Polarizing film, and method of producing polarizing film
The described method enhances polarizing film performance by incorporating controlled stretching and drying processes, achieving high visibility correction and surface irregularities for improved adhesion and optical properties.
Patent Information
- Application Number
- JP2023055388
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polarizing films lack high optical properties and excellent adhesion, with conventional methods failing to achieve optimal visibility correction and surface unevenness for improved performance.
A polarizing film produced by treating a polyvinyl alcohol resin film with a dichroic dye, involving specific stretching and drying processes in controlled humidity and temperature conditions, resulting in a film with high visibility correction and surface irregularities for enhanced adhesion.
The method produces a polarizing film with visibility correction polarization degree of 99.990% or more and surface unevenness of 0.7 μm or more, ensuring excellent adhesion and improved optical properties.
Smart Images

Figure 2024142961000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film produced from a polyvinyl alcohol-based resin film, and a method for producing a polarizing film. [Background technology]
[0002] Polarizing plates are widely used as polarizing elements in image display devices such as liquid crystal display devices. A polarizing plate generally has a structure in which a transparent resin film (such as a protective film) is bonded to one or both sides of a polarizing film using an adhesive or the like.
[0003] Polarizing films are mainly produced by subjecting a raw film made of a polyvinyl alcohol resin to a process of immersing the film in a dye bath containing a dichroic dye such as iodine, followed by a process of immersing the film in a crosslinking bath containing a crosslinking agent such as boric acid, and uniaxially stretching the film at any stage. The uniaxial stretching includes dry stretching in which stretching is performed in air, and wet stretching in which stretching is performed in a liquid such as the dye bath or crosslinking bath.
[0004] Conventionally, in the manufacturing method of polarizing film, various ideas have been devised to improve the properties of polarizing film. JP2013-148806A (Patent Document 1) describes that by providing a primary drying process for drying a polyvinyl alcohol-based resin film between the boric acid treatment process and the water washing process, it is possible to make the transmitted light have a good hue, that is, to make it closer to neutral gray.
[0005] Japanese Patent Application Laid-Open No. 59-094706 (Patent Document 2) describes that a polarizing film having a small shrinkage rate and good flatness can be obtained by performing a fixing process by irradiating far-infrared rays having a wavelength of 1 μm or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-148806 A [Patent Document 2] Japanese Patent Application Publication No. 59-094706 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a polarizing film having high optical properties and excellent adhesion. Another object of the present invention is to provide a method for producing a polarizing film having high optical properties and excellent adhesion. [Means for solving the problem]
[0008] The present invention provides a polarizing film and a method for producing a polarizing film as described below. [1] A polarizing film in which a dichroic dye is adsorbed and oriented on a polyvinyl alcohol-based resin film, The luminosity-corrected polarization degree is 99.990% or more, The visibility corrected single transmittance is 43.0% or more, A polarizing film having a surface with unevenness with a height difference of 0.7 μm or more. [2] The polarizing film according to [1], having a thickness of 24 μm or less.
[0009] [3] A method for producing the polarizing film according to [1], a treatment step of dyeing and uniaxially stretching the polyvinyl alcohol-based resin film by contacting the film with a treatment liquid; After the treatment step, the polyvinyl alcohol-based resin film is heated at a temperature of 40° C. to 100° C. and an absolute humidity of 80 g / m 3 a drying step of performing a drying treatment under a high-temperature and high-humidity atmosphere as described above, in this order.
[0010] [4] The method for producing a polarizing film according to [3], wherein in the drying step, the polyvinyl alcohol-based resin film is uniaxially stretched at a stretching ratio of 1.01 times or more and 1.4 times or less.
[0011] [5] The treatment step includes a swelling step of immersing the polyvinyl alcohol-based resin film in a swelling bath and a dyeing step of immersing the polyvinyl alcohol-based resin film in a dyeing bath, The method for producing a polarized film according to [3] or [4], wherein in the swelling step, the polyvinyl alcohol-based resin film is uniaxially stretched at a stretching ratio of 1.01 times or more and 2.0 times or less.
[0012] [6] The method for producing a polarized film according to [3] or [4], wherein the polyvinyl alcohol-based resin film has a cumulative stretching ratio of 4.5 times or more in the drying step. Effect of the Invention
[0013] According to the present invention, there is provided a polarizing film having high optical properties and excellent adhesion. Also, according to the present invention, there is provided a method for producing a polarizing film having high optical properties and excellent adhesion. [Brief description of the drawings]
[0014] [Figure 1] 1 is a cross-sectional view that illustrates an example of a polarizing film manufacturing method and a polarizing film manufacturing apparatus used in the method according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates an evaluation sample for measuring adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Polarizing film] The polarizing film according to the present invention (hereinafter, simply referred to as "the polarizing film") is a uniaxially stretched polyvinyl alcohol-based resin film on which a dichroic pigment (iodine or a dichroic dye) is adsorbed and oriented.
