Manufacturing method of double-sided metal-clad laminated plate
By controlling the surface roughness and composition of fluororesin layers with specific weight ratios and thermocompression bonding, the method addresses adhesive strength and thermal expansion issues in double-sided metal-clad laminates, achieving reliable and high-speed communication compatibility.
Patent Information
- Application Number
- JP2023055063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The challenge lies in ensuring sufficient adhesive strength between fluororesin layers containing a high concentration of inorganic filler in a double-sided metal-clad laminate, while maintaining low thermal expansion and dielectric properties suitable for high-speed communication applications.
A method involving the controlled surface roughness and composition of fluororesin layers, with a weight ratio of fluororesin to inorganic filler within specific ranges, and thermocompression bonding to enhance adhesion, is employed.
The method ensures strong adhesive strength and reliability of the bonded surfaces, maintaining low thermal expansion and excellent dielectric properties, making it suitable for high-speed communication standards.
Smart Images

Figure 2024142753000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a double-sided metal-clad laminate useful as, for example, a circuit board material. [Background technology]
[0002] As communication devices have become faster in recent years, development of 5G and even 6G communication is progressing, and circuit board materials that are compatible with high-speed communication standards are being investigated for millimeter wave radar boards, antenna boards, etc. Among such materials, fluororesins have attracted attention because of their low dielectric tangent and the potential for reducing signal transmission loss.
[0003] However, since fluororesins have a large coefficient of thermal expansion (CTE), there is a concern that they may impair the dimensional stability of the substrate. In Patent Document 1, in order to achieve low thermal expansion, which is a required characteristic of an insulating material for circuit boards, while taking advantage of the characteristic of low dielectric tangent, an inorganic filler is blended into the dispersion composition as a coating material. Patent Document 2 discloses that when laminating an adhesive layer on an insulating resin layer containing a fluorine-based resin, the surface roughness of the insulating resin layer is set to 0.5 to 3.0 μm. Patent Document 3 discloses that when laminating a prepreg not containing a fluorine-based resin on an insulating resin layer containing a fluorine-based resin, the arithmetic mean roughness Ra of the insulating resin layer as observed by an atomic force microscope is set to 3.0 μm or more. However, neither Patent Document 2 nor Patent Document 3 discloses blending an inorganic filler into an insulating resin layer containing a fluorine-based resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6891890 [Patent Document 2] Patent No. 6954293 [Patent Document 3] International Publication No. WO2018 / 212285 Summary of the Invention [Problem to be solved by the invention]
[0005] In order to compound fluororesin with inorganic filler and achieve low thermal expansion, it is necessary to compound an amount of inorganic filler that exceeds the weight of the fluororesin. When preparing a double-sided metal-clad laminate, there is a concern that the peel strength between the metal foil and the fluororesin layer may decrease if a low-roughness metal foil and a fluororesin layer containing a large amount of inorganic filler are laminated together by a lamination method. Therefore, it is considered effective to first prepare a single-sided metal-clad laminate in which a fluororesin layer is formed on a metal foil, and then laminate the fluororesin layers of a pair of single-sided metal-clad laminates together. However, when laminating the fluororesin layers of a pair of single-sided metal-clad laminates together, it is necessary to sufficiently ensure the adhesive strength of the lamination joint surface.
[0006] Therefore, an object of the present invention is to provide a double-sided metal-clad laminate having a fluororesin layer containing a high concentration of inorganic filler as part or all of an insulating resin layer, and in which the adhesive strength of the bonding surfaces between the fluororesin layers is sufficiently ensured. [Means for solving the problem]
[0007] As a result of investigations, the inventors have found that when the fluororesin layers of a pair of single-sided metal-clad laminates are bonded together to produce a double-sided metal-clad laminate, the adhesive strength of the bonded joint surface can be sufficiently ensured by controlling the surface roughness of the exposed surfaces of the fluororesin layers, and have thus completed the present invention.
[0008] That is, the method for producing a double-sided metal-clad laminate of the present invention is a method for producing a double-sided metal-clad laminate in which metal layers are laminated on both sides of an insulating resin layer, the method comprising the following steps 1 and 2; Step 1: A step of preparing a single-sided metal-clad laminate comprising an insulating resin layer having a fluororesin layer exposed on a surface thereof, and a metal layer laminated on a surface of the insulating resin layer opposite to the fluororesin layer; Step 2: a step of placing two of the single-sided metal-clad laminates so that the fluororesin layers face each other and performing thermocompression bonding; Contains: The method for producing a double-sided metal-clad laminate of the present invention comprises the steps of: (1) forming a fluororesin layer on at least one of the two single-sided metal-clad laminates; and (2) forming a fluororesin layer on at least one of the two single-sided metal-clad laminates. (1): A resin component having a weight ratio of 50% by weight or more of a fluorine-based resin as component (A) and an inorganic filler as component (B), the weight ratio of component (A) being within the range of 20 to 45% by weight and the weight ratio of component (B) being within the range of 55 to 80% by weight relative to the total amount of components (A) and (B), and (2): The surface roughness (Sq) of the exposed surface is 0.5 μm or more and 5 μm or less. The present invention is characterized in that:
[0009] In the method for producing a double-sided metal-clad laminate of the present invention, the component (B) is a particle having an average particle diameter (D 50 ) may be in the range of 0.1 to 20 μm.
[0010] In the method for producing a double-sided metal-clad laminate of the present invention, component (B) may be spherical amorphous silica.
