The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 12, more preferably 1 to 6. This allows the magnetic metal particles 2 to be dispersed particularly well in the oil-based dispersion medium 4.

[0074] The cyclic structure-containing group is a functional group having a cyclic structure. Examples of the cyclic structure-containing group include an aromatic hydrocarbon group, an alicyclic hydrocarbon group, and a cyclic ether group.

[0075] The aromatic hydrocarbon group is a residue obtained by removing a hydrogen atom from an aromatic hydrocarbon, and preferably has 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon group include an aryl group, an alkylaryl group, an aminoaryl group, and a halogenated aryl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and an indenyl group. Examples of the alkylaryl group include a benzyl group, a methylbenzyl group, a phenethyl group, a methylphenethyl group, and a phenylbenzyl group.

[0076] The alicyclic hydrocarbon group is a residue obtained by removing a hydrogen atom from an alicyclic hydrocarbon, and preferably has 3 to 20 carbon atoms. Examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkylalkyl group. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the cycloalkylalkyl group include a cyclopentylmethyl group and a cyclohexylmethyl group.

[0077] Examples of the cyclic ether group include an epoxy group, a 3,4-epoxycyclohexyl group, and an oxetanyl group.

[0078] The fluoroalkyl group is an alkyl group having from 1 to 16 carbon atoms, which is substituted with one or more fluorine atoms, or a cycloalkyl group having from 3 to 16 carbon atoms. In particular, the fluoroalkyl group is preferably a perfluoroalkyl group.

[0079] The fluoroaryl group is an aryl group substituted with one or more fluorine atoms and having from 6 to 20 carbon atoms. In particular, the fluoroaryl group is preferably a perfluoroaryl group.

[0080] Examples of the hydrolyzable group contained in the coupling agent include an alkoxy group, an acyloxy group, an aryloxy group, an aminoxy group, an amide group, a ketoxime group, an isocyanate group, and a halogen atom.

[0081] Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, and a zirconium coupling agent, with the silane coupling agent being particularly preferred.

[0082] The amount of the coupling agent added is preferably 0.01 part by mass to 1.0 part by mass, and more preferably 0.02 part by mass to 0.10 part by mass, when the amount of the particle body 21 is taken as 1 part by mass.

[0083] 1.2.2. Physical properties of magnetic metal particles The saturation magnetization of the magnetic metal particles 2 is preferably 50 emu / g or more, and more preferably 100 emu / g or more. The saturation magnetization is the value of magnetization when the magnetization of a magnetic material is constant regardless of the magnetic field when a sufficiently large magnetic field is applied from the outside. The higher the saturation magnetization of the magnetic metal particles 2, the more fully the magnetic material can function. Specifically, the moving speed of the magnetic metal particles 2 in a magnetic field can be improved, and thus the responsiveness to the magnetic field can be improved. In addition, the range of viscosity change can be further expanded.

[0084] The upper limit of the saturation magnetization of the magnetic metal particles 2 is not particularly limited, but from the viewpoint of ease of material selection that balances performance and cost, it is preferably 250 emu / g or less, and more preferably 220 emu / g or less.

[0085] The saturation magnetization of the magnetic metal particles 2 can be measured by a vibrating sample magnetometer (VSM) etc. The maximum applied magnetic field when measuring the saturation magnetization is, for example, 1194 [kA / m] (15 [kOe]) or more.

[0086] The average particle size of the magnetic metal particles 2 is preferably 0.05 μm or more and 9.0 μm or less, more preferably 0.1 μm or more and 7.0 μm or less, and even more preferably 0.5 μm or more and 5.0 μm or less. If the average particle size of the magnetic metal particles 2 is within the above range, aggregation and sedimentation of the magnetic metal particles 2 in a state where no magnetic field is applied can be suppressed. Also, a decrease in magnetic field responsiveness can be suppressed.

[0087] If the average particle size of the magnetic metal particles 2 falls below the lower limit, depending on the material of the magnetic metal particles 2, the magnetic metal particles 2 may easily aggregate even when no magnetic field is applied. Also, the range of viscosity change may become small. On the other hand, if the average particle size of the magnetic metal particles 2 exceeds the upper limit, depending on the material of the magnetic metal particles 2, the magnetic metal particles 2 may settle and become unevenly distributed in the dispersion medium 4.