[0016] The luminosity-corrected single transmittance Ty of the polarizing film is 43.0% or more, preferably 47.0% or less, more preferably 43.1% or more and 45.0% or less, and even more preferably 43.4% or more and 45.0% or less, taking into consideration the balance with the luminosity-corrected polarization degree Py. The luminosity-corrected polarization degree Py is 99.990% or more, preferably 99.991% or more, and more preferably 99.996% or more. Usually, the luminosity-corrected polarization degree Py is 99.9999% or less. Ty and Py are measured according to the description in the Examples section described later.
[0017] The polarizing film has unevenness on its surface, with a height difference of 0.7 μm or more, preferably 0.72 μm or more, more preferably 0.9 μm or more. The unevenness with the largest height difference is preferably 5.0 μm or less, more preferably 4.5 μm or less, and even more preferably 3.5 μm or less. The height difference of the unevenness with the largest height difference on the surface of the polarizing film is determined as follows. The polarizing film has streak-like unevenness on its surface. The uneven shape of the surface is measured by line measurement while scanning the surface in a direction perpendicular to the extension direction of the streak. From the measurement results, the height difference is determined by the sum of the depth (H1) of the bottom of the lowest concave portion relative to the average line of the surface and the height (H2) of the top of the higher convex portion of two convex portions adjacent to the lowest concave portion. Here, the convex portion is defined as a region in which there is no position higher than the central top in the range of the scanning line centered on the top. The range of the scanning line is uniformly determined by the microscope magnification during observation. The position where the surface unevenness is measured by scanning the surface in a direction perpendicular to the streak extension direction can be selected so that the position includes the unevenness with the maximum height difference based on the result of pre-observing a specific region. The pre-observation can be performed, for example, by pre-observing the surface state with a surface state observation device (product name: Scanning White Light Interference Microscope (vertscan), manufactured by Hitachi High-Tech Science Corporation), and the position including the unevenness with the maximum height difference can be specified. In this polarizing film, the extension direction of the streak usually coincides with the absorption axis direction. The thickness of this polarizing film is preferably 5 μm or more and 24 μm or less, more preferably 5 μm or more and 20 μm or less.
[0018] [Method of manufacturing polarizing film] According to the method for producing a polarizing film according to the present invention (hereinafter, simply referred to as "the present production method"), the above-mentioned present polarizing film can be produced. In the present production method, a polyvinyl alcohol-based resin film (raw film) is used as a starting material for producing a polarizing film. The polyvinyl alcohol-based resin constituting the polyvinyl alcohol-based resin film is usually obtained by saponifying a polyvinyl acetate-based resin. The saponification degree is usually about 85 mol% or more, preferably about 90 mol% or more, and more preferably about 99 mol% or more. The polyvinyl acetate-based resin can be, for example, polyvinyl acetate, which is a homopolymer of vinyl acetate, or a copolymer of vinyl acetate and other monomers copolymerizable therewith. Examples of the other copolymerizable monomers include unsaturated carboxylic acids, olefins, vinyl ethers, and unsaturated sulfonic acids. The degree of polymerization of the polyvinyl alcohol-based resin is usually about 1000 to 10000, and preferably about 1500 to 5000.
[0019] These polyvinyl alcohol resins may be modified, and for example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc., which are modified with aldehydes may also be used.
[0020] The raw film used in this manufacturing method is an unstretched polyvinyl alcohol-based resin film having a thickness of preferably 65 μm or less, more preferably 50 μm or less, even more preferably 35 μm or less, and even more preferably 30 μm or less. This makes it possible to obtain a thin polarizing film, which is increasingly in demand in the market. The width of the raw film is not particularly limited, and can be, for example, about 400 to 6000 mm. The raw film is prepared, for example, as a roll (raw roll) of a long unstretched polyvinyl alcohol-based resin film.
[0021] The polyvinyl alcohol-based resin film used in the present invention may be laminated on a substrate film that supports it, i.e., the polyvinyl alcohol-based resin film may be prepared as a laminate film of a substrate film and a polyvinyl alcohol-based resin film laminated thereon. In this case, the polyvinyl alcohol-based resin film can be produced, for example, by applying a coating liquid containing a polyvinyl alcohol-based resin to at least one surface of the substrate film and then drying the coating liquid.
[0022] The substrate film may be, for example, a film made of a thermoplastic resin. Specific examples include a film made of a thermoplastic resin having light transmission, preferably an optically transparent thermoplastic resin, such as a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.) or a cyclic polyolefin resin (norbornene resin, etc.); a cellulose resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin such as a methyl methacrylate resin; a polystyrene resin; a polyvinyl chloride resin; an acrylonitrile-butadiene-styrene resin; an acrylonitrile-styrene resin; a polyvinyl acetate resin; a polyvinylidene chloride resin; a polyamide resin; a polyacetal resin; a modified polyphenylene ether resin; a polysulfone resin; a polyethersulfone resin; a polyarylate resin; a polyamideimide resin; a polyimide resin, etc.
[0023] The polarizing film can be continuously manufactured as a long polarizing film by continuously conveying the long raw film from the raw film roll along the film conveying path of the polarizing film manufacturing apparatus, immersing the film in a treatment liquid (hereinafter also referred to as a "treatment bath") contained in a treatment tank, withdrawing the film, and then drying the film. The treatment is not limited to the method of immersing the film in the treatment bath as long as the treatment is performed by contacting the film with the treatment liquid, and may be a method of treating the film by attaching the treatment liquid to the film surface by spraying, flowing, dropping, or the like. When the treatment is performed by immersing the film in the treatment bath, the treatment bath for one treatment is not limited to one, and one treatment may be completed by sequentially immersing the film in two or more treatment baths.
