Ferritic stainless steel plate and producing method thereof
By controlling hot rolling and heating processes to achieve uniform Cr carbide distribution and equiaxed ferrite grains, the manufacturing method addresses the challenges of high strength and anisotropy in ferritic stainless steels, resulting in a cost-effective solution for appliance frames.
Patent Information
- Application Number
- JP2023055427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing ferritic stainless steels do not meet the requirements of high strength, minimal bending anisotropy, and cost-effectiveness for frame components in home appliances under stringent bending conditions, particularly in L and C directions, due to inadequate control of carbide distribution and grain structure.
A method of manufacturing ferritic stainless steel by controlling the hot rolling end temperature and subsequent heating and holding to ensure a uniform distribution of fine Cr carbides and equiaxed ferrite grains, combined with specific chemical compositions to enhance strength and reduce bending anisotropy.
The resulting steel exhibits high strength and minimal bending anisotropy in both L and C directions, ensuring shape accuracy and rigidity while being cost-effective.
Smart Images

Figure 2024142991000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel sheet and a method for producing the same. [Background technology]
[0002] Portable notebook computers, televisions and other home appliances are becoming ever more affordable, smaller and lighter, and there is also a demand for frame components to be thinner and have more complex shapes.
[0003] Materials used in the frames of home appliances are required to be high strength to ensure the rigidity of the product as a structural part. In addition to ensuring bending workability that can handle increasingly complex shapes of parts and products, they are also required to have small bending anisotropy due to differences in bending direction in order to achieve high accuracy of shape and dimensional accuracy. The bending direction refers to bending in which the bending ridgeline is perpendicular to the rolling direction of the steel plate (hereinafter referred to as L-direction bending) and bending processing in which the bending ridgeline is parallel to the rolling direction of the steel plate (hereinafter referred to as C-direction bending). It is required that no cracks occur at the bending ridgeline when bending is performed.
[0004] Stainless steel is used as the material for the frame.
[0005] Patent Document 1 discloses an austenitic stainless steel that is excellent in L- and C-direction bending workability and has high strength, but contains a large amount of expensive Ni and Mo, and is more expensive than ferritic stainless steel. Patent Documents 2 and 3 disclose inexpensive alloy-saving ferritic stainless steels with small bending anisotropy, but the bending conditions used for evaluation in these documents cannot be said to be the strict conditions required in recent years. Patent Document 4 discloses a ferritic stainless steel that is an intermediate material for high-strength martensitic stainless steel and a manufacturing method thereof. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-124131 A [Patent Document 2] International Publication No. WO2005 / 014873 [Patent Document 3] JP 2018-145484 A [Patent Document 4] Patent Publication No. 2021-050386 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a ferritic stainless steel sheet which has high strength, is free of bending anisotropy in the L and C directions under the severe bending conditions required in recent years, and requires less alloying, and a method for producing the same. [Means for solving the problem]
[0008] The inventors have conducted extensive research into alloy-saving ferritic stainless steel suitable for components used in the frames of home appliances, and have clarified the characteristics of the metal structure that not only ensures a specified hardness, but also eliminates bending anisotropy in the L and C directions.
[0009] We have found that strengthening by particle dispersion strengthening of fine Cr carbides, which has not been used in the field of ferritic stainless steels, can be used for specific steel components. We have also found that the required strength can be secured by combining grain refinement strengthening and particle dispersion strengthening of fine Cr carbides. On the other hand, we have also found that even if a large amount of carbides are dispersed in the ferritic matrix, they do not adversely affect bending workability as long as they are fine. In conventional stainless steels, coarse carbides precipitate at the grain boundaries where diffusion is easy, so they do not contribute to strengthening and often have an adverse effect on workability.
[0010] In addition, they discovered that by making the aspect ratio of ferrite in the steel sheet cross section parallel to the rolling direction of the steel sheet equiaxed to a specified value or less, the same workability can be ensured in C-direction bending as in L-direction bending. They clarified the characteristics of the steel composition and metal structure that can achieve this effect.
