Composite sheet for forming resin film, kit and method for manufacturing workpiece processed product with resin film

The composite sheet with a support sheet and adhesive layer addresses the challenge of picking up small-sized workpieces with resin films by maintaining low adhesive force post-heating, ensuring reliable separation and enhancing manufacturing efficiency in semiconductor device production.

JP2024142714APending Publication Date: 2024-10-11LINTEC CORP

Patent Information

Application Number
JP2023055005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The challenge in manufacturing semiconductor devices is the inability to efficiently pick up small-sized workpieces with resin films from support sheets due to insufficient heat resistance and adhesive properties, leading to peeling issues during high-temperature processing, especially when using thermosetting resin films.

Method used

A composite sheet for forming resin films with a support sheet and adhesive layer that maintains low adhesive force after high-temperature heating, allowing easy pickup of workpieces without curing the adhesive layer, and includes features like block-type crosslinking agents and energy ray-curable properties to enhance adhesion and peeling resistance.

Benefits of technology

The solution enables normal pickup of workpieces with resin films even at high temperatures, preventing peeling from fixing jigs and ensuring reliable separation from the support sheet, thus improving manufacturing efficiency and yield in semiconductor device production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142714000001_ABST
    Figure 2024142714000001_ABST
Patent Text Reader

Abstract

To provide: a composite sheet for forming a resin film, capable of normally picking up a workpiece processed product with a resin film from an adhesive layer without energy ray-curing the adhesive layer in a support sheet after heating and capable of suppressing the peeling of the support sheet from a fixing jig for other purposes; a kit; and a method for manufacturing a workpiece processed product with a resin film.SOLUTION: There is provided a composite sheet 1 for forming a resin film or a kit. The composite sheet 1 for forming a resin film includes a support sheet 10 including a base material 11 and an adhesive layer 12, and a thermosetting resin film forming film 13. An adhesive force (Z2) between the adhesive layer 12 and the resin film after heating at 140°C is 1,500 mN / 25 mm or less, and an adhesive force (Y0) between the adhesive layer 12 and a stainless steel plate is 2,000 mN / 25 mm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite sheet for resin film formation, a kit, and a method for manufacturing a workpiece with a resin film. [Background technology]

[0002] 2. Description of the Related Art Some workpieces such as semiconductor wafers, insulator wafers, and semiconductor device panels have circuits formed on one surface (circuit surface) and further have protruding electrodes such as bumps on that surface (circuit surface).

[0003] In a manufacturing process of a semiconductor device using a mounting method called a face-down method, a protective film-forming film is used to protect the back surface of a workpiece formed by dicing the workpiece, and a protective film-forming composite sheet is used, which is a combination of a support sheet formed by laminating an adhesive layer on one side of a base material and a protective film-forming film. Also, a film-like adhesive is used to bond the back surface of the workpiece to a lead frame or an organic substrate, and a dicing die bonding sheet, which is a combination of a support sheet and a film-like adhesive, is also used when dicing the workpiece. The protective film-forming film and the film-like adhesive are attached to the back surface of the workpiece.

[0004] Hereinafter, in this specification, the thermosetting protective film-forming film or film-like adhesive is referred to as the thermosetting resin film-forming film, and the protective film-forming composite sheet or dicing die bonding sheet is referred to as the resin film-forming composite sheet. The protective film formed by the protective film-forming film or the bonding film formed by the film-like adhesive is referred to as the resin film.

[0005] In the manufacturing process of a workpiece with a resin film, a thermosetting resin film-forming film for forming a protective film or a bonding film is attached to the back surface of the workpiece. The thermosetting resin film-forming film may be attached to the back surface of the workpiece in the form of a composite sheet for resin film formation in which the thermosetting resin film-forming film is laminated on a support sheet. The thermosetting resin film-forming film may be attached to the back surface of the workpiece without being laminated on a support sheet, and then attached to the support sheet.

[0006] The thermosetting resin film-forming film attached to the back surface of the workpiece is thermally cured on a support sheet formed of a substrate and an adhesive layer, for example, to form a resin film. When the thermosetting resin film-forming film attached to the back surface of the workpiece is thermally cured on the support sheet, a first laminated composite sheet, which is formed by laminating the substrate, adhesive layer, thermosetting resin film-forming film, and workpiece in this order in the thickness direction, is heated and cooled while the peripheral portion of the support sheet is attached to a fixing jig such as a ring frame. Thereafter, in a dicing process on the support sheet, the workpiece is divided, the resin film is cut, and the workpiece is picked up as a workpiece with a resin film (see Patent Document 1). Patent Document 1 describes that the first laminated composite sheet is heated at 130° C. for 2 hours to thermally cure the resin film-forming film and form a resin film.

[0007] As a support sheet that is heat resistant and suitable for heating, a support sheet (sheet for work processing) has been disclosed that has a base material and an adhesive layer, and in which the Young's modulus of the base material at 23°C after heating at 120°C for 4 hours and the storage modulus E' of the base material at 120°C are both specified within specific ranges (see Patent Document 2). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2015 / 178346 [Patent Document 2] JP 2021-119592 A Summary of the Invention [Problem to be solved by the invention]

[0009] For example, Patent Document 1 describes a method of dicing a semiconductor wafer having a diameter of 8 inches into chips having a chip size of 9 mm×9 mm. Patent Document 2 describes a method of dicing a semiconductor wafer having a diameter of 8 inches into chips having a chip size of 3 mm×3 mm.

[0010] In the manufacturing process of resin-coated chips, semiconductor wafers with larger diameters are being used, and the chip size is tending to become smaller. When the chip size is small, dicing at a faster feed rate is required to improve production efficiency.

[0011] On the other hand, the support sheet may be heated to remove foreign matter such as low molecular weight resin components attached to the surface of the workpiece with the resin film-forming film attached thereto, in addition to the heating for the purpose of thermally curing the resin film-forming film with the workpiece attached thereto. In addition, the support sheet may be heated to dry the workpiece with the resin film, etc., after washing and removing fine foreign matter that occurs during processing such as dicing the workpiece with the resin film-forming film and that is attached to the surface of the workpiece with the resin film-forming film with water. In addition, it is preferable that these heating processes are usually performed with the upper limit of the heating temperature being about 140°C. However, if the heat resistance of the support sheet is insufficient, when the support sheet with the workpiece with the resin film-forming film attached thereto is heated at such a temperature, it may be impossible to finally pick up the workpiece with the resin film from the support sheet.

[0012] When the chip size of the resin-filmed workpiece obtained by thermal curing at about 130° C. is relatively large, the resin-filmed workpiece may not be picked up from the support sheet, but a resin-filmed workpiece with a small chip size of, for example, 1.5 mm×1.5 mm may be able to be picked up. However, when heated at a high temperature of about 140° C., even if the resin-filmed workpiece has a small chip size of 1.5 mm×1.5 mm, it may not be possible to pick up the resin-filmed workpiece from the support sheet.

[0013] It is also known that when the adhesive layer is energy ray curable, the adhesive layer is cured with energy rays to reduce the adhesion between the cured product and the resin film-attached workpiece, making it easier to pick up the resin film-attached workpiece. However, there is also a demand to omit the step of curing the adhesive layer with energy rays for small chip-sized resin film-attached workpieces.

[0014] If the adhesive layer's adhesiveness is reduced to make it easier to pick up the resin-coated workpiece from the support sheet, there is a risk that after the support sheet is affixed to a fixing jig such as a ring frame, the workpiece may peel off from the fixing jig due to its own weight during transport, etc.

[0015] It is therefore desirable to achieve normal pick-up of such resin-film-coated workpieces and to prevent the support sheet from peeling off from the fixing jig for an unintended purpose.

[0016] The present invention aims to provide a composite sheet for resin film formation and a kit, which, when a thermosetting resin film-forming film and a workpiece are processed on a support sheet having a substrate and an adhesive layer provided on one side of the substrate to produce a resin-film-attached workpiece, can be normally picked up from the adhesive layer even when the thermosetting resin film-forming film and the workpiece are heated on the support sheet at a high temperature of 140° C. or higher, without curing the adhesive layer in the support sheet after heating with energy rays, and can also suppress peeling of the support sheet from a fixing jig for an unintended purpose. Another aim is to provide a method for producing a resin-film-attached workpiece using the composite sheet for resin film formation or the kit. [Means for solving the problem]

[0017] In order to solve the above problems, the present invention employs the following configuration. [1] A composite sheet for resin film formation, comprising: a support sheet having a substrate and an adhesive layer provided on one surface of the substrate; and a thermosetting resin film-forming film provided on the adhesive layer of the support sheet, The thermosetting resin film-forming film in the composite sheet for resin film formation is heated at 140° C. to form a resin film, and when the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less, A composite sheet for forming a resin film, in which the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the stainless steel plate with the support sheet is left to stand for 30 minutes at a temperature of 23°C, and the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, and the adhesive strength (Y0) is 2000 mN / 25 mm or more. [2] The composite sheet for resin film formation according to [1], wherein the pressure-sensitive adhesive layer contains a block type crosslinking agent (β1). [3] The composite sheet for resin film formation according to [1] or [2], wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more.

[0018] [4] The composite sheet for forming a resin film according to any one of [1] to [3], wherein when the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less. [5] The composite sheet for resin film formation according to any one of [1] to [4], wherein the pressure-sensitive adhesive layer is energy ray-curable. [6] The composite sheet for forming a resin film described in [5], wherein when the thermosetting resin film-forming film in the composite sheet for forming a resin film is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is cured with energy rays, and the adhesive strength (Z1) between the energy-ray-cured product of the pressure-sensitive adhesive layer and the resin film is measured, the adhesive strength (Z1) is 500 mN / 25 mm or less.

[0019] [7] A kit comprising a first laminate formed by laminating a first release film and a thermosetting resin film-forming film, a base material and a pressure-sensitive adhesive layer provided on one surface of the base material, and a support sheet used to support a workpiece to which the thermosetting resin film-forming film is to be attached and the thermosetting resin film-forming film, The pressure-sensitive adhesive layer in the support sheet and the thermosetting resin film-forming film are attached to form a second laminate, and the thermosetting resin film-forming film in the second laminate is heated at 140° C. to form a resin film. When the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less, A kit, wherein the support sheet is attached to a surface of a stainless steel plate by the adhesive layer, the stainless steel plate with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, and the adhesive strength (Y0) is 2000 mN / 25 mm or more. [8] The kit described in [7], wherein the adhesive layer contains a block type crosslinking agent (β1). [9] The kit described in [7] or [8], wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more.

[0020]

[10] The kit described in any one of [7] to [9], wherein when the support sheet is attached to a surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less.

[11] The kit according to any one of [7] to

[10] , wherein the pressure-sensitive adhesive layer is energy ray-curable.

[12] The kit described in

[11] , wherein when the thermosetting resin film-forming film in the second laminate is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is energy ray-cured, and the adhesive strength (Z1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the resin film is measured, the adhesive strength (Z1) is 500 mN / 25 mm or less.

[0021]

[13] A method for manufacturing a resin-film-attached workpiece, comprising: a workpiece; and a resin film provided on a rear surface of the workpiece, [1]-[6]: The exposed surface of the thermosetting resin film-forming film in the composite sheet for resin film formation described in any one of the above items is attached to the back surface of the workpiece, and the peripheral portion of the adhesive layer in the composite sheet for resin film formation is attached to a fixing jig; or [7]-

[12] : The exposed surface of the thermosetting resin film-forming film in the kit described in any one of the above items is attached to the back surface of the workpiece, and the peripheral portion of the adhesive layer in the support sheet of the kit is attached to a fixing jig, thereby fixing the first laminated composite sheet, which is configured by laminating the base material, the adhesive layer, the thermosetting resin film-forming film, and the workpiece in this order in the thickness direction, to the fixing jig; A processing step of dividing the work in the first laminated composite sheet and cutting the thermosetting resin film-forming film to produce a second laminated composite sheet in which a plurality of workpieces with a resin film-forming film are fixed on the base material and the adhesive layer; a heating step of heating the second laminated composite sheet with the peripheral portion of the adhesive layer attached to a fixing jig to harden the thermosetting resin film-forming film and form the resin film, thereby producing a third laminated composite sheet in which the base material, the adhesive layer, and a plurality of workpieces with resin films are laminated in this order in the thickness direction; A method for manufacturing a workpiece with a resin film, comprising: a pick-up process for picking up the workpiece with the resin film in the third laminated composite sheet by separating it from the adhesive layer. Effect of the Invention

[0022] According to the present invention, when a thermosetting resin film-forming film and a workpiece are processed on a support sheet having a substrate and an adhesive layer on one side of the substrate to produce a resin-film-attached workpiece, even if the thermosetting resin film-forming film and the workpiece are heated on the support sheet at a high temperature of 140° C. or higher, the adhesive layer in the support sheet after heating can be cured with energy rays, and the resin-film-attached workpiece can be normally picked up from the adhesive layer, and peeling of the support sheet from a fixing jig for an unintended purpose can be suppressed. Also provided is a composite sheet for resin film formation and a kit. Also provided is a method for producing a resin-film-attached workpiece using the composite sheet for resin film formation or the kit. [Brief description of the drawings]

[0023] [Figure 1] 1 is a cross-sectional view showing a schematic example of a composite sheet for resin film formation according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view illustrating an example of a kit according to one embodiment of the present invention. [Figure 3A]1 is a cross-sectional view for illustrating a schematic diagram of a portion of an example of a method for manufacturing a workpiece with a resin film according to an embodiment of the present invention. [Figure 3B] 1 is a cross-sectional view for illustrating a schematic diagram of a portion of an example of a method for manufacturing a workpiece with a resin film according to an embodiment of the present invention. [Figure 3C] 1 is a cross-sectional view for illustrating a schematic diagram of a portion of an example of a method for manufacturing a workpiece with a resin film according to an embodiment of the present invention. [Figure 3D] 1 is a cross-sectional view for illustrating a schematic diagram of a portion of an example of a method for manufacturing a workpiece with a resin film according to an embodiment of the present invention. [Figure 3E] 1 is a cross-sectional view for illustrating a schematic diagram of a portion of an example of a method for manufacturing a workpiece with a resin film according to an embodiment of the present invention. [Figure 4A] 10A to 10C are cross-sectional views for illustrating a schematic view of a portion of an example of a method for manufacturing a workpiece with a resin film according to another embodiment of the present invention. [Figure 4B] 10A to 10C are cross-sectional views for illustrating a schematic view of a portion of an example of a method for manufacturing a workpiece with a resin film according to another embodiment of the present invention. [Figure 4C] 10A to 10C are cross-sectional views for illustrating a schematic view of a portion of an example of a method for manufacturing a workpiece with a resin film according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] ◇Composite sheet for forming resin film A composite sheet for forming a resin film according to one embodiment of the present invention comprises a support sheet having a substrate and an adhesive layer provided on one side of the substrate, and a thermosetting resin film-forming film provided on the adhesive layer of the support sheet. When the thermosetting resin film-forming film in the composite sheet for forming a resin film is heated at 140°C to form a resin film, and the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating (sometimes simply referred to as "adhesive strength (Z2)" in this specification) is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less. The support sheet is attached to the surface of a stainless steel plate by the adhesive layer, and the stainless steel plate with the support sheet is left to stand for 30 minutes at a temperature of 23°C. When the adhesive strength (Y0) between the adhesive layer and the stainless steel plate (sometimes simply referred to as "adhesive strength (Y0)" in this specification) is measured, the adhesive strength (Y0) is 2000 mN / 25 mm or more.

[0025] The composite sheet for resin film formation of this embodiment can be used, for example, to manufacture a workpiece with a resin film, as described later.

[0026] In the composite sheet for resin film formation of this embodiment, since the adhesive strength (Z2) is 1500 mN / 25 mm or less, even if the thermosetting resin film-forming film and the workpiece are heated at a high temperature of 140° C. or more on the support sheet when preparing the workpiece with a resin film, the workpiece with a resin film can be normally picked up from the adhesive layer without curing the adhesive layer in the support sheet with energy rays after heating. Also, since the adhesive strength (Y0) is 2000 mN / 25 mm or more, peeling of the support sheet from the fixing jig for an unintended purpose can be suppressed.

[0027] In this specification, "room temperature" means a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 18 to 28°C.

[0028] In this embodiment, the workpiece may be, for example, a wafer, a semiconductor device panel, or the like.

[0029] Examples of the wafer include semiconductor wafers made of elemental semiconductors such as silicon, germanium, and selenium, and compound semiconductors such as GaAs, GaP, InP, CdTe, ZnSe, and SiC; and insulating wafers made of insulators such as sapphire and glass. A circuit is formed on one surface of the workpiece, which is typically a wafer, and in this specification, the surface of the workpiece on which the circuit is formed is referred to as the "circuit surface," and the surface of the workpiece opposite the circuit surface is referred to as the "rear surface." The wafer is divided into chips by dicing or other means. In this specification, as in the case of the wafer, the surface of the chip on which the circuit is formed is referred to as the "circuit surface," and the surface of the chip opposite the circuit surface is referred to as the "back surface." It is preferable that the circuit surface of each workpiece is provided with protruding electrodes such as bumps, pillars, etc. The protruding electrodes are preferably made of solder.

[0030] The semiconductor device panel is handled during the manufacturing process of a semiconductor device, and a specific example thereof is a configuration in which a semiconductor device in which one or more electronic components are sealed with sealing resin is used, and multiple such semiconductor devices are arranged in a planar manner within an area of ​​a circular, rectangular, or other shape.

[0031] In this embodiment, the resin film-coated workpiece is obtained by processing a workpiece with a resin film-forming film. For example, when the workpiece is a wafer, the resin film-coated workpiece may be a chip with a resin film, and when the workpiece is a semiconductor wafer, the resin film-coated workpiece may be a semiconductor chip with a resin film.

[0032] In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, or an LED lamp as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays. In this specification, the term "non-curable" refers to a property that does not cure by any means, such as heating or irradiation with energy rays.

[0033] Fig. 1 is a cross-sectional view showing an example of a composite sheet for resin film formation according to an embodiment of the present invention. In addition, the drawings used in the following description may show the main parts enlarged for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0034] The composite sheet 1 for forming a resin film shown here comprises a support sheet 10 having a substrate 11 and an adhesive layer 12 provided on one surface 11a of the substrate 11, and a thermosetting resin film forming film 13 provided on the adhesive layer 12 of the support sheet 10. In the composite sheet 1 for resin film formation, the adhesive strength (Z2) is 1500 mN / 25 mm or less, and the adhesive strength (Y0) is 2000 mN / 25 mm or more.

[0035] In the composite sheet for resin film formation 1 of this embodiment, the substrate 11 and the adhesive layer 12 are approximately the same size. The thermosetting resin film-forming film 13 is smaller than the substrate 11 and the adhesive layer 12 so that the adhesive layer 12 can be attached to a fixing jig such as a ring frame 18 outside the peripheral portion of the thermosetting resin film-forming film 13.

[0036] The composite sheet for resin film formation of the present embodiment is not limited to the one shown in Fig. 1, and may adopt the form of a known composite sheet for resin film formation. That is, within the scope that does not impair the effect of the present invention, a part of the configuration shown in Fig. 1 may be changed, deleted, or added.

[0037] 1 includes a substrate 11, a pressure-sensitive adhesive layer 12, a thermosetting resin film-forming film 13, and a release film 15. The composite sheet for resin film formation of this embodiment may include other layers that do not fall under any of the substrate, pressure-sensitive adhesive layer, thermosetting resin film-forming film, and release film.

[0038] The composite sheet 1 for resin film formation shown in Figure 1 has a release film 15, but in the composite sheet for resin film formation of this embodiment, the release film has an optional configuration, and the composite sheet for resin film formation of this embodiment does not need to have a release film.

[0039] In the composite sheet for resin film formation of this embodiment, it is preferable that the substrate and the pressure-sensitive adhesive layer are provided in direct contact with each other, the pressure-sensitive adhesive layer and the thermosetting resin film-forming film are provided in direct contact with each other, and the thermosetting resin film-forming film and the release film are provided in direct contact with each other.

[0040] Next, each layer constituting the composite sheet for resin film formation of this embodiment will be described in detail.

[0041] <<Thermosetting resin film>> The thermosetting resin film-forming film is used by being attached to the back surface of a workpiece in a method for manufacturing a workpiece with a resin film. The thermosetting resin film-forming film is preferably a protective film-forming film used to protect the back surface of a workpiece obtained by dividing the workpiece. The protective film-forming film of the present embodiment has thermosetting properties and functions as a protective film by the thermal curing. In this specification, a resin film-formed film at room temperature is heated to a temperature higher than room temperature and then cooled to room temperature to obtain a resin film-formed film after heating and cooling, and when the hardness of the resin film-formed film after heating and cooling is compared with the hardness of the resin film-formed film before heating at the same temperature, if the resin film-formed film after heating and cooling is harder, then this resin film-formed film is thermosetting.

[0042] By using the composite sheet for resin film formation or the kit including the support sheet and the thermosetting resin film-forming film, a workpiece with a resin film can be manufactured by a manufacturing method of a workpiece with a resin film, which will be described later. For example, when the workpiece is a wafer, a chip with a resin film can be manufactured by using the composite sheet for resin film formation or the kit, which includes a chip and a resin film provided on the back of the chip.