[0024] Examples of the treatment liquid include a swelling liquid, a dyeing liquid, a crosslinking liquid, and a cleaning liquid. Examples of the treatment process include a swelling process in which a swelling liquid is brought into contact with the raw film to perform a swelling process, a dyeing process in which a dyeing liquid is brought into contact with the film after the swelling process to perform a dyeing process, a crosslinking process in which a crosslinking liquid is brought into contact with the film after the dyeing process to perform a crosslinking process, and a cleaning process in which a cleaning liquid is brought into contact with the film after the crosslinking process to perform a cleaning process. In addition, between these series of treatment processes (i.e., before and after any one or more treatment processes and / or during any one or more treatment processes), a uniaxial stretching process is performed in a wet or dry manner. Other treatment processes may be added as necessary.
[0025] Hereinafter, an example of a method for producing a polarizing film according to the present invention will be described in detail with reference to Fig. 1. Fig. 1 is a cross-sectional view that typically illustrates an example of a method for producing a polarizing film according to the present invention and a polarizing film production apparatus used therein. The polarizing film production apparatus shown in Fig. 1 is configured such that an original (unstretched) film 10 made of a polyvinyl alcohol-based resin is transported along a film transport path while being continuously unwound from an original roll 11, and the film is passed through a swelling bath (swelling liquid contained in a swelling tank) 13, a dyeing bath (dyeing liquid contained in a dyeing tank) 15, a first crosslinking bath (first crosslinking liquid contained in a crosslinking tank) 17a, a second crosslinking bath (second crosslinking liquid contained in a crosslinking tank) 17b, and a washing bath (washing liquid contained in a washing tank) 19 provided on the film transport path in order, and finally passes through a drying furnace 21. In this specification, the treatment in the swelling bath 13 is referred to as the swelling step, the treatment in the dyeing bath 15 as the dyeing step, the treatment in the first crosslinking bath 17a as the first crosslinking step, the treatment in the second crosslinking bath 17b as the second crosslinking step, and the treatment in the washing bath 19 as the washing step, and the swelling step, dyeing step, first crosslinking step, second crosslinking step, and washing step are collectively referred to as the treatment steps.
[0026] The obtained polarizing film 23 can be transported directly to the next polarizing plate production process (a process of laminating a protective film to one or both sides of the polarizing film 23). The arrow in Fig. 1 indicates the transport direction of the film.
[0027] In the description of Fig. 1, "treatment tank" is a general term including a swelling tank, a dyeing tank, a crosslinking tank, and a washing tank, "treatment liquid" is a general term including a swelling liquid, a dyeing liquid, a crosslinking liquid, and a washing liquid, and "treatment bath" is a general term including a swelling bath, a dyeing bath, a crosslinking bath, and a washing bath. The swelling bath, the dyeing bath, the crosslinking bath, and the washing bath respectively constitute a swelling section, a dyeing section, a crosslinking section, and a washing section in the production apparatus of the present invention.
[0028] The film transport path of the polarizing film manufacturing apparatus can be constructed by arranging, in addition to the above-mentioned treatment baths, guide rolls 30-48, 60, 61 that support the film being transported or can further change the film transport direction, and nip rolls 50-55 that press and pinch the film being transported and can apply a driving force to the film by rotating it or can further change the film transport direction at appropriate positions. The guide rolls and nip rolls can be arranged before, after, or within each treatment bath, and this allows the film to be introduced into, immersed in, and removed from the treatment bath (see FIG. 1). For example, one or more guide rolls can be provided in each treatment bath, and the film can be immersed in each treatment bath by transporting the film along these guide rolls.
[0029] The polarizing film manufacturing apparatus shown in FIG. 1 has nip rolls disposed before and after each treatment bath (nip rolls 50 to 54), which makes it possible to carry out inter-roll stretching in one or more treatment baths, in which longitudinal uniaxial stretching is performed by applying a peripheral speed difference between the nip rolls disposed before and after the treatment bath.
[0030] (Swelling process) The swelling process is carried out for the purposes of removing foreign matter on the surface of the raw film 10, removing plasticizers in the raw film 10, imparting ease of dyeing, plasticizing the raw film 10, etc. The treatment conditions are determined within a range in which the purposes can be achieved and in which defects such as extreme dissolution or devitrification of the raw film 10 do not occur.
[0031] 1, the swelling step can be performed by continuously unwinding raw film 10 from raw film roll 11, transporting raw film 10 along a film transport path, immersing raw film 10 in swelling bath 13 for a predetermined time, and then pulling it out. In the example of FIG. 1, from when raw film 10 is unwound until when it is immersed in swelling bath 13, raw film 10 is transported along a film transport path formed by guide rolls 60, 61 and nip roll 50. In the swelling treatment, raw film 10 is transported along a film transport path formed by guide rolls 30 to 32 and nip roll 51.