[0011] In the method for producing a double-sided metal-clad laminate of the present invention, the component (A) may be a tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA).
[0012] The method for producing a double-sided metal-clad laminate of the present invention comprises the steps of: a) applying a dispersion composition containing a fluorine-based resin powder and an inorganic filler of component (B) onto a metal foil to form a coating film; and b) a step of subjecting the obtained coating film to a heat treatment in a nitrogen atmosphere at a temperature within a range of +10 to +100°C higher than the inflection point temperature of the storage modulus of the molten fluororesin to melt the fluororesin powder and form a fluororesin layer on the metal foil; The method may include: Effect of the Invention
[0013] In the method of the present invention, the fluororesin layers of a pair of single-sided metal-clad laminates with controlled surface roughness (Sq; root mean square height) of the exposed surfaces are bonded together to produce a double-sided metal-clad laminate, so that the adhesive strength of the bonded surfaces is sufficiently guaranteed. Therefore, the double-sided metal-clad laminate obtained by the method of the present invention is less likely to peel off at the bonded surfaces and has high reliability. In addition, by using a single-sided metal-clad laminate as the material for the double-sided metal-clad laminate, the adhesion between the metal foil and the insulating resin layer can be ensured. Moreover, the double-sided metal-clad laminate achieves both excellent dielectric properties due to the fluororesin and low thermal expansion due to the addition of a high concentration of inorganic filler. Therefore, the double-sided metal-clad laminate obtained by the method of the present invention is useful as a circuit board material that can comply with high-speed communication standards. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic process diagram of a method for producing a double-sided metal-clad laminate according to the first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate.
[0016] [Manufacturing of double-sided metal-clad laminates] A method for producing a double-sided metal-clad laminate according to one embodiment of the present invention is a method for producing a double-sided metal-clad laminate in which metal layers are laminated on both sides of an insulating resin layer, and includes the following steps 1 and 2.
[0017] <Process 1> Step 1 is a step of preparing a single-sided metal-clad laminate. First, as shown in FIG. 1(a), a single-sided metal-clad laminate 30A in which a metal layer 10A and an insulating resin layer 20A are laminated, and a single-sided metal-clad laminate 30B in which a metal layer 10B and an insulating resin layer 20B are laminated are prepared. Each of the single-sided metal-clad laminates 30A and 30B has an exposed surface S on which a fluororesin layer is exposed. The single-sided metal-clad laminates 30A and 30B may have the same configuration or different configurations as long as they have a fluororesin layer exposed on the surface.
[0018] (insulating resin layer) The insulating resin layers 20A and 20B are each composed of a single layer or multiple layers and each have a fluorine-based resin layer. In Fig. 1, the insulating resin layers 20A and 20B each are each composed of a fluorine-based resin layer, but the insulating resin layers 20A and 20B may each have any resin layer other than a fluorine-based resin layer.
[0019] The fluororesin layer satisfies the following conditions (1) and (2). At least one of the fluororesin layers of the two single-sided metal-clad laminates 30A, 30B may satisfy conditions (1) and (2), but it is preferable that both of the fluororesin layers of the two single-sided metal-clad laminates 30A, 30B satisfy conditions (1) and (2).
[0020] Condition (1): The composition contains component (A) a resin component having a weight ratio of 50% or more of a fluorine-based resin, and component (B) an inorganic filler, and the weight ratio of component (A) is within the range of 20 to 45% by weight and the weight ratio of component (B) is within the range of 55 to 80% by weight, relative to the total amount of components (A) and (B). The fluororesin is a polymer containing fluorine atoms, and the type is not particularly limited, but examples thereof include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-tetrafluoroethylene-hexafluoropropylene copolymer (EFEP), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), and the like. These may be used in combination of two or more kinds, and may contain a monomer unit based on perfluoroolefin having a functional group in a part of the fluororesin. As the functional group, a carbonyl group-containing group, a hydroxy group, an epoxy group, an amide group, an amino group, and an isocyanate group are preferable. Among these fluororesins, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and tetrafluoroethylene-hexafluoropropylene copolymer (FEP) are more preferable as those exhibiting a low dielectric tangent.
[0021] The component (B) is an inorganic filler, and the type thereof is not particularly limited. However, from the viewpoint of reducing the coefficient of thermal expansion (CTE) of the fluororesin layer, for example, silicon dioxide (silica), aluminum oxide (alumina), magnesium oxide (magnesia), beryllium oxide, niobium oxide, titanium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, magnesium fluoride, potassium silicofluoride, talc, glass, barium titanate, and the like are preferable. These may be used in combination of two or more. Among these, silicon dioxide (silica), aluminum oxide, boron nitride, aluminum fluoride, glass, and the like are more preferable as materials having a low coefficient of thermal expansion (CTE). When the component (B) is silica, it may be either crystalline silica or amorphous silica, but from the viewpoint of being able to reduce the coefficient of thermal expansion (CTE) without impairing the dielectric properties in the film state, and being able to reduce the difference between the coefficient of thermal expansion (CTE) in the thickness direction and the plane direction, amorphous silica is preferable, and spherical amorphous silica is particularly preferable. The shape of component (B) is not particularly limited, but is preferably, for example, spherical, crushed spherical, etc., since it can reduce the difference in the coefficient of thermal expansion (CTE) between the thickness direction and the plane direction. Component (B) may also be hollow. In addition, from the viewpoint of reducing the dielectric constant and adhesion to the fluorine-based resin, the inorganic filler of component (B) is preferably surface-treated with a coupling agent, etc. Examples of coupling agents used for the surface treatment include 3-aminopropylethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropylethoxysilane, 3-isocyanatopropylethoxysilane, and hexamethyldisilazane.
