Covering material, and coating layer formation method
A coating material with a specific binder composition forms a stable carbonized heat insulating layer, addressing shrinkage and peeling issues, providing enhanced heat-resistant protection by maintaining adhesion to the base material at high temperatures.
Patent Information
- Application Number
- JP2023054975
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing coating materials form carbonized heat insulating layers that suffer from shrinkage or peeling when exposed to high temperatures, compromising their heat-resistant protection performance.
A coating material comprising a binder with a copolymer resin of a vinyl alkyl monomer and a resin different from it, along with components like polyol and isocyanate, forms a stable carbonized heat insulating layer with excellent adhesion to the base material, even at high temperatures.
The coating material maintains excellent adhesion and forms a stable carbonized heat insulating layer, ensuring superior heat-resistant protection by foaming and adhering to the base material, even at temperatures above 200°C.
Smart Images

Figure 2024142706000001 
Figure 2024142706000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel coating material and a method for forming a coating. [Background technology]
[0002] For the purpose of protecting substrates such as steel, concrete, wood, and synthetic resin from fire, various coating materials have been proposed that foam when the temperature rises during a fire or the like, forming a carbonized insulating layer. Known coating materials include synthetic resins mixed with foaming agents, carbonizing agents, flame retardants, etc. The heat-resistant protective performance of such coating materials is often determined by the coating thickness, and in order to obtain the desired heat-resistant protective performance, it is important to apply the coating uniformly at a specified thickness, and in particular, the selection of the synthetic resin is important.
[0003] For example, Patent Document 1 describes a synthetic resin obtained from a specific ethylenically unsaturated monomer as the resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special table 2019-522701 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when using a resin such as that in Patent Document 1 above, there is a risk that problems may arise, such as the carbonized insulation layer (foam layer) shrinking when the temperature rises or the carbonized insulation layer peeling off from the substrate, and there is still room for improvement in order to obtain the desired heat resistance protection performance. The present invention has been made in consideration of these problems, and aims to provide a coating material that foams when the temperature rises to form an excellent carbonized insulation layer, has excellent adhesion between the substrate and the carbonized insulation layer, and can form a stable carbonized insulation layer, thereby ensuring excellent heat-resistant protective performance. [Means for solving the problem]
[0006] In order to solve these problems, the present inventors conducted extensive research and discovered that by using, as a binder, a copolymer resin (A) of a vinyl monomer group containing an alkyl acid vinyl monomer (a1) and a resin (B) different from the copolymer resin (A), it is possible to ensure excellent adhesion between the substrate and the carbonized insulation layer even when the temperature rises, and excellent heat-resistant protective performance, thereby completing the present invention.
[0007] That is, the present invention has the following features. 1. A coating material that forms a carbonized heat insulating layer at temperatures of 200°C or higher. The coating material includes a binder and a heat resistance imparting component, The coating material is characterized in that the binder contains a copolymer resin (A) of a vinyl monomer group containing an alkyl acid vinyl monomer (a1) and a resin (B) different from the copolymer resin (A). 2. The coating material according to 1., wherein the resin (B) contains a polyol (b1) and an isocyanate (b2). 3. A coating material that forms a carbonized heat insulating layer at temperatures of 200°C or higher, The coating material is characterized by having a base material containing a copolymer resin (A) of a vinyl monomer group containing an alkyl acid vinyl monomer (a1), a polyol (b1) and a heat resistance imparting powder, and a curing agent containing an isocyanate (b2). 4. The coating material according to claim 3, wherein the base agent further contains a water absorbing agent. 5. The coating material according to 1. or 3., wherein the copolymer resin (A) is a copolymer resin of a vinyl monomer group including an alkyl acid vinyl monomer (a1) and an aromatic-containing vinyl monomer (a2). 6. The coating material according to 1. or 3., wherein the copolymer resin (A) is a copolymer resin of a vinyl monomer group containing 3% by weight or more and less than 60% by weight of an alkyl acid vinyl monomer (a1). 7. The coating material according to 1 or 3, wherein the heat resistance imparting component includes at least one selected from the group consisting of a foaming agent, a carbonizing agent, a flame retardant, and a filler. 8. A coating forming method for forming a coating by applying a coating material to a substrate, comprising the steps of: The coating material is a coating material according to any one of 1. to 4., 9. A coating forming method for forming a coating by applying a coating material to a substrate, comprising the steps of: The coating material is the coating material according to any one of 1. to 4., and is applied in one or more recoating steps, and the dry film thickness per step is 300 μm or more. Effect of the Invention
[0008] The coating material of the present invention foams when the temperature rises to form an excellent carbonized heat insulating layer, and has excellent adhesion between the substrate and the carbonized heat insulating layer, ensuring excellent heat-resistant protective performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below based on the embodiments.
[0010] The present invention relates to a coating material whose coating forms a carbonized insulating layer at a temperature of 200°C or higher, and the coating material comprises a binder and a heat resistance-imparting powder, and is characterized in that the binder contains a copolymer resin (A) (hereinafter also referred to as "component (A)") of a vinyl monomer group containing alkyl acid vinyl monomer (a1) (hereinafter also referred to as "component (a1)"), and a resin (B) (hereinafter also referred to as "component (B)") different from component (A). The coating formed by the coating material of the present invention has excellent foaming properties at temperatures of 200° C. or higher (preferably 250° C. or higher), and can improve the heat-resistant protective performance of the substrate by forming a carbonized insulating layer.
[0011] The present invention contains components (A) and (B) as binders, which foam when the temperature rises to form an excellent carbonized insulation layer, and which also has excellent adhesion between the substrate and the carbonized insulation layer, allowing the formation of a stable carbonized insulation layer and ensuring excellent heat resistance protection performance. Although the details of the manifestation of such an effect are unknown, when the temperature starts to rise, the (a1) component segment in the (A) component is thermally decomposed from the alkyl acid-derived side chain segment, and is detached from the main chain, increasing the acidity, while the main chain structure of the (A) component is maintained, and it is easy to form a state that is easy to foam while maintaining adhesion to the substrate. Furthermore, by including a (B) component different from the (A) component, it has a different thermal decomposition temperature, carbonization formation speed, etc. from the (A) component, and as a result, it is thought that the carbonized insulation layer formed by foaming can be made strong. In other words, by including the (A) component and the (B) component, it is thought that it is possible to foam and form an excellent carbonized insulation layer, and to ensure excellent adhesion between the substrate and the carbonized insulation layer, and excellent heat resistance protection performance.
[0012] The component (A) of the present invention is a copolymer resin of a vinyl monomer group containing the component (a1) and, if necessary, other vinyl monomers.
[0013] Examples of the component (a1) include vinyl versatate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl palmitate, vinyl stearate, vinyl 2-ethylhexanoate, vinyl pivalate, vinyl crotonate, and vinyl benzoate, and one or more of these can be used. In the present invention, it is particularly preferable that the vinyl ester compound contains at least one selected from vinyl versatate, vinyl acetate, and vinyl 2-ethylhexanoate.