[0032] As the swelling liquid for the swelling bath 13, in addition to pure water, it is also possible to use an aqueous solution containing boric acid (JP Patent Publication No. 10-153709), chlorides (JP Patent Publication No. 06-281816), inorganic acids, inorganic salts, water-soluble organic solvents, alcohols, etc., in an amount of about 0.01 to 10% by weight.
[0033] The temperature of the swelling bath 13 is, for example, about 10 to 50° C., preferably about 10 to 40° C., and more preferably about 15 to 30° C. The immersion time of the raw film 10 is preferably about 10 to 300 seconds, and more preferably about 20 to 200 seconds. When the raw film 10 is a polyvinyl alcohol resin film that has been stretched in advance in a gas, the temperature of the swelling bath 13 is, for example, about 20 to 70° C., and preferably about 30 to 60° C. The immersion time of the raw film 10 is preferably about 10 to 300 seconds, and more preferably about 30 to 240 seconds.
[0034] In the swelling process, the original film 10 is likely to swell in the width direction, causing wrinkles in the film. As one means for conveying the film while removing the wrinkles, the guide rolls 30, 31 and / or 32 may be rolls having a width-widening function, such as expander rolls, spiral rolls, and crown rolls, or other width-widening devices, such as cross guiders, bend bars, and tenter clips. Another means for suppressing the occurrence of wrinkles is to perform a stretching process. For example, a uniaxial stretching process can be performed in the swelling bath 13 by utilizing the difference in peripheral speed between the nip rolls 50 and 51. In the swelling process, it is preferable to uniaxially stretch the film at a ratio of preferably 1.01 times or more and 2.0 times or less, more preferably 1.2 times or more and 1.7 times or less, and even more preferably 1.3 times or more and 1.7 times or less.
[0035] In the swelling treatment, the film also swells and expands in the film transport direction, so if the film is not actively stretched, it is preferable to take measures such as controlling the speed of nip rolls 50, 51 disposed before and after the swelling bath 13 in order to eliminate slack in the film in the transport direction. Also, for the purpose of stabilizing the film transport in the swelling bath 13, it is useful to control the water flow in the swelling bath 13 with an underwater shower or to use an EPC device (Edge Position Control device: a device that detects the edge of the film and prevents the film from meandering) in combination.
[0036] In the example shown in FIG. 1, the film pulled out from the swelling bath 13 passes through a guide roll 32, a nip roll 51 and a guide roll 33 in this order, and is introduced into the dyeing bath 15.
[0037] (dying process) The dyeing process is carried out for the purpose of adsorbing and orienting a dichroic dye on the polyvinyl alcohol-based resin film after the swelling process. The treatment conditions are determined within a range in which the purpose can be achieved and in which defects such as extreme dissolution or devitrification of the film do not occur. With reference to FIG. 1, the dyeing process can be carried out by conveying the film along a film conveying path constructed by a nip roll 51, guide rolls 33 to 36, and a nip roll 52, immersing the film after the swelling process in a dye bath 15 (a treatment liquid contained in a dyeing tank) for a predetermined time, and then pulling it out. In order to enhance the dyeability of the dichroic dye, it is preferable that the film to be subjected to the dyeing process is a film that has been subjected to at least some degree of uniaxial stretching, or it is preferable to perform a uniaxial stretching process during the dyeing process instead of or in addition to the uniaxial stretching process before the dyeing process.
[0038] When iodine is used as the dichroic dye, the dyeing solution of the dye bath 15 may be, for example, an aqueous solution having a concentration of iodine / potassium iodide / water=0.003-2 / 0.1-10 / 100 by weight ratio. Instead of potassium iodide, other iodides such as zinc iodide may be used, or potassium iodide may be used in combination with other iodides. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may be allowed to coexist. When boric acid is added, it is distinguished from the crosslinking treatment described below in that it contains iodine, and any aqueous solution containing about 2 parts by weight or more of iodine per 100 parts by weight of water can be considered as the dye bath 15. The temperature of the dye bath 15 when the film is immersed is usually about 10 to 45°C, preferably 10 to 40°C, more preferably 20 to 35°C, and the immersion time of the film is usually about 30 to 600 seconds, preferably 50 to 300 seconds.
[0039] When a water-soluble dichroic dye is used as the dichroic pigment, the dyeing solution of the dye bath 15 may be, for example, an aqueous solution having a concentration of dichroic dye / water=0.001 to 0.1 / 100 by weight ratio. The dye bath 15 may contain a dyeing assistant, for example, an inorganic salt such as sodium sulfate or a surfactant. Only one dichroic dye may be used alone, or two or more dichroic dyes may be used in combination. The temperature of the dye bath 15 when the film is immersed is, for example, about 20 to 80° C., preferably 30 to 70° C., and the immersion time of the film is usually about 30 to 600 seconds, preferably about 60 to 300 seconds.
[0040] As described above, in the dyeing step, the film can be uniaxially stretched in the dye bath 15. The film can be uniaxially stretched by, for example, providing a difference in peripheral speed between the nip rolls 51 and 52 disposed before and after the dye bath 15.