[0022] Component (B) has an average particle diameter (D 50 The average particle diameter (D) of the inorganic filler of component (B) is preferably in the range of 0.1 to 20 μm, more preferably in the range of 3 to 15 μm, and most preferably in the range of 5 to 15 μm. 50 By having the average particle diameter (D) in the range of 0.1 to 20 μm, even when the inorganic filler is homogeneously and highly concentrated in the fluororesin layer, it becomes easy to control the surface roughness (Sq) and coefficient of thermal expansion (CTE) of the exposed surface S of the fluororesin layer. 50 If D ) is out of the above range, it becomes difficult to control the surface roughness (Sq) of the exposed surface S of the fluororesin layer within the desired range. In addition, the surface roughness (Sq) of the exposed surface S can be controlled within the desired range by surface treatment of the exposed surface S, but even when the surface treatment is performed, D 50 If the thickness is less than 0.1 μm, the surface cannot be roughened to the desired extent. 50 If the surface roughness exceeds 20 μm, the roughness cannot be reduced to the desired range.
[0023] The weight percentage of the fluororesin in the resin component of component (A) is 50% by weight or more, and preferably in the range of 60 to 100% by weight. If the weight percentage of the fluororesin is less than 50% by weight, it becomes difficult to sufficiently lower the dielectric tangent of the insulating resin layer 20 (20A, 20B). By making the weight percentage of the fluororesin 50% by weight or more, the dielectric tangent of the insulating resin layer 20 (20A, 20B) can be sufficiently lowered, and the double-sided metal-clad laminate produced can have excellent transmission characteristics for high-frequency signals. The weight percentage of component (A) is within the range of 20 to 45% by weight, preferably within the range of 25 to 40% by weight, based on the total amount of components (A) and (B). The weight percentage of component (B) is within the range of 55 to 80% by weight, preferably within the range of 60 to 75% by weight, based on the total amount of components (A) and (B). If the weight percentage of component (A) is less than 20% by weight, it becomes difficult to achieve both low dielectric tangent and film formation, and if the weight percentage of component (B) is more than 80% by weight, it becomes difficult to form a film due to embrittlement, making it difficult to apply to high-frequency signal transmission. On the other hand, if the weight percentage of component (A) is more than 45% by weight or the weight percentage of component (B) is less than 55% by weight, it becomes difficult to sufficiently lower the coefficient of thermal expansion (CTE) when formed into a film, making it difficult to ensure dimensional stability when applied to a circuit board.
[0024] The amount of component (A) relative to the total weight of the fluororesin layer is preferably 20% by weight or more, and more preferably within the range of 25 to 40% by weight. If the amount of component (A) in the fluororesin layer is less than 20% by weight, it becomes difficult to reduce the dielectric tangent of the insulating resin layer 20 (20A, 20B) and to ensure adhesion between the insulating resin layers 20 (20A, 20B). If the amount of component (A) in the fluororesin layer is more than 40% by weight, it becomes difficult to control the coefficient of thermal expansion (CTE). The amount of component (B) relative to the total weight of the fluororesin layer is preferably 60% by weight or more, and more preferably within the range of 60 to 75% by weight. If the amount of component (B) in the fluororesin layer is less than 60% by weight, it becomes difficult to reduce the thermal expansion of the insulating resin layer 20 (20A, 20B), and if it exceeds 75% by weight, it becomes difficult to form a film due to embrittlement.
[0025] Examples of the resin component of component (A) other than fluorine-based resins include polyimide, polyphenylene ether, liquid crystal polymer, cycloolefin polymer, cycloolefin copolymer, styrene-butadiene copolymer, and styrene-divinylbenzene copolymer.
[0026] The fluororesin layer has a dielectric loss tangent (Df) at 60 GHz measured by a split cylinder resonator after 24 hours of conditioning under conditions of a temperature of 22 to 24°C and a humidity of 45 to 55%, which is preferably 0.0025 or less, more preferably 0.0020 or less, and even more preferably 0.0015 or less. Also, the relative dielectric constant (Dk) measured under the same conditions is preferably 4.0 or less, more preferably 3.5 or less. If the dielectric loss tangent (Df) and the relative dielectric constant (Dk) exceed the above values, this leads to an increase in dielectric loss when applied to a circuit board, and is likely to cause inconveniences such as loss of electrical signals on the transmission path of high-frequency signals in the GHz band (e.g., 1 to 80 GHz).
[0027] In order to ensure dimensional stability, the coefficient of thermal expansion (CTE) of the fluororesin layer is preferably within a range of 10 to 50 ppm / K, and more preferably within a range of 15 to 30 ppm / K.
[0028] The thickness of the fluororesin layer is not particularly limited, but when used as an insulating resin layer for a circuit board, taking into consideration application to high-frequency signal transmission, the thickness is preferably within the range of 30 to 150 μm, more preferably within the range of 75 to 150 μm.