[0014] The other vinyl monomers are not particularly limited, but include, for example, Aromatic-containing vinyl monomers such as styrene, α-methylstyrene, 2-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 2,4,6-trimethylstyrene, monofluorostyrene, difluorostyrene, monochlorostyrene, dichlorostyrene, methoxystyrene, t-butoxystyrene, 1-vinylnaphthalene, and 2-vinylnaphthalene; Hydroxyalkyl vinyl ethers such as hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, and hydroxypentyl vinyl ether; hydroxyallyl ethers such as ethylene glycol monoallyl ether, diethylene glycol monoallyl ether, and triethylene glycol monoallyl ether; hydroxyl group-containing vinyl monomers such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 4-hydroxyethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; Carboxyl group-containing vinyl monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, salicylic acid, and cinnamic acid; silyl group-containing vinyl monomers such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri-n-butoxysilane, vinyltris(β-methoxyethoxy)silane, allyltrimethoxysilane, trimethoxysilylethyl vinyl ether, triethoxysilylethyl vinyl ether, trimethoxysilylpropyl vinyl ether, triethoxysilylpropyl vinyl ether, γ-(meth)acryloyloxypropyl trimethoxysilane, γ-(meth)acryloyloxypropyl triethoxysilane, γ-(meth)acryloyloxypropyl methyldimethoxysilane, vinylmethyldimethoxysilane, methyldimethoxysilylethyl vinyl ether, and methyldimethoxysilylpropyl vinyl ether; Amino group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate and dimethylaminopropyl (meth)acrylate; Amide group-containing vinyl monomers such as (meth)acrylamide and ethyl(meth)acrylamide; carbonyl group-containing vinyl monomers such as diacetone acrylamide; Nitrile group-containing vinyl monomers such as acrylonitrile, glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate; Sulfonic acid-containing vinyl monomers such as vinyl sulfonic acid, Chlorine-containing vinyl monomers such as vinyl chloride, vinylidene chloride, and chloroprene; Fluorine-containing vinyl monomers such as perfluoromethyl methacrylate, perfluoroisononylmethyl methacrylate, 2-perfluorooctylethyl acrylate, 2-perfluorooctylethyl methacrylate, trifluoroethyl acrylate, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, vinyl fluoride, and vinylidene fluoride. Vinyl monomers such as ethylene, propylene, and isobutylene Methyl acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, t-pentyl (meth)acrylate, 1-ethylpropyl (meth)acrylate, 2-methylbutyl (meth)acrylate, 3-methylbutyl (meth)acrylate, (meth)acrylic acid alkyl (meth)acrylates such as n-hexyl acrylate, cyclohexyl acrylate, 2-ethylbutyl (meth)acrylate, 2-methylpentyl (meth)acrylate, 4-methylpentyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl methacrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, and n-lauryl (meth)acrylate; etc., and one or more of these can be used.
[0015] The component (A) of the present invention can be produced using the component (a1) and, if necessary, other vinyl monomers as described above, by a known vinyl polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, slurry polymerization, or dispersion polymerization. The form of the resin is not particularly limited, and can be appropriately set and used as a solvent-soluble resin, a solvent-dispersed resin, a solventless resin, a powder resin, etc. The powder resin can be used, for example, by dissolving and / or dispersing it in a solvent or the like described below.
[0016] The mixing ratio of the (a1) component in the (A) component is preferably 3% by weight or more and less than 60% by weight, further preferably 5% by weight or more and 55% by weight or less, and even further preferably 7% by weight or more and 51% by weight or less, based on the total amount of vinyl monomers used in the production of the (A) component. By being in this range, when the temperature rises, it foams to form an excellent carbonized insulation layer, and the adhesion between the substrate and the carbonized insulation layer is excellent, so a stable carbonized insulation layer can be formed, and excellent heat resistance protection performance can be ensured. The other vinyl monomers preferably include aromatic-containing vinyl monomers. By including an aromatic vinyl monomer, the foamed shape is easily maintained when the temperature rises, and an excellent carbonized heat insulating layer can be formed. The mixing ratio of the aromatic-containing vinyl monomer is preferably 40% by weight or more and 97% by weight or less, more preferably 45% by weight or more and 95% by weight or less, and even more preferably 49% by weight or more and 93% by weight or less, based on the total amount of vinyl monomers used in producing component (A). In addition, when a vinyl monomer other than the aromatic-containing vinyl monomer (a1) is used, the amount of the vinyl monomer is preferably 0% by weight or more and less than 30% by weight, more preferably 0% by weight or more and less than 20% by weight, and even more preferably 0% by weight or more and less than 10% by weight, based on the total amount of vinyl monomers used in the production of the copolymer resin.
[0017] The mixing amount of the component (A) is preferably from 5% by weight to 40% by weight, and more preferably from 10% by weight to 20% by weight, based on the total amount of the binder.
[0018] Examples of the component (B) of the present invention include vinyl polymer resins that do not contain the component (a1), urethane resins, epoxy resins, silicone resins, and fluororesins. In the present invention, it is particularly preferable to use, as the component (B), a copolymer resin obtained by using the above-mentioned other vinyl monomer group not including the component (a1), and / or a resin containing a polyol (b1) and an isocyanate (b2).
[0019] The vinyl polymer resin not containing the component (a1) is a copolymer resin not containing the component (a1) and obtained by using the above-mentioned other vinyl monomer group, and for example, it is preferable to use a copolymer resin containing an aromatic vinyl monomer as the vinyl monomer. The copolymer resin containing an aromatic vinyl monomer is likely to retain the foamed shape when the temperature rises, and can form an excellent carbonized heat insulating layer.
[0020] The resin containing polyol (b1) and isocyanate (b2) is a resin obtained by reacting polyol (b1) and isocyanate (b2). It may be a resin obtained by reacting polyol (b1) with isocyanate (b2) in advance, or it may be a resin obtained by reacting polyol (b1) with isocyanate (b2) after application to form the resin. In such a resin, even when the softening and foaming of the component (A) has progressed to a certain extent during temperature rise, the polyol-isocyanate bond remains, and therefore, in the initial stage of temperature rise, the formation of the carbonized heat insulation layer proceeds with the polyol-isocyanate bond remaining. Therefore, it is possible to suppress the decrease in adhesion and strength of the carbonized heat insulation layer caused by the softening of the component (A) in the initial stage of temperature rise, and an excellent carbonized heat insulation layer can be effectively formed.
[0021] Examples of the polyol (b1) include polyether polyol, fluorine-containing polyol, polyester polyol, acrylic polyol, epoxy-containing polyol, silicone-containing polyol, castor oil, castor oil-modified polyol, polycarbonate polyol, polylactone polyol, polybutadiene polyol, polypentadiene polyol, etc., and one or more selected from these can be used. In the present invention, it is particularly preferable to use polyether polyol and / or fluorine-containing polyol.
[0022] The molecular weight of the polyether polyol is preferably 1000 or more (more preferably 3000 to 20000, even more preferably 5000 to 18000, particularly preferably 6000 to 15000, and most preferably 6500 to 12000). By including such a polyether polyol as the polyol, the coating exhibits excellent foaming properties due to the temperature rise of the coating (preferably the coating surface temperature is 200° C. or more, more preferably 250° C. or more), and the heat-resistant protection performance of the substrate can be improved. In the present invention, the molecular weight of the polyol is a number average molecular weight (Mn), which is a so-called polystyrene-equivalent molecular weight determined by gel permeation chromatography using a polystyrene polymer as a reference.