[0041] In the dyeing process, in order to transport the polyvinyl alcohol-based resin film while removing wrinkles from the film, similarly to the swelling process, rolls having a width-expanding function such as expander rolls, spiral rolls, and crown rolls may be used as the guide rolls 33, 34, 35, and / or 36, or other width-expanding devices such as cross guiders, bend bars, and tenter clips may be used. Another means for suppressing the occurrence of wrinkles is to perform a stretching process, similarly to the swelling process.
[0042] In the example shown in FIG. 1, the film drawn out from the dye bath 15 passes through a guide roll 36, a nip roll 52, and a guide roll 37 in this order, and is introduced into a first crosslinking bath 17a.
[0043] (Crosslinking process) The crosslinking step is a treatment carried out for the purpose of making the film water-resistant by crosslinking, adjusting the hue (preventing the film from becoming bluish, etc.), etc. In the example shown in FIG. 1, two crosslinking baths are arranged as crosslinking baths for carrying out the crosslinking step, and the first crosslinking step for making the film water-resistant is carried out in the first crosslinking bath 17a, and the second crosslinking step for adjusting the hue is carried out in the second crosslinking bath 17b. Referring to FIG. 1, the first crosslinking step can be carried out by conveying the film along a film conveying path constructed by a nip roll 52, guide rolls 37 to 40, and a nip roll 53a, immersing the film after the dyeing process in the first crosslinking bath 17a (first crosslinking liquid contained in a crosslinking tank) for a predetermined time, and then pulling it out. The second crosslinking step can be carried out by conveying the film along a film conveying path formed by nip roll 53a, guide rolls 41-44, and nip roll 53b, immersing the film after the first crosslinking step in second crosslinking bath 17b (second crosslinking liquid contained in a crosslinking tank) for a predetermined time, and then pulling it out. Hereinafter, the crosslinking bath includes both the first crosslinking bath 17a and the second crosslinking bath 17b, and the crosslinking liquid includes both the first crosslinking liquid and the second crosslinking liquid.
[0044] The crosslinking liquid may be a solution in which a crosslinking agent is dissolved in a solvent. Examples of the crosslinking agent include boron compounds such as boric acid and borax, glyoxal, and glutaraldehyde. These may be used alone or in combination of two or more. The solvent may be, for example, water, and may further contain an organic solvent compatible with water. The concentration of the crosslinking agent in the crosslinking solution is not limited thereto, but is preferably in the range of 1 to 20% by weight, and more preferably 6 to 15% by weight.
[0045] The crosslinking liquid may be an aqueous solution containing, for example, 1 to 10 parts by weight of boric acid per 100 parts by weight of water. When the dichroic dye used in the dyeing process is iodine, the crosslinking liquid preferably contains an iodide in addition to boric acid, and the amount of the iodide may be, for example, 1 to 30 parts by weight per 100 parts by weight of water. Examples of the iodide include potassium iodide and zinc iodide. In addition, compounds other than iodide, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, and sodium sulfate, may be allowed to coexist.
[0046] In the crosslinking treatment, the concentrations of boric acid and iodide and the temperature of the crosslinking bath 17 can be appropriately changed depending on the purpose. For example, in the case of the first crosslinking liquid in which the purpose of the crosslinking treatment is to make the film water-resistant by crosslinking, the first crosslinking liquid can be an aqueous solution having a concentration of boric acid / iodide / water=3-10 / 1-20 / 100 by weight ratio. If necessary, other crosslinking agents may be used instead of boric acid, or boric acid may be used in combination with other crosslinking agents. The temperature of the first crosslinking bath 17a when the film is immersed is usually about 50-70°C, preferably 53-65°C, and the immersion time of the film is usually about 10-600 seconds, preferably 20-300 seconds, more preferably 20-200 seconds. In addition, when the dyeing treatment and the first crosslinking treatment are performed in this order on the polyvinyl alcohol-based resin film that has been stretched before the swelling treatment, the temperature of the first crosslinking bath 17a is usually about 50-85°C, preferably 55-80°C.
[0047] In the second crosslinking liquid for adjusting the hue, for example, when iodine is used as a dichroic dye, the concentration can be boric acid / iodide / water=1-5 / 3-30 / 100 by weight ratio. The temperature of the second crosslinking bath 17b when the film is immersed is usually about 10-45° C., and the immersion time of the film is usually about 1-300 seconds, preferably 2-100 seconds.
[0048] The crosslinking treatment may be carried out multiple times, usually 2 to 5 times. In this case, the composition and temperature of each crosslinking bath used may be the same or different as long as they are within the above range. The crosslinking treatment for water resistance by crosslinking and the crosslinking treatment for color adjustment may each be carried out in multiple steps.
[0049] The uniaxial stretching treatment can be performed in the first crosslinking bath 17a by utilizing the difference in peripheral speed between the nip roll 52 and the nip roll 53a. Also, the uniaxial stretching treatment can be performed in the second crosslinking bath 17b by utilizing the difference in peripheral speed between the nip roll 53a and the nip roll 53b.
[0050] In the crosslinking treatment, in order to transport the polyvinyl alcohol-based resin film while removing wrinkles from the film, similarly to the swelling treatment, rolls having a width-expanding function such as expander rolls, spiral rolls, and crown rolls may be used as the guide rolls 38, 39, 40, 41, 42, 43, and / or 44, or other width-expanding devices such as cross guiders, bend bars, and tenter clips may be used. Another means for suppressing the occurrence of wrinkles is to perform a stretching treatment, similarly to the swelling treatment.
