Nitride semiconductor element and manufacturing method of nitride semiconductor element
The nitride semiconductor device addresses cladding layer deterioration and carrier injection efficiency issues by employing a second conductivity type cladding layer with a discontinuous impurity concentration profile, enhancing device performance.
Patent Information
- Application Number
- JP2023056078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Niride semiconductor devices, such as laser diodes, suffer from insufficient suppression of cladding layer deterioration and suboptimal carrier injection efficiency.
A nitride semiconductor device with a second conductivity type cladding layer having a discontinuous concentration profile of carbon or oxygen, formed under specific temperature and pressure conditions, to improve carrier injection efficiency while suppressing cladding layer deterioration.
The solution effectively suppresses cladding layer deterioration and enhances carrier injection efficiency, resulting in improved performance of nitride semiconductor devices.
Smart Images

Figure 2024143415000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nitride semiconductor device and a method for manufacturing a nitride semiconductor device. [Background technology]
[0002] Conventionally, nitride semiconductors have been used as materials for forming light emitting diodes (LEDs) and laser diodes (LDs). Nitride semiconductors have a direct transition recombination mode, and therefore are suitable as materials for LEDs and LDs in that they can provide high recombination efficiency and high optical gain. As an example of a laser diode using such a nitride semiconductor, a technology for oscillating a current injection type laser diode in the ultraviolet region has been disclosed (for example, Non-Patent Document 1). [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] Zhang et at., Applied Physics Express 12, 124003(2019) Summary of the Invention [Problem to be solved by the invention]
[0004] Although the nitride semiconductor devices such as the laser diodes described above can improve the efficiency of carrier (electron or hole) injection, they do not sufficiently suppress deterioration of the cladding layer. An object of the present disclosure is to provide a nitride semiconductor device that can suppress deterioration of a cladding layer while improving carrier injection efficiency, and a method for manufacturing the nitride semiconductor device. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems, a nitride semiconductor device according to one aspect of the present disclosure includes a nitride semiconductor substrate containing Al, and a semiconductor laminate portion disposed on the nitride semiconductor substrate. The semiconductor laminate portion includes a first-conductivity-type cladding layer containing a first-conductivity-type nitride semiconductor, a light-emitting layer disposed on the first-conductivity-type cladding layer and formed of a nitride semiconductor containing one or more quantum wells, and a second-conductivity-type cladding layer disposed on the light-emitting layer and formed of a second-conductivity-type nitride semiconductor containing Al. The second-conductivity-type cladding layer has at least one region in which the concentration profile of carbon or oxygen contained in the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the nitride semiconductor substrate.
[0006] In addition, a manufacturing method for a nitride semiconductor device according to another aspect of the present disclosure includes forming a first conductivity type cladding layer including a first conductivity type nitride semiconductor on a nitride semiconductor substrate including Al, forming a light emitting layer on the first conductivity type cladding layer using a nitride semiconductor including one or more quantum wells, forming a part of a second conductivity type cladding layer including a second conductivity type nitride semiconductor under conditions where the wafer temperature is from 900°C to 1000°C and the reactor pressure is from 15 mbar to 350 mbar, and forming the remaining part of the second conductivity type cladding layer under conditions where the wafer temperature is from 1030°C to 1100°C and the reactor pressure is from 15 mbar to 350 mbar, thereby forming a semiconductor stack on the nitride semiconductor substrate. It should be noted that the above summary of the invention does not list all of the features of the invention according to the present disclosure. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a nitride semiconductor device that can suppress deterioration of a cladding layer while improving carrier injection efficiency, and a method for manufacturing the nitride semiconductor device. [Brief description of the drawings]
[0008] [Figure 1] 1 is a graph showing an example of an Al composition ratio in a nitride semiconductor device according to an embodiment of the present disclosure. [Figure 2A]4 is an AFM image showing the structure of the upper surface of a second conductivity type cladding layer of a nitride semiconductor device according to an embodiment of the present disclosure. [Figure 2B] 4 is an SEM photograph showing the structure of the upper surface of a second conductivity type cladding layer of a nitride semiconductor device according to an embodiment of the present disclosure. [Diagram 3] 1 is an AFM photograph showing the structure of the upper surface of a second conductivity type cladding layer of a conventional nitride semiconductor device. [Figure 4] 1 is a schematic plan view showing a configuration example of a nitride semiconductor device according to an embodiment of the present disclosure. [Diagram 5] 1 is a schematic cross-sectional view showing a configuration example of a nitride semiconductor device according to an embodiment of the present disclosure. [Figure 6] 1 is a schematic cross-sectional view showing a configuration example of a nitride semiconductor device according to an embodiment of the present disclosure. [Figure 7] 1 is a schematic cross-sectional view showing a configuration example of a nitride semiconductor device according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The nitride semiconductor device according to the present disclosure will be described below through embodiments, but the following embodiments do not limit the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention. In the following description, "up" and "down" do not necessarily mean the vertical direction relative to the ground. In other words, the directions of "up" and "down" are not limited to the direction of gravity. "Up" and "down" are merely convenient expressions for specifying the relative positional relationship of a surface, a film, a substrate, etc., and do not limit the technical idea of the present invention. For example, if the paper surface is rotated 180 degrees, "up" will of course become "down" and "down" will become "up."