[0023] Polyether polyols can be obtained, for example, by addition polymerization of polyhydric alcohols such as trimethylolpropane, glycerin, hexanetriol, pentaerythritol derivatives, sorbitol, and neopentyl glycol with alkylene oxides such as ethylene oxide and propylene oxide. In the present invention, a polymer obtained by addition polymerization of the above polyhydric alcohols with ethylene oxide and / or propylene oxide is preferred, and one having ethylene oxide and / or propylene oxide added to the terminal is more preferred. Furthermore, the above polyether polyol preferably contains a polyether polyol having three or more functional groups having active hydrogen atoms (functional group number 3 or more). In this case, the curability is excellent and a coating can be stably formed, so that the effect of the present invention is easily obtained. A hydroxyl group is preferred as the functional group having an active hydrogen atom.
[0024] The hydroxyl value (solid content) of the polyether polyol is preferably 3 to 150 mgKOH / g (more preferably 5 to 100 mgKOH / g, even more preferably 7 to 40 mgKOH / g, and most preferably 10 to 30 mgKOH / g). By using such a polyether polyol, more excellent foaming properties can be exhibited, and the heat-resistant protection performance of the substrate can be improved. In the present invention, the hydroxyl value is a value (mgKOH / g) represented by the number of mg of potassium hydroxide equivalent to the moles of hydroxyl groups contained in 1 g of solid content, and "α to β" is synonymous with "α or more and β or less".
[0025] The content of the polyether polyol is preferably 50% by weight or more and 100% by weight or less (more preferably 60 to 99% by weight, and even more preferably 70 to 98% by weight) based on the total amount of the polyol.
[0026] Fluorine-containing polyols are preferably used because they have excellent foaming properties when the temperature of the coating is increased (preferably when the coating surface temperature is 200°C or higher, and more preferably 250°C or higher), and they can form a stable carbonized insulation layer by suppressing incineration, shrinkage, etc. of the carbonized insulation layer, and can enhance the heat-resistant protection of the substrate.
[0027] The fluorine-containing polyol is not particularly limited, but is, for example, one obtained by copolymerizing a fluorine-containing monomer such as a fluoroolefin monomer or a fluoroalkyl group-containing acrylic monomer, a hydroxyl group-containing vinyl monomer, and, if necessary, other polymerizable monomers. Examples of the fluoroolefin monomer include perfluoroolefins such as tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene, vinyl fluoride, and vinylidene fluoride. Examples of fluoroalkyl group-containing acrylic monomers include perfluoromethyl methacrylate, perfluoroisononylmethyl methacrylate, 2-perfluorooctylethyl acrylate, 2-perfluorooctylethyl methacrylate, trifluoroethyl acrylate, etc. These can be used alone or in combination of two or more. In the present invention, it is preferable to use one or more selected from tetrafluoroethylene and chlorotrifluoroethylene, and more preferably chlorotrifluoroethylene. As the hydroxyl group-containing vinyl monomer, the above-mentioned hydroxyl group-containing vinyl monomers can be mentioned, and one or more of these can be used. The other polymerizable monomers include the above-mentioned vinyl monomers excluding the above-mentioned hydroxyl group-containing vinyl monomers, and one or more of these can be used.
[0028] As for such a fluorine-containing polyol, the fluorine content in the fluorine-containing polyol solid content is preferably 10 to 50% by weight (more preferably 15 to 40% by weight, and further preferably 20 to 35% by weight). In addition, the hydroxyl value (solid content) is preferably 5 to 100 mgKOH / g (more preferably 10 to 80 mgKOH / g). Furthermore, the molecular weight [number average molecular weight (Mn)] is preferably 5,000 to 100,000 (more preferably 8,000 to 60,000). By including such a fluorine-containing polyol, in the event of a temperature rise due to a fire or the like, the coating exhibits excellent foaming properties and forms a carbonized heat insulating layer, and incineration and shrinkage can be suppressed even in a high-temperature atmosphere, thereby improving the heat-resistant protection performance of the substrate. In addition, the exothermic peak of the coating can be shifted to the high-temperature side, the flame retardancy of the coating can be increased, and decomposition at temperatures below 200°C can be suppressed, and it is considered that the effects of the present invention can be fully exhibited.
[0029] The content of the fluorine-containing polyol is preferably 0.1 to 30% by weight (more preferably 0.5 to 20% by weight, and even more preferably 1 to 10% by weight) in terms of solid content relative to the total amount of polyol. By satisfying this range, the heat-resistant protective performance of the substrate can be improved and the adhesion with the topcoat material can be sufficiently ensured.
[0030] The polyols used in the present invention are preferably liquid at 20°C, and each of them preferably has a viscosity of 0.05 to 100 Pa·s (more preferably 0.1 to 50 Pa·s). This makes it easier to obtain the effects of the present invention. The viscosity of the polyol component is the viscosity at 20 rpm (index value at the fifth rotation) measured with a BH type viscometer at a temperature of 20°C.
[0031] The isocyanate (b2) is one having two or more NCO groups in one molecule, and examples thereof include toluene diisocyanate (TDI), 4,4-diphenylmethane diisocyanate (pure-MDI), polymeric MDI, xylylene diisocyanate (XDI), hexamethylene diisocyanate (HMDI), isophorone diisocyanate (IPDI), hydrogenated XDI, hydrogenated MDI, and the like, or derivatives thereof obtained by allophanating, biureting, dimerizing (uretdione), trimerizing (isocyanurating), adducting, or carbodiimiding them; and blocked isocyanates obtained by blocking these with alcohols, phenols, ε-caprolactam, oximes, active methylene compounds, or the like. One or more selected from these can be used.
[0032] In the present invention, it is particularly preferable that the isocyanate (b2) contains hexamethylene diisocyanate (HMDI) and / or its derivatives (hereinafter also referred to as "HMDIs"). The content of the HMDIs is preferably 90% by weight or more (more preferably 95% by weight or more) based on the total amount of isocyanate. In addition, an embodiment in which the isocyanate consists only of HMDIs is also preferable. In addition, as the derivative, a biuret and / or an isocyanurate is preferable. In such a case, the formed coating has excellent curing properties, and exhibits better foaming properties when the temperature rises, thereby improving the heat resistance protection of the substrate.
[0033] In the present invention, it is preferable that the isocyanate (b2) has an isocyanate group content of 10% by weight or more (preferably 15% by weight or more and 30% by weight or less) in the solid content. In such a case, the formed coating can exhibit excellent curing effect, and a stable coating can be formed. In the present invention, the isocyanate group content is defined as the content (wt%) of isocyanate groups contained in the solid content of the isocyanate compound, and is a value obtained by back titration with hydrochloric acid after neutralizing the isocyanate groups with an excess amine.
[0034] In the present invention, the mixing ratio of polyol (b1) and isocyanate (b2) is preferably 1 or more (preferably 1.2 to 3.5, more preferably 1.5 to 3.0) in terms of NCO / OH equivalent ratio. In such a case, regardless of the coating environment, a coating film having excellent curability and a uniform thickness of a desired thickness can be formed. In addition, when the coating material is applied in layers, the coating film has excellent adhesion between layers and can stably form a thick film. Furthermore, the formed coating film has excellent foaming properties in the event of a temperature rise due to a fire or the like, and can form a stable carbonized insulation layer to enhance the heat-resistant protection performance of the substrate. Furthermore, the formed coating film has excellent durability (for example, waterproofness, water permeability resistance, crack resistance, base following ability, etc.), can maintain the initial appearance (beauty) for a long period of time, and can fully exert the effects of the present invention in the event of a temperature rise due to a fire or the like.