[0051] In the example shown in FIG. 1, the film pulled out from the second crosslinking bath 17b passes through a guide roll 44 and a nip roll 53b in this order, and is introduced into a washing bath 19.
[0052] (Cleaning process) In the example shown in Fig. 1, a cleaning step is included after the crosslinking step. The cleaning treatment is performed for the purpose of removing excess chemicals such as boric acid and iodine attached to the polyvinyl alcohol-based resin film. The cleaning step is performed, for example, by immersing the crosslinked polyvinyl alcohol-based resin film in a cleaning bath 19. Note that the cleaning step can also be performed by spraying a cleaning liquid onto the film as a shower, instead of immersing the film in the cleaning bath 19, or by combining immersion in the cleaning bath 19 with spraying the cleaning liquid.
[0053] 1 shows an example of a case where a cleaning treatment is performed by immersing a polyvinyl alcohol-based resin film in a cleaning bath 19. The temperature of the cleaning bath 19 in the cleaning treatment is usually about 2 to 40° C., and the immersion time of the film is usually about 1 to 120 seconds.
[0054] In addition, in the cleaning treatment, for the purpose of transporting the polyvinyl alcohol-based resin film while removing wrinkles, a roll having a width expanding function such as an expander roll, a spiral roll, or a crown roll, or other width expanding devices such as a cross guider, a bend bar, or a tenter clip, may be used as the guide rolls 45, 46, 47, and / or 48. In addition, in the film cleaning treatment, a stretching treatment may be performed to suppress the occurrence of wrinkles.
[0055] (Stretching process) As described above, the raw film 10 is uniaxially stretched in a wet or dry manner during the series of processing steps (i.e., before and after any one or more processing steps and / or during any one or more processing steps). Specific methods of uniaxial stretching include, for example, inter-roll stretching in which longitudinal uniaxial stretching is performed by applying a peripheral speed difference between two nip rolls (e.g., two nip rolls arranged before and after a processing bath) constituting a film transport path, hot roll stretching as described in Japanese Patent No. 2731813, tenter stretching, etc., and preferably inter-roll stretching. The uniaxial stretching step can be performed multiple times from the raw film 10 until the polarizing film 23 is obtained. As described above, the stretching process is also advantageous in suppressing the occurrence of wrinkles in the film.
[0056] The cumulative stretching ratio of the polarizing film 23 before being subjected to the drying step, based on the original film 10, is preferably 4.5 to 7.0 times, more preferably 5.0 to 6.5 times, and even more preferably 5.5 to 6.5 times. The stretching step may be performed in any of the processing steps, and even when the stretching treatment is performed in two or more processing steps, the stretching treatment may be performed in any of the processing steps.
[0057] (drying process) After the washing step, the polyvinyl alcohol-based resin film is dried. There is no particular limitation on the drying method, but it can be performed using a drying oven 21 as shown in the example of FIG. 1. The drying oven 21 can be equipped with a hot air dryer, for example. In the drying oven 21, the temperature is 40° C. or higher and 100° C. or lower, preferably 50° C. or higher and 98° C. or lower, and the absolute humidity is 80 g / m 3 More than 82g / m 3 More than 200g / m 3 Less than 85g / m 3 More than 180g / m 3 More preferably, 140 g / m 3 More than 180g / m 3 The drying time is, for example, 30 to 600 seconds.
[0058] According to the manufacturing method in which the drying step is performed under the above conditions, a polarizing film having unevenness on the surface with a height difference of 0.7 μm or more can be easily obtained. In addition, according to the manufacturing method in which the drying step is performed under the above conditions, uniaxial stretching can be performed in the drying step without breaking the polyvinyl alcohol-based resin film. The method of uniaxial stretching in the drying step is not limited, and includes the above-mentioned methods such as inter-roll stretching, hot roll stretching, and tenter stretching, and preferably inter-roll stretching. The uniaxial stretching in the drying step is preferably performed at a magnification of 1.01 times or more and 2.0 times or less, more preferably 1.01 times or more and 1.5 times or less. By performing uniaxial stretching in the drying step, a polarizing film with better optical properties (Py, Ty) can be obtained.
[0059] The obtained polarizing film may be wound up on a winding roll to form a roll, or may be directly subjected to the polarizing plate production process (a process of laminating a protective film or the like on one or both sides of the polarizing film) without being wound up.
[0060] (Other processing steps for polyvinyl alcohol-based resin film) Treatments other than those described above may also be added. Examples of treatments that can be added include a treatment of immersion in an aqueous iodide solution not containing boric acid (complementary color treatment) performed after the crosslinking step, and a treatment of immersion in an aqueous solution not containing boric acid but containing zinc chloride or the like (zinc treatment).
[0061] <Polarizing plate> A polarizing plate can be obtained by bonding a protective film to at least one side of the polarizing film produced as described above via an adhesive. Examples of the protective film include films made of acetylcellulose-based resins such as triacetylcellulose and diacetylcellulose; films made of polyester-based resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate-based resin films, cycloolefin-based resin films; acrylic-based resin films; and films made of linear olefin-based resins such as polypropylene-based resins.