[0043] When the thermosetting resin film-forming film is a protective film-forming film, by using the composite sheet for resin film formation (i.e., composite sheet for protective film formation) or the kit comprising the support sheet and the protective film-forming film, a workpiece with a protective film can be manufactured by the manufacturing method for a workpiece with a resin film described below, which comprises a workpiece and a protective film provided on the back surface of the workpiece.

[0044] Furthermore, by using the workpiece with the resin film, a substrate device can be manufactured. In this specification, the term "substrate device" refers to a device configured by connecting a resin-coated workpiece to a circuit board. For example, a substrate device may be configured by flip-chip connecting a protruding electrode on a circuit surface of a workpiece with a protective film to a connection pad on a circuit board. For example, if a semiconductor wafer is used as the workpiece, a substrate device may be a semiconductor device equipped with a resin-coated semiconductor chip.

[0045] The thermosetting resin film-forming film may be made of one layer (single layer) or may be made of two or more layers. When the thermosetting resin film-forming film is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.

[0046] The thickness of the thermosetting resin film-forming film is preferably 1 to 100 μm, more preferably 5 to 60 μm, and even more preferably 10 to 50 μm. When the thickness of the thermosetting resin film-forming film is equal to or greater than the lower limit, a resin film with higher protective performance can be formed. When the thickness of the thermosetting resin film-forming film is equal to or less than the upper limit, the resin film can be prevented from becoming excessively thick. Here, "the thickness of the thermosetting resin film-forming film" means the thickness of the entire thermosetting resin film-forming film, and for example, the thickness of a thermosetting resin film-forming film consisting of multiple layers means the total thickness of all layers constituting the thermosetting resin film-forming film.

[0047] The thermosetting resin film-forming film can be formed using a resin film-forming composition containing its constituent materials (i.e., a thermosetting resin film-forming composition for forming a thermosetting resin film). For example, the thermosetting resin film-forming film can be formed by applying a thermosetting resin film-forming composition to the surface to be formed and drying it as necessary. The ratio of the contents of the components that do not vaporize at room temperature in the thermosetting resin film-forming composition is usually the same as the ratio of the contents of the components in the thermosetting resin film-forming film.

[0048] In particular, a thermosetting protective film-forming film, which is an example of a thermosetting resin film-forming film, can be formed using a protective film-forming composition (III-1) described below.

[0049] <Protective film forming composition (III-1)> Examples of compositions for forming resin films include a composition for forming a protective film (III-1) (sometimes abbreviated in this specification as "composition for forming a protective film (III-1)") containing a polymer component (A) and a thermosetting component.

[0050] (Polymer component (A)) The polymer component (A) is a polymer compound for imparting film-forming properties, flexibility, and the like to the thermosetting protective film-forming film. The polymer component (A) contained in the protective film-forming composition (III-1) and the thermosetting protective film-forming film may be one type or two or more types, and if there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0051] The polymer component may also be a thermosetting component. In this specification, when the composition for forming a protective film contains a component that corresponds to both a polymer component and a thermosetting component, the composition for forming a protective film is considered to contain a polymer component and a thermosetting component.

[0052] As the polymer component, it is possible to use acrylic resin, urethane resin, phenoxy resin, silicone resin, saturated polyester resin, etc. As the polymer component, it is preferable to use acrylic resin.

[0053] The weight average molecular weight (Mw) of the polymer component is preferably from 10,000 to 2,000,000, and more preferably from 100,000 to 1,200,000. When the weight average molecular weight of the polymer component is equal to or more than the lower limit, the adhesive strength (Z2) and the adhesive strength (Z1) tend to be more easily decreased.

[0054] The glass transition temperature (Tg) of the polymer component is preferably in the range of -60 to 50°C, more preferably -50 to 40°C, further preferably -40 to 20°C, and particularly preferably -30 to -1°C. When the glass transition temperature of the polymer component is equal to or higher than the lower limit, the adhesive strength (Z2) and the adhesive strength (Z1) tend to be lower. When the glass transition temperature of the polymer component is equal to or lower than the upper limit, the risk of cracking (cracking) when the protective film-forming film is rolled and bent is reduced.

[0055] From the viewpoints of adhesion, adhesion and film-forming properties, the preferred content of the polymer component is 5 to 50 parts by mass, 10 to 45 parts by mass, 14 to 40 parts by mass, or 18 to 35 parts by mass relative to 100 parts by mass of the total solid content constituting the protective film-forming film.

[0056] The glass transition temperature (Tg) of the resin constituting the polymer component can be calculated using the Fox formula shown below. 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+...+(Wm / Tgm) (wherein Tg is the glass transition temperature of the resin constituting the polymer component, Tg1, Tg2,...Tgm are the glass transition temperatures of the homopolymers of the monomers that are the raw materials of the resin constituting the polymer component, and W1, W2,...Wm are the mass fractions of the monomers. However, W1+W2+...+Wm=1.) The glass transition temperature of the homopolymer of each monomer in the Fox formula can be the value described in the Polymer Data Handbook, the Adhesive Handbook, the Polymer Handbook, etc. For example, the glass transition temperatures of homopolymers are 10°C for methyl acrylate, 105°C for methyl methacrylate, -54°C for n-butyl acrylate, -70°C for 2-ethylhexyl acrylate, 41°C for glycidyl methacrylate, and -15°C for 2-hydroxyethyl acrylate.

[0057] Examples of monomers constituting the acrylic resin include (meth)acrylic acid ester monomers or derivatives thereof. For example, alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, butyl (meth)acrylate, etc., can be mentioned. In addition, (meth)acrylates having a cyclic skeleton, specifically cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. can be mentioned. Furthermore, examples of functional group-containing monomers include 2-hydroxyethyl (meth)acrylate having a hydroxyl group, etc.; and other examples include glycidyl (meth)acrylate having an epoxy group, etc. As the acrylic resin, an acrylic polymer containing a structural unit having a hydroxyl group is preferable because it has good compatibility with the thermosetting component described later. In addition, the acrylic polymer may be copolymerized with acrylic acid, methacrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, etc.

[0058] (thermosetting component) The protective film-forming composition (III-1) preferably contains a thermosetting component, which allows the protective film-forming film to be thermosetting.

[0059] By using a thermosetting protective film-forming film, the variation in curing property depending on the thickness can be relatively small even if the protective film-forming film is made thick. In the heat curing process, a large number of second laminated composite sheets can be heated at the same time.

[0060] As the thermosetting component, a thermosetting resin (B) and a thermosetting agent (C) are used. Examples of the thermosetting resin include epoxy resin, thermosetting polyimide resin, unsaturated polyester resin, etc., and epoxy resin is preferred. In this specification, the thermosetting polyimide resin is a general term for a polyimide precursor and a thermosetting polyimide, which form a polyimide resin by thermal curing.

[0061] As the epoxy resin, a conventionally known epoxy resin can be used. Specific examples of the epoxy resin include polyfunctional epoxy resins, dicyclopentadiene type epoxy resins, bisphenol A type epoxy resins, and other epoxy compounds having two or more functional groups in the molecule. These can be used alone or in combination of two or more.

[0062] The preferred content of the thermosetting component is 1 to 75 parts by mass, more preferably 2 to 60 parts by mass, and even more preferably 3 to 50 parts by mass, relative to 100 parts by mass of the total solid content constituting the protective film-forming film, and may be, for example, 4 to 40 parts by mass, 5 to 35 parts by mass, or 6 to 30 parts by mass. When the content of the thermosetting component is equal to or more than the lower limit, the protective film can obtain sufficient adhesion to the workpiece, and the protective film has excellent performance in protecting the workpiece.When the content of the thermosetting component is equal to or less than the upper limit, the protective film has excellent storage stability during storage.

[0063] The thermosetting agent (C) functions as a curing agent for the thermosetting resin (B), particularly for epoxy resins. A preferred thermosetting agent is a compound having two or more functional groups in one molecule that can react with an epoxy group. The functional groups include phenolic hydroxyl groups, alcoholic hydroxyl groups, amino groups, carboxyl groups, and acid anhydrides. Of these, preferred are phenolic hydroxyl groups, amino groups, and acid anhydrides, and more preferred are phenolic hydroxyl groups and amino groups.

[0064] Specific examples of phenol-based hardeners include polyfunctional phenol resins and novolac-type phenol resins.Specific examples of amine-based hardeners include DICY (dicyandiamide).These can be used alone or in combination of two or more.

[0065] The content of the thermosetting agent (C) is preferably 0.1 to 500 parts by mass, more preferably 0.5 to 200 parts by mass, even more preferably 1 to 50 parts by mass, and particularly preferably 1 to 30 parts by mass, relative to 100 parts by mass of the thermosetting resin (B). When the content of the thermosetting agent is equal to or greater than the lower limit, the thermosetting agent is sufficiently cured and protective performance is easily obtained. When the content of the thermosetting agent is equal to or less than the upper limit, the moisture absorption rate of the protective film is suppressed, and the adhesive reliability between the workpiece and the protective film tends to be easily improved. The protective film-forming composition (III-1) may contain the following components in addition to the above-mentioned polymer component (A) and thermosetting component (that is, the thermosetting resin (B) and the thermosetting agent (C)).

[0066] (energy ray curable component) The protective film-forming composition (III-1) may contain an energy ray-curable component. As the energy ray-curable component, a low molecular weight compound (energy ray-polymerizable compound) that contains an energy ray-polymerizable unsaturated group and is polymerized and cured when irradiated with energy rays such as ultraviolet rays and electron beams can be used. Specific examples of such energy ray-polymerizable compounds include acrylate-based compounds such as dipentaerythritol hexaacrylate, 1,6-hexanediol diacrylate, and urethane acrylate-based oligomers. Such compounds have at least one energy ray-polymerizable unsaturated group in the molecule, and usually have a weight average molecular weight of 100 to 30,000, preferably about 300 to 10,000. The content of the energy ray-curable component is preferably 1 to 30 parts by mass, more preferably 5 to 25 parts by mass, relative to 100 parts by mass of the total solid content constituting the protective film-forming film.

[0067] In addition, as the energy ray curable component, an energy ray curable polymer having an energy ray polymerizable unsaturated group bonded to the main chain or side chain of a polymer component may be used. Such an energy ray curable polymer has both a function as a polymer component and a function as a curable component.

[0068] The main skeleton of the energy ray curable polymer is not particularly limited, and may be an acrylic polymer, which is widely used as a polymer component, or may be polyester, polyether, or the like. However, it is particularly preferable to use an acrylic polymer as the main skeleton because of ease of synthesis and control of physical properties.

[0069] Specific examples of the energy ray-polymerizable unsaturated group bonded to the main chain or side chain of the energy ray-curable polymer include a (meth)acryloyl group, etc. The energy ray-polymerizable unsaturated group may be bonded to the energy ray-curable polymer via an alkylene group, an alkyleneoxy group, or a polyalkyleneoxy group.

[0070] The weight average molecular weight (Mw) of the energy ray curable polymer is preferably 10,000 to 2,000,000, and more preferably 100,000 to 1,200,000. The glass transition temperature (Tg) of the energy ray curable polymer is preferably in the range of -60 to 50°C, more preferably -50 to 40°C, and particularly preferably -40 to 20°C.

[0071] The energy beam curable polymer is obtained by reacting an acrylic resin containing a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, or an epoxy group with a substituent reactive with the functional group and an unsaturated group-containing compound having 1 to 5 energy beam polymerizable unsaturated groups per molecule. Examples of the substituent reactive with the functional group include an isocyanate group, a glycidyl group, and a carboxyl group.

[0072] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate.

[0073] The acrylic resin containing a functional group is preferably a copolymer consisting of a (meth)acrylic monomer or a derivative thereof having a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, or an epoxy group, and another (meth)acrylic acid ester monomer or a derivative thereof copolymerizable therewith.

[0074] Examples of the (meth)acrylic monomer having a functional group such as a hydroxy group, a carboxyl group, an amino group, a substituted amino group, or an epoxy group, or a derivative thereof, include 2-hydroxyethyl (meth)acrylate having a hydroxy group; acrylic acid having a carboxyl group; and glycidyl methacrylate having an epoxy group.

[0075] Examples of other (meth)acrylic acid ester monomers copolymerizable with the above monomers or derivatives thereof include alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, butyl (meth)acrylate, etc.; and (meth)acrylates having a cyclic skeleton, specifically cyclohexyl (meth)acrylate, isobornyl acrylate, etc. In addition, the above acrylic resins may be copolymerized with vinyl acetate, acrylonitrile, styrene, etc.

[0076] (Colorant (G)) The protective film-forming film preferably contains a colorant (G). By blending a colorant in the protective film-forming film, when the semiconductor device is incorporated into an apparatus, infrared rays and the like generated from the surrounding devices can be shielded, and malfunction of the semiconductor device due to them can be prevented. In a semiconductor device or semiconductor chip on which a protective film is formed, a product number and the like are usually printed on the surface of the protective film by a laser marking method, but when the protective film contains a colorant, a sufficient contrast difference is obtained between the part of the protective film marked by the laser light and the part that is not, and visibility is improved. As the colorant, organic or inorganic pigments and dyes are used. Pigments are preferable from the viewpoint of heat resistance and the like. As the pigment, carbon black, iron oxide, manganese dioxide, aniline black, activated carbon, etc. are used, but are not limited to these. Among them, carbon black is particularly preferable from the viewpoint of handling and dispersibility. The colorant may be used alone or in combination of two or more kinds.

[0077] The content of the colorant is preferably 0.05 to 35 parts by mass, more preferably 0.1 to 25 parts by mass, and particularly preferably 0.2 to 15 parts by mass, based on 100 parts by mass of the total solid content constituting the protective film-forming film.

[0078] (Cure accelerator (D)) The curing accelerator (D) is used to adjust the curing speed of the protective film-forming film. The curing accelerator is preferably used in particular when an epoxy resin and a heat curing agent are used in combination in the thermosetting component.

[0079] A preferred curing accelerator is 2-phenyl-4,5-dihydroxymethylimidazole, etc. These may be used alone or in combination of two or more.

[0080] The curing accelerator is preferably contained in an amount of 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the thermosetting component. By containing the curing accelerator in the amount within the above range, the adhesive has excellent adhesive properties even when exposed to high temperature and high humidity, and can achieve high adhesive reliability even when exposed to severe reflow conditions.

[0081] (Coupling agent (F)) The coupling agent (F) may be used to improve the adhesive reliability of the protective film to the workpiece. In addition, the use of the coupling agent can improve the water resistance of the protective film obtained by curing the protective film-forming film without impairing the heat resistance of the protective film.

[0082] As the coupling agent, a compound having a group that reacts with a functional group of a polymer component, a thermosetting component, etc. is preferably used. As the coupling agent, a silane coupling agent is preferable. Examples of such coupling agents include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, etc. These can be used alone or in combination of two or more.

[0083] The coupling agent is usually contained in an amount of 0.1 to 20 parts by mass, preferably 0.2 to 10 parts by mass, and more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the polymer component and the thermosetting component combined. If the content of the coupling agent is less than 0.1 part by mass, the above effect may not be obtained, and if it exceeds 20 parts by mass, it may cause outgassing.

[0084] (Filling material (E)) By blending the filler (E) into the protective film-forming film, it becomes possible to adjust the thermal expansion coefficient of the protective film after curing, and by optimizing the thermal expansion coefficient of the protective film after curing with respect to the semiconductor chip, it is possible to improve the adhesive reliability between the workpiece and the protective film. As the filler, an inorganic filler is preferable. It is also possible to reduce the moisture absorption rate of the protective film after curing.

[0085] Preferred inorganic fillers include silica, alumina, talc, calcium carbonate, titanium oxide, iron oxide, silicon carbide, boron nitride, and the like powders, beads obtained by shaping these into spheres, single crystal fibers, and glass fibers. Among these, silica filler and alumina filler are preferred. The inorganic fillers can be used alone or in combination of two or more. The content of the inorganic filler can be 1 to 85 parts by mass, 5 to 80 parts by mass, 10 to 75 parts by mass, 20 to 70 parts by mass, or 30 to 66 parts by mass, relative to 100 parts by mass of the total solid content constituting the protective film-forming film.

[0086] By making the content of the inorganic filler equal to or less than the upper limit, the risk of cracks (fissures) occurring when the protective film-forming film is bent into a roll can be reduced, and by making the content equal to or more than the lower limit, the heat resistance of the protective film can be improved, and the adhesive strength (Z1) tends to be lower.

[0087] (Photopolymerization initiator) When the protective film-forming film contains an energy ray-curable component, the protective film-forming film is irradiated with energy rays such as ultraviolet rays during use to cure the energy ray-curable component. In this case, by including a photopolymerization initiator in the composition, the polymerization and curing time and the amount of light irradiation can be reduced.

[0088] Specific examples of such photopolymerization initiators include 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, phenyl-1-hydroxycyclohexyl-ketone, etc. The photopolymerization initiators may be used alone or in combination of two or more.

[0089] The blending ratio of the photopolymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the energy ray curable component. If it is equal to or more than the lower limit, photopolymerization can be performed to obtain satisfactory protective performance, and if it is equal to or less than the upper limit, generation of residues that do not contribute to photopolymerization can be suppressed, and the curability of the protective film-forming film can be sufficient.

[0090] (Crosslinking agent) In order to adjust the adhesive strength and cohesiveness of the protective film-forming film with the workpiece, a crosslinking agent may be added. Examples of the crosslinking agent include an organic polyvalent isocyanate compound and an organic polyvalent imine compound.

[0091] Examples of the organic polyisocyanate compound include aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, and trimers of these organic polyisocyanate compounds, as well as isocyanate-terminated urethane prepolymers obtained by reacting these organic polyisocyanate compounds with polyol compounds.

[0092] An example of the organic polyisocyanate compound is trimethylolpropane adduct tolylene diisocyanate.

[0093] The organic polyvalent imine compound may, for example, be N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide).

[0094] The crosslinking agent is usually used in a ratio of 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of the polymer component and the energy ray curable polymer.

[0095] (General purpose additive) In addition to the above, various additives may be blended into the protective film-forming film as necessary. Examples of the various additives include tackifiers, leveling agents, plasticizers, antistatic agents, antioxidants, ion trapping agents, gettering agents, and chain transfer agents.

[0096] (solvent) The composition for forming a protective film preferably further contains a solvent. A composition for forming a protective film containing a solvent has good handleability. The solvent is not particularly limited, but preferred examples include hydrocarbons such as toluene; alcohols such as ethanol; esters such as ethyl acetate; and ketones such as acetone and methyl ethyl ketone. The composition for forming a protective film may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio of the solvents can be selected arbitrarily.

[0097] The solvent contained in the composition for forming a protective film is preferably methyl ethyl ketone or the like, since the components contained in the composition can be mixed more uniformly.

[0098] The protective film-forming film obtained by applying and drying the protective film-forming composition composed of the above-mentioned components has adhesion and curability, and is pressed onto a workpiece in an uncured state. The protective film-forming film may be heated during pressing. After curing, a protective film with high impact resistance can be finally obtained, and the film has excellent adhesion and can maintain sufficient protective performance even under harsh conditions of high temperature and high humidity. The protective film-forming film may have a single layer structure, or may have a multilayer structure as long as it contains at least one layer containing the above-mentioned components.

[0099] Method for producing resin film-forming composition A resin film-forming composition such as the protective film-forming composition (III-1) can be obtained by blending the respective components constituting the composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to pre-dilute the ingredients, or the solvent may be used by mixing it with any of the other ingredients without pre-diluting the ingredients. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component may be appropriately adjusted taking into consideration conditions under which each blended component is unlikely to deteriorate, but a temperature of 15 to 30°C is preferred.

[0100] <<Adhesive layer>> The pressure-sensitive adhesive layer is in the form of a sheet or film, and may be energy ray-curable or non-energy ray-curable. In particular, when the adhesive layer is energy ray curable, the adhesive layer can adjust its physical properties before and after curing. After energy ray curing, the adhesive strength between the energy ray cured product of the adhesive layer and the resin film is further reduced, so that not only small-sized (e.g., 1.5 mm×1.5 mm) workpieces with resin film but also relatively large-sized (e.g., 2.5 mm×2.5 mm) workpieces with resin film can be picked up.

[0101] In this specification, the support sheet after the adhesive layer has cured may be referred to as a "cured support sheet" particularly to distinguish it from a support sheet in which the adhesive layer is not cured.

[0102] The adhesive layer may consist of one layer (single layer), or may consist of two or more layers. If it consists of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited.

[0103] In this specification, not limited to the case of pressure-sensitive adhesive layers, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials and thicknesses of each layer is different from each other".

[0104] The thickness of the adhesive layer is not particularly limited, but from the viewpoint of improving embedding of the adhesive layer into the matte surface of the substrate when embedding is required, and from the viewpoint of making it easier to properly pick up the workpiece, the thickness is preferably 1 to 100 μm, more preferably 3 to 60 μm, even more preferably 5 to 30 μm, and particularly preferably 8 to 25 μm. Here, "the thickness of the adhesive layer" means the thickness of the entire adhesive layer, and for example, the thickness of an adhesive layer consisting of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0105] In this specification, the term "thickness", not limited to that of the adhesive layer, means, unless otherwise specified, a value expressed as the average of thicknesses measured at five randomly selected points on the object, and can be obtained using a constant pressure thickness gauge in accordance with JIS K7130.