[0088] The average particle size of the magnetic metal particles 2 can be determined by measuring the volumetric particle size distribution by a laser diffraction / dispersion method and then calculating from the cumulative distribution curve obtained from this particle size distribution. Specifically, the particle size (median diameter) at which the cumulative value from the small diameter side is 50% in the cumulative distribution curve is the average particle size D50 of the magnetic metal particles 2. An example of an apparatus for measuring particle size distribution by a laser diffraction / dispersion method is the MT3300 series manufactured by Microtrack Bell.

[0089] In addition, in the cumulative distribution curve of the particle size distribution obtained for the magnetic metal particles 2, the particle diameter at which the cumulative value from the small diameter side is 90% is defined as the 90% particle diameter D90 of the magnetic metal particles 2. In the magnetic metal particles 2, the ratio D90 / D50 of the 90% particle diameter D90 to the average particle diameter D50 is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.7 or less. This reduces the content of coarse magnetic metal particles 2, so that the coarse magnetic metal particles 2 attract and aggregate the surrounding relatively small magnetic metal particles 2, and the generation of aggregates can be suppressed. If aggregates are generated, they tend to settle due to their own weight, and there is a risk that the viscosity change range of the magnetorheological fluid 1 will decrease or the viscosity change range will become unstable.

[0090] The average circularity of the magnetic metal particles 2 is preferably 0.78 to 1.00, more preferably 0.80 to 0.98, and even more preferably 0.82 to 0.97. This reduces the specific surface area of ​​the magnetic metal particles 2, thereby preventing the formation of aggregates. As a result, the range of viscosity change of the magnetorheological fluid 1 can be stabilized.

[0091] If the average circularity falls below the lower limit, the average circularity decreases, which may reduce the range of change in viscosity of the magnetorheological fluid 1. On the other hand, if the average circularity exceeds the upper limit, the manufacturing difficulty increases, and the manufacturing efficiency of the magnetorheological fluid 1 may decrease.

[0092] The average circularity of the magnetic metal particles 2 is measured as follows. First, an image (secondary electron image) of the magnetic metal particles 2 is captured by a scanning electron microscope (SEM). Next, the obtained image is loaded into image processing software. For example, image analysis type particle size distribution measurement software "Mac-View" manufactured by Mountech Co., Ltd. is used as the image processing software. The imaging magnification is adjusted so that 50 to 100 particles are captured in one image. Then, multiple images are acquired so that a total of 300 or more particle images are obtained.

[0093] Next, using software, the circularity of 300 or more particle images is calculated and the average value is obtained. The obtained average value is the average circularity of the magnetic metal particles 2. Note that when the circularity is e, the area of ​​the particle image is S, and the perimeter of the particle image is L, the circularity e can be obtained by the following formula. e=4πS / L 2

[0094] The content of the magnetic metal particles 2 is preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and even more preferably 60% by mass or more and 85% by mass or less, of the entire magnetorheological fluid 1. This allows the magnetorheological fluid 1 to have an appropriate viscosity when a magnetic field is applied and when the magnetic field is removed, and also allows the range of viscosity change in the magnetorheological fluid 1 to be sufficiently large.

[0095] Additives Examples of additives 3 include settling inhibitors, detergents, dispersants, antioxidants, antiwear agents, extreme pressure agents, friction modifiers, surfactants, thixotropy-imparting agents (thickeners), viscosity reducers, etc., and one or a mixture of two or more of these is used.

[0096] Examples of the sedimentation inhibitor include solid particles composed of non-magnetic materials such as fumed silica, clay powders such as bentonite and hectorite, and one or a mixture of two or more of these is used. Such solid particles are particles of a non-magnetic material whose constituent material is different from that of the magnetic metal particles 2, and suppress the sedimentation of the magnetic metal particles 2. This makes it possible to suppress a decrease in the viscosity change range even if a long period of time continues in which a magnetic field is not applied.

