Infrared-absorbing particle, infrared-absorbing particle dispersion liquid, infrared-absorbing particle dispersion, and infrared-absorbing laminate

Infrared absorbing particles with a composite oxide composition of potassium, barium, and niobium address the challenge of selectively absorbing near-infrared rays, achieving effective temperature control and transparency, enhancing indoor comfort.

JP2024142722APending Publication Date: 2024-10-11SUMITOMO METAL MINING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023055016
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional infrared absorbing materials lack the ability to selectively absorb near-infrared rays while maintaining transparency in the visible light region, leading to inadequate control over indoor temperature due to sunlight penetration through windows.

Method used

Development of infrared absorbing particles composed of a composite oxide containing potassium, barium, and niobium, with specific ratios of these elements to achieve absorption peaks in the 1400 nm to 2100 nm range, ensuring high absorption in the infrared region and transparency in the visible light region.

Benefits of technology

The novel infrared absorbing particles effectively block near-infrared rays, reducing indoor temperature rise while maintaining visible light transmission, providing a comfortable indoor environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142722000001_ABST
    Figure 2024142722000001_ABST
Patent Text Reader

Abstract

To provide a novel infrared-absorbing particle.SOLUTION: An infrared-absorbing particle includes complex oxides. The complex oxides include, as elements, potassium, barium, and niobium. When the amount of substance of potassium included in the complex oxides is defined as x1, the amount of substance of barium is defined as x2, and the amount of substance of niobium is defined as y, the following relationships hold: 0.002≤(x1+x2) / y≤1.5, 0.05≤x1≤1, and 0.001≤x2≤1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to infrared absorbing particles, an infrared absorbing particle dispersion, an infrared absorbing particle dispersion, and an infrared absorbing laminate. [Background technology]

[0002] Near-infrared rays contained in sunlight penetrate window materials and the like and enter indoor spaces, raising the surface temperatures of the walls and floors inside the rooms and causing the indoor air temperature to rise. In order to make the indoor thermal environment more comfortable, it has been conventional to use light-shielding materials in window materials and the like to block the near-infrared rays that enter through the windows and thereby prevent the indoor air temperature from rising.

[0003] Patent Document 1 proposes a light-shielding film containing black fine powder including inorganic pigments such as carbon black and titanium black, and organic pigments such as aniline black, as a light-shielding material used in windows and the like.

[0004] Patent Document 2 discloses a thermal insulation sheet made of a woven fabric in which a belt-shaped film having infrared reflectivity and a belt-shaped film having infrared absorbing properties are used as warp and weft, respectively. It also discloses that the belt-shaped film having infrared reflectivity is made by depositing aluminum on a synthetic resin film and further laminating another synthetic resin film.

[0005] The present applicant has proposed in Patent Document 3 an infrared-shielding material microparticle dispersion in which infrared material microparticles are dispersed in a medium, the infrared material microparticles containing tungsten oxide microparticles and / or composite tungsten oxide microparticles, and the dispersed particle diameter of the infrared material microparticles being 1 nm or more and 800 nm or less. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-029314 A [Patent Document 2] Japanese Patent Application Publication No. 9-107815 [Patent Document 3] International Publication No. 2005 / 037932 Summary of the Invention [Problem to be solved by the invention]

[0007] Meanwhile, in order to enable the selection of an optimum material depending on the application, there is a demand for new infrared absorbing particles having optical properties different from those of conventional materials.

[0008] Therefore, an object of one aspect of the present invention is to provide novel infrared absorbing particles. [Means for solving the problem]

[0009] In one aspect of the present invention, there is provided an infrared absorbing particle containing a complex oxide, the complex oxide comprising: Contains the elements potassium, barium, and niobium, When the amount of substance of the potassium contained in the composite oxide is x1, the amount of substance of the barium is x2, and the amount of substance of the niobium is y, Provided is an infrared absorbing particle that satisfies the relationships: 0.002≦(x1+x2) / y≦1.5, 0.05≦x1≦1, and 0.001≦x2≦1. Effect of the Invention

[0010] In one aspect of the present invention, novel infrared absorbing particles can be provided. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a graph showing the transmitted light profile of the infrared absorbing particle dispersion liquids according to Example 1 and Reference Example 2. [Diagram 2] FIG. 2 is a schematic diagram of an infrared absorbing particle dispersion liquid. [Diagram 3] FIG. 3 is a schematic diagram of an infrared absorbing particle dispersion. [Figure 4] FIG. 4 is a schematic diagram of an infrared absorbing substrate. [Diagram 5] FIG. 5 is a schematic diagram of an infrared absorbing laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, [1] infrared absorbing particles, [2] a method for producing infrared absorbing particles, [3] infrared absorbing particle dispersion, [4] infrared absorbing particle dispersion, and [5] infrared absorbing laminate will be described in detail in that order. [1] Infrared absorbing particles The present inventors have conducted research into novel infrared absorbing particles. The infrared absorbing particles according to the present invention are preferably near infrared absorbing particles that absorb, in particular, near infrared rays within the infrared region.

[0013] In examining new infrared absorbing particles, the inventors of the present invention focused on oxides of group 5 elements. However, since there are no effective free electrons or holes in the pentoxides of group 5 elements (V2O5, Nb2O5, Ta2O5), they have little absorption and reflection characteristics in the infrared region and are not effective as infrared absorbing materials. However, when a composite oxide is made by adding an electropositive element to the above oxide, free electrons or holes are generated in the composite oxide, and absorption characteristics derived from the free electrons or holes are expressed in the infrared region. Therefore, it was found that new infrared absorbing particles can be made.

[0014] Furthermore, the inventors of the present invention have found that there is a specific range of the composition of the complex oxide that is particularly effective as an infrared absorbing particle. Specifically, they have found that by setting the composition range of the complex oxide within a specific range, the complex oxide is transparent in the visible light region and absorbs in the infrared region.

[0015] The inventors of the present invention further conducted extensive research and found that by controlling the composition of the complex oxide within a specific range, it is possible to provide strong absorption of the light wavelengths that cause scorching heat on human skin, even in the infrared region. It is believed that the heat felt by sunlight on the skin (so-called scorching sensation) is largely due to the influence of infrared rays with wavelengths of 1500 nm to 2100 nm (see, for example, Yoshikazu Ozeki et al., Automotive Engineers of Japan, Inc., Preprint Collection No. 33-99, 13 (1999)). For this reason, in order for infrared absorbing particles to absorb the light wavelengths that cause scorching heat on human skin and reduce the amount of transmission, it is preferable that the infrared absorbing particles reduce or block infrared rays in the wavelength region from about 1400 nm to 2100 nm or less, taking practicality into consideration.

[0016] Therefore, by giving the particle a light absorption peak in the wavelength range of 1400 nm or more and 2100 nm or less, it is possible to create infrared absorbing particles that are transparent in the visible light range, but have high absorption of light wavelengths in the infrared range that cause a burning sensation on human skin.

[0017] On the other hand, infrared absorbing particles that are transparent in the visible light region and have a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less have not been widely known.

[0018] In other words, the inventors discovered that by providing a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less, it is possible to create new infrared absorbing particles with optical properties different from those of conventional materials, thereby completing the present invention. (Composition of the composite oxide) The infrared absorbing particles of this embodiment may contain a composite oxide.

[0019] The composite oxide contained in the infrared absorbing particles of this embodiment can contain potassium (K), barium (Ba), and niobium (Nb) as elements.

[0020] When the amount of substance of potassium contained in the composite oxide is x1, the amount of substance of barium is x2, and the amount of substance of niobium is y, it is preferable that the relationships of 0.002≦(x1+x2) / y≦1.5, 0.05≦x1≦1, and 0.001≦x2≦1 are satisfied.

[0021] The infrared absorbing particles of the present embodiment may be composed only of the composite oxide. However, even in this case, the infrared absorbing particles of the present embodiment may contain inevitable impurities that are mixed in during the manufacturing process or the like.

[0022] As described above, by adding potassium and barium, which are electropositive elements, to an oxide containing niobium to form the above composite oxide, infrared absorbing properties can be exhibited.

[0023] Furthermore, by simultaneously adding potassium and barium to an oxide containing niobium and setting the composition within a predetermined range, infrared absorbing particles containing the composite oxide can have a light absorption peak in the wavelength region of 1400 nm to 2100 nm. This is believed to be because free electrons or holes with a density suitable for having a light absorption peak in the wavelength region of 1400 nm to 2100 nm are generated if the composition of potassium and barium is within the predetermined range.

[0024] By setting the value of (x1 + x2) / y, which represents the content ratio of the total amount of potassium and barium to niobium in the composite oxide, to 0.002 or more, a sufficient amount of free electrons or holes is generated in the composite oxide, and the desired infrared absorption effect can be obtained. And, the greater the contents of potassium and barium, the greater the supply amount of free electrons and the higher the infrared absorption efficiency. However, the effect also saturates when the value of (x1 + x2) / y is about 1.5. Also, if the value of (x1 + x2) / y is 1.5 or less, generation of an impurity phase in the infrared absorption particles can be avoided. For this reason, as described above, it is preferable that 0.002 ≦ (x1 + x2) / y ≦ 1.5, more preferably 0.5 ≦ (x1 + x2) / y ≦ 1.0, and even more preferably 0.7 ≦ (x1 + x2) / y ≦ 1.0.

[0025] The above composite oxide is, for example, represented by the general formula K x1 Ba x2 Nb y O z and can be expressed as such. As shown by the above general formula, the above composite oxide is preferably composed of, for example, potassium, barium, niobium, and oxygen.

[0026] By adding potassium and barium to the niobium-containing oxide, free electrons or holes are supplied to the composite oxide, and infrared absorption characteristics can be exhibited. Therefore, the amount of oxygen contained in the composite oxide is not particularly limited. However, by also setting the amount of oxygen within a predetermined range, the amount of free electrons or holes in the composite oxide can be set to a particularly suitable range from the viewpoint of enhancing the infrared absorption characteristics. Thus, for z / y, which corresponds to the content ratio of oxygen to niobium in terms of the amount of substance in the composite oxide, it is preferable that 1.0 < z / y < 3.5, more preferably 2.0 < z / y < 3.5, even more preferably 2.0 < z / y ≦ 3.0, and most preferably 2.4 ≦ z / y ≦ 3.0. Here, z corresponds to the amount of substance of oxygen contained in the composite oxide.

[0027] As described above, z / y corresponds to the content ratio of the amount of oxygen relative to niobium in the composite oxide, and is a value that affects the amount of oxygen deficiency or excess oxygen in the composite oxide. As described above, the amount of free electrons or holes in the composite oxide can be controlled by the amount of oxygen. For this reason, it is preferable to control the value of z / y according to the required infrared absorbing properties, etc. The value of z / y can be easily controlled by the synthesis conditions of the infrared absorbing particles, etc.