[0010] 1. First embodiment A nitride semiconductor device according to a first embodiment of the present disclosure will be described. The nitride semiconductor device according to this embodiment is, for example, a laser diode. The following describes the case where the nitride semiconductor device is a laser diode.
[0011] (1.1) Structure of a laser diode The laser diode according to this embodiment includes a nitride semiconductor substrate containing Al, and a semiconductor laminate disposed on the nitride semiconductor substrate. The semiconductor laminate includes a first-conductivity-type cladding layer containing a first-conductivity-type nitride semiconductor, a light-emitting layer formed of a nitride semiconductor containing one or more quantum wells and disposed on the first-conductivity-type cladding layer, a first-conductivity-type waveguide layer disposed between the first-conductivity-type cladding layer and the light-emitting layer and confines light to the light-emitting layer, a second-conductivity-type waveguide layer disposed between the second-conductivity-type cladding layer and the light-emitting layer and confines light to the light-emitting layer, and a second-conductivity-type cladding layer disposed on the light-emitting layer and formed of a second-conductivity-type nitride semiconductor. The second-conductivity-type cladding layer has at least one region in which the concentration profile of carbon or oxygen contained in the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the nitride semiconductor substrate. Each layer of the laser diode will now be described in detail.
[0012] <Nitride semiconductor substrate> The nitride semiconductor substrate (hereinafter sometimes referred to as substrate) contains a nitride semiconductor containing Al. The nitride semiconductor containing Al is, for example, AlN. That is, the substrate is preferably an AlN single crystal substrate. The nitride semiconductor containing Al is not limited to AlN, and may be, for example, AlGaN. For example, when the substrate is a nitride semiconductor single crystal substrate such as AlN or AlGaN, the difference in lattice constant with the nitride semiconductor layer formed on the substrate becomes small, and the nitride semiconductor layer is grown in a lattice-matched system, thereby reducing threading dislocations. The threading dislocation density of the substrate is 5×10 4 cm -2 In particular, from the viewpoint of improving the emission intensity and reducing the oscillation threshold current, the threading dislocation density is preferably 1×10 3 More than 1×10 4 cm -2 It is more preferable that: The substrate may be formed on a heterogeneous substrate as long as it contains a nitride semiconductor containing Al. For example, AlN may be grown on a sapphire (Al2O3) substrate.
[0013] Here, the wording "comprises" in the expression "comprises a nitride semiconductor" means that the layer mainly contains a nitride semiconductor, but this expression also includes cases where other elements are included. Specifically, this expression also includes cases where the composition of this layer is slightly changed by adding a small amount of an element other than the nitride semiconductor (for example, elements such as Ga (when Ga is not the main element), In, As, P, or Sb, at a few percent or less). In expressions of the composition of other layers, the wording "comprises" has a similar meaning. Also, the small amount of elements contained is not limited to the above.
[0014] The substrate preferably has a thickness of 100 μm or more and 600 μm or less. The surface orientation may be c-plane (0001), a-plane (11-20), m-plane (10-10), etc., with a c-plane (0001) substrate being more preferable. Furthermore, the substrate may be formed on a surface tilted at some angle (for example, -4° to 4°, preferably -0.4° to 0.4°) from the normal direction of the c-plane (0001), but is not limited thereto.
[0015] <Buffer layer> A buffer layer may be formed on the substrate, i.e., between the substrate and the first conductive type cladding layer. The buffer layer is preferably formed on the entire surface of the substrate. By providing the buffer layer, a nitride semiconductor layer having small lattice constant differences and thermal expansion coefficient differences and few defects is formed on the buffer layer. The buffer layer is preferably a nitride semiconductor layer containing Al, and is formed of, for example, a nitride semiconductor such as AlN, AlGaN, etc. The buffer layer may also contain impurities such as C, Si, Fe, Mg, etc.
