Method for producing water-based pigment dispersion, method for producing aqueous inkjet ink, and water-based pigment composite
A crosslinked structure on pigment surfaces using a polyfunctional compound addresses stability issues in water-based inks, ensuring stable dispersion and improved substrate wetting in aqueous inkjet inks.
Patent Information
- Application Number
- JP2023056071
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Water-based inks face challenges in achieving stable pigment dispersion due to high surface tension and difficulty in wetting various substrates, leading to issues like thickening or gelling when combined with different types of water-soluble organic solvents and surfactants.
A method involving the addition of a polyfunctional compound with multiple (meth)acryloyl groups to a mixture containing a polymer compound, pigment, and water in the presence of a base, forming a crosslinked structure on the pigment surface using a polymer compound with β-dicarbonyl and carboxyl or sulfonic acid groups to enhance dispersibility and stability.
The method provides aqueous pigment dispersions with excellent storage stability, enabling the production of aqueous inkjet inks that maintain stability even with low-polarity solvents, improving wetting and fixing on diverse substrates without gelling or thickening.
Smart Images

Figure 2024143410000001 
Figure 2024143410000002 
Figure 2024143410000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing an aqueous pigment dispersion, a method for producing an aqueous inkjet ink, and an aqueous pigment composite. [Background technology]
[0002] An inkjet recording system is a printing system that performs printing by ejecting highly fluid liquid ink from fine nozzles and depositing it on a substrate. This system is characterized by the ability to print high-resolution, high-quality images at high speed and with low noise using relatively inexpensive equipment. Water-based inks are widely used because they can produce high-quality prints at low cost. Water-based inks have improved drying properties by containing moisture, and also have the advantage of being environmentally friendly. On the other hand, since the solvent for water-based inks is water and water-soluble organic solvents, it is difficult to finely disperse pigments in the water-based inks and ensure the dispersion stability of the pigments, and technological development is desired.
[0003] Patent Document 1 proposes that a dispersant having a crosslinked structure, which is a copolymer of a monomer mixture containing a specific monomer such as a monomer containing a carboxy group, be used to disperse a pigment in an aqueous inkjet ink, thereby improving storage stability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-135519 A Summary of the Invention [Problem to be solved by the invention]
[0005] Water-based inks have a high surface tension and tend to wet poorly on some substrates. As a countermeasure to this, there is a method of improving wettability to substrates by adding a low-polarity water-soluble organic solvent to the water-based ink. In order to provide water-based inks with different types of water-soluble organic solvents, there is a method of preparing water-based pigment dispersions in advance and combining them with water-soluble organic solvents and surfactants suitable for various substrates to provide water-based inks. In this case, depending on the types of water-soluble organic solvents and surfactants, thickening or gelation of the water-based ink may occur, and improvement is expected.
[0006] An object of the present invention is to provide a method for producing an aqueous pigment dispersion capable of providing an ink having excellent storage stability, a method for producing an aqueous ink-jet ink using the same, and an aqueous pigment composite. [Means for solving the problem]
[0007] According to one embodiment, there is provided a method for producing an aqueous pigment dispersion, the method comprising adding a polyfunctional compound having a plurality of (meth)acryloyl groups to a mixture containing a polymer compound, a pigment, and water in the presence of a base, the polymer compound containing a β-dicarbonyl group, and at least one of a carboxy group and a sulfonic acid group.
[0008] According to another embodiment, there is provided a method for producing an aqueous inkjet ink, the method comprising producing the aqueous pigment dispersion according to the above-described production method, and adding a water-soluble organic solvent and a surfactant to the aqueous pigment dispersion.
[0009] According to yet another embodiment, there is provided an aqueous pigment complex comprising a pigment, a polymeric compound, and a polyfunctional compound having a plurality of (meth)acryloyl groups, the polymeric compound comprising a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group, the polymeric compound being adsorbed to the pigment, and the polyfunctional compound having a plurality of (meth)acryloyl groups being bonded to the β-dicarbonyl group of the polymeric compound on the surface of the pigment to form a crosslinked structure. Effect of the Invention
[0010] According to one embodiment of the present invention, it is possible to provide a method for producing an aqueous pigment dispersion capable of providing an ink having excellent storage stability, a method for producing an aqueous inkjet ink using the same, and an aqueous pigment composite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described below using several embodiments, but the present invention is not limited to the examples in the following embodiments.
[0012] (Method of producing aqueous pigment dispersion) A method for producing an aqueous pigment dispersion according to one embodiment includes adding a polyfunctional compound having a plurality of (meth)acryloyl groups to a mixture containing a polymer compound and a pigment in the presence of a base, and the polymer compound is characterized in that it contains a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group.
[0013] Hereinafter, the aqueous pigment dispersion may be simply referred to as a "pigment dispersion" or "dispersion," and the aqueous inkjet ink may be simply referred to as an "aqueous ink" or "ink." In addition, a polyfunctional compound having multiple (meth)acryloyl groups in the presence of a base may be simply referred to as a "polyfunctional compound."
[0014] In this specification, (meth)acryloyl group collectively means methacrylic group, acryloyl group, or a combination thereof, (meth)acrylic acid collectively means methacrylic acid, acrylic acid, or a combination thereof, and (meth)acrylate collectively means methacrylate, acrylate, or a combination thereof. Similar expressions are treated similarly.
[0015] According to one embodiment, it is possible to provide a method for producing an aqueous pigment dispersion capable of providing an ink having excellent storage stability, and a method for producing an aqueous ink-jet ink using the same. The reason for this is explained below, but the present invention is not limited to the following theory.
[0016] Methods for dispersing a pigment in an aqueous ink include a method using a pigment dispersant and a method using an encapsulated pigment in which a pigment is coated with a resin. When the polymer compound used in these methods dissolves in the aqueous medium of the aqueous ink, there is a problem that the aqueous ink thickens or gels. In an aqueous pigment dispersion produced according to a production method of an embodiment and an aqueous ink using the same, the polymer compound can enhance the pigment dispersibility while suppressing the dissolution of the polymer compound into the aqueous medium. When the aqueous ink contains a water-soluble organic solvent, particularly a water-soluble organic solvent with low polarity, the polymer compound is easily dissolved in the solvent. Even in this case, according to an embodiment, the dissolution of the polymer compound can be suppressed and the storage stability can be maintained well.
[0017] In the aqueous pigment dispersion, the polymer compound contains a β-dicarbonyl group and at least one of a carboxyl group and a sulfonic acid group, and thus can act as a dispersant for the pigment. The crosslinked structure of this polymer compound prevents the polymer compound from being detached from the pigment, even when the aqueous ink contains a low-polarity water-soluble organic solvent, and maintains the dispersibility of the pigment. The polymer compound also prevents thickening or gelling of the aqueous ink caused by the detached polymer compound, and excellent storage stability can be obtained over a long period of time. More specifically, the active methylene of the β-dicarbonyl group of the polymer compound is crosslinked on the pigment surface by a Michael addition reaction with a multifunctional compound having multiple (meth)acryloyl groups in the presence of a base, thereby stably forming a coating of the pigment with the polymer compound.
[0018] In the technology disclosed in Patent Document 1, a carboxy group is used as a crosslinking site, but since the carboxy group is a functional group involved in dispersion stabilization by electrostatic repulsion, there is a restriction that an ionic group for dispersion stabilization must be added separately from the crosslinking site. In addition, since the carboxy group is somewhat water-soluble and tends to be located at a position away from the pigment, crosslinking aggregation is likely to occur between pigment particles during crosslinking, and the covering of the pigment with the polymer compound may be insufficient. According to one embodiment, since the polymer compound has a β-dicarbonyl group, interaction by tautomers is expected with the pigment surface, and the adsorption force to the pigment etc. is also expected to be improved by the chelating effect, making it easier to proceed with the crosslinking reaction on the pigment surface. This makes it possible to suppress the increase in particle size of the pigment complex due to crosslinking and the aggregation between pigment particles.