[0028] The above general formula K x1 Ba x2 Nb y O z In the formula, x1, x2, y, and z preferably satisfy 0<(x1+2x2+5y-2z) / y≦3, more preferably satisfy 0<(x1+2x2+5y-2z) / y≦2, and further preferably satisfy 0.1≦(x1+2x2+5y-2z) / y≦1. The above (x1+2x2+5y-2z) / y indicates a guideline for the excess or deficiency of electrons per niobium atom, and when the above range is satisfied, a particularly high infrared absorbing effect can be exhibited. (Crystal structure and lattice constant of complex oxides) According to the study by the inventors of the present invention, when a complex oxide has any one of the crystal structures selected from cubic, tetragonal, and orthorhombic (rectangular), the transmission of light in the visible light region is improved and the absorption of light in the infrared region is improved. However, in order to obtain the effect of improving the transmission of light in the visible light region and improving the absorption of light in the infrared region, it is sufficient that the complex oxide contains a unit structure of a cubic, tetragonal, or orthorhombic crystal structure, and the complex oxide may partially contain amorphous or other structures.

[0029] In the composite oxide, (x1+x2) / y, which indicates the content ratio of the total amount of potassium and barium relative to niobium, is 1.0, and z / y, which indicates the content ratio of the amount of oxygen relative to niobium, is 3.0. In this case, the crystal structure of the composite oxide is a cubic perovskite structure. Specifically, for example, K 0.5 Ba 0.5 NbO3 etc. have a cubic perovskite structure.

[0030] Taking a complex oxide with (x1 + x2) / y = 1.0 and z / y = 3.0 as the basic structure, a complex oxide with a value of (x1 + x2) / y less than 1.0 may have a cubic perovskite structure with a deficiency for one or more elements selected from potassium and barium. Also, a complex oxide with a value of z / y less than 3.0 may have a cubic perovskite structure with an oxygen deficiency. Furthermore, depending on the deficiency state of each element, the complex oxide may have a crystal structure of tetragonal, orthorhombic, or monoclinic in which (K, Ba)NbO3 blocks and NbO blocks are regularly stacked. In addition, a complex oxide with a value of z / y greater than 3.0 and less than 3.5 may have a crystal structure of cubic, tetragonal, or orthorhombic.

[0031] As infrared absorbing particles, materials with high infrared absorption in the infrared region and low visible light absorption in the visible light region are often required. However, since the required performance varies depending on the application and the like, it is not possible to generally determine which of the above crystal structures is preferable.

[0032] K x1 Ba x2 NbO z In the case of (2.0 < z ≤ 3.0), for example, when the value of (x1 + x2) is 0.8 or more and less than 1.0, it may have a cubic perovskite structure with a deficiency of K element and Ba element and, in some cases, further an oxygen deficiency. Also, it may have a crystal structure of tetragonal, orthorhombic, or monoclinic in which (K, Ba)NbO3 blocks and NbO blocks are regularly stacked. In the complex oxide with the above composition and crystal structure, the heat insulation property, which is important for window materials and the like, tends to be high. Note that the heat insulation property means a property determined by the balance between visible light transparency and near-infrared absorbability.

[0033] Thus, since the relationship between the crystal structure and the infrared absorption characteristics also changes depending on the composition of the complex oxide, the crystal structure of the complex oxide contained in the infrared absorbing particles of the present embodiment is not particularly limited and can be selected according to the composition of the complex oxide and the required infrared absorption characteristics and the like.

[0034] The lattice constant of the composite oxide is not particularly limited, but the lattice constant of the a-axis based on a cubic perovskite structure is preferably 3.96 Å to 4.14 Å, more preferably 3.97 Å to 4.14 Å, and even more preferably 3.98 Å to 4.13 Å. The lattice constant can be calculated by Rietveld analysis.

[0035] In addition, when the crystal structure is not cubic (i.e., tetragonal, orthorhombic, etc.), the lattice constant of the a-axis when the cubic perovskite structure is used as a reference (hereinafter, may be referred to as the "pseudocubic lattice constant") can be converted from the value of the lattice constant in the crystal structure. Specifically, the composition of the unit cell of the non-cubic crystal structure is identified. Then, the unit cell volume is calculated based on the lattice constant. Next, the unit cell volume per Nb atom is calculated. The calculated unit cell volume per Nb atom can be converted to the pseudocubic lattice constant by taking the cube root. (Particle characteristics of infrared absorbing particles) The particle characteristics such as particle diameter of the infrared absorbing particles of this embodiment are not particularly limited, and can be arbitrarily selected according to the required infrared absorbing characteristics, etc.

[0036] The infrared absorbing particles of this embodiment preferably have a volume-based cumulative 50% particle size of 1 nm or more and 50 nm or less, and a cumulative 90% particle size of 5 nm or more and 100 nm or less, as measured by a particle size distribution measuring device.

[0037] In general, it is known that materials containing free electrons or holes show a reflection-absorption response to infrared rays around the solar radiation range of wavelengths from 200 nm to 2600 nm due to plasma oscillation. It is also known that if powder particles of such materials are made smaller than the wavelength of light, geometric scattering in the visible light range (wavelengths from 380 nm to 780 nm) is reduced, and transparency in the visible light range is obtained.

[0038] In this specification, the term "transparency" is used to mean "high transmittance with little scattering of light in the visible light region."

[0039] Therefore, when the infrared absorbing particles of this embodiment are used in an application requiring transparency in the visible light region, it is preferable that the cumulative 90% particle diameter based on volume measured by a particle size distribution measuring device is 100 nm or less. This is because particles with a cumulative 90% particle diameter of 100 nm or less do not completely block light due to scattering, and can maintain visibility in the visible light region and efficiently maintain transparency at the same time. In particular, when transparency in the visible light region is important, it is preferable to further consider scattering by the particles.

[0040] When further reduction in scattering by infrared absorbing particles is required, the cumulative 90% particle size is more preferably 70 nm or less, and even more preferably 60 nm or less. If the particle size of the infrared absorbing particles is small, scattering of light in the visible light region with a wavelength of 380 nm or more and 780 nm or less due to geometric scattering or Mie scattering is reduced. Therefore, by setting the cumulative 90% particle size of the infrared absorbing particles to the above range, for example, it is possible to more reliably prevent an infrared absorbing particle dispersion using the infrared absorbing particles from becoming like cloudy glass and not being able to obtain clear transparency. When the cumulative 90% particle size is 70 nm or less, the geometric scattering or Mie scattering is reduced, and the Rayleigh scattering region is reached. And, in the Rayleigh scattering region, the scattered light is proportional to the sixth power of the particle size, so that scattering is reduced and transparency is improved as the particle size decreases.

[0041] Furthermore, if the cumulative 90% particle diameter is 60 nm or less, scattered light is very little, which is preferable. From the viewpoint of avoiding light scattering, it is preferable that the cumulative 90% particle diameter is small, so the lower limit of the cumulative 90% particle diameter is not particularly limited, but the cumulative 90% particle diameter is preferably 5 nm or more. This is because if the cumulative 90% particle diameter is 5 nm or more, industrial production is easy.

[0042] As described above, by setting the cumulative 90% particle size to 100 nm or less, for example, the haze of an infrared absorbing particle dispersion in which the infrared absorbing particles of this embodiment are dispersed in a solid medium can be set to 30% or less at a visible light transmittance of 85% or less. By setting the haze to 30% or less, particularly clear transparency can be obtained.

[0043] From the viewpoint of obtaining particularly excellent infrared absorbing properties, the cumulative 50% particle size of the infrared absorbing particles on a volume basis measured by a particle size distribution measuring device is preferably 1 nm or more. However, from the viewpoint of enhancing transparency in the visible light region, for the same reason as for the cumulative 90% particle size, the cumulative 50% particle size is preferably 50 nm or less.

[0044] The cumulative 50% particle size and cumulative 90% particle size of the infrared absorbing particles can be measured using a particle size distribution measuring device (such as UPA-150 manufactured by Nikkiso Co., Ltd.) based on the dynamic light scattering method analyzed by frequency analysis.

[0045] Particle size distribution data is expressed as cumulative % or frequency % on a particle size scale, but conversely, it may be expressed as particle size on a cumulative % scale. For example, the particle size at the point where the distribution curve expressed as particle size on a cumulative % scale crosses the horizontal axis at 10% is called the cumulative 10% particle size, and the particle size at the point where it crosses the horizontal axis at 50% is called the cumulative 50% particle size. Furthermore, the particle size at the point where it crosses the horizontal axis at 90% is called the cumulative 90% particle size. It is not particularly fixed to 10%, 50%, or 90%, and any cumulative % is used as needed. The 50% particle size is also called the median size and is very commonly used. When comparing the particle size distribution of multiple samples, this median size is often used because it is necessary to represent the size of the measurement target with a single number. For this reason, the median size is often confused with the average particle size, but the definitions are different and the two sizes do not usually match. These two diameters coincide only if the particle size distribution is symmetric about the center (50% diameter).

[0046] The infrared absorbing particles of the present embodiment described above have a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less. Therefore, the infrared absorbing particles of the present embodiment are transparent in the visible light region, while being highly absorbing in the infrared region at light wavelengths that cause scorching heat on human skin.

[0047] Furthermore, the infrared absorbing particles of this embodiment have strong light absorption in the wavelength region of 700 nm or more, and for example, when the visible light transmittance is set to 70%, the transmittance of light in the wavelength region of 700 nm or more and 2100 nm or less can be 20% or less. Therefore, it is possible to suppress the blue color and make the material less subject to restrictions on applications due to color. [2] Manufacturing method of infrared absorbing particles Next, the method for producing infrared ray absorbing particles according to this embodiment will be described. Since the infrared ray absorbing particles described above can be produced by the method for producing infrared ray absorbing particles according to this embodiment, some of the matters already described will not be described.

[0048] The infrared absorbing particles of the present embodiment can be manufactured by a solid-state reaction method. When synthesizing by the solid-state reaction method, for example, a potassium compound or an elemental potassium as a potassium element source, a barium compound or an elemental barium as a barium element source, and a niobium compound or an elemental niobium as a niobium element source can be used as raw materials.

[0049] The method for producing infrared absorbing particles of this embodiment may include a mixed powder preparation step (first mixed powder preparation step) of preparing a mixed powder of a potassium elemental source, a barium elemental source, and a niobium elemental source.

[0050] The potassium source may be one or more selected from potassium compounds and elemental potassium. The potassium compound used as the raw material is preferably one or more selected from oxides, hydroxides, carbonates, nitrates, sulfates, oxalates, organic compounds, sulfides, and chlorides of potassium.