[0106] The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition (I) containing components for constituting the pressure-sensitive adhesive layer. A preferred pressure-sensitive adhesive composition (I) is, for example, a pressure-sensitive adhesive composition containing a blocked crosslinker (β1) (sometimes simply referred to as "crosslinker (β1)" in this specification) or a non-blocked crosslinker (β2) (sometimes simply referred to as "crosslinker (β2)" in this specification). The pressure-sensitive adhesive composition (I) is applied to a surface on which a pressure-sensitive adhesive layer is to be formed, and dried as necessary, to form a pressure-sensitive adhesive layer at a desired site. The ratio of the contents of the components that do not vaporize at room temperature in the pressure-sensitive adhesive composition (I) is usually the same as the ratio of the contents of the components in the pressure-sensitive adhesive layer.

[0107] In the pressure-sensitive adhesive layer, the proportion of the total content of one or more ingredients contained in the pressure-sensitive adhesive layer, which will be described later, relative to the total mass of the pressure-sensitive adhesive layer does not exceed 100 mass %. Similarly, in the pressure-sensitive adhesive composition (I), the ratio of the total content of one or more components contained in the pressure-sensitive adhesive composition (I), which will be described later, to the total mass of the pressure-sensitive adhesive composition (I) does not exceed 100 mass%.

[0108] The pressure-sensitive adhesive composition (I) may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0109] The drying conditions for the pressure-sensitive adhesive composition (I) are not particularly limited. However, when the pressure-sensitive adhesive composition (I) contains a solvent described below, it is preferable to heat-dry it. The pressure-sensitive adhesive composition (I) containing the solvent is preferably heat-dried, for example, at 70 to 130° C. for 10 seconds to 5 minutes.

[0110] When the adhesive layer is provided on the substrate, for example, the adhesive composition (I) may be applied to the substrate and dried as necessary. Alternatively, for example, the adhesive composition (I) may be applied to a release film and dried as necessary to form an adhesive layer on the release film, and the exposed surface of the adhesive layer may be attached to one surface (e.g., a matte surface) of the substrate to laminate the adhesive layer on the substrate. In this case, the release film may be removed at any timing during the manufacturing process or the use process of the support sheet.

[0111] <Crosslinking agent (β1)> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably contain a block type crosslinking agent (β1). The crosslinking agent (β1) is a block type crosslinking agent and may be a known one. Examples of the crosslinking agent (β1) include compounds in which a crosslinkable group such as an isocyanate group reacts with a blocking agent, and the blocking agent masks the group so that the group cannot crosslink. Such crosslinking agents (β1) (blocked crosslinking agents) are relatively stable at room temperature and can be stored for a long period of time, but at high temperatures such as 130°C or higher, the blocking agent dissociates, the mask structure is eliminated, and the crosslinkable group such as an isocyanate group is regenerated and can act as a crosslinking agent.

[0112] More specifically, the crosslinking agent (β1) may be, for example, a crosslinking agent having both a nurate skeleton (isocyanurate skeleton) that can be considered to be formed by trimerization of diisocyanate and a skeleton derived from other diisocyanates. Such a crosslinking agent (β1) is preferably a crosslinking agent having both a nurate skeleton (isocyanurate skeleton) that can be considered to be formed by trimerization of hexamethylene diisocyanate and a skeleton derived from other hexamethylene diisocyanate.

[0113] The number average molecular weight (Mn) of the crosslinking agent (β1) is preferably 15,000 or less, more preferably 13,000 or less, and may be, for example, any of 9,000 or less, 5,000 or less, and 2,500 or less. By using such a crosslinking agent (β1), it becomes easier to set the adhesive strength (Z2) and adhesive strength (Y0) within the range described below. Furthermore, the embedding property of the adhesive layer on the matte surface of the substrate is improved. Furthermore, even if the support sheet with the workpiece attached thereto is heated at a high temperature of 140°C or more, the effect of being able to normally pick up the workpiece from the support sheet is improved. On the other hand, the lower limit of the number average molecular weight (Mn) of the crosslinking agent (β1) is not particularly limited. For example, a crosslinking agent (β1) having a number average molecular weight of 1000 or more is easier to obtain or prepare. The crosslinking agent (β1) is preferably a crosslinking agent whose number average molecular weight is within any of the above ranges and which has both a nurate skeleton (isocyanurate skeleton) that can be considered to have been formed by trimerization of the above diisocyanate and a skeleton derived from another diisocyanate.

[0114] In this specification, the terms "number average molecular weight" and "weight average molecular weight" are polystyrene-equivalent values ​​measured by gel permeation chromatography (GPC) unless otherwise specified.

[0115] Preferred commercially available crosslinking agents (β1) include, for example, Asahi Kasei Corporation's "Duranate (registered trademark) MF-K60B" (number average molecular weight 12000, viscosity at 25°C 220 mPa·s (solids concentration 60 wt%)), Asahi Kasei Corporation's "Duranate (registered trademark) TPA-B80E" (number average molecular weight 2200, viscosity at 25°C 1800 mPa·s (solids concentration 80 wt%)), Asahi Kasei Corporation's "Duranate (registered trademark) SBN-70D" (number average molecular weight 3100, viscosity at 25°C 3300 mPa·s (solids concentration 70 wt%)), and the like.

[0116] In this specification, the viscosity of the crosslinking agent (β1), its solution or its dispersion is a value measured with an E-type viscometer, unless otherwise specified.

[0117] The crosslinking agent (β1) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0118] In the pressure-sensitive adhesive layer, the content of the crosslinking agent (β1) relative to the total mass of the pressure-sensitive adhesive layer is preferably 3% by mass or more, and may be, for example, 7% by mass or more or 11% by mass or more, while the content is preferably 25% by mass or less, and may be, for example, 20% by mass or less. This is equivalent to saying that in the pressure-sensitive adhesive composition (I), the ratio of the content of the crosslinking agent (β1) to the total content of all components other than the solvent is preferably 3 mass% or more, and may be, for example, either 7 mass% or more or 11 mass% or more, while the ratio is preferably 25 mass% or less, and may be, for example, 20 mass% or less. This is based on the fact that in the process of removing the solvent from the resin composition containing the solvent and forming the resin film, the amount of components other than the solvent usually does not change, and the content ratio of the components other than the solvent is the same between the resin composition and the resin film.Therefore, in this specification, not only in the case of the pressure-sensitive adhesive layer, but also in the case of the resin film obtained by removing the solvent from the resin composition, the content of the components other than the solvent is described below.

[0119] In the pressure-sensitive adhesive layer, when the content ratio of the crosslinking agent (β1) relative to the total mass of the pressure-sensitive adhesive layer is 3 mass% or more, it becomes easier to set the adhesive strength (Z2) and adhesive strength (Z1) within the ranges described below. On the other hand, when the ratio is equal to or less than the upper limit, the other properties of the pressure-sensitive adhesive layer become better. In one embodiment, the ratio may be, for example, any one of 3 to 25 mass%, 7 to 25 mass%, and 11 to 25 mass%, or any one of 3 to 20 mass%, 7 to 20 mass%, and 11 to 20 mass%, although these are just examples of the ratio.

[0120] <Crosslinking agent (β2)> The pressure-sensitive adhesive layer preferably further contains a non-blocking crosslinking agent (β2) that does not fall under the category of the crosslinking agent (β1). The crosslinking agent (β2) may be a known one.

[0121] Since the adhesive layer contains the crosslinking agent (β1) and the crosslinking agent (β2), the adhesive strength (Z2), adhesive strength (Z1) and adhesive strength (Y2) tend to be lower, and even when the thermosetting resin film-forming film and the workpiece are heated at a high temperature of 140°C or higher on the support sheet, the adhesive layer in the support sheet after heating has high pick-up properties that allow the resin film-attached workpiece to be picked up normally from the adhesive layer without being cured with energy rays. The heating at this time can be the same as that described above.

[0122] Examples of the crosslinking agent (β2) include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton). Among these, the crosslinking agent (β2) is preferably an adduct of hexamethylene diisocyanate or an isocyanurate-modified product of hexamethylene diisocyanate, since it is easier to set the adhesive strength (Z2) and adhesive strength (Y0) within the ranges described below.

[0123] The crosslinking agent (β2) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0124] When the pressure-sensitive adhesive layer contains a crosslinking agent (β2), the content ratio of the crosslinking agent (β2) to the total mass of the pressure-sensitive adhesive layer is preferably 0.3% by mass or more, and may be, for example, any one of 0.6% by mass or more, 0.9% by mass or more, and 1.2% by mass or more. On the other hand, the ratio is preferably 15% by mass or less, and may be, for example, 10% by mass or less, 5% by mass or less, or 3% by mass or less. When the content of the crosslinking agent (β2) is equal to or more than the lower limit, the effect obtained by using the crosslinking agent (β2) is enhanced. When the content of the crosslinking agent (β2) is equal to or less than the upper limit, excessive use of the crosslinking agent (β2) is suppressed. Furthermore, the embedding property of the matte surface of the substrate is improved. In one embodiment, the content of the crosslinking agent (β2) may be, for example, any one of 0.3 to 15 parts by mass, 0.6 to 15 parts by mass, 0.9 to 15 parts by mass, and 1.2 to 15 parts by mass, or any one of 0.3 to 10 parts by mass, 0.3 to 5 parts by mass, and 0.3 to 3 parts by mass, although these are only examples of the content of the crosslinking agent (β2).

[0125] In the pressure-sensitive adhesive layer, the ratio of the total content of the crosslinking agent (β1) and the crosslinking agent (β2) to the total mass of the pressure-sensitive adhesive layer is preferably 3 mass% or more, and may be, for example, any one of 7 mass% or more, 11 mass% or more, and 13 mass% or more. On the other hand, the ratio is preferably 40 mass% or less, and may be, for example, 30 mass% or less.

[0126] When the content of the crosslinking agent is equal to or more than the lower limit, the effect obtained by using the crosslinking agent is enhanced. Furthermore, it becomes easier to set the adhesive strength (Z2) and the adhesive strength (Z1) in the range described below. When the content of the crosslinking agent is equal to or less than the upper limit, excessive use of the crosslinking agent is suppressed. In one embodiment, the ratio of the total content may be, for example, any one of 3 to 40 mass%, 7 to 40 mass%, 11 to 40 mass%, and 13 to 40 mass%, or any one of 3 to 30 mass%, 7 to 30 mass%, 11 to 30 mass%, and 13 to 30 mass%, but these are just examples of the ratios.

[0127] <Energy ray curable acrylic resin (Ia)> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably further contain an energy ray-curable acrylic resin (also referred to as "energy ray-curable acrylic resin (Ia)" in this specification). By using a pressure-sensitive adhesive layer containing the energy ray-curable acrylic resin (Ia), the crosslinking agent (β1) and the crosslinking agent (β2), it becomes easier to set the adhesive strength (Z2), the adhesive strength (Z1), the adhesive strength (Y2) and the adhesive strength (Y0) in the ranges described below.

[0128] The energy ray-curable acrylic resin (Ia) may, for example, be a resin having a structure in which an unsaturated group is introduced into the side chain of a non-energy ray-curable acrylic resin.

[0129] [Non-energy ray curable acrylic resin] The non-energy ray curable acrylic resin may be, for example, an acrylic polymer having a constituent unit derived from an alkyl (meth)acrylate ester and a constituent unit derived from a functional group-containing monomer.

[0130] In this specification, the term "(meth)acrylic acid" is a concept that includes both "acrylic acid" and "methacrylic acid". The same applies to terms similar to (meth)acrylic acid. For example, the term "(meth)acryloyl group" is a concept that includes both "acryloyl group" and "methacryloyl group", and the term "(meth)acrylate" is a concept that includes both "acrylate" and "methacrylate".

[0131] The (meth)acrylic acid alkyl ester may, for example, be one in which the carbon number of the alkyl group constituting the alkyl ester is 1 to 20. The alkyl group constituting the alkyl ester may be any one of linear, branched, and cyclic, but is preferably linear or branched.

[0132] Among the (meth)acrylic acid alkyl esters, examples of those in which the alkyl group is linear or branched include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), and the like.

[0133] Among the (meth)acrylic acid alkyl esters, examples in which the alkyl group is cyclic include isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate. Among these, from the viewpoint of further reducing the adhesive strength (Z2) and the adhesive strength (Z1), the (meth)acrylic acid alkyl ester is preferably 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, dodecyl acrylate (lauryl acrylate), and dodecyl methacrylate (lauryl methacrylate).

[0134] Examples of the functional group-containing monomer include those in which the functional group reacts with the crosslinking agent (β1) or the crosslinking agent (β2) to become a crosslinking starting point, and those in which the functional group reacts with a group in an unsaturated group-containing compound described below that can bond (react) with a non-energy ray-curable acrylic resin to enable the introduction of an unsaturated group into a side chain of an acrylic polymer.

[0135] Examples of the functional group-containing monomer include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, and an epoxy group-containing monomer.

[0136] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol. Among these, from the viewpoint of making it possible to further reduce the adhesive strength (Z2) and the adhesive strength (Z1), the hydroxyl group-containing monomer is preferably a hydroxyalkyl methacrylate, and more preferably 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, or 2-hydroxybutyl methacrylate.

[0137] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids (monocarboxylic acids having an ethylenically unsaturated bond) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (dicarboxylic acids having an ethylenically unsaturated bond) such as fumaric acid, itaconic acid, maleic acid and citraconic acid; anhydrides of the ethylenically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyalkyl esters such as 2-carboxyethyl methacrylate.

[0138] Examples of the epoxy group-containing monomer include glycidyl group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate.

[0139] The functional group-containing monomer is preferably a hydroxyl group-containing monomer.

[0140] The non-energy ray-curable acrylic resin may have a constituent unit derived from another monomer that does not fall into either the constituent unit derived from an alkyl (meth)acrylate ester or the constituent unit derived from the functional group-containing monomer.

[0141] The other monomer is not particularly limited as long as it is copolymerizable with the (meth)acrylic acid alkyl ester and the like. Examples of the other monomers include styrene, α-methylstyrene, vinyl toluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.

[0142] The constituent units derived from the (meth)acrylic acid alkyl ester, the constituent units derived from the functional group-containing monomer, and the constituent units derived from the other monomers contained in the non-energy ray-curable acrylic resin may each be of only one type or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0143] In the non-energy ray-curable acrylic resin, the content of structural units derived from an alkyl (meth)acrylate is preferably 65 to 99 mass % based on the total amount of structural units.

[0144] In the non-energy ray-curable acrylic resin, the content of the structural unit derived from the functional group-containing monomer is preferably 1 to 35 mass % based on the total amount of the structural units.

[0145] In the non-energy ray-curable acrylic resin, the content of the structural units derived from the other monomers is preferably 0 to 10% by mass based on the total amount of the structural units.

[0146] The energy ray-curable acrylic resin (Ia) can be obtained, for example, by reacting the functional group in the non-energy ray-curable acrylic resin with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group.

[0147] [Unsaturated group-containing compound] The unsaturated group-containing compound is a compound that has, in addition to the energy ray-polymerizable unsaturated group, a group that can bond to the non-energy ray-curable acrylic resin by reacting with a functional group in the non-energy ray-curable acrylic resin. Examples of the energy ray-polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (ethenyl group), and an allyl group (2-propenyl group), and the like, with a (meth)acryloyl group being preferred. Examples of the group capable of bonding to the functional group in the non-energy ray-curable acrylic resin include an isocyanate group and a glycidyl group capable of bonding to a hydroxyl group or an amino group, and a hydroxyl group and an amino group capable of bonding to a carboxy group or an epoxy group.

[0148] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate.

[0149] When the functional group in the non-energy ray curable acrylic resin is reacted with an unsaturated group-containing compound having an energy ray polymerizable unsaturated group to obtain the energy ray curable acrylic resin (Ia), the total number of moles of the functional group-bondable group in the unsaturated group-containing compound relative to the total number of moles of the functional group in the non-energy ray curable acrylic resin is preferably 0.35 to 0.75 times, and may be, for example, 0.5 to 0.75 times, 0.35 to 0.6 times, or 0.5 to 0.6 times. By having the total number of moles of the functional group-bondable group in such a range, the adhesive strength (Z1) can be made smaller, and the pick-up property of the workpiece from the cured support sheet tends to be made higher. On the other hand, the total number of moles of groups capable of bonding to the functional groups in the unsaturated group-containing compound is preferably 1 or less times the total number of moles of the functional groups in the non-energy ray-curable acrylic resin.

[0150] The energy ray-curable acrylic resin (Ia) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0151] When the adhesive layer and the adhesive composition (I) contain the energy ray curable acrylic resin (Ia), the content ratio of the energy ray curable acrylic resin (Ia) in the adhesive layer relative to the total mass of the adhesive layer is preferably 50 to 95 mass%, and may be, for example, any of 65 to 95 mass% and 75 to 95 mass%, or any of 50 to 90 mass%, 50 to 85 mass%, and 60 to 85 mass%, or may be 65 to 85 mass%. When the ratio is equal to or greater than the lower limit, the pick-up property that allows the above-mentioned workpiece to be picked up from the support sheet without any abnormality is improved. When the ratio is equal to or less than the upper limit, the embedding property of the adhesive layer on the matte surface of the substrate is improved.

[0152] <Other ingredients> The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may contain other components that do not fall under any of the energy ray-curable acrylic resin (Ia), the crosslinking agent (β1), and the crosslinking agent (β2), within a range that does not impair the effects of the present invention. Examples of the other components include an energy ray curable compound (α), a photopolymerization initiator (γ), and additives.

[0153] The other components contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0154] <Energy ray curable compound (α)> The energy ray-curable compound (α) is not particularly limited as long as it is an energy ray-curable component that does not fall under the category of the energy ray-curable acrylic resin (Ia).

[0155] Examples of the energy ray-curable compound (α) include monomers or oligomers that have an energy ray-polymerizable unsaturated group and can be cured by irradiation with energy rays. One molecule of the energy ray-curable compound (α) has one or two or more, and may have three or more, energy ray-polymerizable unsaturated groups, but preferably has one or two. An example of the energy ray-polymerizable unsaturated group is a (meth)acryloyl group.

[0156] The molecular weight of the energy ray-curable compound (α) is not particularly limited, but is preferably not more than 500. By using such an energy ray-curable compound (α), the embedding property of the pressure-sensitive adhesive layer on the matte surface of the substrate is improved. The molecular weight of the energy ray curable compound (α) is preferably 100 to 500. When the molecular weight is equal to or more than the lower limit, the structure of the pressure-sensitive adhesive layer becomes more stable. However, these are only examples of the molecular weight of the energy ray curable compound (α).

[0157] The energy ray-curable compound (α) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0158] In the adhesive layer, the content ratio of the energy ray curable compound (α) to the total mass of the adhesive layer is preferably 0 to 5 mass%. The higher the ratio, the higher the effect obtained by using the energy ray curable compound (α). When the ratio is equal to or less than the upper limit, the adhesive layer can embed the matte surface of the substrate more easily, and further, even when the support sheet with the workpiece attached thereto is heated at a high temperature of 140°C or more, the effect of being able to normally pick up the workpiece from the support sheet is improved.

[0159] [Photopolymerization initiator (γ)] When the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) contain either one or both of the energy ray-curable acrylic resin (Ia) and the energy ray-curable compound (α), the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably contain a photopolymerization initiator (γ). The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) containing the photopolymerization initiator (γ) sufficiently undergo a curing reaction even when irradiated with a relatively low-energy energy ray such as ultraviolet light.

[0160] Examples of the photopolymerization initiator (γ) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, and benzoin dimethyl ketal; acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-hydroxy-1-(4-(4- Acetophenone compounds such as (2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-4'-morpholinobutylphenone, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one; bis(2,4,6-trimethylbenzoyl)phenyl acylphosphine oxide compounds such as phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; oxime ester compounds such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); sulfide compounds such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-ketol compounds such as 1-hydroxycyclohexyl phenyl ketone Examples of suitable amines include azo compounds such as azobisisobutyronitrile, titanocene compounds such as titanocene, thioxanthone compounds such as thioxanthone, peroxide compounds, diketone compounds such as diacetyl, benzyl, dibenzyl, benzophenone, 2,4-diethylthioxanthone, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone, and quinone compounds such as 1-chloroanthraquinone and 2-chloroanthraquinone. As the photopolymerization initiator (γ), for example, a photosensitizer such as an amine can be used.

[0161] The photopolymerization initiator (γ) contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0162] The photopolymerization initiator (γ) has high heat resistance even under heating conditions of 140° C. or more, and from the viewpoint of further reducing the adhesive strength (Z1), 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, phenyl-1-hydroxycyclohexyl-ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)phenyl ... It is preferable that the oxime is one or more selected from the group consisting of 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime).

[0163] As these photopolymerization initiators (γ), the following are commercially available products. 2-Hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one: "Omnirad (registered trademark) 127" manufactured by IGM Resins Phenyl-1-hydroxycyclohexyl-ketone (IGM Resins "Omnirad® 184") 2-Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one: "Omnirad (registered trademark) 907" manufactured by IGM Resins 2-Benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone: "Omnirad (registered trademark) 369" manufactured by IGM Resins 2-Dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one: "Omnirad (registered trademark) 379EG" manufactured by IGM Resins 2,4,6-trimethylbenzoyldiphenylphosphine oxide: "Omnirad (registered trademark) TPO H" manufactured by IGM Resins Ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) "Omnirad (registered trademark) OXE02" manufactured by IGM Resins

[0164] When the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) contain a photopolymerization initiator (γ), the content of the photopolymerization initiator (γ) in the pressure-sensitive adhesive layer is preferably 1 to 5 parts by mass relative to 100 parts by mass of the total content of the energy ray curable acrylic resin (Ia) and the energy ray curable compound (α), and may be, for example, any of 1.5 to 4.5 parts by mass and 2 to 4 parts by mass. When the content of the photopolymerization initiator (γ) is equal to or more than the lower limit, the effect obtained by using the photopolymerization initiator (γ) is further enhanced. When the content of the photopolymerization initiator (γ) is equal to or less than the upper limit, excessive use of the photopolymerization initiator (γ) is suppressed. Here, when the adhesive layer does not contain the energy ray curable acrylic resin (Ia), the content of the energy ray curable acrylic resin (Ia) in the adhesive layer is set to 0 parts by mass, and when the adhesive layer does not contain the energy ray curable compound (α), the content of the energy ray curable compound (α) in the adhesive layer is set to 0 parts by mass.