[0097] The content of solid particles is preferably 5.0% by mass or less of the entire magnetorheological fluid 1, and more preferably 0.5% by mass or more and 3.0% by mass or less. This makes it possible to suppress the settling of the magnetic metal particles 2 without affecting the range of viscosity change, and to stabilize the range of viscosity change over a long period of time. Therefore, by adding an appropriate additive 3, the aforementioned rate of change can be optimized.

[0098] Dispersants include, for example, oleates, naphthenates, sulfonates, phosphates, stearic acid, stearates, glycerol monooleate, sorbitan sesquioleate, lauric acid, fatty acids, and fatty alcohols.

[0099] Examples of the anti-wear agent include organic molybdenum compounds such as molybdenum dialkyldithiocarbamate and molybdenum dialkyldithiophosphate, and organic zinc compounds such as zinc dialkyldithiocarbamate and zinc dialkyldithiophosphate.

[0100] The total content of the additives 3 is preferably 10 mass % or less, more preferably 8 mass % or less, and even more preferably 6 mass % or less of the entire magnetorheological fluid 1. This makes it possible to prevent the additives 3 from impairing the function of the magnetic metal particles 2. The additive 3 may be added as necessary and may be omitted.

[0101] 1.2.4.Dispersion medium The dispersion medium 4 is not particularly limited as long as it is a liquid capable of dispersing the magnetic metal particles 2 and the additive 3. Examples of the dispersion medium 4 include oils such as silicone oil, poly-α-olefin base oil, aromatic synthetic oil, paraffin oil, alkylated phenyl ether oil, ether oil, ester oil, polybutene oil, polyalkylene glycols, mineral oil, vegetable oil, and animal oil, organic solvents such as toluene, xylene, and hexane, and ionic liquids (room-temperature molten salts) such as ethylmethylimidazolium salt, 1-butyl-3-methylimidazolium salt, and 1-methylpyrazolium salt. The dispersion medium 4 may be a mixture containing two or more of these, or a mixture containing one or more of these and a liquid other than the above.

[0102] Among these, examples of the ester oil include a diester produced from a monohydric alcohol and a dicarboxylic acid, a polyol ester produced from a polyol and a monocarboxylic acid, and a complex ester produced from a polyol, a monocarboxylic acid, and a polycarboxylic acid.

[0103] Examples of the diester include esters of dibasic acids such as adipic acid, azelaic acid, sebacic acid, and dodecanedioic acid. The dibasic acid is preferably an aliphatic dibasic acid having 4 to 36 carbon atoms. The alcohol residue constituting the ester portion of the ester of the dibasic acid is preferably a monohydric alcohol residue having 4 to 26 carbon atoms. Examples of such diester include dioctyl adipate, dioctyl sebacate, diisodecyl adipate, and dioctyl azelate.

[0104] As the polyol used in the polyol ester and the complex ester, specifically, a hindered alcohol having no β-hydrogen such as trimethylolpropane, pentaerythritol, neopentyl glycol, etc. is preferably used. As the monocarboxylic acid used in the polyol ester and the complex ester, a linear saturated fatty acid such as coconut oil fatty acid and stearic acid, a linear unsaturated fatty acid such as oleic acid, a branched fatty acid such as isostearic acid, etc. are listed.

[0105] As the polycarboxylic acid, straight-chain saturated polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid are preferably used.

[0106] Examples of the alkylated phenyl ether oil include alkylated diphenyl ethers and (alkylated) polyphenyl ethers.

[0107] Examples of polyalkylene glycols include polyethylene glycol, polypropylene glycol, polybutylene glycol, ethylene oxide-propylene oxide copolymer, propylene oxide-butylene oxide copolymer, and derivatives thereof.

[0108] 1.3.Examples of applications of magnetorheological fluids Applications of the magnetorheological fluid 1 include various apparatuses and devices that utilize the difference in stress when the application of a magnetic field is switched. Examples of such apparatuses and devices include vibration control devices such as linear dampers, rotary dampers, and shock absorbers, braking devices such as brakes, power transmission devices such as clutches, muscle parts and end effectors of robots, valves for controlling the flow rate of liquids, tactile presentation devices, audio devices, robot hands for medical and welfare purposes, nursing hands, personal mobility devices, and the like.