[0051] The barium element source may be one or more selected from barium compounds and simple barium elements. The barium compound used as the raw material is preferably one or more selected from oxides, hydroxides, carbonates, nitrates, sulfates, oxalates, organic compounds, sulfides, and chlorides of barium.

[0052] The niobium element source may be one or more selected from niobium compounds and elemental niobium. The niobium element source is preferably one or more selected from niobium pentoxide (Nb2O5), dioxide (NbO2), sesquioxide (Nb2O3), elemental metal (Nb), sulfate, ammonium salt, organic compound, sulfide, chloride, and oxide hydrate obtained by dissolving the chloride in a liquid such as alcohol, adding water to hydrolyze, and evaporating the solvent.

[0053] In the mixed powder preparation step, the specific procedure for obtaining a mixed powder of potassium compounds or potassium elements, barium compounds or barium elements, and niobium compounds or niobium elements is not particularly limited. For example, the potassium compounds or the like which are the potassium element source, the barium compounds or the like which are the barium element source, and the niobium compounds or the like which are the niobium element source are dry-mixed in powder form to obtain a mixed powder. In addition, the potassium compounds or the like which are the potassium element source are dissolved in water, and then wet-mixed with the barium compounds or the like which are the barium element source and the niobium compounds or the like which are the niobium element source, and then dried to obtain a mixed powder.

[0054] In the mixed powder preparation step, it is preferable to mix the potassium, barium, and niobium in the mixed powder obtained so that the ratio of the substance amounts is the same as the ratio of the potassium, barium, and niobium in the target composite oxide. That is, it is preferable to mix so that the ratio of the total substance amount (A) of potassium and barium in the target composite oxide to the substance amount (B) of niobium is satisfied, A:B=(x1+x2):y. As described above, x1, x2, and y are preferably (x1+x2) / y=0.002≦(x1+x2) / y≦1.5, more preferably 0.5≦(x1+x2) / y≦1.0, and even more preferably 0.7≦(x1+x2) / y≦1.0. For this reason, it is preferable to mix the potassium compound, barium compound, and niobium compound so that the above-mentioned preferable range is satisfied.

[0055] In addition, the infrared absorbing particles of this embodiment can be synthesized in multiple stages to obtain infrared absorbing particles containing a composite oxide of the target composition. In this case, in the first mixed powder preparation step, the potassium compound or the like which is the potassium element source, the barium compound or the like which is the barium element source, and the niobium compound or the like which is the niobium element source can be mixed so as to obtain the composition of the intermediate product. When synthesizing the infrared absorbing particles of this embodiment in multiple stages, for example, in the first mixed powder preparation step, a mixture may be prepared using only raw materials of two types of element sources selected from the potassium element source, the barium element source, and the niobium element source. In this case, after the first firing step, an intermediate product containing two types of elements selected from potassium, barium, and niobium is generated.

[0056] The method for producing infrared absorbing particles of this embodiment may include a firing step (first firing step) of firing the mixed powder obtained in the mixed powder preparation step (first mixed powder preparation step).

[0057] The conditions for the firing step are not particularly limited. In the firing step, for example, the mixed powder can be fired in any atmosphere selected from an inert gas atmosphere, a reducing gas atmosphere, a vacuum atmosphere, a mixed gas atmosphere of an inert gas and a reducing gas, and an oxidizing atmosphere containing oxygen.

[0058] For example, in the case of a composite oxide, when oxygen vacancies are introduced and z / y in the general formula described above is made smaller than the stoichiometric ratio, the firing atmosphere is preferably a mixed gas atmosphere of an inert gas and a reducing gas. The reducing gas is not particularly limited, but is preferably, for example, hydrogen gas. In addition, when hydrogen gas is used as the reducing gas, the volume ratio of hydrogen gas is preferably 1% or more, and more preferably 3% or more. The upper limit of the volume ratio of hydrogen gas is not particularly limited, and since it can be reduced gas alone, it can be up to 100%.

[0059] The inert gas is not particularly limited, but one or more types selected from nitrogen gas, rare gases, and the like can be used.

[0060] The oxidizing atmosphere may be any atmosphere containing oxygen, for example, an atmosphere containing oxygen in a volume ratio of 18% to 100%. For example, the atmosphere may be air.

[0061] The firing temperature in the firing step is not particularly limited, but the firing temperature is preferably equal to or higher than the temperature at which the generated composite oxide starts to crystallize and equal to or lower than the melting point of the composite oxide. Specifically, the firing temperature is preferably set to, for example, 1000° C. or higher and 2100° C. or lower.

[0062] In the present embodiment, the infrared absorbing particles can be synthesized in multiple stages to obtain infrared absorbing particles containing a composite oxide of a target composition. When synthesizing in multiple stages, for example, a niobium compound or a simple niobium element, which is a niobium element source, can be added and mixed with the intermediate product obtained in the above-mentioned firing step (first firing step) (second mixed powder preparation step). It is also possible to prepare a plurality of types of intermediate products having different compositions and mix them in the second mixed powder preparation step. In this case, it is also possible to add and mix a niobium compound or a simple niobium element, which is a niobium element source, as necessary. When preparing a plurality of types of intermediate products having different compositions, the above-mentioned mixed powder preparation step (first mixed powder preparation step) and firing step (first firing step) can be performed for each intermediate product. It is also possible that the intermediate product contains two types of elements selected from potassium, barium, and niobium, and does not need to contain any of the three types of elements. In addition, in the second mixed powder preparation step, a potassium element source or a barium element source other than the niobium element source can be added as necessary.

[0063] The niobium compound used in the second mixed powder preparation step is not particularly limited, but may be, for example, the compound already described in the first mixed powder preparation step. In the second mixed powder preparation step, it is preferable to mix so that the ratio of the total amount of substance of potassium and barium in the resulting mixed powder to the amount of substance of niobium is the ratio of the total amount of substance of potassium and barium to the amount of substance of niobium in the target composite oxide. In other words, it is preferable to mix so as to satisfy A:B=(x1+x2):y, which is the ratio of the total amount of substance of potassium and barium (A) to the amount of substance of niobium (B) in the target composite oxide. Since the mixing can be performed in the same manner as in the mixed powder preparation step, a description thereof will be omitted here.

[0064] The obtained mixed powder is then subjected to a firing step (second firing step) to prepare the infrared absorbing particles of this embodiment. The conditions of the second firing step are not particularly limited, but the firing atmosphere and firing temperature can be performed in the same manner as described in the firing step (first firing step), for example, and therefore will not be described here. The firing conditions of the first firing step and the second firing step may be the same or different.

[0065] Although the method for producing infrared absorbing particles containing a composite oxide in two stages has been described as an example here, infrared absorbing particles containing a composite oxide can also be produced in n stages, which is three or more stages. In this case, the above description of the second mixed powder preparation step and the second firing step can be read as the nth mixed powder preparation step and the nth firing step.

[0066] The n-th mixed powder preparation step can be supplied with an intermediate product obtained by firing the mixed powder prepared in the (n-1)th mixed powder preparation step in the (n-1)th firing step.

[0067] In the n-1th mixed powder preparation step, the intermediate product obtained in the n-2nd firing step is used, and the intermediate product can be mixed with a niobium compound or elemental niobium, which is a niobium element source, according to the composition of the intermediate product to be supplied to the nth step. Other than the above, the configuration can be the same as that of the second mixed powder preparation step. Therefore, a description will be omitted. In the n-1th mixed powder preparation step, a potassium element source or a barium element source other than the niobium element source can also be added as necessary.

[0068] In addition, the n-1st firing step can be performed under the same firing conditions as the first firing step and the second firing step, except that the mixed powder prepared in the n-1st mixed powder preparation step is used, so the explanation is omitted. Note that the conditions for each firing step may be the same or different.

[0069] By carrying out the steps described above, the infrared ray absorbing particles of the present embodiment can be obtained. After the firing step is completed, the obtained infrared ray absorbing particles can be crushed, pulverized, sieved, or the like, as necessary, to obtain a desired particle size distribution. [3] Infrared absorbing particle dispersion Next, the infrared absorbing particle dispersion liquid of this embodiment will be described.

[0070] The infrared absorbing particle dispersion of this embodiment can contain a liquid medium and the above-mentioned infrared absorbing particles contained in the liquid medium. That is, for example, as shown in Fig. 2, the infrared absorbing particle dispersion 20 of this embodiment can contain the above-mentioned infrared absorbing particles 21 and a liquid medium 22. The infrared absorbing particles 21 are preferably dispersed in the liquid medium 22.

[0071] 2 is a schematic diagram, and the infrared absorbing particle dispersion of this embodiment is not limited to this form. For example, in FIG. 2, the infrared absorbing particles 21 are represented by circles and described as spherical particles, but the shape of the infrared absorbing particles 21 is not limited to this form and can have any shape. The infrared absorbing particle dispersion 20 can contain other additives as necessary in addition to the infrared absorbing particles 21 and the liquid medium 22.

[0072] The infrared absorbing particle dispersion liquid of this embodiment can be obtained by using the infrared absorbing particles described above, in other words, by using infrared absorbing particles obtained by the infrared absorbing particle manufacturing method described above.

[0073] The infrared absorbing particle dispersion may contain, in addition to the infrared absorbing particles and the liquid medium, a dispersant and other additives as desired. The infrared absorbing particle dispersion may be used as an intermediate product of the infrared absorbing particle dispersion or as a coating liquid.

[0074] The liquid medium means a medium that is liquid at the temperature of use, and is preferably a medium that is liquid at room temperature (27° C.) in particular. The liquid medium is not particularly limited and can be arbitrarily selected depending on the application, etc., but it is preferable that the liquid medium contains one or more selected from water, organic solvents, liquid plasticizers, oils and fats, and compounds that are polymerized by curing.

[0075] The infrared absorbing particle dispersion liquid of this embodiment will be described below in the order of (1) contained materials, (2) a method for producing the infrared absorbing particle dispersion liquid, (3) a method for using the infrared absorbing particle dispersion liquid, and an article using the infrared absorbing particle dispersion liquid. (1) Materials contained (1-1) Infrared absorbing particles The infrared absorbing particle dispersion liquid of this embodiment can contain the infrared absorbing particles described above. The infrared absorbing particles have already been described, so a description thereof will be omitted here. (1-2)Liquid medium (1-2-1) Organic Solvent As the organic solvent used as the liquid medium, for example, one or more types selected from alcohols, ketones, esters, glycol derivatives, amides, aromatic hydrocarbons, and the like can be suitably used.

[0076] Specifically, alcohol-based materials such as methanol, ethanol, 1-propanol, isopropanol, butanol, pentanol, benzyl alcohol, and diacetone alcohol; Ketone-based materials such as acetone, methyl ethyl ketone, dimethyl ketone, methyl propyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone; Ester-based materials such as 3-methyl-methoxy-propionate, n-butyl acetate; Glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol isopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; Amides such as formamide, N-methylformamide, dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone; Aromatic hydrocarbons such as toluene and xylene; The organic solvent may be one or more selected from ethylene chloride, chlorobenzene, and the like.