[0011] Furthermore, in order to obtain a large amount of fine carbides, which are beneficial as described above, a manufacturing method thereof has been clarified. In the ferritic stainless steel of the present invention, it is important that the end temperature of hot rolling is controlled in the austenite single phase region. This controls and maintains the strain distribution state of the austenite after hot rolling, increases the frequency of Cr carbides precipitating from the prior austenite grain boundaries during the heating and holding following hot rolling, and a large amount of fine Cr carbides are randomly distributed. In addition, grain growth of ferrite precipitated together with Cr carbides occurs in the plate thickness direction and the rolling direction, and the ferrite after heating and holding becomes equiaxed. This makes it possible to make the average aspect ratio of ferrite 2.5 or less.
[0012] After the hot rolling, the steel is heated and held continuously. By "continuously," the steel is heated and held at a specified temperature of 600°C or higher and 800°C or lower for 30 minutes or longer and 360 minutes or shorter, without lowering the temperature below 600°C after the hot rolling is completed. This allows the transformation and precipitation of austenite to ferrite and Cr carbides to proceed uniformly, achieving the uniform dispersion of a large amount of fine carbides.
[0013] Based on the above findings, the present invention discloses the following techniques. [1] In mass%, C: 0.16% to 0.45%, Si: 0.01% to 1.00%, Mn: 0.01% to 1.00%, Cr: 11.5% to 15.0%, N: 0.002% to 0.070%, P: 0.040% or less, S: 0.0300% or less, Ni: 0% to 0.80%, the balance being Fe and impurities. The average grain size of the ferrite phase is 10 μm or less, and the average aspect ratio of the ferrite phase is 2.5 or less, A ferritic stainless steel sheet characterized in that the average particle diameter of Cr carbide is 0.25 μm or less, and the residue recovery rate of Cr carbide recovered by an extraction residue method is 1.0 mass% or more. [2] The ferritic stainless steel sheet according to [1], characterized in that in place of a portion of the Fe, one or more of the following are included, by mass%, Al: 0.30% or less, Nb: 0.070% or less, B: 0.0030% or less, Ti: 0.070% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.000% or less, Co: 0.500% or less, Zr: 0.500% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Y: 0.1000% or less, REM: 0.10% or less, and Sb: 0.15% or less. [3] The ferritic stainless steel according to [1] or [2], further characterized in that the hardness is 240 HV or more.
[0014] [4] A method for producing a ferritic stainless steel according to [1] or [2], After the hot rolling is completed at 950°C or more and 1050°C or less, the hot rolling is followed by heating and holding at a temperature of 600°C or more and 800°C or less for 30 minutes to 360 minutes; A method for producing a ferritic stainless steel sheet, further comprising cold rolling and cold-rolled sheet annealing, the cold-rolled sheet annealing temperature being 700°C or higher and 800°C or lower, and the cold-rolled sheet annealing time being 10 s or higher and 300 s or lower. [5] The method for producing a ferritic stainless steel sheet according to [4], further characterized in that the hardness of the ferritic stainless steel sheet is 240 HV or more. Effect of the Invention
[0015] According to the present invention, it is possible to provide a ferritic stainless steel sheet having high strength and extremely small bending anisotropy in the L and C directions. The strength of the ferritic stainless steel sheet is evaluated by hardness (HV). [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram showing a method of a bending test. [Diagram 2] FIG. 2 is a diagram showing the positional relationship between a bending test piece and the rolling direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] 1. Ferritic stainless steel plate The ferritic stainless steel sheet of the present invention will now be described in more detail.
[0018] (Chemical Composition) First, the components contained in the ferritic stainless steel of the present invention will be described. Note that the "%" for the content of each element means % by mass.
[0019] C affects the amount of Cr carbide precipitation and is an element necessary for ensuring the amount of particle dispersion strengthening by Cr carbide. If the C content is less than 0.16%, the amount of carbide precipitation is small, sufficient particle dispersion strengthening cannot be obtained, and strength is insufficient. On the other hand, if the C content exceeds 0.45%, aggregation and coarsening of Cr carbide cannot be avoided, sufficient particle dispersion strengthening cannot be obtained, and strength is insufficient. For the above reasons, the C content is set to 0.16% or more and 0.45% or less. It is preferably 0.26% or more and 0.40% or less, more preferably 0.28% or more and 0.35% or less.