[0109] 1.4. Manufacturing method of magnetorheological fluid In the method for producing the magnetorheological fluid 1, the raw materials of the magnetorheological fluid 1 described above are first mixed and stirred. Examples of the stirring method include stirring with a spatula, a vortex mixer, a high shear mixer, and a low-frequency acoustic resonance mixer. The stirring time is appropriately set depending on the stirring method, but is preferably 5 minutes to 4 hours. The stirring temperature is appropriately set depending on the stirring method, but is preferably 15°C to 70°C.

[0110] 2. Vibration control device Next, a vibration damping device according to an embodiment will be described.

[0111] Fig. 3 is a vertical cross-sectional view showing the vibration damping device 100 according to the embodiment. Note that the posture of the vibration damping device 100 in Fig. 3 during use is not particularly limited, but in the following description, the upper side in Fig. 3 will be referred to as "upper" and the lower side as "lower".

[0112] 3 includes a cylindrical cylinder 200 (container) with closed upper and lower ends, a piston rod 310 that penetrates an upper portion 210 of the cylinder 200 from the outside of the cylinder 200 and extends into the cylinder 200, and a piston 300 that is provided at the lower end of the piston rod 310 and slides up and down within the cylinder 200. A magnetorheological fluid 1 is stored within the cylinder 200.

[0113] Such a vibration damping device 100 operates to expand and contract between a member connected to the upper end of the piston rod 310 and a member connected to the lower end of the cylinder 200. For example, if the upper end of the piston rod 310 is connected to the body of an automobile and the lower end of the cylinder 200 is connected to a wheel or an axle, an expansion and contraction force is applied to the vibration damping device 100 when the distance between the body and the wheel (axle) expands and contracts.

[0114] In the vibration damping device 100, the piston 300 slides in accordance with the expansion and contraction forces applied between the various members, and during this sliding, a resistance force is applied to the piston 300 from the magnetorheological fluid 1 in a direction that relieves the aforementioned expansion and contraction forces. As a result, the piston 300 functions as a shock absorber that relieves and attenuates the expansion and contraction forces applied between the various members.

[0115] The vibration damping device 100 also includes a coil 400 that is provided inside the piston 300 and applies a magnetic field to the magnetorheological fluid 1 contained in the cylinder 200, and a power supply circuit (not shown) that applies a voltage to the coil 400. Thus, the coil 400 and the power supply circuit function as a magnetic field generating device.

[0116] The viscosity of the magnetorheological fluid 1 changes depending on the presence or absence of a magnetic field and its strength. Therefore, the viscosity of the magnetorheological fluid 1 can be adjusted by appropriately setting the presence or absence and strength of the magnetic field generated by the magnetic field generating device described above. By utilizing such characteristics, the vibration damping device 100 becomes a variable damping force damper that can control the damping force. Furthermore, by using the magnetorheological fluid 1, it is possible to obtain a vibration damping device 100 that can maintain good performance for a long period of time.

[0117] Each component of the vibration damping device 100 will be described in detail below. The cylinder 200 shown in FIG. 3 has a two-layer structure (double cylinder type) and is composed of an outer cylinder 220 on the outside and an inner cylinder 230 on the inside.

[0118] Further, the space inside the inner cylinder 230 is divided into a rod side chamber 200a above the piston 300 and a piston side chamber 200b below the piston 300.

[0119] Furthermore, below the piston side chamber 200b, a first reservoir chamber 250 is provided via a base valve 240 that is provided so as to separate the space inside the inner cylinder 230.

[0120] The base valve 240 is provided with an orifice 241 that penetrates the base valve 240, and the piston side chamber 200b and the first reservoir chamber 250 communicate with each other via this orifice 241.

[0121] Moreover, the space between the outer cylinder 220 and the inner cylinder 230 is a second reservoir chamber 260. The first reservoir chamber 250 and the second reservoir chamber 260 are adjacent to each other via the lower end portion of the inner cylinder 230.

[0122] In addition, an orifice 231 that penetrates the portion of the inner tube 230 that separates the first reservoir chamber 250 and the second reservoir chamber 260 is provided, and the first reservoir chamber 250 and the second reservoir chamber 260 are connected to each other via this orifice 231.

[0123] The cylinder 200 is made of a material having excellent mechanical properties and oil resistance, such as various metal materials.