[0019] The method for producing the aqueous pigment dispersion may include adding a polyfunctional compound having a plurality of (meth)acryloyl groups to a mixture containing a polymer compound, a pigment, and water in the presence of a base. The polymer compound may include a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group.
[0020] According to this manufacturing method, in a state where the polymer compound is adsorbed on the pigment, the polymer compound and the polyfunctional compound having a plurality of (meth)acryloyl groups undergo a crosslinking reaction to form a crosslinked structure on the surface of the pigment. The formation of a crosslinked structure on the surface of the pigment makes it possible to suppress the polymer compound from being detached from the pigment and the polymer compound from being dissolved in a solvent.
[0021] The mixture includes a polymer compound, a pigment, and water. The mixture may be obtained by using a polymer compound composition obtained by synthesis of a polymer compound. In this case, the mixture may further include a polymerization initiator, a chain transfer agent, and the like. Each component will be described below.
[0022] The polymeric compound may contain a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group.
[0023] The polymer compound has a β-dicarbonyl group, which allows it to have pigment adsorption properties for various pigments. In addition, the β-dicarbonyl group serves as the starting point for a crosslinking reaction with a polyfunctional compound having multiple (meth)acryloyl groups. As a result, a crosslinked structure is formed on the pigment surface, which makes it possible to suppress the polymer compound from being detached from the pigment. Furthermore, the crosslinked structure makes it possible to suppress the polymer compound from dissolving in a solvent.
[0024] The β-dicarbonyl group may be a β-diketone group (-C(=O)-CC(=O)-), a β-keto acid ester group (-C(=O)-CC(=O)OR, where R is a hydrocarbon group), or a combination thereof. Examples of the β-diketone group include an acetoacetyl group and a propionoacetyl group, and examples of the β-keto acid ester group include an acetoacetoxy group and a propionoacetoxy group. It is sufficient for a polymer compound to contain one type of β-dicarbonyl group per molecule, and it may contain two or more types of β-dicarbonyl groups.
[0025] The β-dicarbonyl group may be derived from a polymerizable compound having a β-dicarbonyl group and contained in the polymer compound. The polymerizable compound having a β-dicarbonyl group may be a monomer or an oligomer, but is preferably a monomer. Hereinafter, the monomer having a β-dicarbonyl group is also simply referred to as monomer (A).
[0026] As the monomer (A) having a β-dicarbonyl group, a compound in which a β-dicarbonyl group has been introduced into (meth)acrylic acid, (meth)acrylate, (meth)acrylamide, an allyl compound, ethylene or a derivative thereof can be used. Among these, a (meth)acrylate having a β-dicarbonyl group is preferred. This makes it possible to provide a copolymer whose main chain is a (meth)acrylic skeleton. The copolymer whose main chain is a (meth)acrylic skeleton has a certain degree of hardness and flexibility on the surface of the pigment and can be preferably used as a polymer compound.
[0027] Examples of the monomer (A) include acetoacetoxyalkyl (meth)acrylates such as acetoacetoxyethyl (meth)acrylate, acetoacetoxypropyl (meth)acrylate, and acetoacetoxybutyl (meth)acrylate; ethylene glycol monoacetoacetate mono(meth)acrylate, 2,3-di(acetoacetoxy)propyl (meth)acrylate, and 2,4-hexadione (meth)acrylate; allyl acetoacetate; vinyl acetoacetate; and acetoacetoxyalkyl (meth)acrylamides such as acetoacetoxyethyl (meth)acrylamide. The monomer (A) may be used alone or in combination of two or more.
[0028] The polymer compound has at least one of a carboxy group and a sulfonic acid group, and thus can contribute to dispersion stabilization by electrostatic repulsion.
[0029] The carboxyl group and the sulfonic acid group may be derived from a polymerizable compound having a carboxyl group and a polymerizable compound having a sulfonic acid group, respectively, and may be included in the polymer compound. The polymerizable compound having a carboxyl group and the polymerizable compound having a sulfonic acid group may be a monomer or an oligomer, respectively, but is preferably a monomer. Hereinafter, the monomer having a carboxyl group and the monomer having a sulfonic acid group are also simply referred to as monomer (B).
[0030] When the main chain of the polymer compound is a carbon chain, the carboxyl group is preferably directly bonded to a carbon atom of the main chain. Examples of the monomer (B) for introducing such a carboxyl group include acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, citraconic acid, etc. Among them, acrylic acid, methacrylic acid, or a combination thereof is preferred.
[0031] The carboxyl group may be introduced into the main chain of the polymer compound via any functional group. Examples of the monomer (B) for introducing such a carboxyl group include β-carboxyethyl (meth)acrylate, 4-[2-(methacryloyloxy)ethoxy]-4-oxo-2-butenoic acid, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl hexahydrophthalic acid, 2-acryloyloxypropyl phthalic acid, 2-acryloyloxypropyl hexahydrophthalic acid, methacryloyloxymethyl succinic acid, methacryloyloxyethyl succinic acid, methacryloyloxyethyl phthalic acid, methacryloyloxyethyl hexahydrophthalic acid, methacryloyloxypropyl phthalic acid, and methacryloyloxypropyl hexahydrophthalic acid.
[0032] Examples of monomers for introducing a sulfonic acid group as monomer (B) include 2-sulfoethyl methacrylate, 3-(meth)acryloyloxypropanesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, 4-vinylbenzenesulfonic acid, allylsulfonic acid, 2-methylallylsulfonic acid, etc. The monomers having a sulfonic acid group may be subjected to synthesis as sodium salts, potassium salts, etc.
[0033] Monomer (B) may be used alone or in combination of two or more. Monomer (B) preferably contains (meth)acrylic acid, (meth)acrylate having a carboxy group or a sulfonic acid group, or a combination thereof. This makes it possible to provide a copolymer whose main chain is a (meth)acrylic skeleton.
[0034] The carboxyl group and sulfonic acid group derived from the monomer (B) may be neutralized from the viewpoint of improving electrostatic repulsion. Representative examples of the neutralizing agent include ammonium hydroxide, sodium hydroxide, and potassium hydroxide. In the aqueous pigment composite, the neutralizing agent is used in a molar ratio of preferably 80 to 120, more preferably 80 to 100, based on the total of the carboxyl group and sulfonic acid group derived from the monomer (B).
[0035] The polymer compound may further contain other units in addition to the units having a β-dicarbonyl group, the units having a carboxyl group, and the units having a sulfonic acid group. The other units may be units having other functional groups in addition to the β-dicarbonyl group, the carboxyl group, and the sulfonic acid group. Examples of the other functional groups include alkyl groups, aromatic hydrocarbon groups, groups having polyoxyalkylene glycol chains, acetate ester groups, and nitrile groups. These functional groups may be contained in the polymer compound alone or in combination of two or more types.
[0036] The other functional group may be derived from a polymerizable compound having another functional group and contained in the polymer compound. The polymerizable compound having another functional group may be a monomer or an oligomer, but is preferably a monomer. Hereinafter, the monomer having another functional group is also simply referred to as monomer (C).
[0037] Specific examples of monomers (C) having other functional groups include (meth)acrylates; styrene-based monomers such as styrene and α-methylstyrene; vinyl ether-based polymers such as vinyl acetate, vinyl benzoate, and butyl vinyl ether; maleic acid esters; fumaric acid esters; acrylonitrile; methacrylonitrile; and α-olefins.
[0038] When at least one of the monomers (A) and (B) is a (meth)acrylate monomer, it is preferable to use a (meth)acrylate as the monomer (C).