[0035] The mixing amount of the component (B) is preferably from 60% by weight to 95% by weight, and more preferably from 80% by weight to 90% by weight, based on the total amount of the binder. When the component (B) is a resin containing a polyol (b1) and an isocyanate (b2), the amount is calculated based on the total amount of the polyol (b1) and the isocyanate (b2).
[0036] In the present invention, a curing catalyst that promotes the reaction between polyol (b1) and isocyanate (b2) can be used in combination. A curing catalyst is a substance that promotes the reaction and curing of isocyanate groups. Examples of the curing catalyst include various types of amine catalysts, organometallic catalysts, and inorganic catalysts. Examples of the amine catalyst include ethylenediamine, triethylenediamine, triethylamine, ethanolamine, diethanolamine, and hexamethylenediamine, or their derivatives or mixtures with solvents. Examples of the organometallic catalyst include organometallic compounds such as dibutyltin dilaurate and dibutyltin diacetate; and organometallic salts such as potassium acetate, zinc stearate, calcium stearate, lead stearate, aluminum stearate, and tin octylate. Examples of the inorganic catalyst include tin chloride. These can be used alone or in combination, and can also be used by mixing with a solvent. In the present invention, it is particularly preferable to include an organometallic catalyst. In this case, the curing is accelerated and the curability of the film-forming component is increased, thereby enhancing the effects of the present invention. The content of the curing catalyst is preferably 0.01 to 3 parts by weight (more preferably 0.05 to 2.5 parts by weight) relative to 100 parts by weight of the solid content of the polyol.
[0037] The coating formed from the binder has an exothermic peak in differential thermal analysis (DTA), and the exothermic peak preferably has a maximum value in the temperature range of 200 to 400° C. (more preferably 250 to 380° C.) In such a case, when the temperature rises due to a fire or the like, the foaming property is further improved, and it is possible to form an excellent carbonized heat insulating layer, thereby improving the heat-resistant protection of the substrate.
[0038] In the present invention, the differential thermal analysis of the coating was performed using a differential thermal analyzer (for example, a "Differential Thermobalance Thermo plus EVO2 TG-DTA Series" manufactured by Rigaku Corporation), in which 3±1 mg of sample was placed in a platinum sample pan, α-alumina was used as a standard substance, and the temperature was increased at a rate of 20°C / min from 100 to 900°C.
[0039] In the coating material of the present invention, the heat resistance imparting powder is a component that forms a carbonized heat insulating layer by interacting with the binder (e.g., at least one of a dehydrating and cooling effect, a non-flammable gas generating effect, a carbonization promotion effect, a carbonized heat insulating layer forming effect, etc.) when the temperature rises during a fire, etc. The heat resistance imparting powder preferably contains, for example, one or more selected from a foaming agent, a carbonizing agent, a flame retardant, a filler, etc.
[0040] The foaming agent imparts a foaming action to the coating due to a temperature rise during a fire or the like, and specifically imparts a foaming action when the temperature of the coating surface is preferably 200° C. or higher. Examples of the foaming agent include melamine and its derivatives, dicyandiamide and its derivatives, azobistetrazole and its derivatives, azodicarbonamide, urea, and thiourea. These can be used alone or in combination of two or more. The content of the foaming agent is preferably 10 to 200 parts by weight (more preferably 20 to 150 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0041] The carbonizing agent is one that, due to a temperature rise during a fire or the like, carbonizes the coating and dehydrates and carbonizes to form a carbonized heat insulating layer. Examples of carbonizing agents include pentaerythritol, dipentaerythritol, trimethylolpropane, starch, casein, and tris(2-hydroxyethyl)isocyanurate. These can be used alone or in combination of two or more. In the present invention, pentaerythritol and dipentaerythritol are particularly preferred because they are excellent in dehydration and cooling effects and in forming a carbonized heat insulating layer. The content of the carbonizing agent is preferably 10 to 200 parts by weight (more preferably 20 to 120 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0042] Examples of the flame retardant include organic phosphorus compounds such as tricresyl phosphate and diphenyl cresyl phosphate; chlorine compounds such as chlorinated polyphenyl, chlorinated polyethylene, diphenyl chloride, triphenyl chloride, chlorinated paraffin, pentachlorinated fatty acid ester, perchloropentacyclodecane, chlorinated naphthalene, and tetrachlorophthalic anhydride; antimony compounds such as antimony trioxide and antimony pentachloride; phosphorus compounds such as phosphorus trichloride, phosphorus pentachloride, ammonium phosphate, ammonium polyphosphate, melamine phosphate, melamine polyphosphate, melam polyphosphate, melem polyphosphate, boron phosphate, boron polyphosphate, aluminum phosphate, and aluminum polyphosphate; and inorganic compounds such as zinc borate and sodium borate. These can be used alone or in combination of two or more. In the present invention, the flame retardant preferably contains at least one phosphorus compound selected from, for example, melamine polyphosphate, melam polyphosphate, a melamine-melam-melem double salt, or a complex compound of a melamine-melam-melem double salt of polyphosphate and dimelam pyrosulfate, and further preferably contains these in combination with ammonium polyphosphate. The content of the flame retardant is preferably 30 to 800 parts by weight (more preferably 50 to 500 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0043] Examples of the filler include talc, calcium carbonate, sodium carbonate, aluminum oxide, titanium oxide, zinc oxide, silica, clay, siliceous sand, mica, silica sand, silica powder, quartz powder, barium sulfate, etc. These can be used alone or in combination of two or more. The content of the filler is preferably 3 to 200 parts by weight (more preferably 5 to 150 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0044] Furthermore, in the present invention, in addition to the above components, metal hydrates, fibers, etc. can also be included. Metal hydrates exhibit endothermic properties due to dehydration reactions, etc., when the temperature rises, and are different from the above fillers. Examples of such metal hydrates include aluminum hydroxide and magnesium hydroxide. These can be used alone or in combination of two or more. The average particle size of the metal hydrate is preferably 0.1 to 20 μm (more preferably 0.2 to 15 μm, even more preferably 0.3 to 8 μm, and most preferably 0.4 to 3 μm). The content of the metal hydrate is preferably 0.1 to 50 parts by weight (more preferably 0.2 to 30 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0045] In the present invention, it is preferable to use a filler and a metal hydrate in combination, and in this case, the content of the metal hydrate is preferably 0.1 to 20% by weight (more preferably 0.3 to 15% by weight, and even more preferably 0.5 to 10% by weight) relative to the filler. In this case, the foamability, particularly the shrinkage of the carbonized insulation layer at high temperatures, can be suppressed, and a stable carbonized insulation layer can be formed, thereby enhancing the effects of the present invention. The average particle size is measured by a laser diffraction particle size distribution analyzer.
[0046] The fibers can improve the coating thickness and suppress cracking of the coating. In addition, the fibers can prevent the coating from sagging during a temperature rise due to a fire or the like, and can also improve the thermal conductivity inside the coating. As a result, the fibers exhibit excellent foaming properties, form a uniform carbonized heat insulating layer, and improve the heat-resistant protection performance of the substrate. Examples of such fibers include organic fibers such as acrylic fibers, acetate fibers, aramid fibers, cuprammonium fibers (cupra), nylon fibers, novoloid fibers, pulp fibers, viscose rayon, vinylidene fibers, polyester fibers, polyethylene fibers, polyvinyl chloride fibers, polychlar fibers, boronosic fibers, polypropylene fibers, and cellulose fibers, and inorganic fibers such as carbon fibers, rock wool fibers, glass fibers, silica fibers, alumina fibers, silica-alumina fibers, slag wool fibers, ceramic fibers, carbon fibers, and silicon carbide fibers. These can be used alone or in combination of two or more.