[0029] Condition (2): The surface roughness (Sq) of the exposed surface S of the fluororesin layer is 0.5 μm or more and 5 μm or less. By having the surface roughness (Sq) of the exposed surface S of the fluororesin layer be 0.5 μm or more and 5 μm or less, the adhesiveness of the exposed surface S to be bonded in the next step 2 is improved. The exposed surface S of the fluororesin layer has fine irregularities formed by controlling the particle size of the inorganic filler of the component (B) contained in the fluororesin layer or by surface treatment. In the method of the present invention, the surface roughness (Sq), which is an index of the size of such irregularities, is controlled within a certain range. This can increase the surface area of the exposed surface S, and since a large number of inorganic fillers are pushed inward from the exposed surface S (i.e., toward each metal layer 10A or 10B) by the pressure during thermocompression bonding, it is assumed that the fusion and integration of the resins contained in both fluororesin layers at the bonding boundary is facilitated by the inorganic filler present at the bonding boundary when cooled and solidified after thermocompression bonding, and a strong adhesive force is easily expressed.
[0030] Preferred methods for controlling the surface roughness (Sq) of the exposed surface S of the fluororesin layer within the above range include, for example, a method of controlling the surface unevenness by forming voids between adjacent inorganic fillers by setting the particle size of the inorganic filler to a certain size or more, or by controlling the particle size distribution of the inorganic filler, surface treatments such as polishing by roughening roll processing, embossing at a temperature above the melting point of the fluororesin layer, corona treatment, plasma treatment, etc., and methods of promoting flow in the initial stage of drying of the coating film by controlling the viscosity and air pressure of the dispersion composition (slurry) during coating. It is also possible to control the surface roughness (Sq) of the exposed surface S by combining two or more of these methods.
[0031] The insulating resin layers 20A and 20B may have an arbitrary resin layer between the fluororesin layer having the exposed surface S and the metal layers 10A and 10B. Examples of such a resin layer include polyimide and polytetrafluoroethylene polymers.
[0032] (metal layer) The material of the metal layers 10A and 10B is not particularly limited, but examples thereof include copper, stainless steel, iron, nickel, beryllium, aluminum, zinc, indium, silver, gold, tin, zirconium, tantalum, titanium, lead, magnesium, manganese, and alloys thereof. Among these, copper or a copper alloy is particularly preferred.
[0033] The thickness of the metal layers 10A and 10B is not particularly limited, but when a metal foil such as a copper foil is used, the thickness is preferably 35 μm or less, and more preferably in the range of 5 to 25 μm. From the viewpoints of production stability and handling, the lower limit of the thickness of the metal foil is preferably 5 μm. When a copper foil is used as the metal foil, it may be a rolled copper foil or an electrolytic copper foil, for example, a peelable copper foil having a release layer formed between a copper foil having a thickness of 5 μm or less and a carrier foil. In addition, a commercially available copper foil may be used as the copper foil.
[0034] <Process 2> Step 2 is a step of bonding together the two single-sided metal-clad laminates 30A, 30B obtained in step 1. As shown in Fig. 1(b), the pair of single-sided metal-clad laminates 30A, 30B are arranged so that the insulating resin layers 20A, 20B face each other, and are subjected to thermocompression bonding to bond the insulating resin layers 20A, 20B together.
[0035] The temperature of the thermocompression bonding is preferably set within a range of +10°C to +100°C higher than the inflection point temperature of the storage modulus of the fluororesin when melted, and more preferably within a range of +20°C to +80°C. If the thermocompression bonding temperature is lower than the inflection point temperature of the storage modulus of the fluororesin +10°C, the fluororesin will not melt sufficiently, and the adhesiveness of the bonding surface will not be obtained. On the other hand, if the thermocompression bonding temperature is higher than the inflection point temperature of the storage modulus of the fluororesin +100°C, the fluidity will be too high, causing the resin to flow out, or the fluororesin may be thermally deteriorated. Note that by controlling the surface roughness (Sq), even if the thermocompression bonding temperature is near the inflection point temperature of the storage modulus of the fluororesin when melted (for example, about the inflection point temperature +10°C), the adhesiveness of the bonding surface is easily obtained due to the anchor effect due to the irregularities of the inorganic filler and the effect of increasing the initial contact points due to the increase in surface area.
[0036] The pressure of the thermocompression bonding is preferably within a range of, for example, 2 MPa to 30 MPa. If the pressure is lower than 2 MPa, adhesion between the bonding surfaces of the fluororesins cannot be obtained. On the other hand, if the pressure is higher than 30 MPa, the fluororesin may flow and flow out to the ends. By controlling the surface roughness (Sq), adhesion between the bonding surfaces can be easily obtained even with a low pressure of thermocompression bonding of about 2 MPa due to the anchor effect of the irregularities of the inorganic filler and the effect of increasing the number of initial contact points due to the increase in surface area.
[0037] In the above manner, as shown in FIG. 1(c), a double-sided metal-clad laminate 100 having a layer structure in which a metal layer 10A / insulating resin layer 20 (however, a layer in which two fluororesin layers are bonded together) / metal layer 10B are laminated in this order can be manufactured. The double-sided metal-clad laminate 100 may have any resin layer other than the fluororesin layer. The double-sided metal-clad laminate 100 not only has excellent adhesion between the metal layers 10A and 10B and the insulating resin layer 20, but also has a strong bond between the bonding surfaces of the fluororesin layers bonded together by thermocompression bonding, and is highly reliable because peeling is unlikely to occur between the metal foil and the insulating resin layer 20 and at the bonding surfaces. Moreover, the insulating resin layer 20 of the double-sided metal-clad laminate 100 has both excellent dielectric properties due to the fluororesin and low thermal expansion due to the addition of a high concentration of inorganic filler. Therefore, the double-sided metal-clad laminate 100 obtained by the method of the present invention is useful as a circuit board material that can comply with high-speed communication standards.