[0039] Examples of the (meth)acrylate as monomer (C) include alkyl (meth)acrylate, cycloalkyl (meth)acrylate, aryl (meth)acrylate, etc. Among them, alkyl (meth)acrylate having 1 to 20 carbon atoms, preferably 1 to 8, more preferably 1 to 4 carbon atoms, cycloalkyl (meth)acrylate having 6 to 20 carbon atoms, preferably 6 to 12 carbon atoms, and aryl (meth)acrylate having 6 to 20 carbon atoms, preferably 6 to 12 carbon atoms are preferred.
[0040] Specific examples of the (meth)acrylate as monomer (C) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate), neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, isododecyl (meth)acrylate, n-stearyl (meth)acrylate, isostearyl (meth)acrylate, and cyclohexyl (meth)acrylate. The monomer (C) may be used alone or in combination of two or more kinds.
[0041] Among the other functional groups, aromatic hydrocarbon groups are preferred because they can further increase the adsorption of polymer compounds to pigments, and groups having polyoxyalkylene glycol chains are preferred because they can further increase the dispersion stability in the aqueous pigment composite due to the three-dimensional structure of the long chain.
[0042] Specific examples of the monomer having an aromatic hydrocarbon group as monomer (C) (hereinafter also referred to simply as monomer (C1)) include phenyl (meth)acrylate, benzyl (meth)acrylate, biphenyl (meth)acrylate, naphthyl (meth)acrylate, etc., and ethylene oxide modified products thereof.
[0043] Examples of ethylene oxide modified products of monomers having aromatic hydrocarbon groups include ethoxylated phenylphenol (meth)acrylate. One example of ethoxylated phenylphenol (meth)acrylic can be synthesized by esterification reaction of polyethylene glycol modified biphenyl alcohol and (meth)acrylic acid. Examples of commercially available products of ethoxylated phenylphenol (meth)acrylate include "A-LEN-10" (trade name) manufactured by Shin-Nakamura Chemical Co., Ltd.
[0044] Examples of the monomer having a polyoxyalkylene glycol chain as monomer (C) (hereinafter, also simply referred to as monomer (C2)) include ethers of (meth)acrylic acid and polyalkylene glycol, (meth)acrylates modified with polyalkylene glycol, etc. Polyalkylene glycol-modified (meth)acrylates can be obtained, for example, by reacting polyalkylene glycol with (meth)acrylates into which functional groups that serve as the starting point of isocyanate groups, etc. have been introduced.
[0045] Specific examples of monomers having a polyoxyalkylene glycol chain include polyethylene glycol mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, ethoxypolyethylene glycol mono(meth)acrylate, polyethylene glycol modified 2-isocyanatoethyl (meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol-propylene glycol-mono(meth)acrylate, polyethylene glycol-trimethylene glycol-mono(meth)acrylate, polyethylene glycol-allyl ether, methoxypolyethylene glycol-allyl ether, polyethylene glycol-polypropylene glycol-allyl ether, polypropylene glycol-allyl ether, and methoxypolyethylene glycol acrylamide.
[0046] Examples of commercially available monomers having a polyoxyalkylene glycol chain include "ADEKA REASOAP ER-20" manufactured by ADEKA CORPORATION, "BLEMMER PME-400", "BLEMMER PME-1000", and "BLEMMER PME-4000" manufactured by NOF CORPORATION, "NK ESTER M-230G" manufactured by Shin-Nakamura Chemical Co., Ltd., and "LIGHT ESTER 041MA" manufactured by Kyoeisha Chemical Co., Ltd. (all trade names).
[0047] Since the polymer compound contains at least one of a carboxy group and a sulfonic acid group, it exhibits anionicity and can exhibit pigment dispersibility. From this viewpoint, it is preferable that the polymer compound does not contain a cationic functional group, and the other functional group is preferably a nonionic group.
[0048] The polymeric compound may be a copolymer of a monomer mixture including monomer (A) and monomer (B). In another example, the polymeric compound may be a copolymer of a monomer mixture including monomer (A), monomer (B), and monomer (C). In yet another example, the polymeric compound may be a copolymer of a monomer mixture including monomer (A), monomer (B), monomer (C1), and monomer (C2).
[0049] From the viewpoints of pigment adsorption and crosslinking reactivity, the unit derived from the monomer (A) is preferably 1 to 50 mol %, more preferably 10 to 35 mol %, and even more preferably 20 to 30 mol % relative to the total units of the polymer compound. When the monomer (A) is 1 mol %, 10 mol % or more, or 20 mol % or more, sufficient starting points for the crosslinking reaction are provided on the surface of the pigment, and the crosslinked structure can further suppress detachment of the polymer compound from the pigment.
[0050] The unit derived from the monomer (B) is preferably 1 to 50 mol %, more preferably 10 to 35 mol %, and even more preferably 20 to 30 mol %, based on all units of the polymer compound, from the viewpoint of pigment dispersibility due to electrostatic repulsion.
[0051] The molar ratio of monomer (A) to the total of monomer (A) and monomer (B) is preferably from 20 to 80 mol %, more preferably from 30 to 70 mol %, and still more preferably from 40 to 60 mol %.
[0052] The amount of units derived from monomer (C1) relative to the total units of the polymer compound is preferably 1 to 50 mol%, more preferably 10 to 30 mol%, and even more preferably 20 to 30 mol%, from the viewpoint of pigment adsorption. The amount of units derived from monomer (C2) relative to the total units of the polymer compound is preferably 1 to 30 mol%, more preferably 5 to 20 mol%, and even more preferably 5 to 15 mol%, from the viewpoint of imparting pigment dispersibility by the three-dimensional structure of the molecular structure. The amount of units derived from monomer (C) relative to the total units of the polymer compound is preferably 1 to 80 mol%, more preferably 10 to 60 mol%, and even more preferably 20 to 40 mol%, as the total amount of other monomers (C).
[0053] The polymer compound is preferably 0.5 to 30% by mass, more preferably 1 to 20% by mass, and even more preferably 5 to 10% by mass, based on the total mass of the aqueous pigment dispersion. By making the content of this polymer compound 0.5%, 1%, or 5% by mass or more, it is possible to further increase the pigment coverage and improve the pigment dispersibility. By making the content of this polymer compound 30% by mass or less, 20% by mass or less, or 10% by mass or less, it is possible to prevent the thickening or gelation of the aqueous ink caused by excess polymer compound.
[0054] From the same viewpoint, the mass ratio of the polymer compound to the pigment is preferably 0.1 to 5, more preferably 0.2 to 3, and even more preferably 0.4 to 1.
[0055] An example of a method for synthesizing a polymer compound will be described below. Note that the polymer compound is not limited to those synthesized by a specific synthesis method.
[0056] An example of a method for synthesizing a polymer compound includes copolymerizing a monomer mixture, the monomer mixture including monomer (A) and monomer (B). The monomer mixture may further include monomer (C). Details of monomer (A), monomer (B) and monomer (C) are as described above.
[0057] The polymer compound can be synthesized by copolymerizing a monomer mixture by known radical polymerization or the like. The polymerization may be any of random copolymerization, block copolymerization, and graft copolymerization. The polymer compound may be a random copolymer, and may contain a block unit in part, and no particular regularity is required. The polymerization may be carried out according to a solution polymerization method, a bulk polymerization method, a suspension polymerization method, an emulsion polymerization method, or the like, and is preferably a solution polymerization method.
[0058] Examples of the polymerization solvent used in the solution polymerization include aliphatic alcohols having 1 to 3 carbon atoms, such as ethanol, 1-propanol, and 2-propanol; ketones, such as acetone and methyl ethyl ketone; and esters, such as ethyl acetate.