[0047] In the present invention, it is preferable that the fibers contain inorganic fibers, and among them, artificial mineral fibers such as rock wool fibers, slag wool fibers, glass fibers, and ceramic fibers are preferable. This can further suppress cracking of the coating. Furthermore, when the temperature rises due to a fire or the like, it is possible to make it difficult for the coating to sag, and to further increase the thermal conductivity inside the coating. As a result, it is possible to form a carbonized insulation layer that exhibits uniform and excellent foaming properties even to the inside (core) of the coating, and has a uniform and excellent strength, and to further improve the heat-resistant protection performance of the substrate.
[0048] The size of the fibers (fiber length and fiber diameter) may be set according to the performance of the coating material, the specifications of the substrate to which it is applied, the application tool, etc., and the average fiber length is preferably within the range of 10 to 1000 μm (more preferably 15 to 800 μm, and even more preferably 20 to 600 μm), and the average fiber diameter is preferably within the range of 0.5 to 10 μm (more preferably 1 to 8 μm). The aspect ratio (fiber length / fiber diameter) is preferably 3 to 300 (more preferably 5 to 200). When the above range is satisfied, the coating is more easily applied, the coating is less likely to crack, and the coating is less likely to drip when the temperature rises due to a fire, etc., and a stable carbonized heat insulating layer can be formed. The content of the fibers is preferably 0.5 to 30 parts by weight (more preferably 1 to 25 parts by weight, and even more preferably 2 to 20 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0049] The coating material of the present invention preferably contains a water absorbing agent. In particular, when a resin containing a polyol (b1) and an isocyanate (b2) is used as the component (B), it is preferable that the coating material contains a water absorbing agent. The water absorbing agent imparts the function of absorbing moisture in the coating material and / or in the air. The moisture in the coating material and / or in the air is particularly likely to react with the above-mentioned isocyanate (b2). Therefore, the coating material is easily affected by the moisture in the air during the coating method and coating environment, particularly when the coating material is spray-coated or coated (film-formed) under high humidity (even in rainy weather or under high temperature and humidity), and the reaction between the isocyanate and the polyol is inhibited, and the curing property (curing speed, coating strength, etc.) and adhesion to the substrate are reduced, and as a result, sufficient heat resistance protection may not be obtained. In the present invention, the water absorbing agent is blended to absorb the moisture in the coating material or in the air, so that the curing property and adhesion to the substrate can be sufficiently secured regardless of the coating method and coating environment, and a thick film can be stably formed.
[0050] The water absorbing agent is not particularly limited as long as it has the above-mentioned effect, and for example, a water binding agent and a dehydrating agent can be used. These can be used alone or in combination of two or more. The water absorbing agent can be in any form, such as pellets, powder, liquid, or paste. In the present invention, pellets and powder are preferred.
[0051] The water binding agent has the effect of removing water from the coating material and / or the air by reacting with water. Examples of such water binding agents include alkyl orthoformates such as methyl orthoformate, ethyl orthoformate, trimethyl orthoformate, triethyl orthoformate, and tributyl orthoformate; trialkyl orthoacetates such as trimethyl orthoacetate, triethyl orthoacetate, and tributyl orthoacetate; trialkyl orthoborates such as trimethyl orthoborate, triethyl orthoborate, and tributyl orthoborate; monoisocyanate compounds such as phenyl isocyanate, p-chlorophenyl isocyanate, benzene Examples of the suitable silanes include monoisocyanate compounds such as toluenesulfonyl isocyanate, p-toluenesulfonyl isocyanate, and isocyanate ethyl methacrylate; alkoxysilanes such as tetraethoxysilane, tetrabutoxysilane, tetraphenoxysilane, tetrakis(2-ethoxybutoxy)silane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, and diphenyldiethoxysilane; and acid anhydrides such as maleic anhydride and phthalic anhydride.
[0052] The dehydrating agent has the function of removing water from the coating material and / or the air by absorbing water as crystal water, adsorbed water, etc. (water adsorption). Furthermore, the dehydrating agent can improve heat-resistant protection because it can dehydrate adsorbed water when the temperature rises (at high temperatures). Examples of such dehydrating agents include silica gel, synthetic zeolite, natural zeolite, synthetic clay, activated alumina, calcium oxide, magnesium sulfate, sodium sulfate, gypsum hemihydrate, anhydrous gypsum, crystalline gypsum, cement, activated carbon, and partially cross-linked acrylic acid polymers (polymer water absorbents).
[0053] In the present invention, the above-mentioned dehydrating agent is preferred as the water absorbing agent. Among them, porous inorganic particles such as silica gel, synthetic zeolite, natural zeolite, and activated alumina are preferred, and the form thereof is preferably in powder form. In particular, powdered synthetic zeolite is preferred in the present invention. The types of synthetic zeolite include A-type, X-type, Y-type, L-type, mordenite type, and chabazide type, and A-type zeolite is preferred in the present invention. In addition, the average pore size of the porous inorganic particles may be larger than the molecular diameter of water molecules (about 2.3 to 3.9 Å), and is preferably 2.3 to 30 Å (more preferably 2.5 to 10 Å, even more preferably 3 to 8 Å, and particularly preferably 3.5 to 5 Å). In this case, the water adsorption is excellent, and the curing properties of the polyol and isocyanate are excellent, and the curing speed and the hardness of the coating can be increased. In addition, it has excellent adhesion to the substrate, can form a uniform coating, and can fully exert the effect of maintaining the heat-resistant protective performance of the substrate without inhibiting the foaming property of the coating (does not adsorb non-flammable gases, etc.) in the event of a temperature rise due to a fire, etc. The average pore size of the porous inorganic particles can be measured, for example, by nitrogen adsorption measurement.
[0054] When the water absorbing agent is in a powder form, the average particle size is preferably 30 to 500 μm (more preferably 40 to 400 μm, and further preferably 50 to 300 μm).
[0055] The content of the water absorbing agent is preferably 0.5 to 50 parts by weight (more preferably 1 to 50 parts by weight, and further preferably 1.5 to 30 parts by weight) relative to 100 parts by weight of the solid content of the binder.
[0056] Other additives may be used as long as they do not significantly impair the effects of the present invention, and examples thereof include pigments, wetting agents, plasticizers, lubricants, preservatives, antifungal agents, anti-algae agents, antibacterial agents, thickeners, leveling agents, dispersants, defoamers, crosslinking agents, silane coupling agents, UV absorbers, light stabilizers, antioxidants, halogen scavengers, diluting solvents, absorbents, dehydrating agents, solvents, etc.
[0057] Among these, the antioxidant is preferably, for example, a phosphorus-based, sulfur-based, or hindered phenol-based antioxidant. These can be used alone or in combination of two or more. By including such an antioxidant, deterioration of the coating can be suppressed not only under normal conditions but also when the temperature rises due to a fire or the like, and the properties of the carbonized heat insulating layer formed by the temperature rise can be improved.