[0062] By constructing a polarizing plate using the polarizing film, the adhesion between the polarizing film and the protective film is improved. In addition, in order to improve the adhesion between the polarizing film and the protective film, the bonding surface of the polarizing film and / or the protective film may be subjected to a surface treatment such as a corona treatment, a flame treatment, a plasma treatment, an ultraviolet irradiation, a primer coating treatment, or a saponification treatment. Examples of adhesives used for bonding the polarizing film and the protective film include active energy ray curable adhesives such as ultraviolet curable adhesives, aqueous solutions of polyvinyl alcohol resins or aqueous solutions containing crosslinking agents, and water-based adhesives such as urethane emulsion adhesives. The ultraviolet curable adhesive may be a mixture of an acrylic compound and a photoradical polymerization initiator, or a mixture of an epoxy compound and a photocationic polymerization initiator. In addition, a cationic polymerizable epoxy compound and a radical polymerizable acrylic compound may be used in combination, and a photocationic polymerization initiator and a photoradical polymerization initiator may be used in combination as the initiator.
[0063] In this specification, when the adhesion of a polarizing film is high, it means that the adhesion between the polarizing film and the film in contact therewith is high, and specifically, it means that the polarizing film and the film in contact therewith are not easily peeled off from each other. EXAMPLES
[0064] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.
[0065] <Example 1> The polarizing film of Example 1 was manufactured from a polyvinyl alcohol-based resin film using the manufacturing apparatus shown in FIG. 1. Specifically, a long polyvinyl alcohol (PVA) raw film (saponification degree 99.9 mol% or more) having a thickness of 45 μm was continuously transported while being unwound from a roll, and was immersed in a swelling bath of pure water at 30° C. for a residence time of 40 seconds (swelling step). In the swelling step, the film was uniaxially stretched 1.63 times longitudinally by inter-roll stretching in the bath. Thereafter, the film pulled out from the swelling bath was immersed in a dyeing bath at 30° C. containing iodine, in which potassium iodide / boric acid / water was 2 / 0.3 / 100 (weight ratio), for a residence time of 54 seconds (dyeing step). Next, the film pulled out from the dye bath was immersed in a first crosslinking bath at 58° C. containing potassium iodide / boric acid / water in a ratio of 11.7 / 4 / 100 (by weight) for a residence time of 35 seconds, and then in a second crosslinking bath at 40° C. containing potassium iodide / boric acid / water in a ratio of 11.8 / 4 / 100 (by weight) for a residence time of 6 seconds (crosslinking step). In the dyeing step and crosslinking step, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath.
[0066] Next, the film pulled out from the second crosslinking bath 17b was immersed in a washing bath 19 made of pure water at 5°C for a residence time of 1 second (washing step). After the washing step was completed, the cumulative stretching ratio of the polyvinyl alcohol-based resin film was 6.05 times based on the original film at the stage of being supplied to the drying step. Thereafter, the film was dried in a drying oven 21 at a temperature of 80°C and an absolute humidity of 87.6 g / m 3At the same time, the film was uniaxially stretched 1.02 times longitudinally by roll-to-roll stretching to obtain a polarizing film. The thickness of the polarizing film was 17.5 μm. The thickness of the polarizing film was measured using a contact-type film thickness measuring device ("MS-5C" manufactured by Nikon Corporation).
[0067] <Examples 2 to 4, Comparative Examples 1 and 2> A polarizing film was produced in the same manner as in Example 1, except that the stretching ratio in the swelling step, the cumulative stretching ratio provided in the drying step, the absolute humidity in the drying oven, and the stretching ratio in the drying step were set to the conditions shown in Table 1. The thickness of the obtained polarizing film was as shown in Table 1.
[0068] [Evaluation of Polarizing Film] (a) Measurement of single unit transmittance and polarization degree For the polarizing films obtained in each of the Examples and Comparative Examples, the MD transmittance and TD transmittance in the wavelength range of 380 to 780 nm were measured using a spectrophotometer equipped with an integrating sphere ("V7100" manufactured by JASCO Corporation), and the values were calculated using the following formula: Single layer transmittance (%) = (MD + TD) / 2 Degree of polarization (%)={(MD-TD) / (MD+TD)}×100 The single transmittance and the degree of polarization at each wavelength were calculated based on the above.
[0069] "MD transmittance" is the transmittance when the direction of polarized light exiting the Glan-Thompson prism is parallel to the transmission axis of the polarizing film sample, and is represented as "MD" in the above formula. "TD transmittance" is the transmittance when the direction of polarized light exiting the Glan-Thompson prism is perpendicular to the transmission axis of the polarizing film sample, and is represented as "TD" in the above formula. The obtained single transmittance and polarization degree were measured in accordance with JIS Z 8701:1999 "Method of displaying color - XYZ color system and XYZ color system". 10 Y 10 Z 10 Luminosity correction was performed using a 2-degree visual field (C light source) in the "Color Space System," and the luminosity-corrected single transmittance (Ty) and luminosity-corrected polarization degree (Py) were calculated. Table 1 shows the luminosity-corrected polarization degree (Py) and luminosity-corrected single transmittance (Ty).