[0165] [Additives] Examples of the additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, colorants (pigments, dyes), sensitizers, tackifiers, reaction retarders, and crosslinking accelerators (catalysts). The reaction retarder is, for example, a component that suppresses the progress of unintended crosslinking reaction in the pressure-sensitive adhesive composition (I) during storage due to the action of a catalyst mixed in the pressure-sensitive adhesive composition (I). Examples of reaction retarders include those that form a chelate complex by chelating with a catalyst, and more specifically, components having two or more carbonyl groups (-C(=O)-) in one molecule.

[0166] The additives contained in the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0167] The content of the additive in the pressure-sensitive adhesive composition (I) is not particularly limited and may be appropriately selected depending on the type of additive.

[0168] [solvent] The pressure-sensitive adhesive composition (I) may contain a solvent. By containing a solvent, the pressure-sensitive adhesive composition (I) has improved suitability for application to a surface to be coated.

[0169] The solvent is preferably an organic solvent, and examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.

[0170] The pressure-sensitive adhesive composition (I) may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0171] The content of the solvent in the pressure-sensitive adhesive composition (I) is not particularly limited and may be appropriately adjusted.

[0172] [Gas Generator] The pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) preferably do not contain a gas generating agent as the other component. The gas generating agent is a component that generates gas by an external stimulus such as heating or light irradiation. By using a pressure-sensitive adhesive layer containing a gas generating agent, gas is generated at the interface between the pressure-sensitive adhesive layer and the adherend, and the peeling force (adhesive force) between the pressure-sensitive adhesive layer or its energy ray cured product and the adherend can be reduced by the pressure of the gas. Therefore, by using a pressure-sensitive adhesive layer containing a gas generating agent, it may be possible to easily pick up the resin-film-attached workpiece from the cured product of the pressure-sensitive adhesive layer in the pick-up step in the manufacturing method of the resin-film-attached workpiece described later. However, when an adhesive layer containing a gas generating agent is used, it may be difficult to adjust the peeling force (adhesive force) between the adhesive layer or its energy ray cured product and the adherend, and excessive fluctuations in the peeling force may not be suppressed. In such a case, the pick-up of the workpiece from the cured product of the adhesive layer in the pick-up process may become unstable. Furthermore, the gas generating agent may remain at the part of the workpiece that was in contact with the cured product of the adhesive layer. In such a case, the gas generating agent may be taken into the interior of the semiconductor device, which is the final target, and the reliability of the semiconductor device may be reduced. Therefore, it is preferable that the pressure-sensitive adhesive layer and the pressure-sensitive adhesive composition (I) do not contain a gas-generating agent.

[0173] Among the gas generating agents, examples of components that generate gas when irradiated with light include carboxylic acid compounds (compounds having a carboxy group), salts of the carboxylic acid compounds, tetrazole, salts of tetrazole, tetrazole derivatives (compounds having a structure in which one or two hydrogen atoms in tetrazole are replaced with groups other than hydrogen atoms), and salts of the tetrazole derivatives. The carboxylic acid compound and its salt generate carbon dioxide gas in response to an external stimulus, and the tetrazole and its salt, and the tetrazole derivative and its salt generate nitrogen gas in response to an external stimulus.

[0174] In this specification, unless otherwise specified, the term "group" includes not only an atomic group formed by bonding multiple atoms, but also a single atom.

[0175] The gas generating agent may be, for example, a component that has heat resistance and does not decompose under temperature conditions of about 200° C. or less, but generates gas when irradiated with light such as ultraviolet light.

[0176] <One embodiment of the pressure-sensitive adhesive layer> An example of a preferred pressure-sensitive adhesive layer and pressure-sensitive adhesive composition (I) includes one containing a crosslinking agent (β1), a crosslinking agent (β2), an energy ray-curable acrylic resin (Ia) and a photopolymerization initiator (γ).

[0177] In terms of obtaining the effects of the present invention more significantly, a more preferred pressure-sensitive adhesive layer is, for example, a pressure-sensitive adhesive layer containing a crosslinking agent (β1) and a crosslinking agent (β2), in which the number average molecular weight of the crosslinking agent (β1) is not more than 15000. Such a pressure-sensitive adhesive layer is energy ray-curable and may further contain an energy ray-curable acrylic resin (Ia) and a photopolymerization initiator (γ).

[0178] In the adhesive layer, the ratio of the total content of the crosslinking agent (β1), the crosslinking agent (β2), the energy ray curable acrylic resin (Ia), and the photopolymerization initiator (γ) to the total mass of the adhesive layer is preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more, and may be, for example, any of 97 mass% or more and 99 mass% or more. When the ratio is equal to or more than the lower limit, the effect of being able to normally pick up the resin film-attached workpiece from the adhesive layer is further enhanced. On the other hand, the ratio is equal to or less than 100 mass%.

[0179] <Method for producing pressure-sensitive adhesive composition (I)> The adhesive composition (I) can be obtained by blending the components for constituting the adhesive composition (I), such as a crosslinking agent (β1) if necessary, a crosslinking agent (β2) if necessary, an energy ray-curable acrylic resin (Ia) if necessary, and the other components (e.g., one or more selected from the group consisting of an energy ray-curable compound (α), a photopolymerization initiator (γ), an additive, and a solvent) if necessary. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0180] <<Base material>> The substrate is in the form of a sheet or film, and examples of the constituent materials thereof include various resins. Examples of the resin include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resin; ethylene-based copolymers (copolymers obtained by using ethylene as a monomer) such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, and ethylene-norbornene copolymer; vinyl chloride-based resins (copolymers obtained by using vinyl chloride as a monomer) such as polyvinyl chloride and vinyl chloride copolymer. resins having aromatic ring groups); polystyrene; polycycloolefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, and wholly aromatic polyesters in which all constituent units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylic acid esters; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene oxides; polyphenylene sulfides; polysulfones; and polyether ketones. The resin may also be a polymer alloy such as a mixture of the polyester and another resin. The polymer alloy of the polyester and another resin is preferably one in which the amount of the resin other than the polyester is relatively small. Examples of the resin include crosslinked resins in which one or more of the resins exemplified above are crosslinked; and modified resins such as ionomers using one or more of the resins exemplified above. Among the above, the resin constituting the substrate is preferably polypropylene or polybutylene terephthalate, in that it provides the substrate with higher heat resistance at high temperatures (eg, 140° C. or higher) and flexibility.

[0181] The resin constituting the substrate may be of only one type, or of two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0182] The substrate may contain, in addition to the main constituent materials such as the resin, various known additives such as fillers, colorants, antioxidants, organic lubricants, catalysts, softeners (plasticizers), and the like.

[0183] In the support sheet, when the pressure-sensitive adhesive layer is energy ray curable, the substrate is preferably one that transmits energy rays, and is preferably transparent.

[0184] At least one surface of a substrate may have a relatively large degree of unevenness and be rough. Such a surface has a relatively low gloss and appears to have been matte-finished, and is therefore sometimes referred to as a "matte surface." The substrate may have at least one matte surface, both matte surfaces, or one matte surface and the other glossy surface with a small degree of unevenness. In the support sheet, the adhesive layer is preferably provided on the matte surface of the substrate. When both sides of the substrate are matte surfaces, the adhesive layer is preferably provided on the matte surface having a larger surface roughness (Ra).

[0185] The matte surface of the substrate is a surface of the substrate having a roughness equal to or greater than a certain value, and has a low gloss, so that it can be clearly identified by its appearance. Substrates having at least one matte surface are commercially available, and can also be prepared by known methods.

[0186] The surface roughness (Ra) of the matte surface of the substrate is preferably 0.05 μm or more, and may be, for example, any one of 0.1 μm or more, 0.4 μm or more, and 0.7 μm or more. When the surface roughness is equal to or more than the lower limit, blocking of the substrates when the substrates are stacked and stored is more easily suppressed. The upper limit of the surface roughness (Ra) of the matte surface of the substrate is not particularly limited. For example, the surface roughness is preferably 2 μm or less so that the surface irregularity does not become excessively large. In one embodiment, the surface roughness (Ra) of the matte surface of the substrate may be, for example, any one of 0.05 to 2 μm, 0.1 to 2 μm, 0.4 to 2 μm, and 0.7 to 2 μm, although these are just examples of the surface roughness.

[0187] In this specification, the term "surface roughness (Ra)" is not limited to the matte surface of the substrate, but means the so-called arithmetic mean roughness determined in accordance with JIS B0601:2001.

[0188] The surface roughness (Ra) of the glossy surface of the substrate is preferably less than 0.05 μm, and may be, for example, 0.04 μm or less. When the surface roughness is in this range, the average light transmittance of the support sheet described below in the wavelength range of 400 to 800 nm becomes higher. The lower limit of the surface roughness (Ra) of the glossy surface of the substrate is not particularly limited. For example, the surface roughness is preferably 0.01 μm or more in order to prevent blocking of the substrate when the substrates are stored in a stacked state. In one embodiment, the surface roughness (Ra) of the glossy surface of the substrate may be, for example, any one of 0.01 μm or more and less than 0.05 μm, and 0.01 to 0.04 μm, although these are just examples of the surface roughness.

[0189] The surface roughness (Ra) of both sides of the substrate can be adjusted, for example, by the molding conditions of the substrate, the surface treatment conditions, etc. Examples of the surface treatment include a roughening treatment such as sandblasting or solvent treatment, and a smoothing treatment such as polishing.

[0190] In order to adjust the adhesiveness with the pressure-sensitive adhesive layer provided thereon, the surface of the substrate may be subjected to oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromic acid treatment, hot air treatment, lipophilic treatment, hydrophilic treatment, etc. The surface of the substrate may be treated with a primer.

[0191] The substrate may consist of one layer (single layer), or may consist of two or more layers. When the substrate consists of multiple layers, the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited.

[0192] The thickness of the substrate is preferably 50 to 300 μm, and more preferably 60 to 100 μm. By setting the thickness of the substrate within this range, the heat resistance (e.g., 140° C. or higher), flexibility, and suitability for attachment to a workpiece of the support sheet are improved. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0193] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.

[0194] <<Release film>> The release film may be a known one. More specifically, the release film may be, for example, a release film substrate having one or both sides treated for release. A polyethylene terephthalate film is preferred as the release film substrate. The release treated surface can be formed by subjecting the surface of the substrate for the release film to a release treatment with a known release treating agent. The thickness of the release film may be, for example, 2 to 300 μm, and is preferably 20 to 100 μm.

[0195] Next, the physical properties of the composite sheet for resin film formation will be described.

[0196] <Adhesive strength (Z2)> The adhesive strength (Z2) is 1500 mN / 25 mm or less, preferably 1300 mN / 25 mm or less, more preferably 1100 mN / 25 mm or less, and even more preferably 900 mN / 25 mm or less. The smaller the adhesive strength (Z2), the more remarkable the effect of being able to normally pick up the resin-film-attached workpiece from the adhesive layer even when the thermosetting resin film-forming film and the workpiece are heated at a high temperature of 140° C. or more on the support sheet when preparing the resin-film-attached workpiece, without curing the adhesive layer in the support sheet with energy rays.

[0197] The lower limit of the adhesive strength (Z2) is not particularly limited. For example, the adhesive strength (Z2) may be 200 mN / 25 mm or more, 350 mN / 25 mm or more, or 500 mN / 25 mm or more. The adhesive strength (Z2) may be, for example, any one of 200 to 1500 mN / 25 mm, 200 to 1300 mN / 25 mm, 350 to 1100 mN / 25 mm, and 500 to 900 mN / 25 mm, although these are just examples of the adhesive strength (Z2).

[0198] The adhesive strength (Z2) can be measured, for example, by the following method. First, a test piece having a width of 25 mm is cut out from the composite sheet for forming a resin film. Next, this test piece (composite sheet for resin film formation) is attached to the mirror surface of a silicon mirror wafer having a thickness of 650 μm by the resin film-forming film in the composite sheet, thereby preparing a silicon mirror wafer with the test piece attached. The attachment is preferably performed at 70° C. and the attachment speed is preferably 300 mm / min.

[0199] Next, the silicon mirror wafer with the test piece attached is heated at 140° C. for 2 hours. Next, the silicon mirror wafer with the test piece after heating is cooled down to 23°C by natural cooling, and then the support sheet consisting of the adhesive layer and the substrate is peeled off from the silicon mirror wafer with the resin film at a peeling speed of 300mm / min at room temperature. At this time, the support sheet is peeled off in its length direction so that the surface of the silicon mirror wafer with the resin film to which the support sheet was attached forms an angle of 180° with the surface of the support sheet to which the resin film was attached, that is, a so-called 180° peeling is performed. Then, the load (peel force) during this 180° peeling is measured, the measurement length is 50mm, and the first 5mm and the last 5mm of the measurement are excluded from the effective value. The average value of the measured values ​​is adopted as the adhesive force (mN / 25mm). In this embodiment, such a peel strength (Z2) measurement may be performed on two or more test pieces (composite sheets for forming a resin film), and the average value of the obtained multiple measured values ​​may be used as the adhesive strength (Z2).

[0200] <Adhesive strength (Z1)> The thermosetting resin film-forming film in the composite sheet for resin film formation is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is energy ray cured, and the adhesive strength (Z1) between the energy ray cured product of the pressure-sensitive adhesive layer and the resin film (in this specification, it may be simply referred to as "adhesive strength (Z1)") is measured. The adhesive strength (Z1) is preferably 500mN / 25mm or less, more preferably 450mN / 25mm or less, and may be, for example, 400mN / 25mm or less. The smaller the adhesive strength (Z1), the higher the pick-up property of the workpiece with the resin film from the cured support sheet tends to be. And, not only a small size (e.g., 1.5mm x 1.5mm) of the workpiece with the resin film, but also a relatively large size (e.g., 2.5mm x 2.5mm) of the workpiece with the resin film can be picked up.

[0201] The lower limit of the adhesive strength (Z1) is not particularly limited. For example, the adhesive strength (Z1) may be 30 mN / 25 mm or more, 40 mN / 25 mm or more, or 50 mN / 25 mm or more. The adhesive strength (Z1) may be, for example, any one of 30 to 500 mN / 25 mm, 35 to 480 mN / 25 mm, 40 to 450 mN / 25 mm, 45 to 420 mN / 25 mm, and 50 to 400 mN / 25 mm, although these are just examples of the adhesive strength (Z1).

[0202] The adhesive strength (Z1) can be measured, for example, by the following method. First, a test piece having a width of 25 mm is cut out from the composite sheet for forming a resin film. Next, this test piece (composite sheet for resin film formation) is attached to the mirror surface of a silicon mirror wafer having a thickness of 650 μm by the resin film-forming film in the composite sheet, thereby preparing a silicon mirror wafer with the test piece attached. The attachment is preferably performed at 70° C. and the attachment speed is preferably 300 mm / min.

[0203] Next, the silicon mirror wafer with the test piece attached is heated at 140° C. for 2 hours. Next, the silicon mirror wafer with the heated test piece was allowed to cool until its temperature reached 23°C, and then it was placed under illumination with an illumination intensity of 230mW / cm 2 , light intensity 200mJ / cm 2 Under the above condition, the adhesive layer in the silicon mirror wafer with the test piece after cooling is irradiated with energy rays through the substrate to harden the adhesive layer in the test piece.

[0204] Next, at room temperature, the support sheet consisting of the adhesive layer and the substrate is peeled off from the resin-coated silicon mirror wafer at a peeling speed of 300 mm / min. At this time, the support sheet is peeled off in its length direction so that the surface of the resin-coated silicon mirror wafer to which the support sheet was attached forms an angle of 180° with the surface of the support sheet to which the resin film was attached, that is, a so-called 180° peeling is performed. Then, the load (peeling force) during this 180° peeling is measured, the measurement length is 50 mm, and the first 5 mm and the last 5 mm of the measurement are excluded from the effective value. The average value of the measured values ​​is adopted as the adhesive force (mN / 25 mm). In this embodiment, such a peel strength (Z1) measurement may be performed on two or more test pieces (composite sheets for forming a resin film), and the average value of the obtained multiple measured values ​​may be used as the adhesive strength (Z1).

[0205] <Adhesive strength (Y0)> The support sheet is attached to the surface of a stainless steel (SUS) plate using the adhesive layer, and the stainless steel plate with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C. When the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, the adhesive strength (Y0) is 2000 mN / 25 mm or more. In the manufacturing method of the resin film-attached workpiece described later, a first laminated composite sheet, which is composed of the support sheet, the thermosetting resin film-forming film, and the workpiece laminated together, is fixed to the fixing jig by the adhesive layer therein. Furthermore, a second laminated composite sheet, in which a plurality of workpieces with the resin film-forming film are held, and a third laminated composite sheet, in which a plurality of workpieces with the resin film are aligned and held, are produced on one support sheet fixed to the fixing jig. In these cases, by using a resin film-forming composite sheet including the support sheet, peeling of the first laminated composite sheet, the second laminated composite sheet, or the third laminated composite sheet fixed to the fixing jig from the fixing jig can be suppressed. For example, even if the device shakes during any process during the manufacture of a resin-film-coated workpiece, or the first laminate composite sheet, the second laminate composite sheet or the third laminate composite sheet fixed to a fixing jig shakes during their transport, peeling of the first laminate composite sheet, the second laminate composite sheet or the third laminate composite sheet fixed to the fixing jig from the fixing jig (in other words, peeling of the support sheet from the fixing jig) can be suppressed.

[0206] The adhesive strength (Y0) may be, for example, any one of 2500 mN / 25 mm or more, 3000 mN / 25 mm or more, 3500 mN / 25 mm or more, and 4000 mN / 25 mm or more. The greater the adhesive strength (Y0), the greater the effect of suppressing peeling of the first laminated composite sheet, the second laminated composite sheet, or the third laminated composite sheet from the fixing jig. The upper limit of the adhesive strength (Y0) is not particularly limited. For example, in terms of compatibility between the adhesive strength (Y0) and other physical properties of the adhesive layer, the adhesive strength (Y0) is preferably 10000 mN / 25 mm or less, may be 9000 mN / 25 mm or less, may be 8000 mN / 25 mm or less, or may be 7000 mN / 25 mm or less. In one embodiment, the adhesive strength (Y0) may be, for example, any one of 2500 to 10000 mN / 25 mm, 3000 to 9000 mN / 25 mm, 3500 to 8000 mN / 25 mm, and 4000 to 7000 mN / 25 mm, although these are just examples of the adhesive strength (Y0).

[0207] The adhesive strength (Y0) can be measured, for example, by the following method. First, a test piece of a support sheet having a width of 25 mm is cut out from a composite sheet for forming a resin film. Next, the test piece (support sheet) is attached to one side of a 1000 μm thick SUS plate by the adhesive layer in the support sheet to prepare a SUS plate with a test piece attached. The attachment is preferably performed at room temperature, at an attachment speed of 290 to 310 mm / min, and with an attachment pressure of 0.3 MPa, using a laminating roller. The SUS plate with the test piece attached is left to stand at a temperature of 23° C. for 30 minutes. Next, at room temperature, the test piece is peeled off from the SUS plate after the static storage at a peeling speed of 300 mm / min. At this time, the test piece is peeled off in the length direction so that the surface of the SUS plate to which the test piece was attached forms an angle of 180° with the surface of the test piece to which the SUS plate was attached, that is, a so-called 180° peel is performed. Then, the load (peel force) at this 180° peel is measured, and the measurement length is set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (Y0) (mN / 25 mm). In this embodiment, such measurements of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measurements may be used as the adhesive strength (Y0).

[0208] <Adhesive strength (Y2)> When the support sheet is attached to the surface of a stainless steel (SUS) plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) (sometimes simply referred to as "adhesive strength (Y2)" in this specification) between the adhesive layer after heating and the stainless steel plate is measured, it is preferable that the adhesive strength (Y2) is 6000 mN / 25 mm or less. In the manufacturing method of the resin film-attached workpiece, which will be described later, a first laminated composite sheet is prepared in which the base material, the adhesive layer, the thermosetting resin film-forming film, and the workpiece are laminated in this order in the thickness direction, and the peripheral portion of the adhesive layer of the first laminated composite sheet is fixed to a fixing jig. Furthermore, a second laminated composite sheet in which a plurality of workpieces with the resin film-forming film are held on one support sheet fixed to the fixing jig, and a third laminated composite sheet in which a plurality of workpieces with the resin film are aligned and held are prepared. By using the resin film-forming composite sheet including the support sheet, the third laminated composite sheet can be peeled off from the fixing jig without further curing the adhesive layer with energy rays, and furthermore, the adhesive layer can be prevented from remaining on the fixing jig. Therefore, after the heated third laminated composite sheet is peeled off from the fixing jig, the first laminated composite sheet can be attached to the fixing jig again and fixed. In this way, the composite sheet for resin film formation, which includes the support sheet, makes it possible to employ a highly versatile method for manufacturing a workpiece with a resin film.