[0058] Of these, suitable solvents are non-aqueous solvents such as aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, ester solvents, and ketone solvents. Examples of the aliphatic hydrocarbon solvent include n-hexane, n-pentane, n-octane, n-nonane, n-decane, n-undecane, and n-dodecane, as well as terpine oil and mineral spirits. Examples of aromatic hydrocarbon solvents include toluene, xylene, solvent naphtha, 1-phenyl-1-xylylethane, 1-phenyl-1-ethylphenylethane, and mixtures of petroleum resins (polymers of aromatic hydrocarbon fractions having 8 to 10 carbon atoms) and styrylxylene. Examples of the ester solvent include acetate compounds such as ethyl acetate and butyl acetate; Phthalate ester compounds such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, dihexyl phthalate, di-2-ethylhexyl phthalate, diisononyl phthalate, diisodecyl phthalate, diundecyl phthalate, and butyl benzyl phthalate; aliphatic dibasic acid ester compounds such as diethyl adipate, dibutyl adipate, diisobutyl adipate, dihexyl adipate, di-2-ethylhexyl adipate, dioctyl adipate, diisononyl adipate, diisodecyl adipate, bis(butyl diglycol) adipate, diethyl sebacate, dibutyl sebacate, dihexyl sebacate, and di-2-ethylhexyl sebacate; adipic acid-based polyesters such as adipic acid-1,3 butylene glycol-based polyesters and adipic acid-1,2 propylene glycol-based polyesters; maleate compounds such as dimethyl maleate, diethyl maleate, dibutyl maleate, dihexyl maleate, di-2-ethylhexyl maleate, diisononyl maleate, and diisodecyl maleate; phosphate compounds such as triethyl phosphate, tributyl phosphate, tri-2-ethylhexyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate; Trimellitate compounds such as tris-2-ethylhexyl trimellitate; Ricinoleic acid ester compounds such as methyl acetyl ricinoleate, Epoxy ester compounds such as di-2-ethylhexyl epoxyhexahydrophthalate, diepoxystearyl epoxyhexahydrophthalate, epoxidized fatty acid butyl, epoxidized fatty acid 2-ethylhexyl, epoxidized soybean oil, and epoxidized linseed oil; Benzoic acid ester compounds such as benzoic acid glycol esters, Examples of the ketone solvent include methyl ethyl ketone, methyl isobutyl ketone, and γ-butyrolactone. These can be used alone or in combination of two or more.
[0059] In the present invention, the solvent may contain a high-boiling point solvent. The high-boiling point solvent is a high-boiling point liquid compound that is liquid at 20°C and has a boiling point of 100°C or higher (more preferably 150°C or higher, and even more preferably 200°C or higher). By containing such a high-boiling point solvent, the dispersion stability of the heat resistance imparting component and the like can be improved. In addition, a good coating film with excellent adhesion is formed, and in particular, the elasticity of the coating film is improved, and cracks of the coating film and the like can be prevented. Furthermore, when the coating film is exposed to high temperatures due to a fire or the like, it contributes to moderate softening of the coating film, further increasing the foaming property, suppressing the falling off (peeling) of the formed carbonized heat insulating layer, and improving the heat resistance protection performance of the substrate.
[0060] Examples of high boiling point solvents include aromatic hydrocarbon solvents such as 1-phenyl-1-xylylethane, 1-phenyl-1-ethylphenylethane, and a mixture of petroleum resin (aromatic hydrocarbon fraction polymer having 8 to 10 carbon atoms) and styrylxylene, ester solvents such as the above-mentioned phthalate ester compounds, aliphatic dibasic acid ester compounds, adipic acid polyesters, maleic acid ester compounds, phosphate ester compounds, trimellitic acid ester compounds, ricinoleic acid ester compounds, epoxy ester compounds, and benzoic acid ester compounds, and ketone solvents such as γ-butyrolactone, and preferably contains at least one selected from phthalate ester compounds, aliphatic dibasic acid ester compounds, and phosphate ester compounds, and further preferably contains at least one selected from phthalate ester compounds and aliphatic dibasic acid ester compounds having an alkyl group with 4 to 11 carbon atoms (more preferably 5 to 10, and even more preferably 6 to 9). Specific examples thereof include diisononyl phthalate and diisononyl adipate.
[0061] The content of the high boiling point solvent is 150 parts by weight or less (preferably 5 parts by weight or more and 100 parts by weight or less, more preferably 8 parts by weight or more and 80 parts by weight or less) relative to 100 parts by weight of the solid content of the binder. When the above range is satisfied, the dispersibility of the powder component is increased, the thick coating property is excellent, and when the temperature rises due to a fire or the like, the foaming property is excellent, and the effect of maintaining the heat-resistant protective performance of the substrate can be fully exhibited. Furthermore, excellent topcoat material suitability can be obtained.
[0062] The coating material of the present invention has a heating residue of preferably 70 to 98% by weight (more preferably 75 to 95% by weight, and even more preferably 80 to 93% by weight). When the heating residue of the coating material satisfies the above range, excellent thick coating properties and good coating workability can be obtained. As a result, sufficient heat resistance protection can be exhibited. The heating residue of the coating material is a value measured by the method of JIS K 5601-1-2, the heating temperature is 105°C, and the heating time is 60 minutes.
[0063] In the present invention, the viscosity of the coating material is preferably 5 to 70 Pa·s (more preferably 7 to 60 Pa·s, even more preferably 10 to 50 Pa·s, and particularly preferably 15 to 40 Pa·s). When the viscosity of the coating material satisfies the above range, the coating material has excellent workability and thick coating properties, and a uniform coating film can be formed. As a result, sufficient heat-resistant protection can be obtained. The viscosity of the coating material is the viscosity at 20 rpm (guideline value at the fifth rotation) measured with a BH viscometer at a temperature of 23°C immediately after the coating material is prepared (after mixing the base agent and curing agent in the case of a two-component type).
[0064] In the present invention, by applying a coating material that satisfies the above ranges of heating residue and viscosity to form a coating, it is possible to form a thick coating, which exhibits good adhesion to the substrate and can be stably formed as a uniform coating. Furthermore, the formed coating exhibits excellent foaming properties when the temperature rises due to a fire or the like, forms a carbonized heat insulating layer, and can maintain the heat-resistant protective performance of the substrate.
[0065] When the coating material of the present invention contains polyol (b1) and isocyanate (b2) as binders, it is preferable that the coating material is a two-liquid type coating material having the base agent containing the above-mentioned (A) component and the above-mentioned polyol (b1), and the above-mentioned curing agent containing the above-mentioned isocyanate (b2). That is, during distribution, the base agent and the curing agent are stored in separate packages, and these are mixed when used (applied). In this case, the heat resistance imparting component (and, if necessary, the water absorbing agent and other additives) may be mixed into at least one of the base agent and the curing agent, but in the present invention, it is preferable to mix them into the base agent. Also, each component can be added when mixing the base agent and the curing agent.
[0066] The coating material of the present invention is suitable as a foamable fireproof coating material applied to the surface coating of structures such as buildings and civil engineering structures. Specifically, it can be applied to various substrates such as walls, pillars, floors, beams, roofs, stairs, ceilings, and doors. Applicable substrates include, for example, concrete, mortar, siding boards, extrusion molding boards, gypsum boards, perlite boards, bricks, plastics, wood, metals, steel frames (steel materials), glass, and porcelain tiles. These substrates may have a coating already formed on their surfaces, may have been subjected to some kind of undercoating treatment (rust prevention treatment, flame retardant treatment, etc.), or may have wallpaper attached thereto.