[0124] The piston rod 310 is made of a rod-shaped member with high rigidity, and passes through the center of the upper portion 210 of the cylinder 200 , extending inside and outside the cylinder 200 .

[0125] The piston 300 is composed of a cylindrical member, and its outer surface is in sliding contact with the inner wall surface of the inner tube 230 of the cylinder 200. As described above, the piston 300 divides the space inside the inner tube 230 into the rod side chamber 200a and the piston side chamber 200b.

[0126] Furthermore, two orifices 320, 330 are provided so as to penetrate the piston 300. Through these orifices 320, 330, the rod side chamber 200a and the piston side chamber 200b communicate with each other.

[0127] A valve body 340 is provided on the upper surface of the piston 300 near the upper end opening of the orifice 320. The valve body 340 is configured to be capable of taking a state in which the magnetorheological fluid 1 cannot flow through the orifice 320 by closing the upper end opening of the orifice 320 (closed state) and a state in which the magnetorheological fluid 1 can flow through the orifice 320 by opening the upper end opening of the orifice 320 (open state). The valve body 340 is a one-way valve that has a function of passing the flow of the magnetorheological fluid 1 from the piston side chamber 200b to the rod side chamber 200a and blocking the flow in the opposite direction. Note that FIG. 3 shows the valve body 340 in an open state.

[0128] The valve body 340 opens and closes using the driving force of the relative flow of the magnetorheological fluid 1 relative to the piston 300 that occurs as the piston 300 slides relative to the cylinder 200. In order for the valve body 340 to transition from the closed state to the open state, the magnetorheological fluid 1 needs to flow faster than a predetermined speed to apply a pressure of a predetermined magnitude or more to the valve body 340. Therefore, the valve body 340 is configured to be able to take the open state only when the piston 300 slides at a speed equal to or faster than the predetermined speed. With this valve body 340, the vibration damping device 100 can have different damping forces when the sliding speed of the piston 300 is low and high.

[0129] A ring-shaped coil 400 (magnetic field generating unit) is provided inside the piston 300. A part of the outer surface of the coil 400 faces each of the orifices 320, 330.

[0130] As described above, the power supply circuit is connected to the coil 400. When a voltage is applied to the coil 400, a magnetic field is generated around the coil 400.

[0131] In addition, in FIG. 3, coil 400 is provided inside piston 300, but the location where coil 400 is provided is not particularly limited.

[0132] 3. Advantages of the above embodiment As described above, the magnetorheological fluid 1 according to the embodiment includes the dispersoid 5 containing the magnetic metal particles 2 and the liquid dispersion medium 4. The coercive force of the dispersoid 5 is 796 [A / m] or less (10 [Oe] or less). When the thickness of the supernatant layer generated when the magnetorheological fluid 1 is contained in a cylindrical container and an acceleration is applied such that the product of acceleration and time is 690 km / s is tA, and the thickness of the supernatant layer generated when the magnetorheological fluid 1 is contained in the cylindrical container and then a magnetic field is applied and the aforementioned acceleration is applied is tB, the fluctuation rate |tA-tB| / tA of the magnetorheological fluid 1 is 10% or less.

[0133] With this configuration, even after a magnetic field is applied and then removed, the dispersoids 5 are well redispersed, resulting in a magnetorheological fluid 1 that exhibits stable characteristics. Even when used in applications where a magnetic field is repeatedly applied and removed, the range of change in viscosity of this magnetorheological fluid 1 is unlikely to decrease, and stable characteristics based on stress changes can be maintained. Therefore, by using this magnetorheological fluid 1, various devices that exhibit high performance over a long period of time can be realized.

[0134] The average particle size of the magnetic metal particles 2 is preferably not less than 0.05 μm and not more than 9.0 μm.

[0135] This makes it possible to suppress aggregation and sedimentation of the magnetic metal particles 2 when no magnetic field is applied, and also makes it possible to suppress a decrease in magnetic field responsiveness.

[0136] The magnetic metal particles 2 may also contain an Fe-based metal material. Fe-based metal materials have higher saturation magnetization, toughness, and strength than ferrite, etc. For this reason, Fe-based metal materials are useful as a constituent material of the magnetic metal particles 2.