[0020] Silicon is an element that improves oxidation resistance. If the silicon content is less than 0.01%, sufficient oxidation resistance may not be obtained. Moreover, if the silicon content is excessively reduced, the manufacturing cost increases. If the silicon content exceeds 1.00%, cracking during manufacturing is promoted. Therefore, the silicon content is set to 0.01% or more and 1.00% or less. It is preferably 0.05% or more and 0.85% or less, and more preferably 0.15% or more and 0.60% or less.
[0021] Mn is used as a deoxidizing element. From the viewpoint of stable production, the Mn content is set to 0.01% or more. On the other hand, if the Mn content exceeds 1.00%, it may form compounds such as sulfides, which may lead to a decrease in corrosion resistance. Therefore, the Mn content is set to 1.00% or less. It is preferably 0.10% or more and 0.85% or less, and more preferably 0.20% or more and 0.70% or less.
[0022] Cr is an element that combines with C to form Cr carbide. It is also an element that improves corrosion resistance. On the other hand, it is also an element that should be regulated in order to make the metal structure mainly austenite at the hot rolling temperature. If the Cr content is less than 11.5%, sufficient corrosion resistance cannot be obtained. On the other hand, if the Cr content exceeds 15.0%, a two-phase structure of austenite and ferrite will be formed in the hot rolling temperature range, and during the heating and holding process, Cr carbide will mainly precipitate from austenite, and the distribution of Cr carbide will become localized, so the average aspect ratio of ferrite will increase. Therefore, the Cr content is set to 11.5% or more and 15.0% or less. It is preferably 12.0% or more and 14.5% or less, and more preferably 12.5% or more and 14.0% or less.
[0023] Ni is an element that improves toughness and may be added as necessary. However, since Ni is a rare and expensive element, excessive addition of Ni leads to an increase in alloy costs and a hindrance to manufacturability. Therefore, the Ni content is set to 0.80% or less. It is preferably 0.60% or less, and more preferably 0.50% or less.
[0024] N is an element that improves corrosion resistance. From the viewpoint of corrosion resistance, the N content is set to 0.002% or more. On the other hand, if the N content is too high, the hot workability is significantly deteriorated. Therefore, the N content is set to 0.070% or less. It is preferably 0.009% or more and 0.06% or less, and more preferably 0.011% or more and 0.050% or less.
[0025] P is an element that reduces formability and corrosion resistance. It is preferable that the content is low. Therefore, the P content is set to 0.040% or less. There is no particular lower limit. However, if the P content is reduced too much, the manufacturing cost increases. Therefore, the P content is preferably 0.005% or more and 0.030% or less. More preferably, it is 0.007% or more and 0.025% or less.
[0026] S promotes cracking during manufacturing. Therefore, the S content is set to 0.0300% or less. It is preferably 0.0100% or less, and more preferably 0.0030% or less. There is no particular lower limit. However, if the S content is excessively reduced, the manufacturing cost increases. From this viewpoint, the S content is preferably 0.0003% or more.
[0027] The ferritic stainless steel of the present invention contains Fe and impurities (including unavoidable impurities) in addition to the above-mentioned elements.
[0028] In addition to the basic composition described above, the ferritic stainless steel of the present disclosure may selectively contain, in place of a portion of Fe, one or more of the following, by mass%, Al: 0.30% or less, Nb: 0.070% or less, B: 0.0030% or less, Ti: 0.070% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.000% or less, Co: 0.500% or less, Zr: 0.500% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Y: 0.1000% or less, REM: 0.10% or less, and Sb: 0.15% or less.
[0029] The elements Al, Nb, B, and Ti do not have to be added. If these elements are added, they have the effect of improving the formability of ferritic stainless steel and suppressing defects during hot rolling. When added, the Al content is 0.30% or less, the Nb content is 0.070% or less, the B content is 0.0030% or less, and the Ti content is 0.070% or less. In order to reliably obtain the above effects, it is preferable that the Al, Nb, and Ti contents are 0.01% or more, and the B content is 0.001% or more.