[0016] The buffer layer has a thickness of, for example, several micrometers. Specifically, the thickness of the buffer layer is preferably greater than 10 nm and less than 10 μm. When the thickness of the buffer layer is greater than 10 nm, the crystallinity of the nitride semiconductor such as AlN becomes higher. Also, when the thickness of the buffer layer is less than 10 μm, cracks are less likely to occur in the buffer layer formed by crystal growth over the entire wafer surface.
[0017] <N-type clad layer> The n-type clad layer is formed on the substrate. Here, for example, in the expression "the n-type clad layer is formed on the substrate", the word "on" means that the n-type clad layer is formed on one surface of the substrate. Also, the above expression includes the case where another layer further exists between the substrate and the n-type clad layer. In the relationship between other layers as well, the word "above" has the same meaning. For example, when the p-type clad layer is formed via an electron blocking layer on the n-type waveguide layer described later, it is also included in the expression "the p-type clad layer is formed on the n-type waveguide layer". Also, in the description of this embodiment, "n-type" and "p-type" each mean a semiconductor indicating a different conductivity type. For example, when one is n-type conductive, the other is p-type conductive.
[0018] The n-type clad layer is a layer of a nitride semiconductor containing Al and Ga. The n-type clad layer is, for example, Al a Ga (1-a) N (0 < a < 1). Thereby, when forming a material corresponding to the bandgap energy in the deep ultraviolet region as the light-emitting layer, it becomes possible to enhance the crystallinity of the light-emitting layer and improve the light-emission efficiency. From the viewpoint of realizing high light-emission efficiency, the nitride semiconductor constituting the n-type clad layer is preferably a mixed crystal of AlN and GaN. Also, from the viewpoint of growing the n-type clad layer and each layer formed in the upper layer with complete strain with respect to the substrate, the n-type clad layer is Al a Ga (1-a)It is more preferably formed by N(0.65 < a ≤ 0.9).
[0019] The first-conductive-type clad layer may be a gradient layer in which the Al composition increases as it moves away from the substrate for the purpose of controlling the longitudinal conductivity. In this case, the above-mentioned limitation on the Al composition can be the Al composition averaged by the film thickness of the first-conductive-type clad layer for the Al composition at the position in the film thickness direction within the first-conductive-type clad layer. When the first-conductive-type clad layer is an n-type conductive semiconductor layer, it may contain impurities such as group V elements other than N such as P, As, and Sb, and C, H, F, O, Mg, Si, etc., but the types of impurity elements are not limited to this. From the viewpoints of reducing electrical resistance and the availability of raw materials, the impurity contained in the first-conductive-type clad layer is preferably Si, and the impurity concentration is 5×10 18 cm -3 or more and 5×10 19 cm -3 or less, which is preferable. Also, the resistivity of the first-conductive-type clad layer is preferably 1×10 -3 Ωcm or more and 5×10 -3 Ωcm or less. Thereby, carrier injection can be efficiently performed.
[0020] The first-conductive-type clad layer preferably has a layer thickness of 250 nm or more and 800 nm or less, and more preferably has a layer thickness of 300 nm or more and 450 nm or less, from the viewpoints of lattice relaxation within the first-conductive-type clad layer and film resistance.
[0021] <Light-emitting layer> The light-emitting layer is a layer of a nitride semiconductor containing Al and Ga. The nitride semiconductor contained in the light-emitting layer is preferably a mixed crystal of, for example, AlN and GaN from the viewpoint of realizing high luminous efficiency. For example, Al b Ga (1-b) N(0 < b < 1). The light-emitting layer may contain impurities such as group V elements other than N such as P, As, and Sb, and C, H, F, O, Mg, Si, etc., but the types of impurity elements are not limited to this.
[0022] The light emitting layer may have either a multiple quantum well structure or a single quantum well structure. The number of quantum well structures is preferably 1 to 5, depending on the longitudinal conductivity of the first and second conductive cladding layers.