[0209] The adhesive strength (Y2) may be, for example, any one of 5000 mN / 25 mm or less, 3800 mN / 25 mm or less, and 2600 mN / 25 mm or less. The smaller the adhesive strength (Y2), the easier it is to peel the second and third laminated composite sheets from the fixing jig, as described above. On the other hand, the adhesive strength (Y2) is preferably 2000 mN / 25 mm or more. By using such a support sheet, when the second laminated composite sheet is heated while being fixed to the fixing jig to produce a third laminated composite sheet in the heating step of the manufacturing method of the resin film-attached workpiece described later, unintended peeling of the third laminated composite sheet from the fixing jig is suppressed. In one embodiment, the adhesive strength (Y2) may be, for example, any one of 2000 to 6000 mN / 25 mm, 2000 to 5000 mN / 25 mm, 2000 to 3800 mN / 25 mm, and 2000 to 2600 mN / 25 mm, although these are just examples of the adhesive strength (Y2).

[0210] The adhesive strength (Y2) can be measured, for example, by the following method. That is, a SUS plate with a test piece is prepared in the same manner as in the measurement of adhesive strength (Y0). Next, the obtained SUS plate with the test piece attached is heated at 140°C for 2 hours. Next, the SUS plate with the test piece is cooled to 23°C by natural cooling, and then the test piece is peeled off from the SUS plate at room temperature at a peeling speed of 300mm / min. At this time, the test piece is peeled off in its length direction so that the surface of the SUS plate to which the test piece was attached forms an angle of 180° with the surface of the SUS plate to which the test piece was attached, that is, a so-called 180° peeling is performed. Then, the load (peel force) at this 180° peeling is measured, and the measurement length is set to 50mm, and the measurement value at the first 5mm length and the measurement value at the last 5mm length are excluded from the effective value. Then, the average value of the measured values ​​is adopted as the adhesive strength (Y2) (mN / 25mm). In this embodiment, such measurement of the peel strength may be performed on two or more test pieces (support sheets), and the average value of the obtained measured values ​​may be used as the adhesive strength (Y2).

[0211] In this specification, the fixing jig is a known one, an example of which is a ring frame. The fixing jig is preferably made of a metal such as SUS.

[0212] <Method of adjusting adhesive strength of adhesive layer> The various adhesive strengths of the pressure-sensitive adhesive layer described above, i.e., the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating at 140°C; the adhesive strength (Z1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the resin film when the pressure-sensitive adhesive layer is energy ray-cured after heating at 140°C; the adhesive strength (Y2) between the pressure-sensitive adhesive layer and the stainless steel plate after heating at 140°C, and the adhesive strength (Y0) between the pressure-sensitive adhesive layer and the SUS plate, can be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer. For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the adhesive strength (Y0) can be increased by including in the adhesive layer an energy ray-curable acrylic resin (Ia) having fewer unreacted functional groups derived from the acrylic polymer (in other words, having fewer functional groups capable of reacting with the crosslinking agent (β2)). For example, by reducing the content of the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the adhesive strength (Y0) can be increased.

[0213] For example, in an adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) having a ring structure, the adhesive strength (Z2), adhesive strength (Z1) and adhesive strength (Y2) tend to be smaller than when a crosslinking agent having a chain structure without a ring structure is used. For example, in a pressure-sensitive adhesive layer containing an energy ray-curable acrylic resin (Ia) and a crosslinking agent (β2), by using a crosslinking agent (β2) that does not have a urethane bond, the adhesive strength (Z2), adhesive strength (Z1) and adhesive strength (Y2) tend to be smaller than when a crosslinking agent having a urethane bond, such as a trimethylolpropane adduct of diisocyanate, is used. For example, when the pressure-sensitive adhesive layer does not contain the energy ray-curable compound (α), the adhesive strength (Z2) and adhesive strength (Y2) can be made smaller than when the pressure-sensitive adhesive layer contains the energy ray-curable compound (α). For example, when using an energy ray-curable acrylic resin (Ia) obtained by reacting a functional group (e.g., a hydroxyl group) in the acrylic polymer with a group capable of bonding to the functional group in the unsaturated group-containing compound (e.g., an isocyanate group in (meth)acryloyloxyethyl isocyanate), the adhesive strength (Z2), adhesive strength (Z1) and adhesive strength (Y2) can be reduced by including in the adhesive layer an energy ray-curable acrylic resin (Ia) having a large amount of unreacted functional groups derived from the acrylic polymer (in other words, having a large amount of functional groups capable of reacting with the crosslinking agent (β1) or the crosslinking agent (β2)). For example, by increasing the total content of the crosslinking agent (β1) and the crosslinking agent (β2) in the pressure-sensitive adhesive layer, the adhesive strength (Z2), the adhesive strength (Z1) and the adhesive strength (Y2) can be reduced.

[0214] <Average light transmittance (400-800 nm) of support sheet (L1)> The average value (L1) of the light transmittance (400-800 nm) of the support sheet (sometimes simply referred to in this specification as "average value (L1) of the light transmittance of the support sheet" or "average value (L1)") is preferably 80% or more, and may be, for example, either 82% or more or 83.5% or more. When the average value (L1) of the light transmittance (400-800 nm) is equal to or more than the lower limit, inspection accuracy is improved when inspecting the resin-coated workpiece for damage such as cracks and chips (e.g. chipping) through the support sheet while the resin-coated workpiece is held on the support sheet. The upper limit of the average light transmittance (L1) of the support sheet is not particularly limited. For example, a support sheet having an average light transmittance (L1) of 95% or less can be more easily manufactured. In one embodiment, the average light transmittance (L1) of the support sheet may be, for example, any one of 80 to 95%, 82 to 95%, and 83.5 to 95%, although these are just examples of the average value (L1). However, in this specification, unless otherwise specified, the light transmittance of the support sheet is not limited to the light transmittance in the wavelength range of 400 to 800 nm, but means the light transmittance of the support sheet in a state in which no release film is provided.

[0215] The average light transmittance (L1) of the support sheet can be calculated, for example, by the method shown below. That is, the support sheet is irradiated with light from the outside of the substrate side, and the light transmittance is measured by direct light reception without using an integrating sphere. The light transmittance value T(1) at a wavelength of n (nm) in 1 nm increments in the wavelength range of 400 to 800 nm is calculated. n (wherein n is an integer of 400 to 800) is measured. Then, T(1) when n is 400 to 800 is measured. n Add up all the values ​​and get the total T(1) 400-800 Calculate the obtained T(1) 400-800 , T(1) n Divide by the number of measurements (i.e., 800-400+1=401) (T(1) 400-800 / 401), the average light transmittance (L1) of the support sheet can be calculated.

[0216] The average light transmittance (L1) of the support sheet can be adjusted, for example, by adjusting the types and contents of the components contained in the substrate, the roughness of both surfaces of the substrate (for example, surface roughness (Ra)), and the like. The average light transmittance (L1) of the support sheet can also be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer.

[0217] <Light transmittance difference> The difference between the average light transmittance (L1) of the support sheet (400-800 nm) and the average light transmittance (L2) of the support sheet after heating at 140° C. for 2 hours (hereinafter, sometimes simply referred to as the “average light transmittance (L2) of the support sheet after heating” or “average light transmittance (L2)”) (hereinafter, sometimes referred to as the “light transmittance difference”) is preferably 30% or more, and may be, for example, any of 34% or more, 38% or more, and 42% or more. When the light transmittance difference ([average light transmittance (L1) of the support sheet)]-[average light transmittance (L2) of the support sheet after heating)]) is the lower limit or more, the support sheet clearly discolors (more specifically, whitens) and changes in appearance when heated at a high temperature of 140° C. or more. Therefore, when the support sheet is heated at such a high temperature, the support sheet becomes more identifiable (the support sheet can be more easily identified), and the history of the support sheet being heated at such a high temperature can be easily confirmed. The upper limit of the light transmittance difference of the support sheet is not particularly limited. For example, a support sheet having a light transmittance difference of 60% or less can be more easily manufactured. In one embodiment, the light transmittance difference may be, for example, any one of 30 to 60%, 34 to 60%, 38 to 60%, and 42% to 60%, although these are just examples of the light transmittance difference.

[0218] The reason why the support sheet heated at a higher temperature turns white is unclear, but it is speculated that this is because the relatively low molecular weight component and the high molecular weight component coexist in the pressure-sensitive adhesive layer after heating, causing phase separation of these components. For example, the relatively low molecular weight component is assumed to be an oligomer, which is a reaction product between crosslinkers (β1), a blocking agent separated from the crosslinker (β1), etc., and for example, the high molecular weight component is assumed to be a crosslinked energy ray curable acrylic resin (Ia), etc.

[0219] The average light transmittance (L2) of the support sheet after heating can be calculated, for example, by the method shown below. That is, the support sheet is heated at 140° C. for 2 hours. Next, the support sheet is cooled to a temperature of 23°C by natural cooling, and then the support sheet after cooling is irradiated with light from the outside of the substrate side, and the light transmittance is measured by direct light reception without using an integrating sphere. Then, in the same manner as in the case of the average light transmittance (L1) of the support sheet, that is, in the wavelength range of 400 to 800 nm, the light transmittance value T(2) at a wavelength of n (nm) at 1 nm intervals is measured. n (wherein n is an integer of 400 to 800). Then, T(2) when n is 400 to 800 is measured. n Add up all the values ​​and get the total T(2) 400-800 Calculate the obtained T(2) 400-800 , T(2) n Divide by the number of measurements (i.e., 800-400+1=401) (T(2) 400-800 / 401), the average light transmittance (L2) of the support sheet after heating can be calculated. Next, the difference between the average light transmittance (L2) of the support sheet after heating and the average light transmittance (L1) of the support sheet is calculated, thereby making it possible to calculate the light transmittance difference.

[0220] The average light transmittance (L2) of the support sheet after heating can be adjusted, for example, by adjusting the types and contents of the components contained in the substrate and the roughness of both surfaces of the substrate (for example, surface roughness (Ra)). The average light transmittance (L2) of the support sheet after heating can also be adjusted by adjusting the types and contents of the components contained in the pressure-sensitive adhesive layer.

[0221] Method for manufacturing support sheet The support sheet can be manufactured by laminating the above-mentioned layers constituting the support sheet so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method of forming each layer is as described above. For example, the pressure-sensitive adhesive composition (I) is applied to one surface of a substrate, and then dried as necessary to produce a support sheet.

[0222] The support sheet can also be produced by applying the pressure-sensitive adhesive composition (I) to one side of a release film, drying it as necessary to form a pressure-sensitive adhesive layer on the release film, and bonding the exposed surface of the pressure-sensitive adhesive layer to one side of a substrate. In this case, the pressure-sensitive adhesive composition (I) is preferably applied to the release-treated surface of the release film.

[0223] The pressure (attachment pressure) applied when attaching the pressure-sensitive adhesive layer to the substrate in this manner is preferably 0.2 to 0.6 MPa. When the pressure is equal to or greater than the lower limit, the adhesive strength between the pressure-sensitive adhesive layer and the substrate can be sufficiently increased. Such bonding of the pressure-sensitive adhesive layer and the substrate is preferably carried out under temperature conditions of, for example, 15° C. or higher, but may be carried out at room temperature.

[0224] The support sheet having the other layer can be produced, for example, by applying a composition for forming the other layer to an appropriate location on the substrate or the pressure-sensitive adhesive layer, drying the composition as necessary to form the other layer, and laminating a further required layer as necessary. The support sheet can also be produced by laminating a film-like other layer to an appropriate location on the substrate or the pressure-sensitive adhesive layer to provide the other layer, and laminating a further required layer as necessary.

[0225] <Method of manufacturing composite sheet for resin film formation> The composite sheet for resin film formation can be produced by laminating the above-mentioned layers so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method for forming each layer is as described above.

[0226] It is possible to directly form a thermosetting resin film-forming film by applying a resin film-forming composition on the pressure-sensitive adhesive layer already laminated on the substrate. In this way, when forming a new layer (hereinafter abbreviated as "second layer") on any layer (hereinafter abbreviated as "first layer") already laminated on the substrate to form a continuous two-layer laminate structure (in other words, a laminate structure of the first layer and the second layer), a method of applying a composition for forming the second layer on the first layer and drying it as necessary can be applied. However, it is preferable to form the second layer in advance on a release film using a composition for forming the second layer, and then bond the exposed surface of the second layer opposite to the side in contact with the release film to the exposed surface of the first layer to form a continuous two-layer laminate structure. In this case, it is preferable to coat the composition on the release-treated surface of the release film. The release film can be removed as necessary after the laminate structure is formed.

[0227] In this way, all layers other than the substrate that constitute the composite sheet for forming a resin film can be formed in advance on a release film and laminated by bonding it to the surface of the desired layer, so that the composite sheet for forming a resin film can be manufactured by appropriately selecting the layers that will undergo such a process as necessary.

[0228] In addition, the composite sheet for resin film formation is usually stored in a state where a release film is attached to the surface of the outermost layer (for example, a thermosetting resin film-forming film) on the opposite side to the support sheet. Therefore, a composition for resin film formation is applied onto this release film (preferably its release-treated surface) and dried as necessary to form a thermosetting resin film-forming film on the release film, and the remaining layers are laminated on the exposed surface opposite to the side in contact with the release film of this thermosetting resin film-forming film by any of the above-mentioned methods, and the release film is not removed and the laminated state is left as it is, thereby obtaining a composite sheet for resin film formation with a release film.

[0229] When the thermosetting resin film-forming film is a protective film-forming film, the composite sheet for forming a protective film is obtained, which includes the support sheet and the protective film-forming film.

[0230] The composite sheet for resin film formation may be in the form of a sheet, and is preferably in the form of a roll.

[0231] ◇Kit A kit according to an embodiment of the present invention comprises a first laminate formed by laminating a first release film and a thermosetting resin film-forming film, and a support sheet having a substrate and an adhesive layer provided on one side of the substrate, the support sheet being used to support a workpiece to which the thermosetting resin film-forming film is to be attached and the thermosetting resin film-forming film. The adhesive layer in the support sheet and the thermosetting resin film-forming film are adhered to form a second laminate, and the thermosetting resin film-forming film in the second laminate is heated at 140°C to form a resin film. When the adhesive strength (Z2) between the adhesive layer and the resin film after heating is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less. The support sheet is attached to the surface of a stainless steel plate by the adhesive layer, and the stainless steel plate with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C. When the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, the adhesive strength (Y0) is 2000 mN / 25 mm or more. When the thermosetting resin film-forming film in the second laminate is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is energy ray-cured, and the adhesive strength (Z1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the resin film is measured, it is preferable that the adhesive strength (Z1) is 500 mN / 25 mm or less.

[0232] The kit according to this embodiment can be used, for example, to manufacture a workpiece having a resin film, as described below.

[0233] In the kit according to the present embodiment, since the adhesive strength (Z2) is 1500 mN / 25 mm or less, when the thermosetting resin film-forming film and the workpiece are heated at a high temperature of 140° C. or more on the support sheet during the preparation of the resin film-attached workpiece, the resin film-attached workpiece can be picked up normally from the adhesive layer without curing the adhesive layer in the support sheet after heating with energy rays. Furthermore, since the adhesive strength (Y0) is 2000 mN / 25 mm or more, peeling of the support sheet from the fixing jig for an unintended purpose can be suppressed. Furthermore, since the adhesive strength (Z1) is 500 mN / 25 mm or less, the pick-up property of the resin film-attached workpiece from the cured support sheet tends to be improved.

[0234] In measuring the adhesive strength (Z2) and the adhesive strength (Z1) in the kit of this embodiment, the second laminate has a structure in which a substrate, an adhesive layer and a thermosetting resin film-forming film are laminated in this order, which is the same as the structure of the composite sheet for forming a resin film.

[0235] The adhesive strength (Z2) in the kit of this embodiment can be measured in the same manner as the adhesive strength (Z2) in the composite sheet for resin film formation, except that the composite sheet for resin film formation is replaced with a second laminate. More specifically, this will be described in the measurement of adhesive strength (Z2) in the evaluation of the kit in the examples. The adhesive strength (Z1) in the kit of this embodiment is also similar to the measurement of adhesive strength (Z1) in the composite sheet for resin film formation. More specifically, this will be described in the measurement of adhesive strength (Z1) in the evaluation of the kit in the examples.

[0236] The adhesive strength (Y0), adhesive strength (Y2), and the average light transmittance (L1) of the support sheet of the kit of this embodiment can be measured in the same manner as the support sheet in the composite sheet for resin film formation in the measurement of the adhesive strength (Y0), adhesive strength (Y2), and the average light transmittance (L1) of the support sheet of the composite sheet for resin film formation. More specifically, the measurement of the adhesive strength (Y0), adhesive strength (Y2), and the average light transmittance (L1) in the evaluation of the kit of the embodiment will be described.

[0237] An example of the kit 3 of this embodiment will now be described with reference to the drawings. FIG. 2 is a cross-sectional view that illustrates an example of the kit 3 of the present embodiment. The kit 3 of this embodiment includes a first laminate 5 in which a first peel-off film 151, a thermosetting resin film-forming film 13, and a second peel-off film 152 are laminated in this order, and a support sheet 10 used to support the workpiece to which the thermosetting resin film-forming film 13 is attached and the thermosetting resin film-forming film 13.

[0238] The thermosetting resin film-forming film 13 shown here has a first release film 151 on one side (sometimes referred to as the "first side" in this specification) 13a, and a second release film 152 on the other side (sometimes referred to as the "second side" in this specification) 13b opposite the first side 13a.

[0239] When the thermosetting resin film-forming film is a protective film-forming film, by using a kit 3 including the support sheet 10 and the protective film-forming film, a workpiece with a protective film can be manufactured by the manufacturing method for a workpiece with a resin film described later, which includes a workpiece and a protective film provided on the back surface of the workpiece.

[0240] The first laminate may be in the form of a sheet. In addition, such a thermosetting resin film-forming film 13 is suitable for storage in the form of a roll, for example. That is, the first laminate is preferably in the form of a roll.

[0241] The thermosetting resin film 13 can be formed by using the above-mentioned resin film-forming composition.

[0242] Both the first release film 151 and the second release film 152 may be of known types. The first release film 151 and the second release film 152 may be the same as each other, or may be different from each other, for example, having different peeling forces required when peeling them from the thermosetting resin film-forming film 13.

[0243] 2, one of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes the surface to be attached to the back surface of the work (not shown). Then, the remaining other of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes the surface to be attached to the support sheet.

[0244] FIG. 2 shows an example in which the release film is provided on both sides (first side 13a, second side 13b) of the thermosetting resin film-forming film 13, but the release film may be provided on only one side of the thermosetting resin film-forming film 13, i.e., only the first side 13a or only the second side 13b (i.e., only the first release film may be provided).

[0245] In the kit 3 shown in Fig. 2, the support sheet 10 has a base material 11 and an adhesive layer 12 provided on one surface 11a of the base material 11. The adhesive layer 12 may be energy ray curable or non-energy ray curable.

[0246] The support sheet 10 may be in the form of a sheet, but is preferably in the form of a roll.

[0247] The preferred properties of the thermosetting resin film-forming film 13 in the kit 3 shown in FIG. 2 are similar to the preferred properties of the thermosetting resin film-forming film 13 in the composite sheet for resin film formation according to the above-mentioned embodiment.

[0248] 2, the configuration of the support sheet 10 is the same as the configuration of the support sheet 10 in the composite sheet for resin film formation according to the above-mentioned embodiment. In the support sheet 10 in the kit 3, the preferred properties of the base material 11 and the pressure-sensitive adhesive layer 12 are also the same as the preferred properties of the base material 11 and the pressure-sensitive adhesive layer 12 of the support sheet 10 in the composite sheet for resin film formation according to the above-mentioned embodiment.

[0249] For example, in the kit 3 according to the present embodiment, when the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140° C., and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, it is preferable that the adhesive strength (Y2) is 6000 mN / 25 mm or less. By using such a support sheet 10, even if the first laminated composite sheet 501 is heated in a state where it is fixed to a stainless steel (SUS) fixing jig such as a ring frame 18 via the adhesive layer 12 in a manufacturing method of a resin film-attached workpiece described later, peeling of the support sheet 10 from the fixing jig such as a ring frame 18 is suppressed.

[0250] ◇ Manufacturing method for workpieces with resin film The composite sheet and kit for resin film formation according to the embodiment of the present invention described above can be used to manufacture a workpiece with a resin film.

[0251] <<Manufacturing method 1>> A method for manufacturing a workpiece with a resin film according to a first embodiment of the present invention is a method for manufacturing a workpiece with a resin film, the method comprising: A bonding process is performed by bonding an exposed surface of the thermosetting resin film-forming film in the composite sheet for resin film formation to the back surface of a workpiece, and bonding a peripheral portion of the adhesive layer in the composite sheet for resin film formation to a fixing jig, thereby fixing a first laminated composite sheet, in which the base material, the adhesive layer, the thermosetting resin film-forming film, and the workpiece are laminated in this order in the thickness direction, to the fixing jig; A processing step of dividing the work in the first laminated composite sheet and cutting the thermosetting resin film-forming film to produce a second laminated composite sheet in which a plurality of workpieces with a resin film-forming film are fixed on the base material and the adhesive layer; a heating step of heating the second laminated composite sheet with the peripheral portion of the adhesive layer attached to a fixing jig to harden the thermosetting resin film-forming film and form the resin film, thereby producing a third laminated composite sheet in which the base material, the adhesive layer, and a plurality of workpieces with resin films are laminated in this order in the thickness direction; and a pick-up step of picking up the resin film-attached workpiece in the third laminated composite sheet by separating it from the adhesive layer. Hereinafter, the manufacturing method according to the first embodiment may be referred to as "manufacturing method 1" in this specification.