[0038] <Manufacturing of single-sided metal-clad laminates> Next, a method for manufacturing the single-sided metal-clad laminates 30A, 30B used in the method of the present invention will be described. The method for manufacturing the single-sided metal-clad laminates 30A, 30B is not particularly limited, but may be a method including a coating film forming step and a melting heat treatment step described below. Here, an example is taken of the production of the single-sided metal-clad laminates 30A, 30B in which a fluororesin layer is laminated as the insulating resin layer 20A or 20B on the metal layer 10A or 10B.
[0039] (Step a; coating film formation step) In this step, a dispersion composition in which a fluorine-based resin powder and component (B) are dispersed in an organic solvent is applied to the metal foil that will become the metal layers 10A and 10B to form a coating film. That is, the dispersion composition is applied to the metal foil so as to have a desired thickness after the melt heat treatment step, and then dried to form a coating film. There are no particular limitations on the method for applying the dispersion composition to the metal foil, and it is possible to apply it using a coater such as a comma, die, knife, or lip coater.
[0040] In addition, the surface roughness (Sq) of the exposed surface S of the fluororesin layer can be controlled by adjusting the air pressure when applying the dispersion composition to 70 Pa to 140 Pa. Specifically, increasing the air pressure in the initial stage of drying the coating film can promote the flow of the coating film surface and promote surface roughening, while decreasing the air pressure can suppress surface roughening.
[0041] The fluororesin powder used in the coating film formation process has an average particle diameter (D 50 ) is preferably in the range of 0.05 to 100 μm, more preferably in the range of 0.5 to 50 μm, and even more preferably in the range of 0.5 to 10 μm. 50 ) can be calculated, for example, by measuring the particle size distribution of powder particles using laser diffraction / scattering methods, calculating a cumulative curve with the total volume of the powder particles as 100%, and then determining the particle diameter at the point on the cumulative curve where the cumulative volume is 50%.
[0042] The weight ratios of the fluororesin powder, the inorganic filler of component (B), and the like in the dispersion composition are adjusted so as to satisfy condition (1).
[0043] The type of organic solvent used in the dispersion composition is not particularly limited, but an organic solvent that is liquid at 25 ° C. is preferred, such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diglyme, triglyme, cresol, methanol, ethanol, isopropanol, methyl ethyl ketone, cyclohexanone, γ-butyrolactone, etc. Among these, for example, high boiling point solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, and N-methyl-2-pyrrolidone (NMP) are more preferred. There are no limitations on the amount of organic solvent as long as the viscosity of the dispersion composition can be adjusted to the desired value, but in order to obtain good dispersibility and good coatability, it is advisable to adjust and blend the amount so that it is preferably within the range of 25 to 50% by weight, more preferably within the range of 30 to 40% by weight, based on the total weight of the composition. The dispersion composition may contain optional components such as a dispersant, a binder resin, an organic filler, a curing agent, a plasticizer, an elastomer, a coupling agent, a pigment, and a flame retardant.
[0044] The viscosity of the dispersion composition is not particularly limited, but for example, when the purpose is to coat a thick film of 30 μm or more, it is preferably in the range of 500 to 50,000 cP, more preferably in the range of 500 to 30,000 cP. In addition, from the viewpoint of controlling the surface roughness (Sq) in the coating and drying process, it is preferable that the viscosity is in the range of 500 to 10,000 cP. If the viscosity is less than 500 cP, the fluidity becomes too high when the dispersion composition is cast on a metal foil, making it difficult to form a thick coating film. In particular, it becomes impossible to form a relatively thick coating film in the range of 30 to 150 μm for high frequency transmission applications. In addition, if the viscosity is less than 500 cP, sedimentation or aggregation of solids may occur. On the other hand, if the viscosity of the dispersion composition exceeds 50,000 cP, the viscosity is too high and it becomes difficult to form a coating film by casting. The viscosity of the dispersion composition can be measured using an E-type viscometer at a temperature of 25° C.
[0045] (Process b: Melt heat treatment process) In this step, the coating film obtained in the coating film forming step is heat-treated to form a fluororesin layer. That is, the coating film is heat-treated together with the metal foil to remove the solvent remaining in the film, and the fluororesin powder (component (A)) is melted to form a film, forming a fluororesin layer on the metal foil. The heat treatment temperature for melting the fluororesin powder may be equal to or higher than the inflection point temperature of the storage modulus of the fluororesin when melted, and is preferably set to a temperature range of +10°C to +100°C higher than the inflection point temperature of the storage modulus. In addition, the melting heat treatment step is preferably performed in an inert gas atmosphere, more preferably in a nitrogen atmosphere, to prevent oxidation of the metal foil.
[0046] When forming multiple fluororesin layers on a metal foil, the melt heat treatment may be performed each time the dispersion composition is applied and dried, or the process of applying and drying the dispersion composition may be repeated multiple times and then the melt heat treatment may be performed all at once.
[0047] After the melting heat treatment, the resulting laminate is cooled and solidified to produce a single-sided metal-clad laminate 30A, 30B having a fluororesin layer as the insulating resin layer 20A or 20B and a metal layer 10A or 10B. A surface treatment such as polishing, embossing at a temperature equal to or higher than the melting point of the fluororesin layer, corona treatment, plasma treatment, or the like may be carried out on the exposed surface S of the fluororesin layer of the resulting single-sided metal-clad laminate 30A, 30B. The surface roughness of the exposed surface S of the fluororesin layer can be controlled by the surface treatment.