[0023] In the laser diode of this embodiment, α, which indirectly represents the potential fluctuation of the nitride semiconductor layer, is preferably 130 meV or more and 350 meV or less. The nitride semiconductor layer represented by such α may be not only the light emitting layer but also a first conductive type waveguide layer or a second conductive type waveguide layer described later. When α of the light emitting layer, the first conductive type waveguide layer, or the second conductive type waveguide layer is 130 meV or more and 350 meV or less, recombination of localized carriers occurs efficiently, and the light emission efficiency can be improved. Here, the "potential fluctuation of the nitride semiconductor layer" is an index for specifying the distribution state of Ga in the surface direction of the nitride semiconductor layer, and "α indirectly expressing the potential fluctuation" is an index showing the deviation from the uniformity of the alloy in the surface direction of the nitride semiconductor layer. When the above-mentioned α is 30 meV (approximately), it indicates that Ga is uniformly distributed in the surface direction of the nitride semiconductor layer, that is, Al and Ga are uniformly arranged. Such potential fluctuation appears in the half-width of the emission spectrum of the nitride semiconductor layer. That is, the closer the nitride semiconductor constituting the nitride semiconductor layer is to a completely uniform crystal, the narrower the half-width of the emission spectrum. On the other hand, the possible values of the half-width of the emission spectrum also differ depending on the Al composition of the nitride semiconductor. Therefore, the potential fluctuation of the nitride semiconductor layer is evaluated using α, which expresses the deviation from the half-width of the emission spectrum in a uniform state at each Al composition. The Al composition x of the nitride semiconductor layer and the half-width FWHM of the emission spectrum at the emission wavelength can be expressed by the formula FWHM (meV) = αx + 10 meV. In this case, if α is large, it can be said that the state is far from uniform, that is, Ga and the like are segregated or localized.
[0024] In addition, at the interface between the well layer and the barrier layer in the light-emitting layer, the thickness of the region where the Al concentration profile changes gradually is preferably 0.3 nm or more and 0.6 nm or less. This can improve the confinement of carriers and the light emission intensity.
[0025] <Waveguide layer> From the perspective of light confinement as a laser diode, the laser diode of this embodiment may be provided with a waveguide layer that is formed above and below the light-emitting layer so as to sandwich the light-emitting layer and has the effect of confining the light emitted from the light-emitting layer within the light-emitting layer. The waveguide layer is preferably composed of two layers, namely, a first-conductivity-type waveguide layer disposed between the first-conductivity-type clad layer and the light-emitting layer, and a second-conductivity-type waveguide layer disposed between the second-conductivity-type clad layer and the light-emitting layer. That is, the laser diode of this embodiment may include, for example, a first-conductivity-type waveguide layer disposed between the first-conductivity-type clad layer and the light-emitting layer to confine light to the light-emitting layer, and a second-conductivity-type waveguide layer disposed between the second-conductivity-type clad layer and the light-emitting layer to confine light to the light-emitting layer.
[0026] From the perspective of light confinement, the waveguide layer is preferably a nitride semiconductor containing Al and Ga having a bandgap higher in energy than the light-emitting layer. The waveguide layer preferably has an Al composition and a film thickness that increase the overlap of the electric field intensity distribution of the light standing in the device and the light-emitting layer. From the perspective of carrier confinement in the light-emitting layer, the light-emitting layer is Al b Ga (1-b) N (0 < b < 1), and when the waveguide layer is Al c Ga (1-c) N (0 < c < 1), it is more preferable that b < c and c ≧ b + 0.05. For example, when taking a light-emitting layer with an emission wavelength of 265 nm as an example, b is 0.52, and c is preferably 0.57 or more. Also, from the perspectives of light confinement and sheet resistance, the total film thickness of the waveguide layer (the sum of the film thicknesses of the first-conductivity-type waveguide layer and the second-conductivity-type waveguide layer) is preferably 70 nm or more and 150 nm or less.
[0027] The waveguide layer may contain impurities such as P, As, Sb, and other V group elements other than N, C, H, F, O, Mg, and Si, but the types of impurity elements are not limited to these. From the viewpoint of reducing electrical resistance and the ease of obtaining raw materials, the impurity contained in the first conductive type waveguide layer is preferably Si, and the impurity concentration is 5×10 18 cm -3 5×10 or more 19 cm -3 It is preferable that:
[0028] The Al composition of each of the first-conductivity-type waveguide layer and the second-conductivity-type waveguide layer is preferably uniform in the thickness direction, but is not limited to this. In order to avoid light absorption by a metal (e.g., a second electrode) present above the second-conductivity-type cladding layer described later, the Al composition of the second-conductivity-type waveguide layer may be higher than the Al composition of the first-conductivity-type waveguide layer. For the same purpose, the thickness of the second-conductivity-type waveguide layer may be thicker than the thickness of the first waveguide.
[0029] <Second conductive type cladding layer> The second conductive clad layer is a nitride semiconductor layer that is formed on the light emitting layer and has a second conductive type and contains Al and Ga. The second conductive clad layer is, for example, Al d Ga (1-d) N (0.1≦d≦1). Specifically, the second conductive type cladding layer is formed on the second conductive type waveguide layer. This allows the second conductive type cladding layer to easily lattice match with the light emitting layer or the waveguide layer, and makes it possible to suppress the threading dislocation density.