[0252] 3A to 3E are cross-sectional views for explaining a method for manufacturing a semiconductor chip with a resin film as an example of a method for manufacturing a workpiece with a resin film. Here, the manufacturing method 1 is explained by taking as an example a case where the composite sheet 1 for resin film formation shown in FIG. 1 is used.

[0253] <Attachment process> In the bonding step of the manufacturing method 1, the release film 15 is removed from the composite sheet 1 for resin film formation shown in FIG. 1, and then, as shown in FIG. 3A, the exposed surface (i.e., the first surface 13a) of the thermosetting resin film-forming film 13 in the composite sheet 1 for resin film formation is bonded to the back surface 9b of the semiconductor wafer 9, and the peripheral portion of the adhesive layer 12 in the composite sheet 1 for resin film formation is bonded to a ring frame 18 as a fixing jig, thereby fixing the first laminated composite sheet 501, which is constituted by laminating the base material 11, the adhesive layer 12, the thermosetting resin film-forming film 13, and the semiconductor wafer 9 in this order in the thickness direction, to the ring frame 18 as a fixing jig. The first surface 13a of the thermosetting resin film-forming film 13 in the composite sheet 1 for resin film formation is bonded to the back surface 9b of the semiconductor wafer 9. The ring frame 18 is made of stainless steel (SUS).

[0254] In Figure 3A, the bumps and the like on the circuit surface 9a of the semiconductor wafer 9 are not shown, and the first laminated composite sheet 501 is shown after the backgrind tape that was attached to the circuit surface 9a has been peeled off.

[0255] While the thermosetting resin film-forming film 13 in the composite sheet 1 for resin film formation is attached to the semiconductor wafer 9, the area of ​​the pressure-sensitive adhesive layer 12 in the support sheet 10 surrounding the thermosetting resin film-forming film 13 in the width direction is attached to a ring frame 18 as a fixing jig. The pressure-sensitive adhesive layer 12 in the support sheet 10 may be attached to the ring frame 18 while being heated, or the thermosetting resin film-forming film 13 may be attached to the semiconductor wafer 9 while being heated. The temperature (heating temperature) at which the thermosetting resin film-forming film 13 is attached to the semiconductor wafer 9 is preferably 50 to 75°C.

[0256] Since the adhesive strength (Y0) is 2000 mN / 25 mm or more, peeling of the first laminate composite sheet 501 from the ring frame 18 is suppressed during the period from the bonding step of manufacturing method 1 until the heating step described below is performed. For example, even if any of the devices including the bonding device vibrates while the first laminate composite sheet 501 is fixed to the ring frame 18, or even if the first laminate composite sheet 501 in this state vibrates when the first laminate composite sheet 501 fixed to the ring frame 18 is transported, peeling of the first laminate composite sheet 501 from the ring frame 18 is suppressed.

[0257] <Processing process> 3A and 3B, in the processing step of manufacturing method 1, the semiconductor wafer 9 in the first laminated composite sheet 501 is divided on the support sheet 10 fixed to the ring frame 18, and the resin film-forming film 13 is cut. The semiconductor wafer 9 is divided into individual pieces into a plurality of semiconductor chips 90.

[0258] The division of the semiconductor wafer 9 and the cutting of the resin film-forming film 13 may be performed by a known method. For example, the division of the semiconductor wafer 9 and the cutting of the resin film-forming film 13 can be performed continuously by dicing such as blade dicing, laser dicing by laser irradiation, or water dicing by spraying water containing an abrasive. In addition, the semiconductor wafer 9 may be a semiconductor wafer 9 on which a modified layer has been formed by stealth dicing (registered trademark) and which has not been divided. The semiconductor wafer 9 may be expanded in a direction parallel to its circuit surface 9a or back surface 9b, whereby the semiconductor wafer 9 can be divided and the resin film-forming film 13 can be cut. The resin film forming film 13 is cut along the outer periphery of the semiconductor chip 90 regardless of the cutting method. Reference numeral 90b denotes the back surface of the semiconductor chip 90, which corresponds to the back surface 9b of the semiconductor wafer 9.

[0259] In this manner, by dividing the semiconductor wafer 9 and cutting the resin film-formed film 13, a plurality of semiconductor chips 901 with a resin film-formed film are obtained, each of which includes a semiconductor chip 90 and a cut resin film-formed film (sometimes simply referred to as a "resin film-formed film" in this specification) 130 provided on the back surface 90b of the semiconductor chip 90. Reference numeral 130b denotes the surface of the cut resin film-formed film 130 that was the second surface 13b of the resin film-formed film 13 (sometimes referred to as the "second surface" in this specification).

[0260] In the processing step of manufacturing method 1, the second laminated composite sheet 502 in which the plurality of semiconductor chips 901 with resin film attached thereto are fixed on the support sheet 10 is produced as described above.

[0261] The manufacturing method 1 according to an embodiment of the present invention uses the composite sheet 1 for forming a resin film of the above-mentioned embodiment, and since the adhesive strength (Y0) is 2000 mN / 25 mm or more, the support sheet 10 can be prevented from peeling off from a fixing jig such as a ring frame 18, even when the sheet goes through a transportation process before the processing process.

[0262] In the second laminated composite sheet 502, in a state where a plurality of semiconductor chips 901 with a resin film forming film are fixed on the support sheet 10, the semiconductor chips 901 with a resin film forming film may be inspected for damage such as cracks or chips (e.g., chipping) through the support sheet 10. Since the average light transmittance (400 to 800 nm) of the support sheet (L1) is 80% or more, the inspection accuracy can be improved.

[0263] <Heating process> After the attachment step of manufacturing method 1, in the heating step of manufacturing method 1, the second laminated composite sheet 502 is heated with the adhesive layer 12 on the periphery of the second laminated composite sheet 502 attached to the ring frame 18 (FIG. 3C). This causes the thermosetting resin film-forming film 130 to harden and form a resin film 130', thereby producing a third laminated composite sheet 503 in which the support sheet 10 (i.e., the base material 11 and the adhesive layer 12), the resin film 130', and the semiconductor wafer 9 are laminated in this order in the thickness direction, as shown in FIG. 3D.

[0264] At this time, the heating of the second laminated composite sheet 502 can remove, by volatilization, foreign matter such as low-molecular-weight resin components adhering to the surface (e.g., circuit surface 9a) of the semiconductor wafer 9. Aside from the heating for the purpose of thermally curing the thermosetting resin film-forming film 13, a heating step for the purpose of removing, by volatilization, foreign matter such as low-molecular-weight resin components may be provided.

[0265] The temperature (heating temperature) at which the first laminated composite sheet 501 is heated is preferably 130 to 145° C., and more preferably 140 to 145° C. When the heating temperature is equal to or higher than the lower limit, the effect of heating can be sufficiently obtained. When the heating temperature is equal to or lower than the upper limit, excessive heating can be avoided, and, for example, deterioration of the second laminated composite sheet 502 can be suppressed.

[0266] In the support sheet 10 in the composite sheet 1 for resin film formation used in this embodiment, when the adhesive strength (Y2) is 6000 mN / 25 mm or less, in the heating step, after the second laminated composite sheet 502 is heated while being fixed to the ring frame 18 as a fixing jig, the third laminated composite sheet 503 can be peeled off from the ring frame 18 as a fixing jig without further curing the adhesive layer 12 in the third laminated composite sheet 503 with energy rays. Furthermore, when the third laminated composite sheet 503 is peeled off from the ring frame 18, the adhesive layer 12 can be suppressed from remaining on the ring frame 18. Therefore, for example, after the heated third laminated composite sheet 503 is peeled off from the ring frame 18, it becomes possible to attach and fix the first laminated composite sheet 501 to the ring frame 18 again. In this way, a highly versatile method can be adopted as a manufacturing method for a workpiece.

[0267] In the third laminated composite sheet 503 shown in FIG. 3D, the symbol 130b' indicates the surface of the resin film 130' that was the second surface 13b of the thermosetting resin film-forming film 13 (sometimes referred to as the "second surface" in this specification).

[0268] When the thermosetting resin film-forming film 13 is a protective film-forming film, the thermosetting resin film-forming film 13 shown in FIG. 3A may be laser-marked by irradiating a laser through the support sheet 10 (transmitting the support sheet 10).

[0269] When the light transmittance difference of the support sheet 10 is 30% or more, the support sheet clearly turns white when heated at a high temperature of 140° C. or more in the heating step, which makes it possible to judge from the appearance of the support sheet whether or not the support sheet has been heated at such a high temperature.

[0270] Next, in the case where the adhesive layer is energy ray curable, in manufacturing method 1, the adhesive layer 12 in the third laminated composite sheet 503 may be irradiated with energy rays through the substrate 11 to cure the adhesive layer after heating with energy rays. At this time, the pressure-sensitive adhesive layer 12 of the support sheet 10 is cured by the energy rays, and becomes an energy-ray-cured product.

[0271] When the adhesive layer 12 is cured with energy rays (when the adhesive layer 12 is irradiated with energy rays), the illuminance of the energy rays is 60 to 320 mW / cm 2 The light amount of the energy beam is preferably 100 to 1000 mJ / cm. 2 It is preferable that: The energy rays are preferably irradiated onto the pressure-sensitive adhesive layer 12 from outside the support sheet 10 through the substrate 11 (via the substrate 11).

[0272] <Pickup process> Next, in the pick-up step of manufacturing method 1, semiconductor chip 901 with resin film in third laminated composite sheet 503 is picked up by being pulled away from support sheet 10 as shown in FIG. 3E.

[0273] The manufacturing method 1 according to an embodiment of the present invention uses the composite sheet 1 for forming a resin film of the above-mentioned embodiment, and since the adhesive strength (Z2) is 1500 mN / 25 mm or less, even if the thermosetting resin film-forming film and the semiconductor chip 901 are heated at a high temperature of 140°C or more on the support sheet 10, the resin film-coated semiconductor chip 901 can be normally picked up from the adhesive layer 12 without curing the adhesive layer 12 in the support sheet 10 with energy rays after heating.

[0274] In the pick-up step, peeling occurs between the second surface 130b' of the resin film 130' in the resin-film-coated semiconductor chip 901 and the first surface 12a of the adhesive layer in the support sheet 10.

[0275] Here, a case is shown in which the semiconductor chip 901 with the resin film is separated in the direction of the arrow P by using the separating means 7. Note that a cross-sectional view of the separating means 7 is omitted here.

[0276] The resin-film-attached semiconductor chip 901 can be picked up by a known method. For example, a vacuum collet or the like can be used as the detachment means 7 for detaching the resin-film-attached semiconductor chip 901 from the adhesive layer 12 of the support sheet 10.

[0277] In this case, the adhesive force (Z2) between the adhesive layer and the resin film 130' after heating is smaller than the adhesive force between the adhesive layer and the substrate 11 after heating, so that the semiconductor chip 901 with the resin film can be easily picked up.

[0278] When the adhesive layer 12 in the support sheet 10 is energy ray curable, the adhesive layer 12 can adjust its physical properties before and after curing. After energy ray curing, the adhesive force (Z1) between the energy ray cured product of the adhesive layer 12 and the resin film 130' can be further reduced. The smaller the adhesive force (Z1), the higher the pick-up property of the resin film-coated workpiece from the cured support sheet tends to be. When the adhesive force (Z1) is 500 mN / 25 mm or less, not only a small-sized (e.g., 1.5 mm x 1.5 mm) resin film-coated semiconductor chip 901 but also a relatively large resin film-coated semiconductor chip 901 (e.g., 2.5 mm x 2.5 mm) can be picked up.

[0279] In the pick-up step, such pick-up of the resin-film-coated semiconductor chips 901 is performed for all of the desired resin-film-coated semiconductor chips 901 .

[0280] In the manufacturing method 1, the intended semiconductor chip 901 with a resin film is obtained by carrying out the steps up to the pick-up step.

[0281] In the manufacturing method 1, the heating step may be performed before the processing step, so long as it is performed after the bonding step. In that case, the processing step may employ a method that does not use relatively strong water washing (e.g., laser dicing, etc.) so as to prevent the semiconductor chip with the resin film from peeling off from the support sheet due to the small adhesive strength (Z2).

[0282] The explanation of manufacturing method 1 so far has been given for the case where a composite sheet 1 for forming a resin film is used, which has a support sheet 10 shown in FIG. 1. However, in manufacturing method 1, a composite sheet for forming a resin film of this embodiment other than the composite sheet 1 for forming a resin film may also be used.

[0283] <<Manufacturing method 2>> A method for manufacturing a workpiece with a resin film according to a second embodiment of the present invention is a method for manufacturing a workpiece with a resin film, the method comprising: A bonding process is performed by bonding the exposed surface of the thermosetting resin film-forming film in the kit to the back surface of the workpiece, and bonding the peripheral portion of the adhesive layer in the support sheet of the kit to a fixing jig, thereby fixing a first laminated composite sheet, in which the base material, the adhesive layer, the thermosetting resin film-forming film, and the workpiece are laminated in this order in the thickness direction, to the fixing jig; A processing step of dividing the work in the first laminated composite sheet and cutting the thermosetting resin film-forming film to produce a second laminated composite sheet in which a plurality of workpieces with a resin film-forming film are fixed on the base material and the adhesive layer; a heating step of heating the second laminated composite sheet with the peripheral portion of the adhesive layer attached to a fixing jig to harden the thermosetting resin film-forming film and form the resin film, thereby producing a third laminated composite sheet in which the base material, the adhesive layer, and a plurality of workpieces with resin films are laminated in this order in the thickness direction; and a pick-up step of picking up the resin film-attached workpiece in the third laminated composite sheet by separating it from the adhesive layer. Hereinafter, the production method according to the second embodiment may be referred to as "production method 2" in this specification.

[0284] 4A to 4C and 3A to 3E are cross-sectional views for typically explaining a method for manufacturing a resin-film-coated semiconductor chip as an example of a method for manufacturing a resin-film-coated workpiece (manufacturing method 2). Here, the production method 2 will be described using the kit 3 shown in FIG. 2 as an example.

[0285] <Attachment process> In the attachment step of manufacturing method 2, first, a circular punch is applied to the first laminate 5 of kit 3 shown in FIG. 2 from the side of first release film 151, which is the light-surface release film, to peel off the first release film 151 and remove the circular outer side of the thermosetting resin film-forming film 13 together with the first release film 151, thereby exposing the first surface 13a of the resulting circular thermosetting resin film-forming film 13 (FIG. 4A). Next, the exposed surface (reverse surface 9b) of the semiconductor wafer 9 provided with the backgrind tape 17 is attached to the exposed surface (first surface 13a) of the obtained circular thermosetting resin film-forming film 13 to produce a first laminated film 401 in which the thermosetting resin film-forming film 13 and the semiconductor wafer 9 are laminated in their thickness direction (Figure 4B).

[0286] Next, the second release film 152 is removed from the first laminate film 401 (FIG. 4C), thereby exposing the second surface 13b of the thermosetting resin film-forming film 13.

[0287] Here, the case is shown in which the first release film 151 is removed from the first laminate 5 of the kit 3 shown in Figure 2 and the first surface 13a of the thermosetting resin film-forming film 13 is attached to the back surface 9b of the semiconductor wafer 9, but the second release film 152 may be removed from the thermosetting resin film-forming film 13 of the kit 3 shown in Figure 2 and the back surface 9b of the semiconductor wafer 9 may be attached to the second surface 13b of the thermosetting resin film-forming film 13.

[0288] Next, the exposed surface (i.e., the second surface 13b) of the thermosetting resin film-forming film 13 in the kit 3 is attached to the back surface 9b of the semiconductor wafer 9, and the peripheral portion of the adhesive layer 12 in the support sheet 10 of the kit 3 is attached to a stainless steel ring frame 18 (a stainless steel fixing jig).

[0289] The thermosetting resin film-forming film 13 can be attached to the semiconductor wafer 9 by a known method. For example, the thermosetting resin film-forming film 13 may be attached to the semiconductor wafer 9 while being heated. In this case, the attachment temperature (heating temperature) to the semiconductor wafer 9 is preferably 50 to 75°C.

[0290] This fixes the first laminated composite sheet 501, which is composed of the substrate 11, adhesive layer 12, thermosetting resin film-forming film 13 and semiconductor wafer 9 stacked in this order in the thickness direction, to the ring frame 18 (Figure 3A).

[0291] The support sheet 10 shown here is configured to include a base material 11 and an adhesive layer 12 provided on one surface 11a of the base material 11, and the adhesive layer 12 in the support sheet 10 is attached to a thermosetting resin film-forming film 13. A first surface 12a of the adhesive layer 12 on the thermosetting resin film-forming film 13 side is the same as the first surface 10a of the support sheet 10.

[0292] In manufacturing method 2, the first laminated composite sheet 501 is the same as the first laminated composite sheet 501 in manufacturing method 1 (FIG. 3A).

[0293] In the manufacturing method 2, the processing step can be performed in the same manner as in the manufacturing method 1 (FIG. 3B).

[0294] In the manufacturing method 2, the heating step can be carried out in the same manner as in the heating step in the manufacturing method 1 (FIGS. 3C and 3D).

[0295] The manufacturing method 2 according to an embodiment of the present invention uses the kit 3 according to the above-mentioned embodiment, and since the adhesive strength (Y0) is 2000 mN / 25 mm or more, the support sheet 10 can be prevented from peeling off from the fixing jig such as the ring frame 18, even when the support sheet 10 goes through a transportation process before the processing process.

[0296] In the manufacturing method 2, the pick-up step can be performed in the same manner as in the pick-up step in the manufacturing method 1 (FIG. 3E).

[0297] In the manufacturing method 2, the heating step may be performed before the processing step, so long as it is performed after the bonding step. In that case, the processing step may employ a method that does not use relatively strong water washing (e.g., laser dicing, etc.) so as to prevent the semiconductor chip with the resin film from peeling off from the support sheet due to the small adhesive strength (Z2).

[0298] The manufacturing method 2 according to an embodiment of the present invention uses the kit 3 according to the above-mentioned embodiment, and since the adhesive strength (Z2) is 1500 mN / 25 mm or less, the resin film-coated semiconductor chip 901 can be properly picked up from the adhesive layer after heating. In addition, the manufacturing method 2 according to the embodiment can achieve the same effects as the manufacturing method 1 according to the embodiment.

[0299] ◇ Manufacturing method of substrate device (method of using workpiece with resin film) After a workpiece with a resin film is obtained by the above-mentioned manufacturing method, a substrate device can be manufactured in the same manner as the conventional substrate device manufacturing method, except that this workpiece with a resin film is used in place of the conventional substrate device.

[0300] For example, when the thermosetting resin film-forming film is a protective film-forming film and the resin film-coated workpiece is a semiconductor chip with a protective film, an example of a method for manufacturing a substrate device includes a manufacturing method having a flip-chip connection step of picking up a protective film-coated semiconductor chip obtained using the protective film-forming film from a support sheet, and contacting a protruding electrode on the protective film-coated semiconductor chip with a connection pad on a circuit board, thereby electrically connecting the protruding electrode and the connection pad on the circuit board.

[0301] When the thermosetting resin film-forming film is a film-like adhesive and the resin film-coated workpiece is a semiconductor chip with a film-like adhesive, an example of a method for manufacturing a substrate device includes a manufacturing method having a connection step in which a semiconductor chip with a film-like adhesive obtained using the film-like adhesive is picked up from a support sheet and adhered to a circuit board via the film-like adhesive. EXAMPLES

[0302] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0303] The ring frame used in the following Examples, Comparative Examples, and Reference Examples is made of SUS. The shape of the ring frame is a substantially circular ring shape in which two arcs in a part of the outer periphery of the ring, which are symmetrical with respect to the center of the ring, are cut into straight lines. The ring frame for 8-inch wafers has an outer diameter of 296 mm, a width of the straight portion of 276 mm, an inner diameter of 250 mm, and a thickness of 1.2 mm. The ring frame for 12-inch wafers has an outer diameter of 400 mm, a width of the straight portion of 380 mm, an inner diameter of 350 mm, and a thickness of 1.5 mm.

[0304] <Raw materials for resin production> The full names of the raw materials for producing the resins, which are abbreviated in the present examples and comparative examples, are shown below. 2EHA: 2-ethylhexyl acrylate 2EHMA: 2-Ethylhexyl methacrylate HEA: 2-hydroxyethyl acrylate HEMA: 2-hydroxyethyl methacrylate MOI: 2-Methacryloyloxyethyl isocyanate

[0305] <Raw materials for producing adhesive composition> In the present examples and comparative examples, the raw materials used in producing the pressure-sensitive adhesive compositions are shown below. [Energy ray curable compound (α)] (α)-1: 2-(2-phenoxyethoxy)ethyl acrylate ("AMP-20GY" manufactured by Shin-Nakamura Chemical Co., Ltd., viscosity 18 mPa·s at 23°C (measured using a single-cylinder B-type (Brookfield type) rotational viscometer), molecular weight 236.1) [Crosslinker (β1)] (β1)-1: A block-type crosslinking agent having both a nurate skeleton formed by the trimerization of hexamethylene diisocyanate and a skeleton derived from other hexamethylene diisocyanate ("Duranate (registered trademark) MF-K60B" manufactured by Asahi Kasei Corporation, number average molecular weight 12000, viscosity at 25°C 220 mPa s). [Crosslinker (β2)] (β2)-1: Isocyanurate modified hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) (β2)-2: Trimethylolpropane adduct of 1,6-hexamethylene diisocyanate ("Coronate HL" manufactured by Tosoh Corporation) [Photopolymerization initiator (γ)] (γ)-1: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one (Omnirad® 127, manufactured by IGM Resins) (γ)-2: Phenyl-1-hydroxycyclohexyl-ketone (IGM Resins, "Omnirad (registered trademark) 184")

[0306] The viscosity of the above crosslinking agent (β1) is a value measured by an E-type viscometer.