[0048] The single-sided metal-clad laminates 30A, 30B obtained as described above are obtained by applying the dispersion composition directly onto a metal foil by a casting method, and then heat treating the same to form fluororesin layers as insulating resin layers 20A, 20B. Therefore, the single-sided metal-clad laminates 30A, 30B have excellent adhesion between the metal layers 10A, 10B and the fluororesin layers, and can be preferably used as materials for manufacturing a double-sided metal-clad laminate 100.
[0049] [Circuit board manufacturing] As described above in detail, the double-sided metal-clad laminate 100 obtained by the method of the present invention is preferably used mainly as a circuit board material for flexible circuit boards (FPCs), rigid-flex circuit boards, etc. That is, by subjecting the metal layer 10A and / or the metal layer 10B of the double-sided metal-clad laminate 100 to wiring and circuit processing such as etching, a circuit board such as a single-sided circuit board or a double-sided circuit board can be manufactured. EXAMPLES
[0050] The features of the present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to the examples. In the following examples, various measurements and evaluations are as follows, unless otherwise specified.
[0051] [Particle size measurement of amorphous silica filler and fluororesin powder] Using a laser diffraction particle size distribution analyzer (Malvern, product name: Mastersizer 3000), particle size was measured by laser diffraction / scattering method under conditions of water as a dispersion medium and a particle refractive index of 1.54.
[0052] [Measurement of copper foil surface roughness] The surface roughness of the copper foil was measured in tapping mode using an AFM (Bruker AXS, product name: Dimension Icon type SPM) and a probe (Bruker AXS, product name: TESPA (NCHV), tip curvature radius 10 nm, spring constant 42 N / m) in an area of 80 μm x 80 μm on the copper foil surface, and the ten-point average roughness (Rzjis) was calculated. The ten-point average roughness (Rzjis) is based on JIS B 0601-2001.
[0053] [Viscosity measurement] The viscosity at 25°C was measured at a rotation speed of 100 rpm using an E-type viscometer (Brookfield, product name: DV-II+Pro, rotor type: spindle rotor).
[0054] [Evaluation of surface roughness (Sq; root mean square height) of exposed surface S of fluororesin layer] The shape of any part of the exposed surface S of the fluororesin layer of the prepared single-sided copper-clad laminate was measured using a shape analysis laser microscope (product name: VK-X160, manufactured by Keyence Corporation) under the conditions of objective lens: 100x, laser wavelength: 658nm, measurement size: 1024μm×768μm, and after obtaining a fully focused image, the surface roughness (Sq) was measured under the conditions of ISO25178 selected as the analysis condition, S-filter: 0.5μm, L-filter: 0.1mm, and automatic surface inclination correction. At this time, measurements were taken at three arbitrary points, and the average value of the three points was taken as the surface roughness (Sq).
[0055] [Measurement of inflection point temperature of storage modulus of fluororesin when melted] After laminating copper foil (electrolytic copper foil, thickness: 12 μm, ten-point average roughness (Rzjis) of the resin layer side; 0.6 μm) on the exposed surface S of the fluororesin layer of the single-sided copper-clad laminate, it was placed in a batch press machine and heated to 360 ° C under vacuum. After reaching 360 ° C, it was pressed at a pressure of 8 MPa for 5 minutes to obtain a double-sided copper-clad laminate with a dielectric thickness of 50 μm. The copper foil of the obtained double-sided copper-clad laminate was etched and removed using an aqueous ferric chloride solution to obtain a fluororesin film, which was then cut to a size of 5 mm × 70 mm. Measurements were performed using a dynamic viscoelasticity measuring device (DMA: manufactured by TA Instruments, product name: RSA G2) at a heating rate of 4 ° C / min from 30 ° C to 400 ° C and a frequency of 10 Hz. The inflection point temperature of the storage elastic modulus at the time of melting was obtained from the contact point when a tangent was drawn before and after the inflection of the storage elastic modulus obtained by the measurement.
[0056] [Adhesion evaluation of bonded surfaces] A 10cm square single-sided copper-clad laminate was pressed onto the remaining area without applying pressure to a 1cm wide area from one edge of the laminate, and then peeled off from the unpressurized area after pressing. Those where the peeling surface was a cohesive failure within the copper foil surface or fluororesin layer were rated as ○ (good), those where there was a mixture of cohesive failure within the copper foil surface or fluororesin layer and interfacial peeling at the bonding surface were rated as △ (passable), and those where there was interfacial peeling or no adhesion at the bonding surface were rated × (unacceptable).
[0057] [Measurement of coefficient of thermal expansion (CTE)] The fluororesin film obtained from the double-sided copper-clad laminate cut to a size of 3 mm x 20 mm was set in a thermomechanical analyzer (Hitachi High-Technologies Corporation (formerly Seiko Instruments Inc.), product name: TMA / SS7100). At this time, the distance between the device jigs (effective measurement length) was 15 mm. Next, the temperature was raised from 30°C to 260°C at a constant heating rate while applying a load of 5.0 g, and then the temperature was held for 10 minutes, and then cooled at a rate of 5°C / min, and the average thermal expansion coefficient (thermal expansion coefficient) from 200°C to 100°C was obtained.
[0058] [Measurement of dielectric properties] The dielectric constant (Dk) and dielectric loss tangent (Df) of a fluororesin film obtained from a double-sided copper-clad laminate were measured at 60 GHz using a split cylinder resonator (SCR resonator). The film used for the measurement was left to stand for 24 hours under conditions of temperature: 22 to 24° C. and humidity: 45 to 55%, and then the measurement was performed.