[0077] Among the above organic solvents, one or more selected from dimethyl ketone, methyl ethyl ketone, methyl isobutyl ketone, toluene, propylene glycol monomethyl ether acetate, n-butyl acetate, and the like can be more preferably used. (1-2-2)Oils and fats The oil or fat used as the liquid medium is not particularly limited, but vegetable oil or a compound derived from vegetable oil can be preferably used.

[0078] As the vegetable oil, one or more types selected from drying oils such as linseed oil, sunflower oil, tung oil, and perilla oil, semi-drying oils such as sesame oil, cottonseed oil, rapeseed oil, soybean oil, rice bran oil, and poppy oil, and non-drying oils such as olive oil, coconut oil, palm oil, and dehydrated castor oil can be preferably used.

[0079] As the compound derived from vegetable oil, one or more selected from fatty acid monoesters obtained by direct esterification of fatty acids of vegetable oil with monoalcohols, ethers, and the like can be preferably used.

[0080] Commercially available petroleum-based solvents can also be used as the oils and fats.

[0081] Commercially available petroleum-based solvents that can be used include Isopar (registered trademark) E, Exxor (registered trademark) (hereinafter the same), Hexane, Heptane, E, D30, D40, D60, D80, D95, D110, and D130 (all manufactured by ExxonMobil). (1-2-3) Liquid plasticizers Examples of the liquid plasticizer used as the liquid medium include one or more selected from the group consisting of plasticizers that are compounds of monohydric alcohols and organic acid esters, ester-based plasticizers such as polyhydric alcohol organic acid ester compounds, and phosphoric acid-based plasticizers such as organic phosphoric acid-based plasticizers. Note that any of these plasticizers that are liquid at room temperature are preferred.

[0082] Among them, a plasticizer that is an ester compound synthesized from a polyhydric alcohol and a fatty acid can be preferably used. The ester compound synthesized from the polyhydric alcohol and the fatty acid is not particularly limited, but for example, a glycol-based ester compound obtained by reacting a glycol with a monobasic organic acid can be preferably used. As the glycol, one or more selected from triethylene glycol, tetraethylene glycol, tripropylene glycol, etc. can be preferably used. In addition, as the monobasic organic acid, one or more selected from butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, pelargonic acid (n-nonylic acid), decyl acid, etc. can be preferably used.

[0083] Also, ester compounds of tetraethylene glycol, tripropylene glycol, and monobasic organic acids can be preferably used. Among them, one or more selected from fatty acid esters of triethylene glycol, such as triethylene glycol dihexanate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-octanate, and triethylene glycol di-2-ethylhexanoate, can be preferably used. Furthermore, fatty acid esters of triethylene glycol can also be preferably used. (1-2-4) Compounds that become polymerized by curing As the compound that is polymerized by curing and is used in the infrared absorbing particle dispersion liquid of this embodiment, a monomer or oligomer that forms a polymer by a polymerization reaction or the like caused by heat, light, or water can be suitably used.

[0084] Specific examples of compounds that can be polymerized by curing include methyl methacrylate monomers, acrylate monomers, and styrene resin monomers.

[0085] The liquid media described above may be used in combination of two or more kinds. Furthermore, if necessary, an acid or an alkali may be added to these liquid media to adjust the pH. (1-3) Dispersants In the infrared absorbing particle dispersion liquid of this embodiment, in order to further improve the dispersion stability of the infrared absorbing particles and to prevent the particle size from increasing due to re-aggregation, the infrared absorbing particle dispersion liquid of this embodiment may also contain various dispersants, surfactants, coupling agents, and the like.

[0086] The dispersant, coupling agent, and surfactant can be selected according to the application, but it is preferable that the material has one or more functional groups selected from an amine-containing group, a hydroxyl group, a carboxyl group, a phosphate group, and an epoxy group. These functional groups adsorb to the surface of the infrared absorbing particles to prevent aggregation and disperse uniformly. A polymer dispersant having one or more functional groups selected from these functional groups in the molecule can be more preferably used as the dispersant.

[0087] Specific examples of commercially available dispersants include SOLSPERSE (registered trademark) 3000, 5000, 9000, 11200, 12000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000SC, 24000GR, 26000, 27000, and 280 manufactured by Lubrizol Japan. 00, 31845, 32000, 32500, 32550, 32600, 33000, 33500, 34750, 35100, 35200, 36600, 37500, 38500, 39000, 41000, 41090, 53095, 55000, 56000, 71000, 76500, J180, J200, M387, etc.; SOLPLUS (registered trademark) (hereinafter the same) D5 10, D520, D530, D540, DP310, K500, L300, L400, R700, etc.; Disperbyk (registered trademark) manufactured by BYK Japan (hereinafter the same) -101, 102, 103, 106, 107, 108, 109, 110, 111, 112, 116, 130, 140, 142, 145, 154, 161, 162, 163, 164, 165, 16 6, 167, 168, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 191, 192, 2000, 2001, 2009, 2020, 2025, 2050, 2070, 2095, 2096, 2150, 2151, 2152, 2155, 2163, 2164, Anti-Terra (registered trademark) (hereinafter the same)-U, 203, 204, etc.;BYK (registered trademark) (hereinafter the same)-P104, P104S, P105, P9050, P9051, P9060, P9065, P9080, 051, 052, 053, 054, 055, 057, 063, 065, 066N, 067A, 077, 088, 141, 220S, 300, 302, 306, 307, 310, 315, 320, 322, 323, 325, 330, 331, 333, 337, 340, 345, 346, 347, 348, 350, 354, 355, 358N, 361N, 370, 375, 377, 378, 380N, 381, 392, 410, 425, 430, 1752, 4510, 6919, 9076, 9077, W909, W935, W940, W961, W966, W969, W972, W980, W985, W995, W996, W9010, D ynwet800, Cyclean3700, UV3500, UV3510, UV3570, etc.; EFKA Additives' EFKA (registered trademark) (hereinafter the same) 2020, 2025, 3030, 3031, 3236, 4008, 4009, 4010, 4015, 4020, 4046, 4047, 4050, 4055, 4060, 4080, 4300, 4310, 4320, 4330, 43 40, 4400, 4401, 4402, 4403, 4500, 5066, 5220, 6220, 6225, 6230, 6700, 6780, 6782, 7462, 8503, etc.; JONCRYL (registered trademark) manufactured by BASF Japan Ltd. (hereinafter the same); 67, 678, 586, 611, 680, 682, 690, 819, -JDX5050, etc.; TERPLUS (registered trademark) manufactured by Otsuka Chemical Co., Ltd. (hereinafter the same) MD1000, D 1180, D 1130, etc.; Ajisper (registered trademark) (hereinafter the same) PB-711, PB-821, PB-822, etc., manufactured by Ajinomoto Fine-Techno Co., Ltd.; Disparlon (registered trademark) (hereinafter the same) 1751N, 1831, 1850, 1860, 1934, DA-400N, DA-703-50, DA-325, DA-375, DA-550, DA-705, DA-725, DA-1401, DA-7301, DN-900, NS-5210, NVI-8514L, etc., manufactured by Kusumoto Chemicals Co., Ltd.;Examples of such products include Arphon (registered trademark) (hereinafter the same) UH-2170, UC-3000, UC-3910, UC-3920, UF-5022, UG-4010, UG-4035, UG-4040, and UG-4070, and Reseda (registered trademark) (hereinafter the same) GS-1015, GP-301, and GP-301S, manufactured by Toagosei Co., Ltd.; and Dianale (registered trademark) (hereinafter the same) BR-50, BR-52, BR-60, BR-73, BR-77, BR80, BR-83, BR-85, BR-87, BR-88, BR-90, BR-96, BR-102, BR-113, and BR-116, manufactured by Mitsubishi Chemical Corporation.

[0088] In addition, a liquid dispersant having a glass transition temperature lower than room temperature can be used instead of the liquid medium. That is, the infrared absorbing particle dispersion of this embodiment can contain infrared absorbing particles and a liquid dispersant, or can be composed of infrared absorbing particles and a liquid dispersant. Preferable specific examples of commercially available liquid dispersants include SOLSPERSE (registered trademark) 20000 manufactured by Lubrizol Japan, Disparlon (registered trademark) (hereinafter the same) DA234, DA325, DA375 manufactured by Kusumoto Chemicals, etc. (1-4) Other additives The infrared absorbing particle dispersion of this embodiment may contain additives such as various surfactants and resin components in order to control the coating property, leveling property, and drying property. When the additive is added, the infrared absorbing particle dispersion preferably contains the additive in a small amount within the range of 5% by mass or less of the dispersion. The surfactant may be anionic, cationic, nonionic, or amphoteric.

[0089] Furthermore, in order to impart flexibility to the infrared absorbing particle dispersion obtained by using the infrared absorbing particle dispersion, the dispersion may contain one or more organic resins selected from silicone resins, acrylic resins, polyester resins, polyurethane resins, hydrophilic organic resins containing a polyoxyalkylene group, epoxy resins, etc. When the organic resin is added, the infrared absorbing particle dispersion preferably contains a small amount of the organic resin in the range of 5% by mass or less of the infrared absorbing particle dispersion.

[0090] In addition, in order to impart crack prevention to the infrared absorbing particle dispersion prepared using the infrared absorbing particle dispersion, the infrared absorbing particle dispersion may contain one or more resins selected from thermosetting resins, thermoplastic resins, ultraviolet curing resins, etc. When the resin is added, the infrared absorbing particle dispersion preferably contains the resin in an amount of 20 mass% or less of the dispersion. More specifically, examples of the resin include acrylic resins, epoxy resins, polyester resins, amino resins, urethane resins, furan resins, silicone resins, and modified products of these resins. (2) Method for producing infrared absorbing particle dispersion The manufacturing method of the infrared absorbing particle dispersion liquid of this embodiment is not particularly limited. The infrared absorbing particle dispersion liquid of this embodiment can be prepared, for example, by adding and dispersing the infrared absorbing particles described above and, if necessary, a dispersant or other additives into the liquid medium described above. Note that, instead of the liquid medium as described above, a liquid dispersant can also be used.

[0091] The method for dispersing infrared absorbing particles and the like in a liquid medium is not particularly limited, and examples thereof include pulverization and dispersion methods using devices such as a bead mill, a ball mill, a sand mill, a paint shaker, an ultrasonic homogenizer, etc. Among these, media agitation mills such as a bead mill, a ball mill, a sand mill, and a paint shaker using media such as beads, balls, and Ottawa sand can be preferably used because they can give the infrared absorbing particles a desired particle size in a short period of time.