[0307] [Example 1] <<Kit manufacturing>> The following procedure was used to prepare a kit comprising a support sheet having a substrate and an adhesive layer provided on one side of the substrate, and a first laminate in which a first release film, a protective film-forming film which is a thermosetting resin film-forming film, and a second release film were laminated in this order.

[0308] <Production of energy ray curable acrylic resin (Ia)> The acrylic polymer (1) was added with MOI, and the addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-1. The acrylic polymer (1) was a copolymer of 2EHA (35 parts by mass), 2EHMA (45 parts by mass), and HEMA (20 parts by mass). The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.55 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-1 was 400,000, and the glass transition temperature was -26°C.

[0309] <Production of Pressure-Sensitive Adhesive Composition (I)> The energy ray curable adhesive composition (I)-1 was prepared at room temperature, containing energy ray curable acrylic resin (Ia)-1 (100 parts by mass), crosslinking agent (β1)-1 (13.5 parts by mass), crosslinking agent (β2)-1 (2 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further containing methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent was 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0310] <Formation of adhesive layer> A release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been subjected to a release treatment by silicone treatment, was used. The pressure-sensitive adhesive composition (I)-1 obtained above was applied to the release-treated surface, and the resultant was dried by heating at 100°C for 2 minutes to form an energy ray-curable pressure-sensitive adhesive layer having a thickness of 15 μm.

[0311] <Manufacture of Support Sheet> Next, at room temperature, a polypropylene film (manufactured by Diaplus Film Co., Ltd., thickness 80 μm) was attached as a substrate to the exposed surface of the pressure-sensitive adhesive layer at a sticking speed of 5 m / min and a pressure of 0.4 MPa. One surface of the polypropylene film was a matte surface with a surface roughness (Ra) of 0.90 μm, and the other surface was a slightly matte surface with a surface roughness (Ra) of 0.12 μm, and the pressure-sensitive adhesive layer was attached to the matte surface of the polypropylene film. In this manner, the desired support sheet was obtained.

[0312] <Production of protective film-forming composition> The following components were mixed in the following formulation (solid content equivalent) and diluted with methyl ethyl ketone to a solid content concentration of 61 mass % to prepare a composition for forming a protective film. (A) Polymer component: an acrylic polymer obtained by copolymerizing 10 parts by mass of n-butyl acrylate, 70 parts by mass of methyl acrylate, 5 parts by mass of glycidyl methacrylate, and 15 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 400,000, glass transition temperature: -1°C) (B-1) Bisphenol A type epoxy resin ("jER828" manufactured by Mitsubishi Chemical Corporation, liquid at 23°C and 1 atm, molecular weight 370, softening point 93°C, epoxy equivalent 183-194g / eq) (B-2) Bisphenol A type epoxy resin ("jER1055" manufactured by Mitsubishi Chemical Corporation, solid at 23°C and 1 atm, molecular weight 1600, epoxy equivalent 800-900g / eq) (B-3) Dicyclopentadiene type epoxy resin (DIC "Epicron HP-7200HH", solid at 23℃・1atm, softening point 88~98℃, epoxy equivalent 255~260g / eq)

[0313] (C-1) Heat-activated latent epoxy resin hardener (dicyandiamide, ADEKA "ADEKA Hardener EH-3636AS", active hydrogen content 21g / eq) (D) Curing accelerator: 2-phenyl-4,5-dihydroxymethylimidazole ("Curesol 2PHZ" manufactured by Shikoku Chemical Industry Co., Ltd.) (E-1) Silica filler ("SC2050MA" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm) (F) Silane coupling agent ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0314] (G-1) Colorant (blue pigment): A pigment made by using a phthalocyanine blue pigment (Pigment Blue 15:3) in an amount such that the mass ratio of the pigment component to the styrene-acrylic resin was 1 / 3. (G-2) Colorant (yellow pigment): A pigment obtained by using an isoindolinone yellow pigment (Pigment Yellow 139) in an amount such that the mass ratio of the pigment component to the styrene-acrylic resin was 1 / 3. (G-3) Colorant (red pigment): A pigment obtained by using a diketopyrrolopyrrole red pigment (Pigment Red 264) in an amount such that the mass ratio of the pigment component to the styrene-acrylic resin was 1 / 3.

[0315] Ingredients (solid content of protective film-forming composition) (A): 150 parts by mass (B-1): 60 parts by mass (B-2): 10 parts by mass (B-3): 30 parts by mass (C-1):2 parts by mass (D): 2 parts by mass (E-1): 320 parts by mass (F): 2 parts by mass (G-1): 5.7 parts by mass (G-2): 2.6 parts by mass (G-3): 6.5 parts by mass Total: 590.8 parts by mass

[0316] <Production of First Laminate> A release film (second release film, "SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been treated for release by silicone treatment, was used, and the protective film forming composition obtained above was applied to the release-treated surface, followed by drying at 100°C for 2 minutes to produce a thermosetting protective film-forming film having a thickness of 25 μm.

[0317] Furthermore, a release-treated surface of a release film (first release film, "SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) was bonded to the exposed surface of the obtained thermosetting protective film-forming film that did not have a second release film, thereby obtaining a first laminate comprising a thermosetting protective film-forming film, a first release film provided on one surface of the thermosetting protective film-forming film, and a second release film provided on the other surface of the thermosetting protective film-forming film.

[0318] <<Kit Evaluation>> In the evaluation of the support sheet in the following kit evaluation, the release film on the adhesive layer was peeled off as appropriate before evaluation. For example, when the support sheet was attached to each adherend to measure the adhesive strength, when the light transmittance was measured, and when evaluations were performed to confirm each effect, the release film was peeled off before use in the evaluation.

[0319] <Measurement of adhesive strength (Z2) between adhesive layer and resin film (protective film) after heating> Under application temperature conditions of 70°C (laminating roller temperature 70°C, silicon mirror wafer temperature 70°C), application speed of 300 mm / min, and application pressure of 0.3 MPa, the first release film was removed from the first laminate obtained above, and the exposed surface of the thermosetting protective film-forming film was applied to the entire mirror surface of a silicon mirror wafer (thickness 650 μm), and then the remaining second release film was removed to obtain a silicon mirror wafer with a thermosetting protective film-forming film (i.e., the first laminate film). Further, a test piece having a width of 25 mm was cut out from the support sheet obtained above.

[0320] Under application temperature conditions of 23°C (laminating roller temperature 23°C, first laminated film temperature 23°C), application speed 300 mm / min, and application pressure 0.3 MPa, the adhesive layer surface of a test piece of a 25 mm wide support sheet was attached to the exposed surface of the thermosetting protective film-forming film of the first laminated film while removing the release film, to obtain a first laminated composite sheet (wherein the support sheet width was 25 mm) composed of the substrate, the adhesive layer, the thermosetting protective film-forming film, and the silicon mirror wafer stacked in this order in the thickness direction.

[0321] This first laminated composite sheet was placed inside an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. The thermosetting protective film-forming film was thermally cured to become a protective film, and the silicon mirror wafer with the thermosetting protective film-forming film on the support sheet (i.e., the first laminated composite sheet) was changed into a silicon mirror wafer with a protective film.

[0322] Next, the silicon mirror wafer with the protective film after heating was taken out from the oven and allowed to cool down to a temperature of 23°C. Next, the test piece (support sheet) was peeled off from the silicon mirror wafer with the protective film after cooling, using a precision universal testing machine Autograph (Shimadzu Corporation, AG-IS) at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer with the protective film to which the test piece was attached and the surface of the test piece to which the protective film was attached made an angle of 180° (180° peeling was performed). Then, the load (peeling force) at the time of this 180° peeling was measured, the measurement length was 50 mm, and the first 5 mm and the last 5 mm of the measurement were excluded from the effective value. The average value of the measured values ​​was adopted as the adhesive force (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (Z2) (mN / 25 mm) between the adhesive layer and the resin film (protective film) after heating. The results are shown in Table 1.

[0323] In addition, in Table 1, "content (mass%) of crosslinking agent (β1) in pressure-sensitive adhesive layer" means "proportion (mass%) of the content of crosslinking agent (β1) in the pressure-sensitive adhesive layer relative to the total mass of the pressure-sensitive adhesive layer." This also applies to the following tables.

[0324] <Evaluation of pick-up ability of chips with resin film (protective film) from support sheet> (Manufacturing silicon chips with resin film (protective film)) An 8-inch silicon wafer (thickness 350 μm) with one side polished with #2000 was prepared. While removing the first release film from the first laminate obtained above, the exposed surface of the thermosetting protective film-forming film was attached to the polished surface of the 8-inch silicon wafer under a 70°C attachment temperature condition (laminating roller temperature 70°C, silicon wafer temperature 70°C), attachment speed 300 mm / min, and attachment pressure 0.3 MPa. Thereafter, the remaining second release film was removed to produce a first laminated film in which the thermosetting protective film-forming film and the silicon wafer were laminated in the thickness direction.

[0325] The adhesive layer of the support sheet obtained above was attached to the exposed surface of the thermosetting protective film-forming film of the first laminated film and to the ring frame. This produced a first laminated composite sheet in which the base material, the adhesive layer, the thermosetting protective film-forming film, and the silicon wafer were laminated in this order in the thickness direction. The attachment was performed at a temperature of 23°C (laminating roller temperature 23°C, first laminated film temperature 23°C), at an attachment speed of 300mm / min, and at an attachment pressure of 0.3MPa.

[0326] Next, a dicing device (DISCO Corp.'s "DFD6362") was used to dice the silicon wafer and protective film-forming film in the first laminated composite sheet fixed to the ring frame, to produce multiple silicon chips with protective film-forming films measuring 1.5 mm x 1.5 mm. At this time, a dicing blade "ZH05-SD2000-N1-90 CC" manufactured by DISCO Corp. was used as the dicing blade, and the blade rotation speed was set to 35,000 rpm, the blade feed speed was set to 30 mm / s, and the blade height was set to 0.06 mm. The blade was inserted into the first laminated composite sheet from the surface on the silicon wafer side, and cut into the substrate to a depth of 20 μm from the surface on the adhesive layer side. This produced a second laminated composite sheet in which multiple chips with protective film-forming films were stacked in this order in the thickness direction on the support sheet (i.e., the substrate and adhesive layer).

[0327] Next, the second laminated composite sheet fixed to the ring frame was placed in an oven and heated at 140° C. for 2 hours. The third laminated composite sheet fixed to the ring frame was removed from the oven and allowed to cool until its temperature reached 23° C. This caused the thermosetting protective film-forming film to harden and form a protective film.

[0328] In this manner, a third laminated composite sheet was produced in which a plurality of silicon chips with protective film were aligned and held on a single support sheet (that is, the base material and the adhesive layer).

[0329] (Pickup ability of silicon chips with resin film (protective film) before energy beam irradiation) Next, using a pick-up die bonding device (Canon Machinery's "BESTEM D-02"), the silicon chips with protective film of the third laminated composite sheet were picked up by being pulled away from the support sheet under the following pick-up conditions. This pick-up was performed on a total of 100 silicon chips with protective film on the support sheet in 10 rows in two orthogonal directions divided from the center of the silicon wafer before dicing and its neighboring areas, and one silicon chip with protective film was pushed up from the support sheet side by one pin, and the silicon chip with protective film was pulled away from the support sheet by using a collet (pick-up). Then, the pick-up property was evaluated according to the following evaluation criteria. The results are shown in Table 1.

[0330] (Pickup conditions) Temperature conditions: 23℃ Expansion amount (table push-up height): 4mm Needle height: 0.7mm Push-up needle speed: 5mm / s Hold time 300ms Curvature radius of the pin tip: 0.75 mm

[0331] (Evaluation criteria for pick-up ability) A: All 100 silicon chips with protective film were successfully picked up. B: 1 to 4 silicon chips with protective film could not be picked up successfully, but all other silicon chips with protective film (96 to 99 chips) could be picked up successfully. C: Five or more silicon chips with protective film could not be picked up.

[0332] <Measurement of adhesive strength (Y0) between adhesive layer and SUS plate> A test piece having a width of 25 mm was cut out from the support sheet obtained above. Under application temperature conditions of 23°C (laminating roller temperature 23°C, SUS plate temperature 23°C), application speed 300mm / min, and application pressure 0.3MPa, this test piece was attached via its adhesive layer to the #1200 polished surface of a SUS plate ("SUS304 #1200HL, thickness 1000μm, size 70mm x 150mm" manufactured by Partec) to obtain a SUS plate with a test piece attached.

[0333] Next, the SUS plate with the test piece was left to stand at 23° C. for 30 minutes. Next, the test piece was peeled off from the SUS plate after the static storage at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the SUS plate to which the test piece was attached and the surface of the test piece to which the SUS plate was attached made an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (Y0) (mN / 25 mm) between the adhesive layer and the SUS plate. The results are shown in Table 1.

[0334] <Evaluation of the effect of preventing the peeling of the support sheet from the ring frame in the first laminated composite sheet> A 12-inch silicon wafer (thickness 600 μm) with one side polished with #2000 was prepared. While removing the first release film from the first laminate obtained above, the exposed surface of the thermosetting protective film-forming film was attached to the polished surface of the 12-inch silicon wafer under a 70°C attachment temperature condition (laminating roller temperature 70°C, silicon wafer temperature 70°C), an attachment speed of 300 mm / min, and an attachment pressure of 0.3 MPa. Thereafter, the remaining second release film was removed to produce a first laminated film in which the thermosetting protective film-forming film and the silicon wafer were laminated in the thickness direction. The adhesive layer of the support sheet obtained above was attached to the exposed surface of the thermosetting protective film-forming film of the first laminated film and to the ring frame. This produced a first laminated composite sheet in which the base material, the adhesive layer, the thermosetting protective film-forming film, and the silicon wafer were laminated in this order in the thickness direction. The attachment was performed at a temperature of 23°C (laminating roller temperature 23°C, first laminated film temperature 23°C), at an attachment speed of 300mm / min, and at an attachment pressure of 0.3MPa.

[0335] Next, the first laminated composite sheet fixed to the ring frame was arranged so that the exposed surface of the silicon wafer (the surface opposite to the side with the support sheet) was horizontal. Then, assuming the vibration of the manufacturing device during the manufacture of silicon chips and the vibration of the first laminated composite sheet fixed to the ring frame during its transportation, vibration was applied to the ring frame under the conditions of a frequency of 100 Hz and an amplitude of 0.05 m, and the first laminated composite sheet fixed to the ring frame was placed in such a vibration environment at 23 ° C for 2 hours. Furthermore, the vibration was released, and the first laminated composite sheet fixed to the ring frame was left at 23 ° C for 2 hours. The first laminated composite sheet fixed to the ring frame was again placed in the vibration environment as described above at 23 ° C for 2 hours, and then the vibration was released and the sheet was left at 23 ° C for 2 hours. This storage cycle was repeated four times, and the storage cycle was performed five times in total.

[0336] Next, the first laminated composite sheet fixed to the ring frame was visually checked from the outside of the substrate side of the support sheet to see whether the support sheet peeled off from the ring frame, and if peeled off, the extent of peeling. When the first laminated composite sheet fixed to the ring frame is arranged as described above, when the support sheet peels off from the ring frame, it peels off from the inner circumference side of the ring frame. Therefore, when the support sheet peels off from the ring frame, the peeled part where the distance from the inner circumference of the ring frame to the edge of the peeled part of the support sheet is the longest, that is, the peeled part having the maximum peel distance, was specified, and the effect of suppressing peeling of the support sheet from the ring frame was evaluated according to the following criteria based on this maximum peel distance in addition to the presence or absence of peeling. The results are shown in Table 1. (Evaluation Criteria) A: There is no peeling of the support sheet from the ring frame, or even if peeling occurs, the maximum peeling distance is 2 mm or less, and the peeling prevention effect is high. B: The support sheet peels off from the ring frame, and the maximum peel distance is more than 2 mm and 5 mm or less, so the product can still be used in the next process, but the peeling prevention effect is relatively low. For example, if dicing is performed using a dicing blade in the next process, there is a risk of the peeling problem progressing (increasing the peeling distance) due to infiltration of cleaning water into the peeled area of ​​more than 2 mm. C: The support sheet peeled off from the ring frame, the maximum peeling distance exceeded 5 mm, and the peeling suppression effect was particularly low.

[0337] <Calculation of the average light transmittance (L1) of the support sheet, and evaluation of embeddability of the adhesive layer on the matte surface of the substrate> Using a UV-vis measurement device (Shimadzu Corporation's "UV-vis-NIR3600"), the support sheet obtained above was irradiated with light from the outside of the substrate side, and the light transmittance was measured by direct light reception without using an integrating sphere. The wavelength range of the measurement was 190 to 2000 nm. Then, in the wavelength range of 400 to 800 nm in the visible light region, the light transmittance values ​​were summed up every 1 nm, and the sum was divided by the number of summed light transmittance values ​​(i.e., 800-400+1=401) to calculate the average light transmittance (400 to 800 nm) (L1) (%) of the support sheet. Then, from this average value (L1), the embeddability of the adhesive layer on the matte surface of the substrate was evaluated according to the following criteria. These results are shown in Table 1.

[0338] (Evaluation Criteria) A: The average light transmittance (L1) of the support sheet is 80% or more, and the matte surface of the substrate has a high embedding property with the adhesive layer. B: The average light transmittance (L1) of the support sheet is less than 80%, and the matte surface of the substrate is not sufficiently embedded by the adhesive layer.

[0339] <Measurement of adhesive strength (Y2) between adhesive layer and SUS plate after heating at 140℃> A stainless steel plate with a test piece was prepared in the same manner as in the measurement of the adhesive strength (Y0) above. The SUS plate with the test piece attached was placed inside an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. Next, the SUS plate with the test piece attached was taken out of the oven and allowed to cool until its temperature reached 23°C.

[0340] Next, the test piece was peeled off from the cooled SUS plate at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the SUS plate to which the test piece was attached and the surface of the test piece to which the SUS plate was attached formed an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, and the measurement length was set to 50 mm, and the measurement value at the first 5 mm length and the measurement value at the last 5 mm length were excluded from the effective value. Then, the average value of the measured values ​​was adopted as the adhesive strength (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (Y2) (mN / 25 mm) between the adhesive layer and the SUS plate after heating at 140° C. The results are shown in Table 1.

[0341] <Measurement of adhesive strength (Z1) between the energy ray cured adhesive layer and the resin film (protective film)> Using the same method as in measuring the adhesive strength (Z2) above, the release film of a 25 mm wide test piece was removed and the adhesive layer surface was attached to the exposed surface of the thermosetting protective film-forming film of a silicon mirror wafer with a thermosetting protective film-forming film (i.e., the first laminated film), to obtain a first laminated composite sheet (wherein the support sheet width was 25 mm) composed of the substrate, the adhesive layer, the thermosetting protective film-forming film and the silicon mirror wafer laminated in this order in the thickness direction.

[0342] This first laminated composite sheet was heated at 140°C for 2 hours in the same manner as in the measurement of the adhesive strength (Z2) above, and then the silicon mirror wafer with the protective film after heating was removed from the oven and allowed to cool until its temperature reached 23°C. Then, using an ultraviolet irradiation device ("RAD-2000UV" manufactured by Lintec Corporation), the wafer was exposed to an ultraviolet ray irradiation device with an illuminance of 230mW / cm2. 2 , light intensity 200mJ / cm 2Under the above conditions, the adhesive layer in the removed silicon mirror wafer with protective film after heating was irradiated with ultraviolet light through the substrate to ultraviolet-cure the adhesive layer in the silicon mirror wafer with protective film after heating, thereby obtaining a laminate in which the protective film and the silicon mirror wafer were laminated in this order in the thickness direction on the energy ray-cured product of the substrate and the adhesive layer.

[0343] Next, the test piece (support sheet) was peeled off from the laminate after ultraviolet irradiation using a precision universal testing machine Autograph (Shimadzu Corporation, AG-IS) at a peeling speed of 300 mm / min in an environment of 23°C. At this time, the test piece was peeled off in its length direction so that the surface of the silicon mirror wafer with protective film to which the test piece was attached and the surface of the test piece to which the protective film was attached made an angle of 180° (180° peeling was performed). Then, the load (peeling force) at this 180° peeling was measured, the measurement length was 50 mm, and the first 5 mm and the last 5 mm of the measurement were excluded from the effective value. The average value of the measured values ​​was adopted as the adhesive force (mN / 25 mm). The adhesive strength was measured twice, and the average value was used as the adhesive strength (Z1) (mN / 25 mm) between the energy ray-cured adhesive layer and the resin film (protective film). The results are shown in Table 1.