[0070] (b) Measurement of the height difference of the unevenness on the surface of the polarizing film The obtained polarizing film was observed at a magnification of 5x in an area of 7.8 mm in the transmission axis direction (MD direction) and 12 mm in the absorption axis direction (TD direction) with a surface condition observation device (product name: scanning white light interference microscope (vertscan), manufactured by Hitachi High-Tech Science Corporation), and the unevenness with the largest height difference was extracted. Then, the unevenness shape of the surface was measured by line measurement while scanning a range of 10 mm in the absorption axis direction (TD direction) in the TD direction so as to include this unevenness. From the measurement results, the sum of the depth (H1) of the lowest concave portion relative to the average line of the surface and the height (H2) of the top of the higher convex portion of the two convex portions adjacent to each of the lowest concave portions was calculated, and this value was taken as the height difference of the unevenness. Table 1 shows the height difference of the unevenness.
[0071] (c) Adhesion strength measurement A protective film (cycloolefin polymer film manufactured by Zeon Corporation) was attached to one side of the obtained polarizing film using an adhesive to obtain a laminate A of "polarizing film / adhesive / protective film". Next, the above-mentioned laminate A was attached with the polarizing film side facing each other through an epoxy-based ultraviolet-curing adhesive, and the epoxy-based ultraviolet-curing adhesive was cured to obtain a laminate B. Thereafter, the laminate B was cut into a size of 200 mm in length x 25 mm in width so that the absorption axis direction was parallel to the long side to obtain an evaluation sample. An evaluation sample of the laminate B was attached to the surface of a glass substrate through an adhesive, and the adhesion force was measured.
[0072] Fig. 2 is a schematic diagram showing the layer structure of laminate B bonded onto glass substrate 7. As shown in Fig. 2, laminate B has a layer structure of, from the side farthest from glass substrate 7, protective film 1, adhesive layer 2, polarizing film 3, epoxy-based ultraviolet-curing adhesive layer 5, polarizing film 3, adhesive layer 2, and protective film 1, and is bonded onto glass substrate 7 via adhesive layer 6. In each of the laminates B in Examples 1 to 4 and Comparative Examples 1 and 2, the members other than the polarizing film were made of the same material.
[0073] The adhesion was measured by making a cut at interface X of laminate B, and peeling in a 180° direction from the cut at a peel speed of 300 mm / min. The peel strength (adhesion) at this time was measured using an Autograph AGS-50NX manufactured by Shimadzu Corporation. Table 1 shows the measurement results of adhesion.
[0074] [Table 1]
[0075] As shown in Table 1, the polarizing films of Examples 1 to 4 had a height difference of 0.7 μm or more and were excellent in adhesion. [Explanation of symbols]
[0076] 10 raw film made of polyvinyl alcohol resin, 11 raw film roll, 13 swelling bath, 15 dyeing bath, 17a first crosslinking bath, 17b second crosslinking bath, 19 cleaning bath, 21 drying furnace, 23 polarizing film, 30 to 48, 60, 61 guide rolls, 50 to 52, 53a, 53b, 54, 55 nip rolls.
Claims
1. A polarizing film in which a dichroic dye is adsorbed and oriented on a polyvinyl alcohol-based resin film, The luminosity-corrected polarization degree is 99.990% or more, The visibility corrected single transmittance is 43.0% or more, A polarizing film having irregularities on its surface with a height difference of 0.7 μm or more.
2. The polarizing film according to claim 1 , which has a thickness of 24 μm or less.
3. A method for producing the polarizing film of claim 1, comprising the steps of: a treatment step of dyeing and uniaxially stretching the polyvinyl alcohol-based resin film by contacting the film with a treatment liquid; After the treatment step, the polyvinyl alcohol-based resin film is heated at a temperature of 40° C. to 100° C. and an absolute humidity of 80 g / m 3 a drying step of performing a drying treatment under a high-temperature and high-humidity atmosphere as described above, in this order.
4. The method for producing a polarizing film according to claim 3 , wherein in the drying step, the polyvinyl alcohol-based resin film is uniaxially stretched at a stretching ratio of 1.01 times or more and 1.4 times or less.
5. The treatment step includes a swelling step of immersing the polyvinyl alcohol-based resin film in a swelling bath and a dyeing step of immersing the polyvinyl alcohol-based resin film in a dyeing bath, The method for producing a polarizing film according to claim 3 or 4, wherein in the swelling step, the polyvinyl alcohol-based resin film is uniaxially stretched at a stretching ratio of 1.01 times or more and 2.0 times or less.
6. The method for producing a polarizing film according to claim 3 or 4, wherein the polyvinyl alcohol-based resin film has a cumulative stretching ratio of 4.5 times or more provided in the drying step.
Citation Information
Patent Citations
Method for manufacturing polarizing film
JP2017106969A
Method and device for manufacturing polarizing film
JP2018032023A
Polarizing plate and production method therefor
WO2017030144A1
Manufacture of polarizing film
JP1984094706A
Polarizing film and manufacturing method thereof and polarizer
JP2013148806A