[0067] (Film formation method) The coating formation method of the present invention involves applying the coating material to a substrate to form a coating. The coating method is not particularly limited, and various methods can be used, such as brush coating, trowel coating, roller coating, and spray coating (air spray, airless spray), etc.
[0068] The coating material of the present invention is also suitable for spray coating (air spray, airless spray). The coating material can be applied at temperatures of -10 to 45°C, and good coating workability and curing properties can be obtained even at high temperatures of 30°C or higher (even 35°C or higher). The humidity during coating is not particularly limited, but good coating workability, curing properties, and adhesion to the substrate can be obtained even under high humidity conditions (including rainy weather) of 70% Rh or higher (even 80% Rh or higher). As a result, a coating film with excellent heat resistance protection can be formed. Even if the curing (drying) environment of the coating material after coating is high and humid, good curing properties and adhesion to the substrate can be obtained, and a coating film with excellent heat resistance protection can be formed.
[0069] When the coating material of the present invention is applied to a substrate, it may be applied by one or several steps by the above method, but it is preferable to apply the coating so that the dry film thickness per step is preferably 300 μm or more (more preferably 400 to 8000 μm). Even when the coating material of the present invention is applied so that the dry film thickness per step exceeds 1000 μm, it is possible to obtain excellent curing properties and adhesion to the substrate, and to form a coating with excellent heat-resistant protection. In addition, the coating thickness finally formed may be appropriately set depending on the desired functionality, application site, etc., but is preferably about 0.4 to 8 mm.
[0070] (undercoating material) In addition, in the present invention, if necessary, before applying the coating material, the substrate can be subjected to surface treatment or a primer can be applied. This can improve adhesion to the substrate and corrosion resistance (rust resistance), etc. Surface treatment of the substrate can be performed, for example, by surface treatment with a solvent or acid, or scraping with a disk sander, wire foil, scraper, wire brush, sandpaper, etc.
[0071] As the undercoat material, for example, a sealer, a primer, a base conditioner, a surfacer, a putty, etc., as well as a flat-type paint can be applied. These may be either clear type or colored type. In addition, either water-based or solvent-based may be used, and can be appropriately selected according to the painting location, etc., and one or more types can be used. As the undercoat material, for example, it is preferable to contain a resin component such as an acrylic resin, a urethane resin, an epoxy resin, etc., and in addition to the above-mentioned resin components, various additives can be blended to an extent that does not affect the effect of the present invention. Examples of such additives include anti-rust pigments, extender pigments, coloring pigments, plasticizers, preservatives, anti-mold agents, anti-algae agents, defoamers, leveling agents, pigment dispersants, anti-settling agents, anti-sagging agents, antioxidants, catalysts, crosslinking agents, etc.
[0072] The undercoat material can be applied by various methods, such as brush coating, roller coating, spray coating, etc. The amount of application is preferably 30 to 500 g / m2 (More preferably 50 to 300 g / m 2 The number of times the undercoat material is applied may be appropriately determined depending on the surface condition of the substrate, etc., but is preferably 1 to 2 times.
[0073] (Finishing materials) In the present invention, a finishing material layer can be laminated on the coating material layer (coating) formed by the above coating material. Such a finishing material layer is not particularly limited as long as it does not inhibit the above coating material layer from foaming and forming a carbonized insulation layer when the temperature rises due to a fire or the like, and any known finishing material can be laminated. Such a finishing material layer can be laminated by applying a topcoat material or by attaching various sheet materials.
[0074] As the above-mentioned topcoat material, any of clear type or colored type, glossy type or matte type, hard type or elastic type, thin film type or thick film type can be used. In addition, it may be either water-based or solvent-based, and can be appropriately selected according to the desired purpose. In addition, it is preferable that the topcoat material of the present invention contains a resin component. Examples of the form of such a resin include solvent-soluble resin, non-water-dispersed resin, solventless resin, water-dispersed resin, water-soluble resin, etc. Examples of the type of resin include acrylic resin, urethane resin, epoxy resin, vinyl chloride resin, vinyl acetate resin, acrylic silicone resin, fluororesin, silicon resin, polyvinyl alcohol, cellulose derivatives, etc., or composites thereof. These can be used alone or in combination of two or more. In particular, in the present invention, it is preferable to include one or more selected from urethane resin, epoxy resin, acrylic resin, and acrylic silicone resin.
[0075] Furthermore, the resin component may have crosslinking reactivity. When the resin component is a crosslinking reactive resin, the water resistance, durability, and adhesion of the formed coating are improved, and the occurrence of swelling and peeling of the coating due to rainfall, condensation, etc. and the decrease in heat resistance can be suppressed. Such a crosslinking reactive resin may be either one that causes a crosslinking reaction by itself or one that causes a crosslinking reaction by a crosslinking agent that is mixed separately. Such crosslinking reactivity can be imparted by combining reactive functional groups such as, for example, a hydroxyl group and an isocyanate group, a carbonyl group and a hydrazide group, an epoxy group and an amino group, an aldo group and a semicarbazide group, a keto group and a semicarbazide group, alkoxyl groups, a carboxyl group and a metal ion, a carboxyl group and a carbodiimide group, a carboxyl group and an epoxy group, a carboxyl group and an aziridine group, or a carboxyl group and an oxazoline group. Among these, it is preferable to include one or more crosslinking reactive resins selected from a hydroxyl group-isocyanate group, a carbonyl group and a hydrazide group, and an epoxy group and an amino group.
[0076] As components other than the resin component of the above-mentioned topcoat material, for example, color pigments, extender pigments, aggregates, etc. can be mixed. By appropriately blending such components, it is possible to express the desired color and texture. The amount of color pigments, extender pigments, aggregates, etc. to be mixed is not particularly limited as long as it is within a range that does not inhibit the effects of the above-mentioned coating material (foamability, heat-resistant protection, etc.), but is preferably 1 to 2000 parts by weight (more preferably 5 to 1000 parts by weight) relative to 100 parts by weight of the solid content of the resin component.
[0077] In the present invention, it is particularly preferable to use pigments having infrared reflectivity and / or infrared transmittance as the color pigments and extender pigments, which can further enhance the effects of heat resistance protection and the like.
[0078] Examples of pigments having infrared reflectivity include aluminum flakes, titanium oxide, barium sulfate, zinc oxide, iron oxide, calcium carbonate, silicon oxide, magnesium oxide, zirconium oxide, yttrium oxide, indium oxide, alumina, iron-chromium composite oxide, manganese-bismuth composite oxide, manganese-yttrium composite oxide, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, and the like, and one or more of these can be used.
[0079] Examples of pigments having infrared transmittance include perylene pigments, azo pigments, yellow lead, titanium red, cadmium red, quinacridone red, isoindolinone, benzimidazolone, phthalocyanine green, phthalocyanine blue, cobalt blue, indanthrene blue, ultramarine, and Prussian blue, and one or more of these can be used.
[0080] Furthermore, the topcoat material can also contain various additives that can be used in normal paints. Examples of such additives include thickeners, film-forming assistants, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, defoamers, adsorbents, ultraviolet absorbers, light stabilizers, antioxidants, fibers, low-pollution agents, hydrophilizing agents, water repellents, coupling agents, catalysts, etc.