[0059] In the polymerization, various additives such as a radical polymerization initiator, a polymerization chain transfer agent, and a RAFT agent can be used. As the radical polymerization initiator, for example, an azo compound such as 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl-2,2'-azobisbutyrate, 2,2'-azobis(2-methylbutyronitrile), and 1,1'-azobis(1-cyclohexanecarbonitrile) can be preferably used. In addition, as the radical polymerization initiator, an organic peroxide such as t-butyl peroxyoctoate, di-t-butyl peroxide, and dibenzoyl oxide can be used. The amount of the radical polymerization initiator to be added is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the monomer.
[0060] Examples of the polymerization chain transfer agent include mercaptans such as octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-tetradecyl mercaptan, and 2-mercaptoethanol; xanthogen disulfides such as dimethyl xanthogen disulfide and diisopropyl xanthogen disulfide; thiuram disulfides such as tetramethyl thiuram disulfide and tetrabutyl thiuram disulfide; halogens such as carbon tetrachloride and ethylene bromide; Examples of unsaturated cyclic hydrocarbon compounds include: fluorinated hydrocarbons; hydrocarbons such as pentaphenylethane; unsaturated cyclic hydrocarbon compounds such as acrolein, methacrolein, allyl alcohol, 2-ethylhexylthioglycolate, turbinolene, α-terpinene, γ-terpinene, dipentene, α-methylstyrene dimer, 9,10-dihydroanthracene, 1,4-dihydronaphthalene, indene, and 1,4-cyclohexadiene; and unsaturated heterocyclic compounds such as 2,5-dihydrofuran.
[0061] The polymerization conditions can be appropriately adjusted depending on the monomers used, additives such as a radical polymerization initiator, the polymerization solvent, etc. Usually, the polymerization temperature is preferably 30 to 120°C, more preferably 50 to 100°C. The polymerization time is preferably 10 minutes to 20 hours, more preferably 1 hour to 10 hours. The reaction atmosphere is preferably a non-oxidizing atmosphere, more preferably an inert atmosphere, specifically, a nitrogen atmosphere, an argon atmosphere, etc.
[0062] The weight average molecular weight of the polymer compound is not particularly limited, but the weight average molecular weight (Mw) of the polymer compound before the crosslinking reaction is preferably 10,000 to 300,000, more preferably 20,000 to 200,000, and even more preferably 30,000 to 100,000. When the weight average molecular weight of the polymer compound before the crosslinking reaction is 10,000 or more, a sufficient interparticle repulsion effect can be obtained, and the storage stability can be maintained better. When the weight average molecular weight of the polymer compound before the crosslinking reaction is 100,000 or less, the increase in the ink viscosity of the aqueous ink using this aqueous pigment dispersion can be suppressed, and the ejection property can be further improved. Here, the weight average molecular weight of the polymer compound before the crosslinking reaction is a value obtained by gel permeation chromatography (GPC) method in terms of standard polystyrene.
[0063] After synthesis of the polymer compound, the composition containing the polymer compound may be used as it is as an aqueous pigment dispersion, or the composition containing the polymer compound may be subjected to solvent removal or solvent replacement and optionally purified before being used as a part of the aqueous pigment dispersion.
[0064] As the pigment, organic pigments such as azo pigments, phthalocyanine pigments, polycyclic pigments, and dye lake pigments, and inorganic pigments such as carbon black and metal oxides can be used. As the azo pigment, soluble azo lake pigments, insoluble azo pigments, and condensed azo pigments can be used. As the phthalocyanine pigment, metal phthalocyanine pigments and metal-free phthalocyanine pigments can be used. As the polycyclic pigment, quinacridone pigments, perylene pigments, perinone pigments, isoindoline pigments, isoindolinone pigments, dioxazine pigments, thioindigo pigments, anthraquinone pigments, quinophthalone pigments, metal complex pigments, and diketopyrrolopyrrole (DPP) can be used. As the carbon black, furnace carbon black, lamp black, acetylene black, channel black, and the like can be used. As the metal oxide, titanium oxide and zinc oxide can be used.
[0065] From the viewpoints of ejection property and dispersion stability, the average particle size of the pigment is preferably 300 nm or less, and more preferably 200 nm or less. Here, the average particle size of the pigment is the average particle size on a volume basis, and is a value measured by a dynamic light scattering method.
[0066] The pigment may be used alone or in combination of two or more kinds. The content of the pigment is not particularly limited, but is preferably 1 to 30 mass %, more preferably 5 to 25 mass %, and further preferably 10 to 20 mass %, based on the total mass of the aqueous pigment dispersion.
[0067] The aqueous pigment dispersion may contain water. The water is not particularly limited, but is preferably one that does not contain ionic components as much as possible. In particular, from the viewpoint of pigment dispersion stability, it is preferable that the content of polyvalent metal ions such as calcium is small. As the water, for example, ion-exchanged water, distilled water, ultrapure water, etc. may be used.
[0068] The amount of water is not particularly limited, but is preferably 20 to 90% by mass, more preferably 40 to 80% by mass, and even more preferably 50 to 70% by mass, based on the total mass of the aqueous pigment dispersion.
[0069] The aqueous pigment dispersion may further contain a water-soluble organic solvent. For example, the water-soluble organic solvent may be a water-soluble organic solvent used in the synthesis of the polymer compound. The water-soluble organic solvent may be a water-soluble organic solvent that can be used in an aqueous ink, which will be described later. The water-soluble organic solvent is not particularly limited, and may be 0.1 to 30% by mass, 1 to 20% by mass, or 5 to 10% by mass relative to the total mass of the aqueous pigment dispersion.
[0070] The mixture can be obtained by mixing the polymer compound, the pigment, and water. The mixture may further contain optional additives such as a water-soluble organic solvent and a neutralizing agent.
[0071] A method of adding a polyfunctional compound having multiple (meth)acryloyl groups to the above mixture in the presence of a base is described below. By reacting a polymer compound with a polyfunctional compound in the presence of a base, the β-dicarbonyl groups of the polymer compound and the (meth)acryloyl groups of the polyfunctional compound selectively react with each other, making it possible to form a crosslinked structure on the surface of the pigment starting from the β-dicarbonyl groups.
[0072] A polyfunctional compound having a plurality of (meth)acryloyl groups is a compound having two or more (meth)acryloyl groups, and the number of (meth)acryloyl groups in one molecule may be 2 to 10, 2 to 6, or 2 to 4. A polyfunctional compound having two or three (meth)acryloyl groups is more preferred, and a polyfunctional compound having two (meth)acryloyl groups is even more preferred. Here, the number of functional groups in a polyfunctional compound is the number of (meth)acryloyl groups in one molecule.
[0073] The polyfunctional compound is preferably a polyfunctional (meth)acrylate compound having a plurality of (meth)acryloyloxy groups. Examples of the polyfunctional (meth)acrylate compound include a bifunctional (meth)acrylate compound, a trifunctional (meth)acrylate compound, a tetrafunctional (meth)acrylate compound, and a pentafunctional or higher polyfunctional (meth)acrylate compound.
[0074] The polyfunctional (meth)acrylate compound is preferably a low molecular weight compound. The molecular weight of the polyfunctional (meth)acrylate compound is preferably less than 1000, and may be 100 to 800 or 200 to 500. The polyfunctional (meth)acrylate compound may be either a monomer or an oligomer, but is preferably a monomer.
[0075] Examples of the polyfunctional (meth)acrylate compound include esters of polyhydric alcohols such as diols, triols, tetraols, and polyalkylene glycols with (meth)acrylic acid. In particular, the moiety derived from the polyhydric alcohol is preferably a hydrocarbon group, a hydrocarbon group having an ether bond, or a combination thereof. As the hydrocarbon group, a linear or branched, chain or alicyclic alkyl group is preferred, and a linear or branched chain alkyl group is more preferred. As the hydrocarbon group having an ether bond, an oxyalkylene group, a polyoxyalkylene group, or the like may be used.