[0030] The elements Sn, Cu, W, Co, and Zr do not have to be added. These elements have the effect of improving corrosion resistance. When added, the Sn content is 0.12% or less, the Cu content is 0.40% or less, the W content is 1.000% or less, the Co content is 0.500% or less, and the Zr content is 0.500% or less. In order to reliably obtain the above effects, it is preferable that the Sn, Cu, Co, and Zr contents are 0.01% or more, and the W content is 0.1% or more.
[0031] The elements Ca, Mg, Y, REM and Sb do not have to be added. These elements have the effect of changing inclusions such as oxides and sulfides to suppress defects during hot rolling. When added, the Ca content is 0.0050% or less, the Mg content is 0.0050% or less, the Y content is 0.1000% or less, the REM content is 0.10% or less, and the Sb content is 0.15% or less. In order to reliably obtain the above effects, it is preferable that the Ca and Mg contents are 0.0001% or more, and the Y and REM contents are 0.01% or more. In the present invention, "REM" refers to elements (lanthanoids) having atomic numbers of 57 to 71, such as Ce, Pr, and Nd, but does not include Y.
[0032] (Average grain size and average aspect ratio of ferrite phase) In order to ensure the strength required for the material used in the above applications, the average crystal grain size of the ferrite phase must be 10 μm or less. The average crystal grain size is preferably 6 μm or less, and more preferably 4 μm or less. On the other hand, the lower limit of the average crystal grain size is not particularly limited, but is set to 1 μm or more based on past experience. On the other hand, if the average crystal grain size exceeds 10 μm, there is a high possibility that the strength cannot be ensured. The average crystal grain size of the ferrite phase can be calculated as the average circle equivalent diameter of the observed crystal grains.
[0033] On the other hand, in order to ensure workability in the C-direction bending equivalent to that in the L-direction bending, the average aspect ratio of the ferrite phase needs to be 2.5 or less. The average aspect ratio is preferably 2.3 or less, and more preferably 2.1 or less. The average aspect ratio of the ferrite phase means the average value of the "long axis length ÷ short axis length" of the ferrite phase crystal grains.
[0034] (average particle diameter of Cr carbide, residue recovery rate) In order to ensure the strength of the material used in the above applications, it is necessary that Cr carbides of a certain size or less and at least a certain amount are precipitated, and almost all of the C added to the ferritic stainless steel of the present invention exists as Cr carbides. On the other hand, if either the size or the amount of precipitation of the Cr carbides does not satisfy the specified range, the material strength cannot be ensured. Note that the Cr carbides are 23 Any composition is acceptable, including C6.
[0035] The average particle diameter of the Cr carbide is preferably 0.25 μm or less. The average particle diameter is preferably 0.20 μm or less, and more preferably 0.17 μm or less. On the other hand, the lower limit of the average particle diameter is not particularly limited, but is set to 0.01 μm or more based on past experience. On the other hand, if the average particle diameter exceeds 0.25 μm, the material strength cannot be ensured. In addition, there is an increased possibility that defects will occur during processing and the processability will deteriorate. The average particle diameter of the Cr carbide can be obtained as the average value of the circle equivalent diameters of the observed Cr carbides.
[0036] The amount of precipitated Cr carbide must be 1.0 mass% or more in terms of residue recovery rate when recovered by the extraction residue method, and the residue recovery rate of Cr carbide is preferably 2.0 mass% or more, and more preferably 3.0 mass% or more.
[0037] (Presence of phases other than ferrite and carbides) The metal structure of the ferritic stainless steel of the present invention is composed of ferrite and numerous fine carbides at room temperature, which account for only a small proportion of the carbides. However, the presence of other phases can be tolerated to a certain extent. For example, in the ferritic stainless steel of the present invention, there is no problem if the ferritic stainless steel contains phases other than the main phase ferrite, such as austenite and martensite, in an area ratio of 5% or less in total at room temperature.
[0038] 2. Manufacturing method of ferritic stainless steel sheet (Manufacturing method) The method for producing the ferritic stainless steel sheet of the present invention will now be described.