[0081] In the coating method of the present invention, the topcoat material can be applied by repainting, or two or more types of topcoat materials can be laminated and applied. When two or more types of topcoat materials are laminated, it is preferable that the first topcoat material (intermediate coating material) contains one or more resin components selected from urethane resin, epoxy resin, acrylic resin, and acrylic silicone resin (particularly preferably, urethane resin, epoxy resin, etc.). This can further increase the adhesion between the layers of the coating material and the topcoat material. Furthermore, a topcoat material coating with excellent coating properties can be formed.
[0082] The topcoat material may be applied by a known application method, for example, by using various methods such as brush coating, roller coating, and spray coating. The amount of coating is preferably 30 to 5000 g / m2 (more preferably 50 to 3000 g / m2). The number of coats of the topcoat material may be appropriately set depending on the surface condition of the substrate, but is preferably 1 to 2 times. In addition, drying may be preferably performed at room temperature.
[0083] Examples of the sheet material include decorative films, decorative sheets, sheet building materials, wallpapers, etc. The thickness of the sheet material is preferably 0.01 to 30 mm (more preferably 0.05 to 20 mm). These may be attached via a known adhesive (pressure-sensitive adhesive) or the like. EXAMPLES
[0084] The following examples will clarify the features of the present invention, but the present invention is not limited to these examples.
[0085] <Manufacture of Coating Materials 1-3, 13-14> The raw materials shown in Table 1 were mixed in a conventional manner according to the formulation shown in Table 2 to obtain a coating material. <Manufacture of coating materials 4-12, 15-16> The base material was prepared by mixing the raw materials shown in Table 1 in the usual manner according to the composition shown in Table 2. Next, the curing agent was mixed so as to obtain the NCO / OH equivalent ratio shown in Table 1, to obtain a coating material.
[0086] <Evaluation> A coating material was sprayed onto the entire surface of a steel plate (150 mm long x 70 mm wide x 1.6 mm thick) that had previously been coated with an anti-rust paint under standard conditions (temperature 23°C, relative humidity 50%) to give a dry film thickness of 1.5 mm, and after curing for 16 hours, the same coating material was sprayed onto the plate to give a dry film thickness of 1.5 mm, and then cured for 7 days. This was designated as test specimen A, and the following evaluations were carried out. The results are shown in Table 2.
[0087] Based on the ISO 5660-1 cone calorimeter method, an electric heater (CONEIII, manufactured by Toyo Seiki Co., Ltd.) was used to apply 50 kW / m to the surface of the test specimen. 2 The foaming rate (foaming ratio) and the temperature of the bottom surface of the steel plate were measured when the radiant heat of 1000 g was radiated for 30 minutes, and the density and adhesion were evaluated. The evaluation criteria are as follows: <Evaluation 1 (foaming)> A: Expansion ratio over 20 times B: Expansion ratio: 15 times or more and 20 times or less C: Foaming ratio more than 10 times and less than 15 times D: Foaming ratio 10 times or less <Evaluation 2 (reverse surface temperature)> A: Less than 470℃ B: 470℃ or higher and less than 500℃ C: 500℃ or higher but lower than 550℃ D: Over 550℃ <Rating 3 (Density)> The test specimen for which the expansion ratio was measured was cut, and the density of the carbonized insulation layer on the cross section was visually confirmed. The evaluation criteria were a four-level evaluation (A>B>C>D: poor), with "A" being high density and "D" being low density. <Evaluation 4 (Adhesion 1: Adhesion to substrate)> The adhesion of the carbonized insulation layer formed after 30 minutes of radiant heat was checked near the substrate. The evaluation criteria were visually evaluated for the presence or absence of separation between the substrate and the carbonized insulation layer, with a four-level evaluation (A>B>C>D: poor) ranging from "A" for no separation to "D" for severe separation. <Evaluation 5 (Adhesion 2: Adhesion of coating material)> The coating layer side of the steel jig and test specimen A were attached using a two-liquid epoxy resin adhesive, and left to stand for one week under standard conditions. The adhesive strength was measured using an autograph (AGX type, manufactured by Shimadzu Corporation) according to the procedure in JIS A 6909:2014 "Architectural Finish Coating Materials" 7.10 (loading speed: 1764 N / min). The evaluation criteria are as follows: A: Adhesion strength 0.4N / mm 2 The above (fracture in the coating layer of the test specimen) B: Adhesion strength 0.4N / mm 2The above (interface fracture between the steel plate and coating layer of the test specimen) C: Adhesion strength 0.2N / mm 2 More than 0.4N / mm 2 Less than (interface fracture between the steel plate and coating layer of the test specimen) D: Adhesion strength 0.2N / mm 2 Less than (interface fracture between the steel plate and coating layer of the test specimen)
[0088] The coating material was sprayed onto the entire surface of a steel material (H400×200×8×13mm, L=1200mm) that had been previously coated with an anti-rust paint under standard conditions (temperature 23°C, relative humidity 50%) so that the dry film thickness was 4.8mm, and the material was left to cure for 7 days to form test specimen B, which was then subjected to the following evaluations. The results are shown in Table 2. <Rating 6 (fire resistance)> The prepared specimen B was subjected to a 120-minute heating test in accordance with the standard heating curve of ISO834. The evaluation criteria were a visual inspection of the substrate and the carbonized insulation layer to see if there was any separation, and a four-level evaluation was used (A>B>C>D: poor), with no separation being given an "A" and severe separation being given a "D."
[0089] [Table 1]
[0090] [Table 2]
Claims
1. A coating material that forms a carbonized heat insulating layer at a temperature of 200°C or higher, The coating material includes a binder and a heat resistance imparting component, The coating material is characterized in that the binder contains a copolymer resin (A) of a vinyl monomer group containing an alkyl acid vinyl monomer (a1) and a resin (B) different from the copolymer resin (A).
2. The coating material according to claim 1, characterized in that the resin (B) contains a polyol (b1) and an isocyanate (b2).
3. A coating material that forms a carbonized heat insulating layer at a temperature of 200°C or higher, The coating material is characterized by having a base material containing a copolymer resin (A) of a vinyl monomer group containing an alkyl acid vinyl monomer (a1), a polyol (b1) and a heat resistance imparting powder, and a curing agent containing an isocyanate (b2).
4. The coating material according to claim 3 , wherein the base material further contains a water absorbing agent.
5. 4. The coating material according to claim 1, wherein the copolymer resin (A) is a copolymer resin of a vinyl monomer group including an alkyl acid vinyl monomer (a1) and an aromatic group-containing vinyl monomer (a2).
6. 4. The coating material according to claim 1, wherein the copolymer resin (A) is a copolymer resin of a vinyl monomer group containing 3% by weight or more and less than 60% by weight of an alkyl acid vinyl monomer (a1).
7. 4. The coating material according to claim 1, wherein the heat resistance imparting component comprises at least one selected from the group consisting of a foaming agent, a carbonizing agent, a flame retardant, and a filler.
8. A coating forming method for forming a coating by applying a coating material to a substrate, comprising the steps of:
5. A method for forming a coating film, comprising the step of: forming a coating material according to claim 1 on a substrate;
9. A coating forming method for forming a coating by applying a coating material to a substrate, comprising the steps of: The coating material is the coating material according to any one of claims 1 to 4, and is applied in one or more recoating steps, and the dry film thickness per step is 300 μm or more.
Citation Information
Patent Citations
Solvent-based binders for thermally expandable coatings
JP2019522701A
Cited By