[0059] The compounds used in the synthesis examples and dispersion composition preparation examples are shown below. <Silica filler> Silica filler (1) to silica filler (5) shown in Table 1 below were used. The amount of surface treatment is expressed as a weight ratio relative to the weight of the silica filler.
[0060] [Table 1]
[0061] <Fluoroplastic resin powder (1)> Fluon+ (Fluon is a registered trademark) EA-2000PW 10: Fluorine-based resin powder manufactured by AGC, average particle size: 2 to 3 μm, melting point: 300° C. <Dispersant (1)> Futergent 710FL: Neos nonionic fluorine-containing dispersant (dispersant component: 50% by weight, ethyl acetate: 50% by weight) <dmac> N,N-Dimethylacetamide
[0062] (Dispersion Composition Preparation Example 1) 70.4 g of fluororesin powder (1), 169.6 g of silica filler (1), 12 g of dispersant (1) (6 g of dispersant component), and 14.7 g of DMAc were added to the container of TKHIVIS MIX (model 2P-03) manufactured by Primix Corporation (formerly Tokushu Kika Kogyo Co., Ltd.), and stirred at room temperature for 5 minutes at 20 rpm. The device was then stopped, and the kneaded material was scraped off from the stirring blades and the side walls of the container. The above stirring and scraping of the kneaded material from the stirring blades and the side walls of the container after stopping the device were performed three times.
[0063] Next, in order to finely adjust the ratio of the fluororesin powder (1) and the silica filler (1) to the total amount, a small amount of DMAc was added to the kneaded product, and the mixture was stirred at 30 rpm for 5 minutes, and the state of the kneaded product was confirmed. This operation was repeated until the kneaded product became a lump with no powdery parts. In this study, the mixture became a lump when the total mass ratio of the fluororesin powder (1) and the silica filler (1) was 85 mass% (i.e., [[fluororesin powder (1)] + [silica filler (1)]] / [[fluororesin powder (1)] + [silica filler (1)] + [DMAc]] = 85 mass%) relative to the amount of DMAc added to them, and no powdery parts were observed inside the lump of the kneaded product. From the lump-like state, kneading at 30 rpm was started, stopped at 15-minute intervals, and the kneaded product was scraped off from the stirring blade and the side wall of the container. This operation was performed four times in total for a total of 60 minutes, and a dispersion composition (resin composition) 1-1 was obtained. Dispersion Composition 1-1 was determined to be a "solid" since it had no fluidity and the viscosity could not be measured.
[0064] Thereafter, dispersion composition 1-1 was gradually diluted and stirred with DMAc so that the total ratio of fluororesin powder (1) and silica filler (1) was 67.5% by weight relative to the amount of DMAc added, thereby obtaining dispersion composition (resin composition) 1-2 having a viscosity of 1020 cP (1020 mPa S) when measured at 100 rpm (25°C).
[0065] (Dispersion Composition Preparation Examples 2 to 5) Dispersion compositions 2-1 to 5-1, and dispersion compositions 2-2 to 5-2 were prepared using the same method as in Dispersion Composition Preparation Example 1, except that the type of silica filler was changed to silica filler (2) to silica filler (5). That is, dispersion composition 2-1 was obtained in the same manner as dispersion composition 1-1 except that silica filler (1) was changed to silica filler (2), and dispersion composition 2-2 was obtained by diluting and stirring this in the same manner as dispersion composition 1-2. Dispersion composition 3-1 was obtained in the same manner as dispersion composition 1-1 except that silica filler (1) was changed to silica filler (3), and dispersion composition 3-2 was obtained by diluting and stirring this in the same manner as dispersion composition 1-2. Similarly, dispersion composition 4-1 to dispersion composition 5-1, dispersion composition 4-2 to dispersion composition 5-2 were obtained by changing silica filler (1) to silica filler (4) to silica filler (5), respectively. In addition, Dispersion Compositions 2-1 to 5-1 all had no fluidity and the viscosity could not be measured, so they were judged to be "solids." In addition, the viscosities (25°C) of Dispersion Compositions 2-2 to 5-2 measured at 100 rpm are shown in Table 2 below.
[0066] [Table 2]
[0067] <Example 1> Dispersion composition 1-2 was applied onto copper foil (electrolytic copper foil, thickness: 12 μm, ten-point average roughness (Rzjis) of the resin layer side: 0.6 μm), and then the copper foil coated with dispersion composition 1-2 was attached onto a polyimide film passed through a drying oven, and a drying process was performed at 90 ° C. for 1 minute and at 120 ° C. for 3 minutes in a drying oven with an air pressure of 80 Pa under atmospheric conditions, and then the copper foil having a coating film of dispersion composition 1-2 was peeled off from the polyimide film. Next, a hot air oven in a nitrogen atmosphere (oxygen concentration 0.1% by volume or less) was used to increase the temperature from 40 ° C. to 240 ° C. at 10 ° C. / min, and from 240 ° C. to 360 ° C. at 5 ° C. / min, and the temperature was held at 360 ° C. for 5 minutes, and then cooled to 40 ° C. by performing a nitrogen heat treatment to obtain a single-sided copper-clad laminate (fluororesin metal-clad laminate) 1 having a fluororesin layer of dispersion composition 1-2 on one side of the copper foil. Two single-sided copper-clad laminates 1 obtained as described above were prepared, and the resin surfaces of the fluororesin layers of each were placed together in a batch press machine, heated to 320°C under vacuum, and pressed at a pressure of 2 MPa for 5 minutes to obtain a double-sided copper-clad laminate 1 having a dielectric thickness of 100 μm formed by thermocompression bonding two fluororesin layers. The adhesiveness of the bonded surfaces of the obtained double-sided copper-clad laminate 1 was evaluated, and the result was cohesive failure in the resin layer near the copper foil, and the adhesion of the bonded surfaces was ◯ (good). In addition, the surface roughness (Sq) of the exposed surface S of the fluororesin layer of the single-sided copper-clad laminate 1 used for thermocompression bonding was 2.50 μm.