[0076] Examples of bifunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,3-propanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, decamethylene glycol (meth)acrylate, 1,12-dodecanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, 4,4'-biphenol di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, 2-hydroxy-3-methacrylpropyl acrylate, and the like.
[0077] Examples of trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerin tri(meth)acrylate, ethoxylated glycerin tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, and tris-2-hydroxyethyl isocyanurate tri(meth)acrylate.
[0078] Examples of tetrafunctional or higher polyfunctional (meth)acrylates include pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, ditrimethylolpropane hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and the like.
[0079] Among them, alkylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylic, trimethylolpropane tri(meth)acrylate, or a combination thereof is preferred, and polyalkylene glycol di(meth)acrylate is more preferred. More specifically, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylic, trimethylolpropane tri(meth)acrylate, or a combination thereof is preferred, and polyethylene glycol di(meth)acrylate is more preferred. The number of moles added of polyethylene glycol di(meth)acrylate is preferably 2 to 6, more preferably 3 to 5, and may be 4 on average in the mixture of polyethylene glycol di(meth)acrylate.
[0080] Examples of commercially available products include Kyoei Chemical Co., Ltd.'s Light Acrylate "Light Acrylate 4EG-A" (PEG#200 dimethacrylate), Light Acrylate "Light Ester 4EG" (PEG200# diacrylate), and Light Acrylate "Light Acrylate TMP-A" (trimethylolpropane triacrylate).
[0081] The polyfunctional compound having a plurality of (meth)acryloyl groups may be a polyfunctional (meth)acrylamide compound having a plurality of (meth)acryloyl groups. Examples of the polyfunctional (meth)acrylamide compound include bifunctional (meth)acrylamide compounds such as methylene diacrylamide and ethylene bisacrylamide, and trifunctional (meth)acrylamide compounds such as bis(2-acrylamidoethyl)acrylamide. Examples of commercially available polyfunctional (meth)acrylamide compounds include "FOM-03006, FOM-03007, FOM-03008, FOM-03009" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0082] The polyfunctional compound having a plurality of (meth)acryloyl groups may be used alone or in combination of two or more kinds.
[0083] The base may be either an inorganic base or an organic base. Examples of the base include inorganic bases such as ammonium hydroxide, sodium hydroxide, potassium hydroxide, sodium hydrogen carbonate, potassium carbonate, and calcium carbonate; and amines such as aminomethylpropanol, aminoethylpropanol, dimethylethanolamine, triethylamine, diethylethanolamine, dimethylaminopropanol, triethanolamine, diazabicyclononene, and diazabicycloundecene. The base may be used alone or in combination of two or more.
[0084] Among them, the inorganic base is preferably a carbonate, specifically, potassium carbonate, calcium carbonate, etc. The organic base is preferably a nitrogen-containing base, more preferably a tertiary amine, specifically, triethylamine, diazacyclononene, etc.
[0085] As a method for adding the polyfunctional compound to the mixture in the presence of a base, for example, a base and a polyfunctional compound can be added to the mixture and heated to carry out a crosslinking reaction.
[0086] In the aqueous pigment dispersion, it is preferable that the degree of crosslinking, which is expressed by the ratio of the (meth)acryloyl groups of a polyfunctional compound having a plurality of (meth)acryloyl groups to the β-dicarbonyl groups of a polymer compound, satisfies the following formula. Degree of crosslinking = (molar concentration of (meth)acryloyl groups) / (molar concentration of β-dicarbonyl groups)) x 100 = 50 to 200 (%)
[0087] When the degree of crosslinking is 200 mol% or less, 150 mol% or less, or 100 mol% or less, crosslinking between pigment particles is suppressed, and aggregation of the pigment is prevented, so that storage stability can be further improved. When the degree of crosslinking is 50 mol% or more, 80 mol% or more, or 90 mol% or more, coverage of the pigment with the polymer compound is promoted, and storage stability can be further improved. For example, the degree of crosslinking is preferably 50 to 200 mol%, 80 to 150 mol%, or 90 to 100 mol%. The degree of crosslinking is preferably in the range of 50 to 200 mol%, but may be 10 to 500 mol%, or may be 30 to 250 mol%.
[0088] The content of the polyfunctional compound having a plurality of (meth)acryloyl groups is preferably 0.1 to 10 mass%, 0.5 to 5 mass%, or 1 to 2 mass% based on the total mass of the aqueous pigment dispersion. The content of the base is preferably 0.1 to 5 mass%, 0.3 to 2 mass%, or 0.5 to 1 mass% based on the total mass of the aqueous pigment dispersion. The content of the base here does not include the content of the neutralizing agent used for neutralizing the polymer compound.
[0089] (Method of manufacturing water-based inkjet ink) A method for producing an aqueous pigment dispersion according to one embodiment is characterized in that it includes producing an aqueous pigment dispersion according to the production method of the embodiment described above, and adding a water-soluble organic solvent and a surfactant to the aqueous pigment dispersion.
[0090] According to one embodiment, it is possible to provide a method for producing an aqueous inkjet ink that can provide an ink having excellent storage stability.
[0091] The aqueous ink is produced using an aqueous pigment dispersion. The aqueous ink is produced by adding a water-soluble organic solvent and a surfactant to the aqueous pigment dispersion. The aqueous ink may be produced by using the aqueous pigment dispersion as is, or may be produced by adding water to the aqueous pigment dispersion. The water-soluble organic solvent may be one or both of a highly polar water-soluble organic solvent and a low polar water-soluble organic solvent. The components that the aqueous ink may contain are described below.
[0092] The aqueous ink may contain water. The water is contained in the aqueous pigment dispersion, but may be added additionally to the aqueous pigment dispersion. From the viewpoint of adjusting the viscosity of the aqueous ink, the water is contained in an amount of preferably 20 to 90% by mass, more preferably 40 to 80% by mass, and even more preferably 50 to 70% by mass, based on the total mass of the aqueous ink.
[0093] The water-based ink may contain a water-soluble organic solvent. The water-soluble organic solvent is preferably compatible with water. As the water-soluble organic solvent, an organic compound that is liquid at room temperature and can be dissolved or mixed in water may be used from the viewpoint of wettability and moisture retention, and it is preferable to use a water-soluble organic solvent that can be uniformly mixed with the same volume of water at 20°C under 1 atmosphere.
[0094] The boiling point of the water-soluble organic solvent is preferably 170 to 250° C. When the boiling point of the water-soluble organic solvent is 170° C. or higher, more preferably 200° C. or higher, the evaporation of the water-soluble organic solvent from the aqueous ink can be suppressed, and the on-press stability can be further improved. When the boiling point of the water-soluble organic solvent is 250° C. or lower, the drying property of the printed matter can be further improved.
[0095] Examples of the water-soluble organic solvent include glycols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,2-hexanediol; glycerins such as glycerin, diglycerin, triglycerin, and polyglycerin; acetins such as monoacetin and diacetin; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene Glycol ethers such as glycol monopropyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol mono-n-butyl ether, tetraethylene glycol monomethyl ether, tetraethylene glycol monoethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-butyl ether; 1-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, β-thiodiglycol, sulfolane, trimethylolpropane, etc. The water-soluble organic solvent may be used alone or in combination of two or more as long as it forms a single phase.
[0096] From the viewpoints of wettability, moisturizing effect, and adjustment of ink viscosity, the water-soluble organic solvent is preferably contained in an amount of 1 to 80 mass % relative to the total amount of the ink, more preferably 10 to 50 mass %, and even more preferably 20 to 40 mass %.