[0039] A steel having the above composition is melted and cast to produce an ingot. The ingot is then heated. The heating temperature may be any temperature generally used in stainless steel manufacturing. The heating temperature is 1150°C or higher, preferably 1180°C or higher, and more preferably 1200°C or higher. There is no particular upper limit. However, if the heating temperature is excessively high, there is a concern that uneven patterns may occur on the surface of the cold-rolled annealed sheet. From this viewpoint, the heating temperature is preferably 1350°C or lower.
[0040] Next, the heated ingot is hot rolled. As described above, in the ferritic stainless steel of the present invention, it is important that the end temperature of the hot rolling is controlled in the austenite single phase region. In the ferritic stainless steel of the present invention, the end temperature of the hot rolling is 950°C or higher. The end temperature is preferably 975°C or higher, more preferably 1000°C or higher. In the hot rolling, it is important that the metal structure is austenite single phase. Note that austenite single phase means that the austenite phase is 95% or more, more preferably 97% or more. The remainder is a ferrite phase and compounds such as carbides.
[0041] When the above two points are satisfied, the strain distribution state of the austenite after hot rolling is controlled, and the frequency of Cr carbides precipitating from the prior austenite grain boundaries during the heating and holding following the hot rolling increases, and the Cr carbides are randomly distributed after the heating and holding. In addition, the grain growth of the ferrite that precipitates together with the Cr carbides occurs in the plate thickness direction and the rolling direction, and the ferrite after the heating and holding becomes equiaxed. By specifying the end temperature of the hot rolling as described above, the average aspect ratio of the ferrite after the heating and holding becomes 2.5 or less. On the other hand, if the end temperature of the hot rolling is less than 950°C, the Cr carbides are distributed in stripes along the rolling direction after the heating and holding. This makes it easier for the ferrite to grow in grains in the rolling direction, and the average aspect ratio of the ferrite after the heating and holding becomes large.
[0042] As described above, in the method for producing ferritic stainless steel of the present invention, it is necessary to control the end temperature of hot rolling, which is a control that has not been carried out in conventional methods for producing ferritic stainless steel because it leads to an increase in production costs.
[0043] After the hot rolling is completed at a hot rolling end temperature of 950°C or more, the material is subsequently heated and held. Here, "subsequently heated and held" means that the material obtained after hot rolling is inserted into a heating furnace without intentionally cooling between the hot rolling and heat holding steps, and without cooling to less than 600°C. Even if the end temperature of the hot rolling is controlled to a predetermined temperature or higher, in the case of a general manufacturing process in the conventional manufacturing method of ferritic stainless steel, that is, a thermal history in which the material is once cooled to room temperature after the hot rolling, reheated, and held at heat, a long time is required for reheating, and Cr carbides become coarse.
[0044] If the heating temperature is less than 600°C, the transformation and precipitation from austenite to ferrite and Cr carbide will be insufficient, and when the steel is cooled to room temperature after the heating, the amount of Cr carbide precipitation will be insufficient. In addition, the metal structure will contain a lot of hard martensite, which may cause the sheet to break during the subsequent process of passing the sheet. On the other hand, if the temperature exceeds 800°C, the transformation and precipitation from austenite to ferrite and Cr carbide will be insufficient, and when the steel is cooled to room temperature after the heating, the amount of carbide precipitation will be insufficient. If the heating time is less than 30 minutes, the transformation and precipitation from austenite to ferrite and Cr carbide will be insufficient, and when the steel is cooled to room temperature after the heating, the amount of carbide precipitation will be insufficient. In addition, the metal structure will contain a lot of hard martensite, which may cause the sheet to break during the subsequent process of cold rolling. On the other hand, if the heating time exceeds 360 minutes, the average particle size of the carbide will become coarse. Therefore, the heating and holding is performed at a temperature of 600°C to 800°C for 30 minutes to 360 minutes. Preferably, the heating and holding is performed at a temperature of 650°C to 770°C for 60 minutes to 300 minutes. More preferably, the heating and holding is performed at a temperature of 700°C to 760°C for 120 minutes to 240 minutes. The cooling rate after the heating and holding is not particularly limited. For example, the cooling rate may be 0.05°C / s or more, or air cooling may be performed.