[0068] Subsequently, the copper foil of the double-sided copper-clad laminate 1 was etched away using an aqueous solution of ferric chloride to prepare a fluororesin film 1-1. The fluororesin film 1-1 had a CTE of 25.6 ppm / K, a relative dielectric constant (Dk) of 2.9, and a dielectric loss tangent (Df) of 0.0010.
[0069] <Examples 2 to 5 and Comparative Example 1> Except for changing the type of dispersant composition and the thermocompression bonding conditions, single-sided copper-clad laminates 2 to 5, double-sided copper-clad laminates 1-2, double-sided copper-clad laminates 2 to 4, and fluorine-based resin films 1-2 and 2 to 4 were produced using the same method as in Example 1. The production conditions and evaluation properties are summarized in Tables 3 and 4.
[0070] [Table 3]
[0071] [Table 4]
[0072] <Comparative Example 2> Copper foil (electrolytic copper foil, thickness: 12 μm, ten-point average roughness (Rzjis) on the resin layer side: 0.6 μm) was laminated on the exposed surface S of the fluororesin layer of the single-sided copper-clad laminate 1, and then the laminate was placed in a batch press and heated to 360°C under vacuum. After reaching 360°C, the laminate was pressed at a pressure of 8 MPa for 5 minutes to obtain a double-sided copper-clad laminate 1' having a dielectric thickness of 50 μm.
[0073] Subsequently, the copper foil on the thermocompression bonded surface of the double-sided copper-clad laminate 1' was etched away using an aqueous ferric chloride solution to prepare a single-sided copper-clad laminate 1'.
[0074] Two single-sided copper-clad laminates 1' obtained as described above were prepared, and the resin surfaces of the fluororesin layers of each were placed together in a batch press machine, heated to 320°C under vacuum, and pressed at a pressure of 2 MPa for 5 minutes after reaching 320°C, but the bonded surfaces did not bond. The surface roughness (Sq) of the exposed surface S of the fluororesin layer of the single-sided copper-clad laminate 1' used for thermocompression bonding was 0.15 μm.
[0075] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment, and various modifications are possible. [Explanation of symbols]
[0076] 10A, 10B...metal layer; 20, 20A, 20B...insulating resin layer; 30A, 30B...single-sided metal-clad laminate; 100...double-sided metal-clad laminate; S...exposed surface (of fluororesin layer)< / dmac>
Claims
1. A method for producing a double-sided metal-clad laminate in which metal layers are laminated on both sides of an insulating resin layer, comprising the following steps 1 and 2; Process 1: A step of preparing a single-sided metal-clad laminate comprising an insulating resin layer having a fluororesin layer exposed on a surface thereof, and a metal layer laminated on a surface of the insulating resin layer opposite to the fluororesin layer; Step 2: a step of placing two of the single-sided metal-clad laminates so that the fluororesin layers face each other and performing thermocompression bonding; Including, At least one of the fluororesin layers of the two single-sided metal-clad laminates meets the following conditions (1) and (2): (1): A resin component having a weight ratio of 50% by weight or more of a fluorine-based resin as component (A) and an inorganic filler as component (B), the weight ratio of component (A) being within the range of 20 to 45% by weight and the weight ratio of component (B) being within the range of 55 to 80% by weight, relative to the total amount of components (A) and (B); and (2): The surface roughness (Sq) of the exposed surface is 0.5 μm or more and 5 μm or less; A method for producing a double-sided metal-clad laminate, comprising the steps of:
2. Component (B) has an average particle diameter (D 50 2. The method for producing a double-sided metal-clad laminate according to claim 1, wherein the thickness of the laminate is in the range of 0.1 to 20 μm.
3. 2. The method for producing a double-sided metal-clad laminate according to claim 1, wherein the component (B) is spherical amorphous silica.
4. 2. The method for producing a double-sided metal-clad laminate according to claim 1, wherein the component (A) is a tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA).
5. The single-sided metal-clad laminate is subjected to the following steps a and b; a) applying a dispersion composition containing a fluorine-based resin powder and an inorganic filler of component (B) onto a metal foil to form a coating film; and b) a step of subjecting the obtained coating film to a heat treatment in a nitrogen atmosphere at a temperature within a range of +10 to +100° C. higher than the inflection point temperature of the storage modulus of the molten fluororesin to melt the fluororesin powder and form a fluororesin layer on the metal foil; The method for producing a double-sided metal-clad laminate according to claim 1, which is produced by a method comprising the steps of:
Citation Information
Patent Citations
Liquid composition and method for producing film and laminate using the liquid composition
JP6891890B2
Metal laminate and its manufacturing method, and printed circuit board manufacturing method
JP6954293B2
Fluorocarbon resin film and laminate, and production method for thermally-pressed laminate
WO2018212285A1