[0092] By the grinding and dispersion process using the media stirring mill, the infrared absorbing particles are dispersed in the liquid medium, and at the same time, the infrared absorbing particles are atomized due to collisions between the infrared absorbing particles and between the medium and the infrared absorbing particles, and the infrared absorbing particles are further atomized and dispersed. In other words, the infrared absorbing particles are ground and dispersed.

[0093] The dispersion concentration of the infrared absorbing particles in the infrared absorbing particle dispersion is preferably 0.01% by mass or more and 80% by mass or less. This is because sufficient infrared absorbing properties can be exhibited by making the content of the infrared absorbing particles 0.01% by mass or more. In addition, by making the content 80% by mass or less, the infrared absorbing particles can be uniformly dispersed in the liquid medium. By selecting a combination of the liquid medium, dispersant, coupling agent, and surfactant, the infrared absorbing particle dispersion of this embodiment can prevent gelation of the dispersion or sedimentation of the particles for more than 6 months even when placed in a thermostatic bath at a temperature of 40°C, and can suppress an increase in particle size. (3) Method of using infrared absorbing particle dispersion liquid and article using infrared absorbing particle dispersion liquid The applications of the infrared absorbing particle dispersion liquid of the present embodiment are not particularly limited, and the infrared absorbing particle dispersion liquid can be used for various applications.

[0094] The infrared absorbing particle dispersion of the present embodiment can be used as an infrared absorbing substrate by, for example, forming a dispersion film by applying it to the surface of a suitable substrate. The dispersion film is a type of infrared absorbing particle dispersion and a type of dried solid of the infrared absorbing particle dispersion.

[0095] In addition, the infrared absorbing particle dispersion liquid of this embodiment can be dried and pulverized as necessary to form a powdered infrared absorbing particle dispersion (sometimes referred to as "dispersed powder" in this specification). In other words, the dispersed powder is a type of infrared absorbing particle dispersion liquid, and is also a type of dried solidified infrared absorbing particle dispersion liquid. The dispersed powder can also be a powdered dispersion liquid in which infrared absorbing particles are dispersed in a solid medium such as a dispersant. Since the dispersed powder contains a dispersant, it is possible to easily redisperse the infrared absorbing particles in the medium by mixing with an appropriate medium.

[0096] The above-mentioned dispersion powder can also be used as a raw material for adding the infrared absorbing particles in a dispersed state to an infrared absorbing product. That is, the dispersion powder in which the infrared absorbing particles of this embodiment are dispersed in a solid medium may be dispersed again in a liquid medium and used as a dispersion liquid for an infrared absorbing product, or the dispersion powder may be kneaded into a resin and used as an infrared absorbing particle dispersion, as described later.

[0097] The infrared absorbing particle dispersion liquid of this embodiment can be used for various applications that utilize light-to-heat conversion.

[0098] For example, a curable ink composition can be prepared by adding an infrared absorbing particle dispersion to an uncured thermosetting resin or by adding an uncured thermosetting resin to an infrared absorbing particle dispersion. The curable ink composition contains the infrared absorbing particles described above, and the infrared absorbing particles function as an auxiliary agent for increasing the amount of heat generated by infrared irradiation such as infrared rays. Since the curable ink composition contains a thermosetting resin, the infrared absorbing particles function as an auxiliary agent for increasing the amount of heat generated by irradiating the curable ink composition with infrared rays, as described above, and the thermosetting resin can be cured. By providing the curable ink composition on, for example, a substrate, the adhesion between the cured product of the curable ink composition and the substrate can be increased when irradiated with infrared rays, etc.

[0099] Therefore, in addition to being used as a conventional ink, the curable ink composition can be suitably used in applications such as stereolithography, in which a three-dimensional object is formed by repeatedly applying the ink and curing it by irradiating it with infrared light or the like to build up the ink.

[0100] Alternatively, a thermoplastic resin-containing ink composition can be obtained by adding the infrared absorbing particles of this embodiment to a thermoplastic resin that has been heated and melted, or by dispersing the infrared absorbing particles of this embodiment in a suitable solvent and then adding a thermoplastic resin that is highly soluble in the solvent.

[0101] For example, by providing a thermoplastic resin-containing ink composition on a substrate and irradiating it with infrared rays or the like, the solvent is removed and the resin is heat-fused, whereby the cured product of the thermoplastic resin-containing ink composition can be adhered to the substrate. In this case, in the thermoplastic resin-containing ink composition, the infrared absorbing particles function as an auxiliary agent that increases the amount of heat generated by irradiation with infrared rays or the like, as in the case of the curable ink composition described above.

[0102] Therefore, in addition to its use as a conventional ink, the thermoplastic resin-containing ink composition can be suitably used in applications such as photolithography, in which a three-dimensional object is formed by repeatedly applying the ink, removing the solvent by irradiating the ink with infrared rays or the like, and heating and fusing the resin.

[0103] The curable ink composition and the thermoplastic resin-containing ink composition described above are also examples of the infrared absorbing particle dispersion liquid of this embodiment. [4] Infrared absorbing particle dispersion Next, the infrared absorbing particle dispersion of this embodiment will be described.

[0104] The infrared absorbing particle dispersion of this embodiment can contain a solid medium and the infrared absorbing particles contained in the solid medium. Specifically, for example, as shown in FIG. 3, the infrared absorbing particle dispersion 30 can contain the infrared absorbing particles 31 and the solid medium 32, and the infrared absorbing particles 31 can be arranged in the solid medium 32. It is preferable that the infrared absorbing particles 31 are dispersed in the solid medium 32. Note that FIG. 3 is a schematic diagram, and the infrared absorbing particle dispersion of this embodiment is not limited to such a form. For example, in FIG. 3, the infrared absorbing particles 31 are represented by circles and described as spherical particles, but the shape of the infrared absorbing particles 31 is not limited to such a form and can have any shape. The infrared absorbing particle dispersion 30 can contain other additives as necessary in addition to the infrared absorbing particles 31 and the solid medium 32.

[0105] The solid medium means a medium that is solid at the temperature of use, and is preferably a medium that is solid at room temperature (27° C.) As the solid medium, resin, glass, etc. can be used.

[0106] As the solid medium, a resin can be particularly preferably used from the viewpoint of ease of handling.

[0107] When a resin is used as the solid medium, the type of resin is not particularly limited, but the resin can be, for example, one type of resin selected from the group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and ultraviolet-curable resin, or a mixture of two or more types of resins selected from the above resin group.

[0108] The content of infrared absorbing particles in the infrared absorbing particle dispersion is not particularly limited, but the infrared absorbing particle dispersion preferably contains infrared absorbing particles at a ratio of 0.001% by mass or more and 80% by mass or less. This is because the infrared absorbing particles contain 0.001% by mass or more, and therefore sufficient infrared shielding function can be exhibited. In addition, by making the content of infrared absorbing particles 80% by mass or less, it is possible to suppress the infrared absorbing particles from agglomerating together in the solid medium, and thus it is possible to maintain particularly good transparency. In addition, it is advantageous in terms of cost because the amount of infrared absorbing particles used can be suppressed. Furthermore, by making the content of infrared absorbing particles 80% by mass or less, the proportion of the solid medium contained in the infrared absorbing particle dispersion can be increased, and the strength of the dispersion can be increased.

[0109] The shape of the infrared absorbing particle dispersion of the present embodiment is not particularly limited and can be arbitrarily selected depending on the application, etc. For example, the infrared absorbing particle dispersion of the present embodiment preferably has any one of a sheet shape, a board shape, and a film shape.

[0110] The infrared absorbing particle dispersion of the present embodiment will be described in the following order: (1) a method for producing the infrared absorbing particle dispersion, (2) an infrared absorbing substrate, and (3) a method for using the infrared absorbing particle dispersion and an article using the infrared absorbing particle dispersion. (1) Method for producing infrared absorbing particle dispersion The method for producing the infrared absorbing particle dispersion is not particularly limited. The infrared absorbing particle dispersion can be produced, for example, by kneading the above-mentioned infrared absorbing particles into a solid medium such as a resin, and molding the mixture into a desired shape such as a film or a board.

[0111] The infrared absorbing particle dispersion can also be produced by mixing the infrared absorbing particle dispersion liquid described above with a solid medium such as a resin. It is also possible to produce an infrared absorbing particle dispersion by adding a powder dispersion in which infrared absorbing particles are dispersed in a solid medium, i.e., the above-described dispersed powder, to a liquid medium and mixing it with a solid medium such as a resin.

[0112] The shape of the infrared absorbing particle dispersion of this embodiment is not particularly limited, but when a resin is used as the solid medium, the dispersion may be in the form of a sheet having a thickness of 0.1 μm or more and 50 mm or less, a board, or a film.

[0113] As described above, when preparing an infrared absorbing particle dispersion by kneading infrared absorbing particles into a solid medium such as a resin, the infrared absorbing particles and the solid medium are heated and mixed at a temperature near the melting point of the solid medium, for example, a resin (for example, about 200° C. or higher and 300° C. or lower), and kneaded together.

[0114] The material obtained by kneading the infrared absorbing particles into a solid medium can be molded into a desired shape, but it is also possible to first pelletize the material and then mold the pellets into a desired shape such as a film or board by various methods.

[0115] The molding method is not particularly limited, and for example, extrusion molding, inflation molding, solution casting, casting, etc. can be used.

[0116] As described above, when the infrared absorbing particle dispersion is in the form of a sheet, board, or film, the thickness is not particularly limited and can be selected depending on the application.

[0117] Furthermore, the amount of filler relative to the solid medium in the infrared absorbing particle dispersion, i.e., the blending amount of the infrared absorbing particles, can be arbitrarily selected depending on the thickness of the infrared absorbing particle dispersion and the optical properties and mechanical properties required for the infrared absorbing particle dispersion. For example, it is generally preferably 80 mass % or less relative to the solid medium, for example, a resin.

[0118] If the amount of filler relative to the solid medium is 80% by mass or less, the infrared absorbing particles in the solid medium can be prevented from granulating with each other, so that particularly good transparency can be maintained. In addition, the amount of infrared absorbing particles used can be reduced, which is advantageous in terms of cost.

[0119] The lower limit of the amount of filler relative to the solid medium is not particularly limited, but from the viewpoint of the infrared absorbing particle dispersion exerting a sufficient infrared shielding function, it is preferably, for example, 0.001 mass % or more.

[0120] The infrared absorbing particle dispersion can also be used in a powder state by further pulverizing the infrared absorbing particle dispersion in which infrared absorbing particles are dispersed in a solid medium. When this configuration is adopted, the infrared absorbing particles are sufficiently dispersed in the solid medium in the powdered infrared absorbing particle dispersion. Therefore, the powdered infrared absorbing particle dispersion can be dissolved in a suitable liquid medium as a so-called master batch, or kneaded with resin pellets or the like, to easily produce a liquid or solid infrared absorbing particle dispersion.