[0097] Although it depends on the material of the substrate, the aqueous ink does not wet the substrate well, and may not be sufficiently fixed to the substrate surface, and may even be repelled from the substrate surface. Examples of the aqueous ink include non-permeable substrates such as plastic substrates and metal substrates. From the viewpoint of enabling printing on such substrates, it is preferable that the aqueous ink contains a low-polarity water-soluble organic solvent. On the other hand, since some resins are soluble in low-polarity water-soluble organic solvents, there is a problem that the resin used as the pigment dispersant dissolves in the solvent. However, as described above, the aqueous pigment dispersion according to one embodiment is designed such that the polymer compound is less likely to dissolve in general solvents including low-polarity water-soluble organic solvents due to the crosslinked structure, and therefore it is possible to use the aqueous pigment dispersion in combination with various water-soluble organic solvents. From this viewpoint, it is possible to use a low-polarity water-soluble organic solvent so as to be compatible with various substrates.
[0098] The low polarity water-soluble organic solvent is preferably a lower alkyl ether of a polyhydric alcohol having 1 to 4 carbon atoms, and is preferably an n-butyl ether of a polyhydric alcohol. For example, the water-soluble organic solvent is preferably ethylene glycol mono-n-butyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol mono-n-butyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol mono-n-butyl ether, etc. The lower alkyl ether of a polyhydric alcohol having 1 to 4 carbon atoms may be used alone or in combination of two or more.
[0099] The SP value is an index of polarity of a water-soluble organic solvent. In one embodiment, a water-soluble organic solvent with a low polarity has an SP value of 13 (cal / cm 3 ) 1 / 2 Below, 12 (cal / cm 3 ) 1 / 2The following water-soluble organic solvents can be used. It is preferable to use a water-soluble organic solvent with low polarity from among the above so as to satisfy this SP value range. From the viewpoint of compatibility with water, the SP value of the water-soluble organic solvent is 7 (cal / cm 3 ) 1 / 2 More than 8 (cal / cm 3 ) 1 / 2 More preferably, the SP value is 13 (cal / cm 3 ) 1 / 2 From the viewpoint of wettability to the substrate, the amount of the low-polarity water-soluble organic solvent is preferably 1 to 30 mass %, more preferably 5 to 25 mass %, and even more preferably 10 to 20 mass %, relative to the total amount of the water-based ink.
[0100] In this specification, the SP value is the SP value calculated by the Fedors formula, specifically, the value calculated by the following formula proposed by Fedors, where Δei is the evaporation energy of an atom or atomic group of the i component, and Δvi is the molar volume of an atom or atomic group of the i component (see Hansen Solubility Parameters: A User's Handbook, Second Edition, Charles M. Hansen, CRC Press, 2007). δ = [(sumΔei) / (sumΔvi)] 1 / 2
[0101] The aqueous ink may further contain a surfactant. The surfactant can further increase the permeability or wettability of the ink into the substrate and further improve the coatability of the ink. As the surfactant, a nonionic surfactant, an anionic surfactant, a cationic surfactant, an amphoteric surfactant, or a combination thereof can be preferably used, and it is more preferable that the aqueous ink contains a nonionic surfactant.
[0102] Examples of nonionic surfactants include silicone surfactants, acetylene glycol surfactants, fluorine surfactants, polyoxyethylene alkyl ether surfactants, polyoxypropylene alkyl ether surfactants, polyoxyethylene alkyl phenyl ether surfactants, polyoxypropylene alkyl phenyl ether surfactants, polyoxyethylene fatty acid ester surfactants, polyoxypropylene fatty acid ester surfactants, sorbitan fatty acid ester surfactants, polyoxyethylene sorbitan fatty acid ester surfactants, polyoxyethylene sorbitol fatty acid ester surfactants, glycerin fatty acid ester surfactants, etc. The nonionic surfactants may be used alone or in combination of two or more.
[0103] The nonionic surfactant preferably includes a silicone surfactant, an acetylene glycol surfactant, or a combination thereof. Commercially available silicone surfactants include, for example, "Silface SAG014" and "Silface SAG002" (trade names, manufactured by Nissin Chemical Industry Co., Ltd.). Commercially available acetylene glycol surfactants include, for example, acetylene glycols "Olfine E1010", "Olfine E1020", and "Surfinol 440" (all trade names, manufactured by Nissin Chemical Industry Co., Ltd.).
[0104] The amount of the surfactant in terms of active ingredient is preferably 0.1 to 5 mass %, and more preferably 0.2 to 2 mass %, relative to the total amount of the water-based ink.
[0105] In addition to the components described above, the aqueous ink may optionally contain various additives such as a pH adjuster, an antifoaming agent, a wetting agent (moisturizing agent), a surface tension adjuster (penetration agent), a preservative, a fixing agent, and an antioxidant.
[0106] The suitable range of viscosity of the aqueous ink varies depending on the nozzle diameter of the ejection head of the inkjet recording system, the ejection environment, etc., but in general, it is preferably 1 to 12 mPa·s, more preferably 5 to 10 mPa·s, and even more preferably 8 to 10 mPa·s at 23° C. The viscosity of the aqueous ink can be measured using a rotational viscometer.
[0107] The method of forming an image on a substrate using an aqueous inkjet ink can be performed using an inkjet printing method. The inkjet printing method can easily and freely form an image on demand without contacting the substrate. The inkjet printing method is not particularly limited, and may be any method such as a piezo method, an electrostatic method, or a thermal method. For example, ink can be ejected from an inkjet head based on a digital signal, and the ejected ink droplets can be attached to the substrate.
[0108] The aqueous inkjet ink according to one embodiment may be used for printing on an untreated substrate, or may be used for printing on a substrate that has been treated with a pretreatment liquid. The pretreatment liquid preferably contains, for example, one or both of water and a water-soluble organic solvent, and a surfactant, a flocculant, inorganic particles, etc., either singly or in combination of two or more thereof.
[0109] After printing the aqueous ink on the substrate, a step of post-treating the substrate to form an overcoat layer may be further provided. The method of post-treating the substrate may be performed by applying a post-treatment liquid to the substrate. As the post-treatment liquid, for example, a post-treatment liquid containing a resin capable of forming a film and an aqueous solvent or an oil-based solvent may be used.
[0110] The aqueous inkjet ink according to an embodiment can use a low-polarity water-soluble organic solvent while maintaining good storage stability, and can have wettability to a substrate. Therefore, it is possible to form a good image on an untreated substrate, and further, it is possible to form a good image on an untreated non-permeable substrate. In addition, since the aqueous ink according to an embodiment contains a low-polarity water-soluble organic solvent, it is possible to further increase the fixability of the image to the substrate, making post-processing after printing unnecessary.
[0111] The aqueous ink can be applied to both permeable and non-permeable substrates. The non-permeable substrate is a substrate in which the liquid does not permeate into the substrate, specifically, a substrate in which most of the liquid in the aqueous ink remains on the surface of the substrate. Examples of the non-permeable substrate include metal substrates such as metal plates of aluminum, iron, copper, titanium, tin, chromium, cadmium, alloys (e.g., stainless steel, steel, etc.); glass substrates such as plate glass such as borosilicate glass, quartz glass, and soda lime glass; resin substrates such as polyester film, polypropylene (PP) film, overhead transparent sheet (OHT sheet), polyester sheet, and polypropylene sheet; resin substrates such as acrylic plate and polyvinyl chloride plate; ceramic substrates such as molded bodies of alumina, zirconia, steatite, and silicon nitride. These substrates may have a plating layer, a metal oxide layer, a resin layer, etc. formed thereon, or may be surface-treated using a corona treatment or the like.