[0045] After the heating and holding is completed, pickling, cold rolling, and cold-rolled sheet annealing can be performed to obtain a steel sheet of a specified thickness. Pickling is a process for removing oxide scale on the surface, cold rolling is a process for obtaining a specified thickness, and cold-rolled sheet annealing is a process for releasing the strain introduced by the cold rolling and softening the sheet, and these are general methods for the production of stainless steel and do not pose a problem.
[0046] If the temperature of the cold-rolled sheet annealing is less than 700°C, the strain introduced by cold rolling is not sufficiently released, and bending workability cannot be ensured. In addition, passing the sheet to the next process or material processing at the customer becomes difficult. On the other hand, if the temperature is higher than 800°C, the austenite phase reaches a stable temperature range, and after cooling, the metal structure becomes hard due to the martensite phase being abundant, and bending workability cannot be ensured. Passing the sheet to the next process or material processing at the customer becomes difficult. Therefore, the temperature of the cold-rolled sheet annealing is 700°C or more and 800°C or less. Preferably, it is 710°C or more and 790°C or less. More preferably, it is 720°C or more and 780°C or less. In addition, if the time of the cold-rolled sheet annealing is less than 10s, the sheet becomes hard and bending workability cannot be ensured. On the other hand, if it exceeds 300s, the average crystal grain size of the ferrite phase becomes coarse. Therefore, the time of the cold-rolled sheet annealing is 10s or more and 300s or less. Preferably, it is 20s or more and 120s or less. More preferably, it is 30 seconds or more and 60 seconds or less. EXAMPLES
[0047] The effect of the ferritic stainless steel sheet of the present invention will be described with reference to examples. A steel having the composition shown in Table 1 was smelted in a laboratory to obtain an ingot having a thickness of 100 mm. This ingot was heated at 1230°C for 100 minutes, and then hot-rolled. The hot-rolling was completed at the hot-rolling end temperature shown in Tables 2 and 3 to obtain a hot-rolled sheet having a thickness of 5.0 mm. The hot-rolled sheet was then heated and held under the conditions shown in Tables 2 and 3 without being cooled to less than 600°C, and air-cooled. Furthermore, after pickling with sulfuric acid and cold rolling at a rolling reduction of 60%, cold-rolled sheet annealing was performed under the conditions shown in Tables 2 and 3 to obtain a steel sheet having a thickness of 2.0 mm. For comparison, a thermal history process was also performed in which the sheet was cooled to room temperature after hot rolling, heated again, and held.
[0048] [Table 1]
[0049] [Table 2]
[0050] [Table 3]
[0051] (Method of measuring average grain size and average aspect ratio of ferrite) The average grain size and average aspect ratio of ferrite were determined by the following method. First, the L-section (cross section perpendicular to the sheet width direction) of the steel sheet sample prepared by electrolytic polishing was measured by EBSD. The measurement area was 300 μm × 300 μm at the position of 1 / 4t of the sheet thickness, and the measurement step size was 0.1 μm. The measurement data was then analyzed using the analysis software "OIM". If the crystal orientation difference between adjacent plot data was less than 15°, they were considered to be the same crystal grain, and if there was an orientation difference of 15° or more, they were considered to be different crystal grains. Among the measurement data, plot data determined to be "BCC", which is the crystal structure of the ferrite phase, was considered to be the ferrite phase. If the measurement area contained phases other than the ferrite phase, only the ferrite phase was extracted and calculated.
[0052] The average crystal grain size and average aspect ratio of the ferrite phase were calculated using the above software. The average crystal grain size was taken as the average circle equivalent diameter of the observed crystal grains. When the aspect ratio was calculated using the above software, the aspect ratio was output as the "short axis length ÷ long axis length" of the crystal grain. On the other hand, the aspect ratio in this specification is defined as the "long axis length ÷ short axis length" of the crystal grain, and is expressed as the reciprocal of the output value of the above software.