[0121] The solid medium that becomes the matrix of the above-mentioned sheet, board, and film is not particularly limited and can be selected according to the application. As mentioned above, resin can be preferably used from the viewpoint of handling. When using a resin as the solid medium, one type of resin selected from the resin group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and ultraviolet curable resin, or a mixture of two or more types of resins selected from the above resin group can be preferably used. In particular, one or more types of resin selected from polyethylene terephthalate resin, acrylic resin, polyamide resin, vinyl chloride resin, polycarbonate resin, polyolefin resin, epoxy resin, polyimide resin, etc. can be preferably used as a resin that is low cost, highly transparent, and has a wide range of versatility. In addition, fluororesin can also be used in consideration of weather resistance. (2) Infrared absorbing substrate The infrared absorbing particle dispersion of this embodiment also includes the form of an infrared absorbing substrate having a substrate and a dispersion film containing the above-mentioned infrared absorbing particles arranged on the surface of the substrate. Specifically, as shown in FIG. 4, which is a cross-sectional schematic diagram along the lamination direction of the substrate and the dispersion film, an infrared absorbing substrate 40 can have a substrate 41 and a dispersion film 42 containing infrared absorbing particles. The dispersion film 42 containing infrared absorbing particles can be arranged on at least one surface 41A of the substrate 41.

[0122] Such an infrared absorbing substrate can be produced, for example, by the following procedure.

[0123] The above-mentioned infrared absorbing particles, a liquid medium such as an organic solvent such as alcohol or water, a resin binder, and optionally a dispersant are mixed to prepare an infrared absorbing particle dispersion (dispersion preparation step).

[0124] Next, the infrared absorbing particle dispersion liquid is applied to a suitable substrate surface (application step).

[0125] The liquid medium is removed or the resin binder is cured to obtain a dispersion film that is an infrared absorbing particle dispersion (dispersion preparation step). Note that both the removal of the liquid medium and the curing of the resin binder may be performed.

[0126] By the above steps, an infrared absorbing substrate is obtained in which the infrared absorbing particle dispersion is directly laminated on the surface of the substrate.

[0127] The resin binder component can be selected according to the application, and examples thereof include ultraviolet curable resins, thermosetting resins, room temperature curable resins, thermoplastic resins, and the like.

[0128] The method for producing the infrared absorbing substrate is not limited to the above method, and may be, for example, a method for coating an infrared absorbing particle dispersion liquid not containing a resin binder component, and laminating the infrared absorbing particle dispersion on the substrate surface. In addition, after forming an infrared absorbing particle dispersion by coating the above-mentioned infrared absorbing particle dispersion liquid not containing a resin binder component, a liquid medium containing a binder component may be coated on the layer of the infrared absorbing particle dispersion.

[0129] Therefore, in the method for producing the infrared absorbing substrate, specifically, first, a liquid infrared absorbing particle dispersion liquid in which infrared absorbing particles are dispersed in one or more liquid media selected from an organic solvent, an organic solvent in which a resin is dissolved, an organic solvent in which a resin is dispersed, and water can be applied to the surface of the substrate. Then, the obtained coating film can be solidified by an appropriate method to obtain the infrared absorbing substrate.

[0130] As the resin, for example, a resin binder can be used. As described above, a liquid infrared absorbing particle dispersion containing a resin binder can be applied to the surface of a substrate, and the resulting coating film can be solidified by an appropriate method to form an infrared absorbing substrate.

[0131] Alternatively, an infrared absorbing substrate can be obtained by mixing an infrared absorbing particle dispersion, in which infrared absorbing particles are dispersed in a powdery solid medium, with a predetermined medium to form a liquid infrared absorbing particle dispersion, applying the liquid infrared absorbing particle dispersion to the surface of a substrate, and solidifying the resulting coating film by an appropriate method.

[0132] Of course, an infrared absorbing substrate can also be prepared by applying an infrared absorbing particle dispersion obtained by mixing two or more of the above-mentioned liquid infrared absorbing particle dispersions onto a substrate surface and solidifying the resulting coating film by an appropriate method.

[0133] The material of the substrate used in the infrared absorbing substrate is not particularly limited as long as it is transparent, but preferably one or more types selected from glass, a resin sheet, a resin board, a resin film, etc. Note that a transparent body is a material that transmits light in the visible light region, and the degree of transmission of light in the visible light region can be arbitrarily selected depending on the application of the infrared absorbing substrate, etc.

[0134] Resins used for resin sheets, resin boards, and resin films are not particularly limited and can be selected according to the required properties such as the surface condition and durability of the sheet, board, or film. Examples of the resin include polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as diacetyl cellulose and triacetyl cellulose, polycarbonate polymers, acrylic polymers such as polymethyl methacrylate, styrene polymers such as polystyrene and acrylonitrile-styrene copolymers, olefin polymers such as polyethylene, polypropylene, polyolefins having a cyclic or norbornene structure, and ethylene-propylene copolymers, vinyl chloride polymers, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, arylate polymers, polyoxymethylene polymers, epoxy polymers, and further transparent polymers such as various binary and ternary copolymers, graft copolymers, and blends thereof. In particular, polyester-based biaxially oriented films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate are preferred in terms of mechanical properties, optical properties, heat resistance, and economic efficiency. The polyester-based biaxially oriented film may be a copolymer polyester-based film. (3) Method of using infrared absorbing particle dispersion and article using infrared absorbing particle dispersion The infrared absorbing particle dispersion and infrared absorbing base material of the present embodiment described above can transmit light in the visible light region and block light in the infrared region. Therefore, for example, they can be used in various buildings and vehicles as window materials for the purpose of blocking light in the infrared region while sufficiently taking in visible light, and suppressing a rise in temperature inside the room while maintaining brightness. In particular, the infrared absorbing particles described above can have a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less. Therefore, according to the infrared absorbing particle dispersion of the present embodiment, it is possible to suppress the intrusion of infrared rays in the above wavelength region into the room, and to suppress the feeling of scorching heat on the human skin.

[0135] Furthermore, the infrared absorbing particle dispersion of this embodiment can be suitably used for filters that block infrared rays emitted forward from a PDP (plasma display panel), and the like.

[0136] In addition, since the infrared absorbing particles of this embodiment have absorption in the infrared region, when an infrared laser is irradiated onto a printed surface containing the infrared absorbing particles, the infrared ray having a specific wavelength is absorbed. Therefore, the counterfeit prevention printed matter obtained by printing the counterfeit prevention ink containing the infrared absorbing particles onto one or both sides of a printed substrate can be judged for authenticity from the difference in the amount of reflection or transmission by irradiating the counterfeit prevention printed matter with infrared rays having a specific wavelength and reading the reflection or transmission. The counterfeit prevention printed matter is an example of the infrared absorbing particle dispersion of this embodiment.

[0137] In addition, the ink obtained by mixing the above-mentioned infrared absorbing particle dispersion liquid and a binder component is applied onto a substrate, the applied ink is dried, and the dried ink is cured to form a photothermal conversion layer. The photothermal conversion layer generates heat at the location irradiated with an infrared laser, and can heat adjacent materials. Therefore, the photothermal conversion layer can generate heat only at the desired location with high positional accuracy by irradiation with an infrared laser. Therefore, the photothermal conversion layer can be applied as a local heating medium in a wide range of fields such as electronics, medicine, agriculture, and machinery. For example, it can be suitably used as a donor sheet used when forming an organic electroluminescence element by a laser transfer method, thermal paper for a thermal printer, or an ink ribbon for a thermal transfer printer. The photothermal conversion layer is an example of the infrared absorbing particle dispersion of this embodiment.

[0138] In addition, the infrared absorbing particles described above are dispersed in a suitable medium, and the dispersion is contained in one or more locations selected from the surface and the inside of the fiber, to produce an infrared absorbing fiber. Since the infrared absorbing fiber contains infrared absorbing particles, it efficiently absorbs near infrared rays from sunlight and the like, and is an infrared absorbing fiber with excellent heat retention. Since the infrared absorbing fiber transmits light in the visible light region, it is an infrared absorbing fiber with excellent design properties.

[0139] As a result, the infrared absorbing fiber can be used for various applications such as textile products requiring heat retention, such as cold weather clothing, sports clothing, stockings, curtains, and other industrial textile products, etc. The infrared absorbing fiber is an example of the infrared absorbing particle dispersion of this embodiment.

[0140] The infrared absorbing particle dispersion of this embodiment can also be applied to materials such as roofs and exterior wall materials of agricultural and horticultural greenhouses. The infrared absorbing particle dispersion of this embodiment transmits visible light, so light necessary for photosynthesis of plants in the agricultural and horticultural greenhouses can be secured. The infrared absorbing particles of this embodiment can efficiently absorb light other than visible light, such as near-infrared light contained in sunlight, so that the infrared absorbing particles can be used as a heat insulating material for agricultural and horticultural facilities having heat insulating properties. The heat insulating material for agricultural and horticultural facilities is an example of the infrared absorbing particle dispersion of this embodiment. [5] Infrared absorbing laminate The infrared absorbing laminate of this embodiment can have a laminated structure including the infrared absorbing particle dispersion and a transparent substrate. For example, the infrared absorbing laminate can be an example in which two or more transparent substrates are laminated with the infrared absorbing particle dispersion. In this case, the infrared absorbing particle dispersion can be disposed between the transparent substrates and used as an intermediate film for infrared absorption.

[0141] In this case, specifically, as shown in Fig. 5 which is a cross-sectional schematic diagram along the lamination direction of the transparent substrate and the infrared absorbing particle dispersion, the infrared absorbing laminate 50 can have a plurality of transparent substrates 511, 512 and an infrared absorbing particle dispersion 52. The infrared absorbing particle dispersion 52 which is an infrared absorbing intermediate film can be disposed between the plurality of transparent substrates 511, 512. Although Fig. 5 shows an example in which two transparent substrates 511, 512 are provided, the present invention is not limited to this embodiment.

[0142] In this case, the infrared absorbing interlayer film preferably has any one of a sheet shape, a board shape, and a film shape.

[0143] The transparent substrate may be one or more selected from glass sheets, plastic sheets, plastic films, etc., which are transparent in the visible light region. The transparent substrate being transparent in the visible light region means that the substrate transmits light in the visible light region. The degree to which the transparent substrate transmits light in the visible light region can be selected as desired depending on the application of the infrared absorbing laminate.

[0144] When plastic is used as the transparent substrate, the material of the plastic is not particularly limited and can be selected according to the application, and can be, for example, one or more types selected from polycarbonate resin, acrylic resin, polyester resin, polyamide resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, ionomer resin, fluororesin, etc. As the polyester resin, polyethylene terephthalate resin can be preferably used.