[0112] Examples of permeable substrates include printing paper such as plain paper, coated paper, and special paper; fabrics such as woven fabrics, knitted fabrics, and nonwoven fabrics; porous building materials for humidity control, sound absorption, and heat insulation; wood, concrete, and porous materials. Plain paper is paper on which an ink receiving layer or a film layer is not formed. Examples of plain paper include fine paper, medium-quality paper, plain paper copy paper (PPC paper), wood paper, and recycled paper. In addition, as coated paper, inkjet coated paper such as matte paper, glossy paper, and semi-glossy paper, and so-called coated printing paper can be preferably used. Here, coated printing paper is printing paper that has been used conventionally in letterpress printing, offset printing, gravure printing, and the like, and is printing paper in which a coating layer is provided on the surface of fine paper or medium-quality paper using a paint containing an inorganic pigment such as clay or calcium carbonate and a binder such as starch. Coated printing paper is classified into lightly coated paper, high-quality lightweight coated paper, medium-quality lightweight coated paper, high-quality coated paper, medium-quality coated paper, art paper, cast coated paper, etc., depending on the amount of paint applied and the coating method.
[0113] Examples of fibers that make up the fabric include at least one type selected from various fibers such as inorganic fibers such as metal fibers, glass fibers, rock fibers, and silicic fibers; regenerated fibers such as cellulose-based and protein-based fibers; semi-synthetic fibers such as cellulose-based fibers; synthetic fibers such as polyamide, polyester, polyvinyl chloride, polyvinylidene chloride, polyacrylonitrile, polyvinyl alcohol, polyurethane, polyethylene, polypropylene, polystyrene, and polyethylene fluoride; and natural fibers such as cotton, hemp, silk, and wool.
[0114] According to one embodiment, it is possible to provide a method for producing a printed material by producing an aqueous inkjet ink according to the manufacturing method of the above-described embodiment and applying the aqueous inkjet ink to a substrate by an inkjet method to produce a printed material.
[0115] (Other embodiments) According to another embodiment, there can be provided an aqueous pigment composite comprising a pigment, a polymeric compound, and a polyfunctional compound having a plurality of (meth)acryloyl groups, the polymeric compound comprising a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group, the polymeric compound being adsorbed to the pigment, and the polyfunctional compound having a plurality of (meth)acryloyl groups being bonded to the β-dicarbonyl group of the polymeric compound on the surface of the pigment to form a crosslinked structure, as described above in detail.
[0116] According to yet another embodiment, an aqueous pigment dispersion containing the above-mentioned pigment complex and water can be provided. A water-soluble organic solvent, a surfactant, and other components can be added to this aqueous pigment dispersion to provide an aqueous ink. Details are as described above.
[0117] The present disclosure includes the following embodiments. <1> A method for producing an aqueous pigment dispersion includes adding a polyfunctional compound having a plurality of (meth)acryloyl groups to a mixture containing a polymer compound, a pigment, and water in the presence of a base, the polymer compound including a β-dicarbonyl group, and at least one of a carboxy group and a sulfonic acid group.
[0118] <2> a crosslinking degree represented by a ratio of the (meth)acryloyl groups of the polyfunctional compound having a plurality of (meth)acryloyl groups to the β-dicarbonyl groups of the polymer compound satisfies the following formula: <1> 13. A method for producing the aqueous pigment dispersion according to claim 12. Degree of crosslinking = (molar concentration of (meth)acryloyl groups) / (molar concentration of β-dicarbonyl groups)) x 100 = 50 to 200 (%)
[0119] <3> a crosslinking reaction between the polymer compound and the polyfunctional compound having a plurality of (meth)acryloyl groups in a state in which the polymer compound is adsorbed on the pigment; <1> or <2> 13. A method for producing the aqueous pigment dispersion according to claim 12.
[0120] <4> the above <1> from <3> and adding a water-soluble organic solvent and a surfactant to the aqueous pigment dispersion.
[0121] <5> A pigment complex comprising a pigment, a polymeric compound, and a polyfunctional compound having a plurality of (meth)acryloyl groups, wherein the polymeric compound comprises a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group, the polymeric compound is adsorbed onto the pigment, and the polyfunctional compound having a plurality of (meth)acryloyl groups is bonded to the β-dicarbonyl group of the polymeric compound on the surface of the pigment to form a crosslinked structure. EXAMPLES
[0122] The present invention will be described in detail below with reference to examples. The present invention is not limited to the following examples. In the following description, "%" means "mass %" unless otherwise specified. The content shown in each table is the total amount of the solution or dispersion of the component blended as a solution or dispersion. In each table, "-" means not added or not measured.
[0123] (Method of synthesizing polymer compounds) Table 1 shows the synthesis recipe for the polymer compounds. The monomers, solvents, and chain transfer agents shown in the table were placed in a four-neck flask, and nitrogen was bubbled through at room temperature for 30 minutes to replace the dissolved oxygen in the liquid with nitrogen. Then, a polymerization initiator was added, and the mixture was heated and stirred at 70°C for 6 hours. The solvent was then removed using an evaporator to obtain polymer compounds. The weight-average molecular weight of the obtained polymer compounds was about 30,000 in each case.
[0124] The components used are as follows: Monomer (A): acrylic acid, 2-sulfoethyl methacrylate, methacrylic acid: all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Monomer (B): AAEM: ethylene glycol monoacetoacetate monomethacrylate, manufactured by Tokyo Chemical Industry Co., Ltd. Monomer (C1): A-LEN-10 (product name): ethoxylated phenylphenol acrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. Monomer (C1): benzyl methacrylate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Monomer (C2): Plenmer PME-1000 (product name): methoxypolyethylene glycol methacrylate, manufactured by NOF Corporation. Monomer (C2): Plenmer PME-400 (product name): methoxypolyethylene glycol methacrylate, manufactured by NOF Corporation. Monomer (C3): Butyl methacrylate: Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0125] The polymerization initiator AIBN (2,2'-azobisbutyronitrile) and the chain transfer agent lauryl mercaptan are both available from Tokyo Chemical Industry Co., Ltd. The solvent 2-propanol is available from Fujifilm Wako Pure Chemical Corporation.
[0126] [Table 1]
[0127] (Method of Preparing Water-Based Pigment Dispersion) Tables 2 to 4 show the formulations of the aqueous pigment dispersions and inks. The pigment (1-1), polymer compound (1-2), water (1-6) of the pigment dispersion formulation, and neutralizing agent shown in the tables were placed in a stirring vessel together with zirconia beads, and dispersed for 3 hours with a rocking mill to obtain a pre-pigment dispersion. After filtering off the zirconia beads, the pre-pigment dispersion was transferred to a glass bottle, and the multifunctional (meth)acrylate compound (1-3) and base shown in the tables were added, and the mixture was heated and stirred with a magnetic stirrer to cause a crosslinking reaction to obtain an aqueous pigment dispersion. The neutralizing agent was used in an amount that would result in a neutralization degree of 100% for the carboxyl groups of the aqueous pigment dispersion. In Comparative Examples 1 and 5, a monofunctional (meth)acrylate compound (1-4) and a multifunctional epoxy compound (1-5) were used instead of the multifunctional (meth)acrylate compound (1-3), respectively.
[0128] The degree of crosslinking shown in the table was calculated from the molar concentration of the (meth)acryloyl group of the polyfunctional (meth)acrylate compound relative to the molar concentration of the β-dicarbonyl group of the polymer compound, using the following formula: In Comparative Example 1, the (meth)acryloyl group of the monofunctional acrylate was used instead of the (meth)acryloyl group of the polyfunctional (meth)acrylate compound, and in Comparative Example 5, the epoxy group of the polyfunctional epoxy was used instead of the (meth)acryloyl group of the polyfunctional (meth)acrylate compound. Degree of crosslinking = ((molar concentration of (meth)acryloyl groups) / (molar concentration of β-dicarbonyl groups)) x 100
[0129] (How to make water-based ink) To the aqueous pigment dispersion obtained above, the highly polar water-soluble organic solvent (2-1), the low polarity water-soluble organic solvent (2-2), the surfactant (2-3), and the water (2-4) of the ink formulation shown in the table were added, and the mixture was filtered through a filter to obtain an aqueous ink.