[0137] In addition, the Fe-based metal material is preferably an amorphous metal material or a microcrystalline metal material. These have higher toughness and strength than, for example, metal oxides, and therefore can effectively suppress wear and damage of the magnetic metal particles 2. As a result, a magnetorheological fluid 1 with a particularly stable viscosity change range can be realized.

[0138] The Fe-based metal material preferably contains Fe as a main component and has a Si content of 1.0 atomic % to 20.0 atomic %. The saturation magnetization of the magnetic metal particles 2 is preferably 50 emu / g to 250 emu / g. With this configuration, the magnetic field response of the magnetic metal particles 2 can be improved.

[0139] Moreover, the magnetic metal particle 2 may have a particle body 21 and an oxide film 22 provided on the surface of the particle body 21 .

[0140] The oxide film 22 can protect the particle body 21 and suppress agglomeration, and can also enhance the moisture absorption resistance and rust prevention properties of the particle body 21.

[0141] The magnetic metal particles 2 may also have a surface modification film 23 (coating) formed on the surface thereof and made of a compound derived from a coupling agent.

[0142] The surface modification film 23 can introduce functional groups onto the surfaces of the magnetic metal particles 2, and therefore can enhance the dispersibility of the magnetic metal particles 2 in the dispersion medium 4.

[0143] The average circularity of the magnetic metal particles 2 is preferably 0.78 or more and 1.00 or less.

[0144] According to this configuration, the specific surface area of ​​the magnetic metal particles 2 can be reduced, so that the generation of aggregates can be suppressed. As a result, the range of viscosity change of the magnetorheological fluid 1 can be stabilized.

[0145] The dispersoid 5 may also contain solid particles made of a non-magnetic material. According to this configuration, the solid particles suppress the settling of the magnetic metal particles 2. This makes it possible to suppress a decrease in the range of change in viscosity even if a long period of time continues in which no magnetic field is applied.

[0146] The content of solid particles in the entire magnetorheological fluid 1 may be 0.5% by mass or more and 3.0% by mass or less.

[0147] According to this configuration, it is possible to suppress the settling of the magnetic metal particles 2 without affecting the range of viscosity change, and to stabilize the range of viscosity change over a long period of time. As a result, it is possible to optimize the aforementioned rate of change.

[0148] The vibration damping device 100 according to the embodiment includes a magnetorheological fluid 1, a cylinder 200 (container), and a coil 400 (magnetic field generating unit). The cylinder 200 stores the magnetorheological fluid 1. The coil 400 generates a magnetic field that acts on the magnetorheological fluid 1 stored in the cylinder 200.

[0149] With such a vibration damping device 100, the viscosity of the magnetorheological fluid 1 can be adjusted by appropriately setting the presence or absence and strength of the magnetic field generated by the coil 400, thereby obtaining a variable damping force damper capable of controlling the damping force. Furthermore, by using the magnetorheological fluid 1, a vibration damping device 100 capable of maintaining good performance for a long period of time can be obtained.

[0150] While the magnetorheological fluid and the vibration damping device of the present invention have been described above based on the preferred embodiments, the present invention is not limited to these.

[0151] For example, the magnetorheological fluid and the vibration damping device of the present invention may be obtained by adding any configuration to the above-described embodiment. Also, the configuration of each part of the vibration damping device according to the above-described embodiment may be replaced with a configuration having the same function as the above. EXAMPLES

[0152] Next, specific examples of the present invention will be described. 4. Preparation of Magnetorheological Fluid 4.1. Example 1 First, magnetic metal particles and additives were dispersed in a dispersion medium to prepare a magnetorheological fluid. The composition of the magnetorheological fluid is shown in Tables 1 and 2. As additives, clay powder, which is a solid particle, and a liquid organomolybdenum compound were used. As a dispersion medium, a mixture of poly-α-olefin base oil and dioctyl sebacate (dioctyl sebacate) was used.

[0153] The magnetic metal particles used had an oxide film and a surface modification film on their surfaces. The Stöber method was used to form the oxide film. The average thickness of the oxide film is shown in Table 1. The surface modification film was a film composed of a compound derived from a silane coupling agent (SC), and methyltrimethoxysilane was used as the silane coupling agent.