[0145] The transparent substrate may contain particles having an infrared absorbing function. As the particles having an infrared absorbing function, for example, the above-mentioned infrared absorbing particles can be used.

[0146] By using the infrared absorbing particle dispersion described above as a constituent member of an intermediate layer sandwiched between multiple transparent substrates, a solar radiation-shielding laminated structure that is a type of infrared absorbing laminate that transmits visible light and has an infrared absorbing function can be obtained.

[0147] The infrared absorbing laminate can also be obtained by bonding and integrating a plurality of transparent substrates facing each other with the infrared absorbing particle dispersion therebetween by a known method.

[0148] When the above-mentioned infrared absorbing particle dispersion is used as an infrared absorbing intermediate film, which is an intermediate layer sandwiched between a plurality of transparent substrates, the solid medium may be the same as that described for the infrared absorbing particle dispersion. However, from the viewpoint of increasing the adhesive strength between the infrared absorbing intermediate film and the transparent substrate, the solid medium is preferably a polyvinyl acetal resin.

[0149] The infrared absorbing interlayer film can be produced by the above-mentioned method for producing an infrared absorbing particle dispersion, and can be in the form of, for example, a sheet, board, or film.

[0150] In addition, when the infrared absorbing intermediate film does not have sufficient flexibility or adhesion to the transparent substrate, it is preferable to add a liquid plasticizer for the medium resin (solid medium). For example, when the medium resin used in the infrared absorbing intermediate film is a polyvinyl acetal resin, the addition of a liquid plasticizer for the polyvinyl acetal resin is beneficial for improving adhesion to the transparent substrate.

[0151] As the plasticizer, a substance that is used as a plasticizer for the medium resin can be used. For example, examples of plasticizers that can be used in an infrared absorbing intermediate film in which the medium resin is made of a polyvinyl acetal resin include a plasticizer that is a compound of a monohydric alcohol and an organic acid ester, an ester-based plasticizer such as a polyhydric alcohol organic acid ester compound, and a phosphoric acid-based plasticizer such as an organic phosphoric acid-based plasticizer. It is preferable that any of the plasticizers is liquid at room temperature. Among them, a plasticizer that is an ester compound synthesized from a polyhydric alcohol and a fatty acid is preferable.

[0152] The infrared absorbing interlayer film may also contain at least one selected from the group consisting of a silane coupling agent, a metal salt of a carboxylic acid, a metal hydroxide, and a metal carbonate. The metal constituting the metal salt of a carboxylic acid, the metal hydroxide, and the metal carbonate is not particularly limited, but is preferably at least one selected from sodium, potassium, magnesium, calcium, manganese, cesium, lithium, rubidium, and zinc. In the infrared absorbing interlayer film, the content of at least one selected from the group consisting of a metal salt of a carboxylic acid, a metal hydroxide, and a metal carbonate is preferably 1% by mass or more and 100% by mass or less relative to the infrared absorbing particles.

[0153] Furthermore, the infrared absorbing interlayer film may contain, in addition to the infrared absorbing particles described above, at least one of oxide particles, composite oxide particles, and boride particles containing two or more elements selected from the group consisting of Sb, V, Nb, Ta, W, Zr, F, Zn, Al, Ti, Pb, Ga, Re, Ru, P, Ge, In, Sn, La, Ce, Pr, Nd, Gd, Tb, Dy, Ho, Y, Sm, Eu, Er, Tm, Tb, Lu, Sr, and Ca. The infrared absorbing interlayer film may contain such particles in an amount of 5% by mass or more and 95% by mass or less, assuming that the total of such particles and the infrared absorbing particles is 100% by mass.

[0154] In the infrared absorbing laminate, at least one of the intermediate layers disposed between the transparent substrates may contain an ultraviolet absorbing agent. The ultraviolet absorbing agent may be one or more selected from a compound having a malonic acid ester structure, a compound having an oxalic acid anilide structure, a compound having a benzotriazole structure, a compound having a benzophenone structure, a compound having a triazine structure, a compound having a benzoate structure, a compound having a hindered amine structure, and the like.

[0155] Of course, the intermediate layer of the infrared absorbing laminate may be composed of only the infrared absorbing intermediate film.

[0156] The infrared absorbing intermediate film described here is also an example of an infrared absorbing particle dispersion. The infrared absorbing laminate of the present embodiment is not limited to the above-mentioned form in which an infrared absorbing particle dispersion is disposed between transparent substrates, and may have any configuration as long as it has a laminate structure including an infrared absorbing particle dispersion and a transparent substrate. EXAMPLES

[0157] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. (Evaluation method) First, the evaluation methods used in the following Examples and Reference Examples will be described. (Cumulative 50% particle size, cumulative 90% particle size) The particle size distribution of the infrared absorbing particles in the examples and reference examples was measured using a particle size distribution measuring device (manufactured by Nikkiso Co., Ltd., model: UPA-150) based on the principle of dynamic light scattering method analyzed by frequency analysis. The measurement conditions were a particle refractive index of 1.81 and a non-spherical particle shape. The background was measured using methyl isobutyl ketone, and the solvent refractive index was 1.40. The volume-based cumulative 50% particle size and cumulative 90% particle size were then calculated from the obtained particle size distribution. (Crystal structure, lattice constant) Using the infrared absorbing particles obtained by removing the solvent from the infrared absorbing particle dispersion liquid prepared in the Examples and Reference Examples, the crystal structure and lattice constant of the composite oxide contained in the infrared absorbing particles were measured.

[0158] The X-ray diffraction pattern of the infrared absorbing particles was measured by powder X-ray diffraction method (θ-2θ method) using a powder X-ray diffractometer (X'Pert-PRO / MPD manufactured by PANalytical, Spectris Co., Ltd.) The crystal structure contained in the particles was identified from the obtained X-ray diffraction pattern, and the lattice constant was calculated by Rietveld analysis.

[0159] The external standard method was used for the Rietveld analysis. The Rietveld analysis of the X-ray diffraction pattern of the Si standard powder (NIST640c) measured at the same time was first performed, and the zero shift value and half width parameters obtained at that time were determined as the instrument parameters, and the Rietveld analysis of the infrared absorbing particles, which was the target, was refined. (Optical properties of dispersion) The optical properties of the infrared absorbing particle dispersions in the examples and reference examples were measured as follows.

[0160] First, the infrared absorbing particle dispersion was diluted with methyl isobutyl ketone as a solvent in a glass cell for measuring a spectrophotometer. At this time, the dilution ratio was set so that the visible light transmittance after dilution was 70%. Next, a transmitted light profile was measured at intervals of 5 nm in a wavelength range of 200 nm to 2600 nm using a spectrophotometer (Hitachi High-Tech Science, model: UH4150). Then, the visible light transmittance and solar transmittance were calculated in a wavelength range of 300 nm to 2100 nm based on JIS R 3106 (2019). At this time, in this measurement, the incident direction of the light of the spectrophotometer was set to a direction perpendicular to the glass cell for measuring. In addition, a blank in which only the solvent methyl isobutyl ketone was put into the glass cell for measuring was used as the baseline of the light transmittance. (Optical properties of infrared absorbing substrate) The optical properties of the infrared absorbing substrate in the examples and reference examples were measured using a spectrophotometer (Hitachi High-Tech Science Corporation, model: UH4150). The transmitted light profile was measured at 5 nm intervals in the wavelength range of 200 nm to 2600 nm, and the visible light transmittance and solar transmittance were calculated in the wavelength range of 300 nm to 2100 nm based on JIS R 3106 (2019). In addition, the wavelength at which the transmittance is the lowest (light absorption is strongest) in the near infrared region (780 nm to 2600 nm) in the measurement range of the transmitted light profile was determined from the transmitted light profile as the "light absorption peak wavelength". (Hayes) The haze value of the infrared absorbing base material was measured using a haze meter (HM-150N manufactured by Murakami Color Research Laboratory Co., Ltd.) and calculated based on JIS K 7136 (2000). [Example 1] (Infrared absorbing particles) The raw materials used were potassium carbonate (K2CO3, manufactured by Kanto Chemical Co., Ltd., purity 99.0% or more), barium carbonate (BaCO3, manufactured by Kanto Chemical Co., Ltd., purity 99.5% or more), and niobium oxide (Nb2O5, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.9% or more).

[0161] The infrared absorbing particles were synthesized in three steps as described below. (First Stage) In the first step, barium niobate (Ba4Nb2O9) was prepared.

[0162] Specifically, first, barium carbonate and niobium oxide were weighed out and mixed among the above raw materials. At this time, they were weighed out and mixed so that the ratio of the amounts of barium (Ba) and niobium (Nb) in the first mixed powder after mixing, Ba:Nb, was 2.0:1.0. In this way, the first mixed powder was prepared (first mixed powder preparation step).

[0163] Next, the first mixed powder was placed in an alumina boat and fired at a temperature of 1400° C. for 2 hours in an air atmosphere to obtain barium niobate having a composition formula of Ba4Nb2O9 as a first intermediate product (first firing step). (Second Stage) The obtained first intermediate product Ba4Nb2O9, niobium oxide, and niobium powder (Nb, Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.5%) were weighed and mixed. At this time, they were weighed and mixed so that the ratio of the amounts of barium (Ba) and niobium (Nb) in the second mixed powder after mixing, Ba:Nb, was 0.9:1.0. In this way, the second mixed powder was prepared (second mixed powder preparation process).

[0164] Next, the second mixed powder was placed in an alumina crucible and sintered at a temperature of 1500° C. for 2 hours under an argon gas flow to obtain a second intermediate product having the composition formula Ba 0.9 Barium niobate NbO3 was obtained (second firing step). (Third Stage) The second intermediate product obtained, Ba 0.9 NbO3 and potassium carbonate were weighed and mixed. At this time, they were weighed and mixed so that the ratio of the amounts of potassium (K), barium (Ba), and niobium (Nb) in the third mixed powder after mixing, K:Ba:Nb, was 0.1:0.9:1.0. In this way, the third mixed powder was prepared (third mixed powder preparation process).

[0165] Next, the third mixed powder was placed in an alumina crucible and fired at 1000°C for 2 hours under a 3% by volume hydrogen gas flow using argon gas as a carrier to prepare the infrared absorption particles according to Example 1 (the third firing step).

[0166] Through the above procedure, particles containing a complex oxide represented by the composition formula K 0.1 Ba 0.9 NbO z (2.4 < z < 3.2) (hereinafter also referred to as "particle A") were obtained. (Infrared absorption particle dispersion liquid) 6% by mass of particle A according to Example 1, 6% by mass of an acrylic polymer dispersant having a group containing an amine as a functional group (acrylic dispersant with an amine value of 48 mg KOH / g and a decomposition temperature of 250°C), and 88% by mass of methyl isobutyl ketone were mixed. Then, the obtained mixed liquid (slurry) was put into a glass bottle together with φ0.3 mm ZrO2 beads, loaded into a paint shaker, and subjected to a grinding and dispersion treatment for 10 hours to obtain the infrared absorption particle dispersion liquid according to Example 1. At this time, particle A becomes the infrared absorption particles.