[0130] The components used are as follows: (1-1: Pigment) MA8: Carbon black pigment, manufactured by Mitsubishi Chemical Corporation. Chromofine 4927: Copper phthalocyanine pigment, manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd. FASTOGEN® SUPER MAGENTA R: quinacridone pigment, manufactured by DIC Corporation. Hansa Brilliant Yellow 5GX: Condensed disazo pigment, manufactured by Clariant. #45: Carbon black pigment, manufactured by Mitsubishi Chemical Corporation.
[0131] (1-2: Polymer compound): The polymer compound synthesized above was used. Solid content: 100% by mass. (1-3: Multifunctional (meth)acrylate compound) Trifunctional acrylate: "Light Acrylate TMP-A" manufactured by Kyoei Chemical Co., Ltd. Bifunctional acrylate: "Light Acrylate 4EG-A" manufactured by Kyoei Chemical Co., Ltd. Bifunctional methacrylate: "Light Ester 4EG" manufactured by Kyoei Chemical Co., Ltd. (1-4: Monofunctional (meth)acrylic compound) Monofunctional acrylate: "Light Acrylate MTG-A" manufactured by Kyoei Chemical Co., Ltd. (1-5: Multifunctional epoxy compound) Multifunctional epoxy: "Denacol EX-521" manufactured by Nagase ChemteX Corporation.
[0132] The neutralizing agent used was sodium hydroxide, and the bases used were calcium carbonate and diazabicyclononene ("DBN" manufactured by San-Apro Co., Ltd.).
[0133] (2-1: Highly polar water-soluble organic solvent) Trimethylolpropane: SP value = 16.38 (cal / cm 3 ) 1 / 2 , manufactured by Fujifilm Wako Pure Chemical Corporation. (2-2: Low polarity water-soluble organic solvent) 1,2-Hexanediol: SP value = 11.8 (cal / cm 3 ) 1 / 2 Manufactured by Tokyo Chemical Industry Co., Ltd. Diethylene glycol monobutyl ether: SP value = 10.51 (cal / cm 3 ) 1 / 2 Manufactured by Tokyo Chemical Industry Co., Ltd. (2-3: Surfactant) Surfynol 440 (product name): acetylene glycol surfactant, manufactured by Nissin Chemical Industry Co., Ltd.
[0134] (Evaluation method) "Molecular weight of polymer compounds" The weight-average molecular weight of the resulting polymer compound was measured by gel permeation chromatography (GPC) as follows. The weight average molecular weight (Mw) of the polymer compound was measured by GPC using a RID (refractive index detector) under the following conditions: standard material: polystyrene, solvent: 10 mM lithium bromide and 50 mM phosphate-containing N-methylpyrrolidone, flow rate: 0.7 ml / min. The measuring instrument used was the "LC-10A series" manufactured by Shimadzu Corporation, and the column used was Shodex GPC KF-804 (Resonac Corporation). The results are shown in Table 1.
[0135] "Storage stability evaluation" First, the viscosity of the ink was measured immediately after the ink was prepared. Next, the ink was placed in a sealed container and left in an environment of 70°C for 4 weeks. After that, the viscosity of the ink was measured and the viscosity change rate was calculated according to the following formula. Then, the storage stability was evaluated according to the following criteria. The ink viscosity was measured at 23°C using an Anton Paar rheometer "MCR302" (cone angle 1°, diameter 50 mm). The results are shown in Tables 2 to 4. Viscosity change rate: [((viscosity after 4 weeks)-(initial viscosity)) / (initial viscosity)] x 100(%)
[0136] AA: Absolute value of viscosity change rate is 5% or less. A: The absolute value of the viscosity change rate is more than 5% and less than 10%. B: The absolute value of the viscosity change rate exceeds 10%, or the ink has gelled and cannot be measured.
[0137] "Printing Evaluation" Using the obtained ink, a print was produced under the following conditions. Printer: Shuttle printer with a piezo printhead with a resolution of 300 npi. Printing substrate: PVC substrate, Avery Dennison MPI3002P WPE. Printing conditions: Resolution: 1200 x 600 dpi, Image: 30cm x 30cm square solid image. The image quality of the obtained prints was visually observed and evaluated according to the following criteria. The results are shown in Tables 2 to 4.
[0138] A: A uniform solid layer is formed. B: Unevenness occurs. C: Poor ejection has occurred and printing cannot be performed correctly.
[0139] [Table 2]
[0140] [Table 3]
[0141] [Table 4]
[0142] As shown in each table, the ink of each example had good storage stability. Furthermore, the prints produced using the ink of each example had good image quality.
[0143] It can be seen from Examples 1 to 8 that the ink storage stability and the image quality of the printed matter are good for various solvents and various pigments. In addition, the ink contains a low polarity solvent, which improves the wettability to the PVC substrate, reduces unevenness in the printed matter, and improves the image quality of the printed matter. It can be seen from Examples 9 to 13 that the ink storage stability and the image quality of the printed matter are good for various bases and various polyfunctional (meth)acrylate compounds and their amounts used. It can be seen from Examples 14 to 16 that the ink storage stability and the image quality of the printed matter are good even when different monomer types are used in the synthesis of the polymer compound.
[0144] In Comparative Example 1, a monofunctional (meth)acrylate compound was used in the aqueous pigment dispersion, and a crosslinked structure was not formed, so the polymer compound was detached from the pigment, which is considered to have deteriorated the storage stability. In Comparative Example 2, the aqueous pigment dispersion did not contain a (meth)acrylate compound, and the storage stability was deteriorated. In Comparative Example 3, the monomer mixture did not contain monomer (A) in the synthesis of the polymer compound, and the electrostatic repulsion in the ink decreased, and the storage stability decreased. In Comparative Example 3, the dispersibility also decreased, and therefore non-ejection occurred in the inkjet ejection. In Comparative Example 4, the monomer mixture did not contain monomer (B) in the synthesis of the polymer compound, and the crosslinked structure was difficult to form in the aqueous pigment dispersion, and the pigment adsorption force also decreased, and the storage stability of the ink decreased. In Comparative Example 5, the polymer compound was an epoxy compound, and the crosslinked structure was different, and the storage stability of the ink decreased.
Claims
1. The method includes adding a polyfunctional compound having a plurality of (meth)acryloyl groups to a mixture containing a polymer compound, a pigment, and water in the presence of a base, The polymer compound contains a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group.
2. 2. The method for producing an aqueous pigment dispersion according to claim 1, wherein a degree of crosslinking represented by a ratio of (meth)acryloyl groups of the polyfunctional compound having a plurality of (meth)acryloyl groups to β-dicarbonyl groups of the polymer compound satisfies the following formula: Degree of crosslinking=(molar concentration of (meth)acryloyl groups) / (molar concentration of β-dicarbonyl groups)×100=50 to 200(%)
3. The method for producing an aqueous pigment dispersion according to claim 1 , wherein the polymer compound is crosslinked with the polyfunctional compound having a plurality of (meth)acryloyl groups in a state in which the polymer compound is adsorbed on the pigment.
4. A method for producing an aqueous inkjet ink, comprising: producing the aqueous pigment dispersion according to the method of claim 1 ; and adding a water-soluble organic solvent and a surfactant to the aqueous pigment dispersion.
5. A pigment complex comprising a pigment, a polymer compound, and a polyfunctional compound having a plurality of (meth)acryloyl groups, the polymer compound contains a β-dicarbonyl group and at least one of a carboxy group and a sulfonic acid group, the polymer compound is adsorbed to the pigment, and the polyfunctional compound having a plurality of (meth)acryloyl groups is bonded to the β-dicarbonyl group of the polymer compound on the surface of the pigment to form a crosslinked structure.
Citation Information
Patent Citations
Water-based inkjet ink and pigment complex
JP2022135519A