[0154] The content of magnetic metal particles in the magnetorheological fluid was 85% by mass, the content of solid particles was 2.0% by mass, and the content of organic molybdenum compound was 3.0% by mass.

[0155] 4.2. Examples 2 to 5 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2.

[0156] 4.3. Example 6 A magnetorheological fluid was obtained in the same manner as in Example 1, except that magnetic metal particles without an oxide film were used and the composition of the magnetorheological fluid was as shown in Tables 1 and 2.

[0157] 4.4. Example 7 A magnetorheological fluid was obtained in the same manner as in Example 1, except that magnetic metal particles without a surface modification film were used and the composition of the magnetorheological fluid was as shown in Tables 1 and 2.

[0158] 4.5. Examples 8 to 12 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2.

[0159] 4.6. Comparative Examples 1 to 3 A magnetorheological fluid was obtained in the same manner as in Example 1, except that the composition of the magnetorheological fluid was changed as shown in Tables 1 and 2.

[0160] 5. Obtaining magnetorheological fluid properties The characteristics of the magnetorheological fluids of the examples and comparative examples were obtained as follows.

[0161] 5.1.Coercive force of dispersoids The coercive force of the dispersoids of the magnetorheological fluids of each of the Examples and Comparative Examples was measured. The measurement results are shown in Table 2.

[0162] 5.2. Fluctuation rate of thickness of skim layer For the magnetorheological fluids of each Example and Comparative Example, the thickness of the supernatant layer was measured by the method described above, and the fluctuation rate was calculated. The calculation results are shown in Table 2. The measurement of the thickness of the supernatant layer and the calculation of the fluctuation rate were performed by changing the product of acceleration and time to four levels: 340 km / s, 520 km / s, 600 km / s, and 690 km / s. Of these, 340 km / s, 520 km / s, and 690 km / s were obtained by applying centrifugal acceleration by a centrifuge for a predetermined period of time, and 600 km / s was obtained by applying gravitational acceleration for a predetermined period of time. The smaller the fluctuation rate, the higher the dispersion stability of the dispersoid in the magnetorheological fluid.

[0163] 6. Evaluation results of magnetorheological fluid The magnetorheological fluids of each of the examples and comparative examples were evaluated as follows.

[0164] 6.1. Evaluation of stability after 30 or 60 magnetic field applications The magnetic field was repeatedly applied and removed for the magnetorheological fluids of each Example and Comparative Example. The maximum shear yield stress after 30 repetitions and the maximum shear yield stress after 60 repetitions were calculated as a multiple of the shear yield stress immediately before the magnetic field was applied. The calculated multiples were evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2.

[0165] A: The multiple is less than 2.0. B: The multiple is 2.0 or more and less than 4.0. C: The ratio is 4.0 to less than 6.0. D: The ratio is 6.0 to less than 12.0. E: The multiple is 12.0 or more.

[0166] The shear yield stress of a magnetorheological fluid is the shear stress measured at a shear rate of 0.01 [ / s]. For example, a rheometer MCR102 manufactured by Anton Paar can be used to measure the shear stress. In addition, a magnetic field application attachment MRD70 manufactured by Anton Paar can be used as a device for applying a magnetic field during measurement.

[0167] The shear stress can be measured by taking a 200μL sample of magnetorheological fluid, placing it between the sample stage and a 20mm diameter rotor of the device, rotating the rotor, and applying a specified shear rate while switching the application of a magnetic field. The magnetic field strength is 0.5T, and the gap between the sample stage and the rotor is 0.5mm.

[0168] When the application and removal of the magnetic field are repeated, the length of the magnetic field application period and the length of the magnetic field removal period are each 80 seconds. When the application of the magnetic field is switched, the shear yield stress also changes accordingly. When switching from the magnetic field removal period to the magnetic field application period, the shear yield stress increases instantaneously. The shear yield stress immediately before this increase is the above-mentioned "shear yield stress immediately before the application of the magnetic field," which refers to the minimum value measured in the period from the first application of the magnetic field to 5 seconds before that (the period from 5 seconds before the first application of the magnetic field to the moment of the first application of the magnetic field). On the other hand, the above-mentioned "maximum shear yield stress" refers to the maximum value of the shear yield stress measured during 30 or 60 repetitions of the application and removal of the magnetic field.