[0053] (Method for measuring the average particle diameter of Cr carbide) The average particle diameter of the carbides was determined by the following method. First, the L-section of the steel plate was mirror-polished, and then the sample was prepared by electrolytic polishing to reveal the grain boundaries and carbides, and then SEM observation was performed. Carbides can be confirmed by EDX. The size and number density of the carbides were measured by SEM observation. The measurement area was a total area of 200 μm × 200 μm at the 1 / 4t position of the plate thickness, and SEM observation was performed at a magnification of 5000 times. The size of the carbides was determined by converting the observed carbides into circle equivalent diameters, and averaging these values to determine the average particle diameter. The carbides confirmed in the ferritic stainless steel of the present invention are (Cr, Fe) 23 Most of the carbide is C6, but some of it may contain (Cr,Fe)7C3. Carbide with a Cr content higher than the average value of the steel composition is considered to be Cr carbide.
[0054] (Method for measuring the residue recovery rate of Cr carbide) The residue recovery rate was determined by the following method. For a steel plate with a thickness (t [mm]), the area from both surfaces of the steel plate to 1 / 4t of the plate thickness was cut to prepare a sample of 30 mmL x 20 mmW x 1 / 2t. The extracted residue was collected by constant current electrolysis using a non-solvent electrolyte (10% acetylacetone-1% tetramethylammonium chloride-methanol). The size of the residue filter used was 0.2 μm. Here, the residue recovery rate of Cr carbide was defined as the value calculated by formula (2). Here, W is the residue recovery rate of Cr carbide (unit: [mass%]), g and G are the mass of the residue collected in the residue filter and the mass change of the sample before and after the extraction residue, respectively (unit: [pieces]). As is clear from the following formula (2), the total amount (g) of the residue collected in the residue filter is Cr carbide. W = g / G × 100 … (2)
[0055] The residue obtained in the ferritic stainless steel sheet of the present invention is (Cr, Fe) 23 The majority of the residue is C6, but it may contain some (Cr,Fe)7C3. The substances that make up the residue can be confirmed by XRD.
[0056] (Hardness measurement method) To evaluate the material strength of the ferritic stainless steel plate, the cross-sectional hardness was measured at 1 / 4t of the plate thickness using a Vickers hardness tester. Ten measurements were performed with a test load of 500g, and if the average value was 240HV or higher, it was determined that the required material strength was met.
[0057] (Method for evaluating the presence or absence of bending anisotropy) A bending test was performed using the V-block method in accordance with JIS Z2248 (see Figure 1. Using a jig 2 and a punch 3, the tip of the punch 3 had a radius of 0.4 mm, θ: 45°). The shape of the bending test piece 1 was 60 mm long and 30 mm short. The bending test piece 1 for the L-direction bending and the bending test piece 1 for the C-direction bending were taken in a positional relationship in which the rolling direction and the long side of the bending test piece 1, and the rolling direction and the short side of the bending test piece 1 coincided, as shown in Figure 2. The bending test was performed with N=3 for the same sample, and samples that did not show any cracks in all three tests were evaluated as "Good", and samples that showed any cracks at least once were evaluated as "Poor". The presence or absence of cracks was judged visually. The presence or absence of bending anisotropy was judged as follows. When both the L-direction bending and the C-direction bending were evaluated as "Good", it was judged that there was no bending anisotropy. On the other hand, when either the L-direction bending or the C-direction bending was evaluated as "Poor", it was judged that there was bending anisotropy.
[0058] (Method to determine the presence or absence of austenite and martensite) The metal structure of the ferritic stainless steel sheet of the present invention is composed of a ferrite phase and numerous fine carbides, which account for only a small proportion of the ferrite phase at room temperature. However, the presence of other phases can be tolerated to a certain extent. For example, the ferritic stainless steel sheet of the present invention can be acceptable at room temperature if it contains a total of 5% or less of phases other than the main phase ferrite, such as austenite and martensite, in terms of area ratio. Here, γ represents the area ratio of austenite (unit: [%]), and F and B represent the number of plots of the FCC structure and the BCC structure obtained by EBSD measurement, respectively (unit: [pieces]). γ = F / (F + B) × 100 … (1)
[0059] Meanwhile, the presence or absence of martensite was judged by Vickers hardness. If 5% or more martensite is present, the hardness exceeds 300HV. Using a Vickers hardness tester, measurements were taken 10 times with a load of 500g, and if the average value was 300HV or less, it was determined that martensite was not present.