[0344] <Evaluation of pick-up ability of chips with resin film (protective film) from support sheet after energy beam irradiation> (Manufacturing silicon chips with resin film (protective film)) Using the same procedure as in the above-mentioned <Evaluation of pick-up ability of chips with protective film from a support sheet>, a third laminated composite sheet was produced in which multiple silicon chips with protective film were aligned and held on a single support sheet. Note that the size of the silicon wafer and protective film was changed from 1.5 mm × 1.5 mm to 2.5 mm × 2.5 mm.

[0345] (Pickup ability of chips with resin film (protective film) from support sheet after energy beam irradiation) Using an ultraviolet irradiation device (RAD-2000UV), the adhesive layer in the third laminated composite sheet was irradiated with light at an intensity of 230 mW / cm from the outside of the substrate side through the substrate. 2 , light intensity 200mJ / cm 2 The pressure-sensitive adhesive layer was cured by irradiating it with ultraviolet light under the conditions of:

[0346] Next, using a pick-up die bonding device (Canon Machinery's "BESTEM D-02"), the protective film-attached silicon chip was picked up by being separated from the cured support sheet (i.e., the energy ray cured product of the substrate and the adhesive layer) under the above pick-up conditions. This pick-up was performed on a total of 100 protective film-attached silicon chips on the cured support sheet in 10 rows in two orthogonal directions divided from the center of the silicon wafer before dicing and its neighboring areas, and one protective film-attached silicon chip was pushed up from the support sheet side by one pin, and the protective film-attached silicon chip was picked up from the support sheet by using a collet. Then, the pick-up property was evaluated according to the same evaluation criteria as the evaluation criteria for pick-up property before energy ray irradiation. The results are shown in Table 1.

[0347] <Calculation of light transmittance difference> The pressure-sensitive adhesive layer in the support sheet obtained above was attached to the mirror surface of a silicon mirror wafer (thickness 650 μm) in the width direction of the central region, and the region surrounding the region attached to the silicon mirror wafer was attached to a ring frame. The pressure-sensitive adhesive layer was attached to the silicon wafer and the ring frame at a temperature of 23° C. (laminating roller temperature 23° C., silicon mirror wafer temperature 23° C.), at a bonding speed of 300 mm / min, and at a bonding pressure of 0.3 MPa. As a result, a silicon mirror wafer with a support sheet, which includes a silicon mirror wafer and a support sheet provided on one side of the silicon mirror wafer, was fixed to the ring frame. The silicon mirror wafer with the support sheet was then placed inside an oven whose temperature was adjusted to 140° C., and heated at this temperature (140° C.) for 2 hours. The silicon mirror wafer with the support sheet was then removed from the oven and allowed to cool until its temperature reached 23° C. A test piece was cut out from a region of the support sheet in the silicon mirror wafer with the support sheet after cooling, where the adhesive layer was exposed, between the region where the adhesive layer was attached to the ring frame and the region where the adhesive layer was attached to the silicon mirror wafer. Using a UV-vis measuring device (Shimadzu Corporation's "UV-vis-NIR3600"), the light transmittance of the test piece (i.e., the support sheet after heating) was measured and the average light transmittance (L2) was calculated in the same manner as when calculating the average light transmittance (L1) of the support sheet above, except that the test piece obtained above was used instead of the support sheet.

[0348] From the obtained values, the light transmittance difference ([average light transmittance of the support sheet (L1)] - [average light transmittance of the support sheet after heating (L2)]) was calculated. The results are shown in Table 1.

[0349] <Evaluation of the discernibility of support sheets heated at 140°C> Before being placed inside an oven whose temperature was adjusted to 140° C., the color of the support sheet of the silicon mirror wafer with the support sheet was visually observed by 10 judges under fluorescent lighting for 3 seconds. Furthermore, among the silicon mirror wafers with support sheets after heating at 140° C. and cooling, the color of the support sheets was visually observed by 10 judges under fluorescent lights for 3 seconds. Ten judges judged the appearance of the support sheet before and after heating in terms of color change, and evaluated the distinctiveness of the support sheet heated at 140° C. according to the following criteria. The results are shown in Table 1.

[0350] (Evaluation Criteria) A: All 10 judges judged that the appearance of the support sheet had changed due to heating. B: 8 to 9 judges determined that the appearance of the support sheet had changed due to heating, and 1 to 2 judges determined that the appearance of the support sheet had not changed due to heating. C: Three or more judges judged that the appearance of the support sheet was not changed by heating.

[0351] [Example 2] <<Production of support sheet and evaluation of kit>> An energy ray curable adhesive composition (I)-2 was prepared, which had the same composition as in Example 1, except that the crosslinking agent (β2)-2 (2 parts by mass) was used instead of the crosslinking agent (β2)-1 (2 parts by mass). A support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (I)-2 was used instead of the adhesive composition (I)-1. The results are shown in Table 1.

[0352] [Example 3] <<Production of support sheet and evaluation of kit>> An energy ray curable adhesive composition (I)-3 was prepared, which had the same composition as in Example 1, except that the photopolymerization initiator (γ)-2 (3 parts by mass) was used instead of the photopolymerization initiator (γ)-1 (3 parts by mass). A support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (I)-3 was used instead of the adhesive composition (I)-1. The results are shown in Table 1.

[0353] [Reference example 1] <<Production of support sheet and evaluation of kit>> <Production of energy ray curable acrylic resin (Ia)> The same acrylic polymer (1) as used in Example 1 was added with MOI, and an addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-2. The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.785 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-2 was 500,000, and the glass transition temperature was -26°C.

[0354] <Production of Pressure-Sensitive Adhesive Composition (R)> The energy ray curable adhesive composition (R)-1 was prepared, which contains energy ray curable acrylic resin (Ia)-2 (100 parts by mass), energy ray curable compound (α)-1 (25 parts by mass), crosslinking agent (β2)-1 (4.12 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further contains methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent is 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0355] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-1 obtained above was used instead of the adhesive composition (I)-1.

[0356] <Kit evaluation> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0357] [Reference example 2] <<Production of support sheet and evaluation of kit>> An energy ray curable adhesive composition (R)-2 was prepared, which had the same composition as in Example 1, except that the content of the crosslinking agent (β1)-1 was 15.5 parts by mass instead of 13.5 parts by mass, and that the crosslinking agent (β2)-1 was not contained. A support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (R)-2 was used instead of the adhesive composition (I)-1. The results are shown in Table 1.

[0358] [Reference example 3] <<Production of support sheet and evaluation of kit>> <Production of energy ray curable acrylic resin (Ia)> The same acrylic polymer (1) as used in Example 1 was added with MOI, and an addition reaction was carried out in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-3. The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.95 times the total number of moles of hydroxyl groups derived from HEMA in the acrylic polymer (1). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-3 was 440,000, and the glass transition temperature was -26°C.

[0359] <Production of Pressure-Sensitive Adhesive Composition (R)> The energy ray curable adhesive composition (R)-3 was prepared containing energy ray curable acrylic resin (Ia)-3 (100 parts by mass), energy ray curable compound (α)-1 (5.7 parts by mass), crosslinking agent (β2)-2 (0.59 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further containing methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent was 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0360] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-3 obtained above was used instead of the adhesive composition (I)-1.

[0361] <Kit evaluation> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0362] [Comparative Example 1] <<Production of support sheet and evaluation of kit>> An energy ray curable adhesive composition (R)-4 was prepared, which has the same composition as in Reference Example 3, except that the content of the crosslinking agent (β2)-2 is 0.53 parts by mass instead of 0.59 parts by mass, and that the energy ray curable compound (α)-1 is not contained. Then, a support sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive composition (R)-4 was used instead of the adhesive composition (I)-1. The results are shown in Table 2.

[0363] [Comparative Example 2] <<Production of support sheet and evaluation of kit>> <Production of energy ray curable acrylic resin (Ia)> The MOI was added to the acrylic polymer (2) and subjected to an addition reaction in an air stream at 50°C for 48 hours to obtain an energy beam curable acrylic resin (Ia)-4. The acrylic polymer (2) is a copolymer of 2EHA (35 parts by mass), 2EHMA (45 parts by mass), and HEA (20 parts by mass). The amount of MOI used was such that the total number of moles of isocyanate groups in the MOI was 0.7 times the total number of moles of hydroxyl groups derived from HEA in the acrylic polymer (2). The weight average molecular weight of the obtained energy beam curable acrylic resin (Ia)-4 was 880,000, and the glass transition temperature was -35°C.

[0364] <Production of Pressure-Sensitive Adhesive Composition (R)> An energy ray curable pressure sensitive adhesive composition (R)-5 was prepared, which contains energy ray curable acrylic resin (Ia)-4 (100 parts by mass), crosslinking agent (β2)-2 (9.26 parts by mass), and photopolymerization initiator (γ)-1 (3 parts by mass), and further contains methyl ethyl ketone as a solvent, and the total concentration of all components other than the solvent is 25% by mass. Note that the contents of all components other than methyl ethyl ketone shown here are the contents of the target product excluding the solvent.

[0365] <Formation of adhesive layer, production of support sheet> An adhesive layer (thickness 15 μm) was formed and a support sheet was produced in the same manner as in Example 1, except that the adhesive composition (R)-5 obtained above was used instead of the adhesive composition (I)-1.

[0366] <Kit evaluation> The support sheet obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0367] [Table 1]

[0368] [Table 2]

[0369] As is clear from the above results, in Examples 1 to 3, the adhesive strength (Z2) was 1500 mN / 25 mm or less. Therefore, even when the thermosetting resin film (protective film)-forming film and the workpiece were heated at a high temperature of 140°C on the support sheet, the resin-film-attached silicon chip could be normally picked up from the adhesive layer without curing the adhesive layer in the support sheet with energy rays after heating. That is, in Examples 1 to 3, the pick-up property of the resin-film-attached workpiece from the adhesive layer was good.

[0370] Moreover, in Examples 1 to 3, the adhesive strength (Y0) was 2000 mN / 25 mm or more, which was sufficiently large. That is, in Examples 1 to 3, it is possible to suppress unintended peeling of the support sheet from the ring frame during the production of the resin-coated chip. In fact, even if vibration occurs in the first laminated composite sheet and the second laminated composite sheet fixed to the ring frame via the support sheet, peeling of the support sheet from the ring frame was suppressed.

[0371] Thus, the kits including the thermosetting resin film-forming film and the support sheet of Examples 1 to 3 had the desired properties. It is clear that a composite sheet for forming a resin film, which has a thermosetting resin film-forming film and a support sheet having the same characteristics, also has good pick-up properties of the workpiece with the resin film from the adhesive layer, and peeling of the support sheet from the ring frame is suppressed.

[0372] In Examples 1 to 3, the matte surface of the substrate had high embedding ability with the adhesive layer. As a result, in Examples 1 to 3, the average light transmittance (400 to 800 nm) of the support sheet (L1) was 82.6% or more, which was sufficiently high, and it was presumed that the chipping inspection accuracy of the support sheet was high.

[0373] Furthermore, in Examples 1 to 3, the adhesive strength (Y2) was 6000 mN / 25 mm or less, which was appropriately small. Therefore, when the thermosetting resin film-forming film and the workpiece were heated at a high temperature of 140° C. on the support sheet fixed to the ring frame using the kits including the thermosetting resin film-forming film and the support sheet of Examples 1 to 3, it was presumed that the second laminated composite sheet could be peeled off from the ring frame without curing the adhesive layer in the support sheet with energy rays after heating, and further, the adhesive layer remaining on the ring frame could be suppressed.

[0374] Furthermore, in Examples 1 to 3, the adhesive strength (Z1) between the energy ray cured product of the adhesive layer and the resin film was 500 mN / 25 mm or less, which was appropriately small. Therefore, by heating the thermosetting resin film-forming film in the composite sheet for resin film formation in Examples 1 to 3 at 140°C to form a resin film, and curing the adhesive layer after heating with energy rays, even a relatively large silicon chip with a resin film of 2.5 mm x 2.5 mm could be picked up well.

[0375] Furthermore, in Examples 1 to 3, the difference between the average light transmittance (L1) of the unheated support sheet and the average light transmittance (L2) of the heated support sheet was 40.2% or more, which was sufficiently large. The support sheets of Examples 1 to 3 were clearly whitened when heated at 140°C, and these support sheets were highly distinguishable when heated at 140°C.

[0376] Thus, the kits including the thermosetting resin film-forming film and the support sheet of Examples 1 to 3 were also excellent in properties other than those intended. The same is true for the composite sheet for resin film formation including the thermosetting resin film-forming film and the support sheet having the same properties.

[0377] In contrast, in Reference Examples 1 to 3 and Comparative Examples 1 to 2, the adhesive strength (Z2) was large, exceeding 1500 mN / 25 mm, and after the thermosetting resin film-forming film and the workpiece were heated at a high temperature of 140°C on the support sheet, many of the resin-coated silicon chips could not be picked up normally from the adhesive layer, and the pick-up performance was significantly inferior.

[0378] Moreover, in Reference Example 1 and Comparative Example 2, the adhesive strength (Y0) was less than 2000 mN / 25 mm, which was too small. That is, in Reference Example 1 and Comparative Example 2, during the production of the chip with the resin film, it was not possible to suppress the unintended peeling of the support sheet from the ring frame. In fact, in Reference Example 1 and Comparative Example 2, when vibration occurred in the first laminated composite sheet and the second laminated composite sheet fixed to the ring frame via the support sheet, the effect of suppressing the peeling of the support sheet from the ring frame was low.

[0379] As described above, the kits provided with the thermosetting resin film-forming film and the support sheet in Reference Examples 1 to 3 and Comparative Examples 1 and 2 did not have the desired properties.

[0380] In Comparative Examples 1 and 2, the matte surface of the substrate was not sufficiently embedded by the adhesive layer, and as a result, the average light transmittance (400-800 nm) (L1) of the support sheet in Comparative Examples 1 and 2 was 79.1% or less, which was low, and it was presumed that the chipping inspection accuracy of the support sheet was poor.

[0381] Furthermore, in Reference Examples 1 and 3 and Comparative Examples 1 to 2, the adhesive strength (Y2) was large, exceeding 6000 mN / 25 mm. Therefore, when the thermosetting resin film-forming film and the workpiece were heated at a high temperature of 140°C on the support sheet fixed to the ring frame using the kits equipped with the thermosetting resin film-forming film and the support sheet of Comparative Examples 1 to 2 and Reference Examples 1 and 3, it was presumed that unless the adhesive layer in the support sheet was cured with energy rays after heating, the second laminated composite sheet and the third laminated composite sheet fixed to the ring frame via the support sheet could not be peeled off from the ring frame.

[0382] Furthermore, in Reference Examples 2 to 3 and Comparative Examples 1 to 2, the adhesive strength (Z1) between the energy ray-cured product of the adhesive layer and the resin film was large, exceeding 500 mN / 25 mm. Therefore, in Reference Examples 2 to 3 and Comparative Examples 1 to 2, when the thermosetting resin film-forming film in the composite sheet for resin film formation was heated at 140°C to form a resin film, even if the adhesive layer after heating was cured with energy rays, a relatively large silicon chip with a resin film of 2.5 mm x 2.5 mm could not be picked up well.

[0383] Furthermore, in Comparative Examples 1 and 2 and Reference Examples 1 and 3, the difference between the average light transmittance (L1) of the unheated support sheet and the average light transmittance (L2) of the heated support sheet was small, being 12.2% or less. The support sheets of Comparative Examples 1 and 2 and Reference Examples 1 and 3 showed a low degree of whitening when heated at 140°C, and these support sheets showed low discernibility when heated at 140°C. [Industrial Applicability]

[0384] The present invention can be used in the manufacture of resin-film-coated workpieces, such as semiconductor chips with resin films. [Explanation of symbols]

[0385] REFERENCE SIGNS LIST 1...resin film forming composite sheet, 3...kit, 10...support sheet, 11...substrate, 11a...one side of substrate, 12...adhesive layer, 13...thermosetting resin film forming film, 17...backgrind tape, 18...ring frame, 9...semiconductor wafer, 90...semiconductor chip, 401...first laminated film, 501...first laminated composite sheet, 502...second laminated composite sheet, 503...third laminated composite sheet

Claims

1. A composite sheet for resin film formation, comprising: a support sheet having a substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate; and a thermosetting resin film-forming film provided on the pressure-sensitive adhesive layer of the support sheet, The thermosetting resin film-forming film in the composite sheet for resin film formation is heated at 140° C. to form a resin film, and when the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less, A composite sheet for forming a resin film, wherein the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the stainless steel plate with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, and the adhesive strength (Y0) is 2000 mN / 25 mm or more.

2. The composite sheet for resin film formation according to claim 1 , wherein the pressure-sensitive adhesive layer contains a block type crosslinking agent (β1).

3. The composite sheet for resin film formation according to claim 1 or 2, wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more.

4. The composite sheet for forming a resin film according to claim 1 or 2, wherein when the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and the adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less.

5. The composite sheet for resin film formation according to claim 1 or 2, wherein the pressure-sensitive adhesive layer is energy ray curable.

6. The composite sheet for forming a resin film according to claim 5, wherein when the thermosetting resin film-forming film in the composite sheet for forming a resin film is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is cured with energy rays, and the adhesive strength (Z1) between the energy-ray cured product of the pressure-sensitive adhesive layer and the resin film is measured, the adhesive strength (Z1) is 500 mN / 25 mm or less.

7. A kit comprising a first laminate formed by laminating a first release film and a thermosetting resin film-forming film, a base material and a pressure-sensitive adhesive layer provided on one surface of the base material, and a support sheet used to support a workpiece to which the thermosetting resin film-forming film is to be attached and the thermosetting resin film-forming film, The pressure-sensitive adhesive layer in the support sheet and the thermosetting resin film-forming film are attached to form a second laminate, and the thermosetting resin film-forming film in the second laminate is heated at 140° C. to form a resin film. When the adhesive strength (Z2) between the pressure-sensitive adhesive layer and the resin film after heating is measured, the adhesive strength (Z2) is 1500 mN / 25 mm or less, a support sheet is attached to a surface of a stainless steel plate by the pressure-sensitive adhesive layer, and the stainless steel plate provided with the support sheet is left to stand for 30 minutes under a temperature condition of 23°C, and when the adhesive strength (Y0) between the adhesive layer and the stainless steel plate is measured, the adhesive strength (Y0) is 2000 mN / 25 mm or more.

8. The kit according to claim 7 , wherein the adhesive layer contains a blocked crosslinker (β1).

9. The kit according to claim 7 or 8, wherein the average light transmittance (L1) of the support sheet in the wavelength range of 400 to 800 nm is 80% or more.

10. The kit according to claim 7 or 8, wherein when the support sheet is attached to the surface of a stainless steel plate by the adhesive layer, the adhesive layer after attachment is heated at 140°C, and an adhesive strength (Y2) between the adhesive layer after heating and the stainless steel plate is measured, the adhesive strength (Y2) is 6000 mN / 25 mm or less.

11. The kit according to claim 7 or 8, wherein the pressure-sensitive adhesive layer is energy ray curable.

12. The kit according to claim 11, wherein when the thermosetting resin film-forming film in the second laminate is heated at 140°C to form a resin film, the pressure-sensitive adhesive layer after heating is energy ray-cured, and an adhesive strength (Z1) between the energy ray-cured product of the pressure-sensitive adhesive layer and the resin film is measured, the adhesive strength (Z1) is 500 mN / 25 mm or less.

13. A method for manufacturing a resin film-attached workpiece, comprising: a workpiece; and a resin film provided on a rear surface of the workpiece, A bonding process for fixing a first laminated composite sheet, which is configured by laminating the base material, the adhesive layer, the thermosetting resin film-forming film, and the workpiece in this order in the thickness direction, to the fixing jig, by attaching the exposed surface of the thermosetting resin film-forming film in the composite sheet for resin film formation described in claim 1 or 2 to the back surface of the workpiece and attaching the peripheral portion of the adhesive layer in the composite sheet for resin film formation to the fixing jig, or by attaching the exposed surface of the thermosetting resin film-forming film in the kit described in claim 7 or 8 to the back surface of the workpiece and attaching the peripheral portion of the adhesive layer in the support sheet of the kit to the fixing jig; A processing step of dividing the work in the first laminated composite sheet and cutting the thermosetting resin film-forming film to produce a second laminated composite sheet in which a plurality of workpieces with a resin film-forming film are fixed on the base material and the adhesive layer; a heating step of heating the second laminated composite sheet with the peripheral portion of the adhesive layer attached to a fixing jig to harden the thermosetting resin film-forming film and form the resin film, thereby producing a third laminated composite sheet in which the base material, the adhesive layer, and a plurality of workpieces with resin films are laminated in this order in the thickness direction; A method for manufacturing a workpiece with a resin film, comprising a pick-up process of picking up the workpiece with the resin film in the third laminated composite sheet by separating it from the adhesive layer.

Citation Information

Patent Citations

  • Dicing tape

    JP2008159998A

  • Dicing sheet with protective film forming layer and chip manufacturing method

    JP2013131593A

  • Dicing sheet with protective film forming layer and method for producing chip

    JP2016219841A

  • Adhesive composition, cured product, and adhesive sheet

    JP2022038777A

  • Support sheet, composite sheet for resin film formation, kit and method for manufacturing resin film-attached chip

    JP2022152297A

Cited By

  • Method for avoiding layering in embedded wafer level ball grid array bonding process

    CN120072668A