[0169] 6.2. Evaluation of long-term stability For the magnetorheological fluids of each Example and Comparative Example, the application and removal of a magnetic field was repeated 100 times. The maximum shear yield stress after 100 repetitions was calculated as a multiple of the shear yield stress immediately before the magnetic field was applied. The calculated multiple was then evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2.

[0170] A: The multiple is less than 2.0. B: The multiple is 2.0 or more and less than 4.0. C: The ratio is 4.0 to less than 6.0. D: The ratio is 6.0 to less than 12.0. E: The multiple is 12.0 or more.

[0171] [Table 1]

[0172] [Table 2]

[0173] As is clear from Table 2, the magnetorheological fluids of each example exhibited a stable range of viscosity change even when a magnetic field was repeatedly applied and removed over a long period of time, and as a result, it was found that the range of change in shear yield stress was also stable.

[0174] Therefore, it was found that the present invention can realize a magnetorheological fluid in which dispersoids are well redispersed and exhibit stable properties even after a magnetic field is applied and then removed. [Explanation of symbols]

[0175] 1...Magnetic rheological fluid, 2...Magnetic metal particles, 3...Additive, 4...Dispersion medium, 5...Dispersoid, 21...Particle body, 22...Oxide film, 23...Surface modification film, 100...Vibration damping device, 200...Cylinder, 200a...Rod side chamber, 200b...Piston side chamber, 210...Upper portion, 220...Outer cylinder, 230...Inner cylinder, 231...Orifice, 240...Base valve, 241...Orifice, 250...First reservoir chamber, 260...Second reservoir chamber, 300...Piston, 310...Piston rod, 320...Orifice, 330...Orifice, 340...Valve body, 400...Coil

Claims

1. A dispersoid containing magnetic metal particles; A liquid dispersion medium; having The coercive force of the dispersoid is 796 [A / m] or less (10 [Oe] or less), The thickness of the supernatant layer generated when the sample is accommodated in a cylindrical container and accelerated such that the product of acceleration and time is 690 km / s is tA. When a magnetic field is applied to the sample contained in the cylindrical container and then the acceleration is applied, the thickness of the supernatant layer generated is defined as tB. A magnetorheological fluid characterized in that the rate of change |tA-tB| / tA is 10% or less.

2. 2. The magnetorheological fluid according to claim 1, wherein the average particle size of the magnetic metal particles is 0.05 μm or more and 9.0 μm or less.

3. The magnetorheological fluid according to claim 1 , wherein the magnetic metal particles comprise an Fe-based metallic material.

4. 4. The magnetorheological fluid according to claim 3, wherein the Fe-based metallic material is an amorphous metallic material or a microcrystalline metallic material.

5. The Fe-based metallic material is Fe is the main component, The Si content is 1.0 atomic % or more and 20.0 atomic % or less, 5. The magnetorheological fluid according to claim 3, wherein the saturation magnetization of the magnetic metal particles is from 50 emu / g to 250 emu / g.

6. The magnetic metal particles are A particle body; 5. The magnetorheological fluid according to claim 1, further comprising an oxide film provided on the surface of the particle body.

7. 5. The magnetorheological fluid according to claim 1, further comprising a coating formed on the surface of said magnetic metal particles and comprising a compound derived from a coupling agent.

8. 5. The magnetorheological fluid according to claim 1, wherein the average circularity of the magnetic metal particles is 0.78 or more and 1.00 or less.

9. 5. The magnetorheological fluid according to claim 1, wherein the dispersoid contains solid particles made of a non-magnetic material.

10. 10. The magnetorheological fluid according to claim 9, wherein the content of the solid particles in the entirety is 0.5% by mass or more and 3.0% by mass or less.

11. A magnetorheological fluid according to any one of claims 1 to 4, A container for storing the magnetorheological fluid; a magnetic field generating unit that generates a magnetic field acting on the magnetorheological fluid stored in the container; A vibration damping device comprising:

Citation Information

Patent Citations

  • Magnetic viscous fluid

    JP1998032114A