[0167] The particle size distribution of the infrared absorption particle dispersion liquid according to Example 1 was measured, and the cumulative 50% particle diameter and cumulative 90% particle diameter were determined. The evaluation results are shown in Table 1.

[0168] Also, when the solvent (dispersion medium) was removed from the infrared absorption particle dispersion liquid and the powder X-ray diffraction pattern of particle A according to Example 1 was measured, diffraction peaks attributed to the crystal phase of the cubic perovskite structure were confirmed. Further, Rietveld analysis was performed based on the cubic perovskite structure to determine the lattice constant. The evaluation results are shown in Table 1.

[0169] The infrared absorption particle dispersion liquid according to Example 1 was diluted with methyl isobutyl ketone as the solvent, and its optical properties were measured. The visible light transmittance was 70% and the solar radiation transmittance was 35%. The transmitted light profile of the infrared absorption particle dispersion liquid is shown in Fig. 1. (Infrared absorption particle dispersion) The infrared absorbing particle dispersion according to Example 1 and an ultraviolet curable resin (Aronix UV-3701, manufactured by Toa Gosei Co., Ltd.) were weighed out so that the mass ratio was 1:1, and mixed and stirred to prepare a dispersion for forming an infrared absorbing substrate. Then, using a bar coater with bar No. 10, the dispersion for forming an infrared absorbing substrate was applied onto a PET (polyethylene terephthalate) film (HPE-50, manufactured by Toyobo Co., Ltd.) having a thickness of 50 μm, and then dried at 70° C. for 1 minute, and irradiated with a high-pressure mercury lamp. By the above operations, an infrared absorbing substrate according to Example 1 was obtained. The infrared absorbing substrate is an example of an infrared absorbing particle dispersion.

[0170] The optical properties of the obtained infrared absorbing substrate according to Example 1 were measured. The evaluation results are shown in Table 2. [Reference example 1] A tin compound solution was prepared by dissolving 54.9 g of SnCl4·5H2O (Wako Pure Chemical Industries, Wako special grade, purity 98% or more) in 340 g of water at 25°C. 12.7 mL of a methanol solution (Yoneyama Chemical Industries, reagent special grade, purity 99.8% or more) in which 4.2 g of an antimony compound SbCl3 (Wako Pure Chemical Industries, JIS special grade, purity 98% or more) was dissolved, and an aqueous NH4OH solution (Wako Pure Chemical Industries, reagent special grade, concentration 30%), which is an alkaline solution diluted to a concentration of 16%, was dropped in parallel to the tin compound solution. Then, a hydroxide containing tin and antimony, which is a precursor of antimony-doped tin oxide (hereinafter abbreviated as ATO) infrared absorbing particles, was generated and precipitated by the parallel dropping.

[0171] From the viewpoint of desired optical properties, the amount of antimony compound added to the tin compound solution was set to 9.5 parts by mass in terms of elemental antimony per 100 parts by mass of tin (IV) oxide. By adding this amount, ATO infrared absorbing particles containing about 68% by mass of Sn element and about 8% by mass of Sb element can be produced.

[0172] As described above, ammonia water was used as the alkaline solution used as the precipitant, and the alkaline concentration was 16%, which is 1.6 times the chemical equivalent required for the tin compound and the antimony compound to become hydroxides.

[0173] The parallel dropping time of the methanol solution and the alkaline solution was 25 minutes, and the parallel dropping was continued until the pH of the solution obtained by dropping reached 7.5. After the dropping was completed, the solution was stirred for 10 minutes to homogenize the system. The temperature of the solution at that time was the same as the temperature during the parallel dropping, 65°C.

[0174] Next, the precipitate was washed by repeatedly decanting until the conductivity of the supernatant of the washing solution in the decantation was 1 mS / cm or less, and then filtered.

[0175] Next, the washed precipitate was wetted with anhydrous ethyl alcohol solution (special grade reagent, purity 99.5% or more, manufactured by Wako Pure Chemical Industries, Ltd.). During the wet treatment, the mass ratio of [filtered precipitate:anhydrous ethyl alcohol solution] was set to 1:4 (corresponding to 80% alcohol), and the filtered precipitate and the anhydrous ethyl alcohol solution were stirred at room temperature for 1 hour to obtain a precursor. After completion of the wet treatment, the precursor was dried at 90°C for 10 hours to obtain a dried product.

[0176] The ATO infrared absorbing particle precursor that had been subjected to the wet treatment was heated to 700° C. in an air atmosphere and baked for 2 hours to produce the ATO infrared absorbing particles of Reference Example 1.

[0177] Except for using the ATO infrared absorbing particles according to Reference Example 1 instead of the particles A as the infrared absorbing particles, an infrared absorbing particle dispersion liquid and an infrared absorbing base material according to Reference Example 1 were prepared in the same manner as in Example 1, and evaluations were performed in the same manner as in Example 1. The evaluation results in Reference Example 1 are shown in Tables 1 and 2. [Reference example 2] (Infrared absorbing particles) The raw materials used in preparing the intermediate product were strontium carbonate (SrCO3, manufactured by Kanto Chemical Co., Ltd., purity 99.5% or higher) and the same niobium oxide as in Example 1. The ratio of the amounts of Sr and Nb in weighing the raw materials was Sr:Nb=2.0:1.0.

[0178] The mixed powder obtained by mixing the raw materials was put into an alumina boat and fired at 1400 °C for 2 hours in an air atmosphere to obtain strontium niobate with the composition formula Sr4Nb2O9 as an intermediate product.

[0179] The obtained intermediate product Sr4Nb2O9, the same niobium oxide as in Example 1, and niobium powder (Nb, manufactured by Fujifilm Wako Pure Chemical Corporation, purity 99.5%) were mixed. At this time, the mixture was carried out so that Sr:Nb, which is the ratio of the amounts of substances of Sr and Nb in the powder after mixing, was 1.0:1.0. The mixed powder was put into an alumina crucible and fired at 1600 °C for 3 hours under a 3% by volume hydrogen gas stream using argon gas as a carrier to prepare the infrared absorption particles according to Reference Example 2.

[0180] By the above procedure, particles containing strontium niobate with the composition formula SrNbO z (1.0 < z < 3.5) were obtained. Also, except for using the infrared absorption particles, an infrared absorption particle dispersion liquid and an infrared absorption base material were obtained in the same manner as in Example 1, and the same evaluation as in Example 1 was carried out. The evaluation results are shown in Table 1 and Table 2. Also, the transmission light profile of the infrared absorption particle dispersion liquid is shown in FIG. 1.

[0181]

Table 1

[0182]

Table 2

[0183] According to the results shown in Table 1 and Table 2, it was confirmed that the infrared absorption particle dispersion liquid and the infrared absorption particle dispersion obtained by using the infrared absorption particles obtained in Example 1 had a high visible light transmittance and could suppress the solar radiation transmittance. That is, it was confirmed that the transmittance in the visible light region was high and the transmittance in the infrared region could be suppressed.

[0184] It was also confirmed that the visible light transmittance and solar radiation transmittance were comparable to or superior to those of ATO of Reference Example 1, which has been conventionally used as an infrared absorbing particle. Furthermore, the light absorption peak wavelength of the infrared absorbing base material of Example 1 was in the range of 1400 nm or more and 2100 nm or less.

[0185] That is, it was clear that the infrared absorbing particles have a strong absorption at the light wavelength that generates a burning sensation on human skin even in the infrared region. Therefore, it was confirmed that the infrared absorbing particles obtained in Example 1 are novel infrared absorbing particles that can be used in practical applications.

[0186] In addition, the light absorption peak wavelength of the infrared absorbing transparent substrate of Reference Example 2 was 1300 nm. Therefore, it was confirmed that the infrared absorbing particles according to one embodiment of the present disclosure of Example 1 and the infrared absorbing substrate containing the infrared absorbing particles are novel substances having optical properties different from those of the conventional infrared absorbing particles of Reference Example 2 and the infrared absorbing substrate containing the infrared absorbing particles. [Explanation of symbols]

[0187] 20 Infrared absorbing particle dispersion 21 Infrared absorbing particles 22 Liquid medium 30 Infrared absorbing particle dispersion 31 Infrared absorbing particles 32 Solid medium 40 Infrared absorbing substrate 41 Base material 42 Dispersion membrane 41A One side 50 Infrared absorbing laminate 511, 512 Transparent base material 52 Infrared absorbing particle dispersion

Claims

1. An infrared absorbing particle containing a complex oxide, the complex oxide comprising: Contains the elements potassium, barium, and niobium, When the amount of substance of the potassium contained in the composite oxide is x1, the amount of substance of the barium is x2, and the amount of substance of the niobium is y, Infrared absorbing particles satisfying the relationships: 0.002≦(x1+x2) / y≦1.5, 0.05≦x1≦1, and 0.001≦x2≦1.

2. 2. The infrared absorbing particles according to claim 1, wherein the volume-based cumulative 50% particle size measured by a particle size distribution measuring device is 1 nm or more and 50 nm or less, and the cumulative 90% particle size is 5 nm or more and 100 nm or less.

3. A liquid medium; An infrared absorbing particle dispersion liquid comprising: the infrared absorbing particles according to claim 1 or 2 contained in the liquid medium.

4. 4. The infrared absorbing particle dispersion liquid according to claim 3, wherein the liquid medium contains at least one selected from the group consisting of water, an organic solvent, a liquid plasticizer, an oil or fat, and a compound that is polymerized by curing.

5. A solid medium; 3. An infrared absorbing particle dispersion comprising: the infrared absorbing particles according to claim 1 or 2 contained in the solid medium.

6. The infrared absorbing particle dispersion according to claim 5 , wherein the solid medium is a resin.

7. 7. The infrared absorbing particle dispersion according to claim 6, wherein the resin is one type of resin selected from the group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and ultraviolet curable resin, or a mixture of two or more types of resins selected from the group.

8. 6. The infrared absorbing particle dispersion of claim 5, having a sheet, board, or film shape.

9. The infrared absorbing particle dispersion according to claim 5 , An infrared absorbing laminate having a laminate structure including a transparent substrate.

Citation Information

Patent Citations

  • Sheet for heat insulation

    JP1997107815A

  • Light shielding film

    JP2003029314A

  • Infrared shielding material microparticle dispersion, infrared shield, process for producing infrared shielding material microparticle, and infrared shielding material microparticle