[0060] The results are shown in Tables 2 and 3. It can be confirmed that No. 1 to 25, in which the average grain size, average aspect ratio, average particle diameter of Cr carbide, and residue recovery rate are within the specified range, ensure the necessary material strength and do not exhibit bending anisotropy. In contrast to the above, No. 26, in which the end temperature of hot rolling is below the specified level, exhibits bending anisotropy because the average aspect ratio of ferrite is greater than the specified level. No. 27, which has a thermal history of being cooled to room temperature after the end of hot rolling and then heated again and held at heat, exhibits insufficient material strength because the average particle diameter of Cr carbide is greater than the specified level. No. 28, which contains too little added C, exhibits insufficient material strength because the residue recovery rate of Cr carbide is less than the specified level. No. 29, which contains too much added C, exhibits insufficient material strength because the size of Cr carbide aggregates and becomes coarse. No. 30, which contained too much Cr, became a two-phase state of austenite and ferrite in the hot rolling temperature range, and Cr carbides precipitated locally, which increased the average aspect ratio of the ferrite and caused bending anisotropy. No. 31, which had been annealed for a longer time than specified, had a larger average grain size of ferrite and an average particle diameter of Cr carbide than specified, and the material strength was insufficient. No. 32, which was obtained by performing temper rolling with a reduction of 60% on the hot rolled sheet, had a larger average aspect ratio of ferrite than specified, and therefore showed bending anisotropy. [Industrial Applicability]
[0061] The ferritic stainless steel sheet of the present disclosure has high strength, is free of bending anisotropy in the L and C directions even under more severe bending conditions than before, and is alloy-saving. That is, for example, it can accommodate more complex shapes and lower costs for components used in the frames of home appliances. [Explanation of symbols]
[0062] 1. Bending test piece 2 Jig 3 Punch
Claims
1. In mass%, C: 0.16% or more and 0.45% or less, Si: 0.01% or more and 1.00% or less, Mn: 0.01% or more and 1.00% or less, Cr: 11.5% or more and 15.0% or less, N: 0.002% or more and 0.070% or less, P: 0.040% or less, S: 0.0300% or less, Ni: 0% or more and 0.80% or less, the balance being Fe and impurities. The average grain size of the ferrite phase is 10 μm or less, and the average aspect ratio of the ferrite phase is 2.5 or less, A ferritic stainless steel plate, characterized in that the average particle diameter of Cr carbide is 0.25 μm or less, and the residue recovery rate of Cr carbide recovered by an extraction residue method is 1.0 mass% or more.
2. In place of a portion of the Fe, the following elements are added, by mass%, Al: 0.30% or less, Nb: 0.070% or less, B: 0.0030% or less, Ti: 0.070% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.000% or less, Co: 0.500% or less, Zr: 0.500% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Y: 0.1000% or less, REM: 0.10% or less, and Sb: 0.15% or less. The ferritic stainless steel sheet according to claim 1, further comprising one or more of the following:
3. The ferritic stainless steel sheet according to claim 1 or 2, further comprising a hardness of 240 HV or more.
4. A method for producing a ferritic stainless steel sheet according to claim 1 or claim 2, After the hot rolling is completed at 950° C. or more and 1050° C. or less, the hot rolling is followed by heating and holding at a temperature of 600° C. or more and 800° C. or less for 30 minutes to 360 minutes or less; A method for producing a ferritic stainless steel sheet, further comprising cold rolling and cold-rolled sheet annealing, the cold-rolled sheet annealing temperature being 700° C. or higher and 800° C. or lower, and the cold-rolled sheet annealing time being 10 s or higher and 300 s or lower.
5. The method for producing a ferritic stainless steel sheet according to claim 4, further characterized in that the hardness of the ferritic stainless steel sheet is 240 HV or more.
Citation Information
Patent Citations
High strength austenitic stainless steel strip having excellent bending workability
JP2004124131A
High strength diplophase stainless steel material excellent in corrosion resistance and flexure processability
JP2018145484A
Ferritic stainless steel and method for producing ferritic stainless steel
JP2021050386A
Work-hardened material from stainless steel
WO2005014873A1