[0030] The second conductive cladding layer is not particularly limited in its conductive type, so long as it has sufficient conductivity to inject carriers (electrons or holes) into the light-emitting layer and can increase the overlap between the electric field intensity distribution of the optical mode existing in the device and the light-emitting layer (i.e., increase the light confinement). The second conductive cladding layer may be, for example, p-type AlGaN doped with Mg. The second conductive cladding layer may also contain impurities such as P, As, Sb, and other V group elements other than N, C, H, F, O, Mg, and Si, but the types of impurity elements are not limited to these.
[0031] From the viewpoint of more efficient carrier injection into the light-emitting layer, the second conductive type cladding layer has a composition gradient such that the Al composition d decreases with increasing distance from the substrate. d Ga (1-d) The compositionally graded layer is formed of N (0.1≦d≦1), and in a portion of the second conductivity type cladding layer, the Al composition d increases with increasing distance from the substrate. The second conductivity type cladding layer preferably has a composition gradient in which the Al composition ratio d changes from 1 to 0.7 with increasing distance from the nitride semiconductor substrate side. The profile (gradient) of the Al composition d in the second conductivity type cladding layer may decrease continuously or may decrease discontinuously. Here, "decreasing discontinuously" means that the second conductivity type cladding layer includes a portion in which the Al composition d is the same (constant in the film thickness direction). In other words, the second conductivity type cladding layer may include a portion in which the Al composition d does not decrease in the direction away from the substrate.
[0032] The thickness of the second conductive type cladding layer is preferably 500 nm or less from the viewpoint of lattice matching, and more preferably 250 nm to 500 nm from the viewpoint of optical confinement.
[0033] The Al composition ratio (shown by the thick line) and the impurity composition ratio (shown by the solid line) in each layer of the laser diode are shown in Fig. 1. Note that Fig. 1 shows a structure without a buffer layer as an example. As shown in Fig. 1, the second conductivity type cladding layer has a composition gradient such that the Al composition d decreases with increasing distance from the substrate. A portion of the second conductivity type cladding layer is doped with impurities such as carbon or oxygen. The impurities are also doped into a composition gradient layer provided between the second conductivity type waveguide layer and the second conductivity type cladding layer, for example, and the concentration profile discontinuously decreases at the start point of the composition gradient layer (the interface on the second conductivity type waveguide layer side). Conventionally, the second conductive type cladding layer is often formed of a nitride semiconductor that is hardly doped with impurities for the purpose of suppressing the diffusion of impurities and improving the injection efficiency, etc. However, in the laser diode according to this embodiment, a part of the second conductive type cladding layer contains a large amount of impurities, so that it is possible to suppress deterioration and improve the injection efficiency in the second conductive type cladding layer at the same time.
[0034] Moreover, the second conductive type cladding layer preferably has at least one region where the concentration profile of carbon or oxygen contained in the second conductive type cladding layer discontinuously decreases with increasing distance from the substrate. That is, the second conductive type cladding layer has a region where the concentration profile of the impurity is convex in the direction of increasing concentration. By having such a discontinuous region, the second conductive type cladding layer has a part of the second conductive type cladding layer that exhibits an effect of suppressing deterioration of the second conductive type cladding layer, and a remaining part of the second conductive type cladding layer that exhibits an effect of improving the injection efficiency of carriers (electrons or holes) into the light emitting layer. In this case, the concentration profile of carbon or oxygen in the second conductive type cladding layer slopes steeply, improving the effect of improving the injection efficiency of carriers into the light emitting layer, and the second conductive type cladding layer can achieve both the effect of suppressing deterioration of the second conductive type cladding layer and the effect of improving the injection efficiency of carriers into the light emitting layer. Generally, if the impurity concentration profile has a region that is convex in the direction in which the concentration increases, this is disadvantageous in terms of the efficiency of carrier injection into the light-emitting layer. However, depending on the thickness of the second cladding layer, providing a region in which the carbon or oxygen concentration profile slopes steeply can be advantageous in terms of the overall efficiency of carrier injection into the light-emitting layer.
[0035] Here, "a region where the concentration profile discontinuously decreases with increasing distance from the substrate (nitride semiconductor substrate) at least at one point" refers to a region where the impurity concentration in a certain region (the impurity concentration measured at a measurement point in the region) differs by a factor of two or more from the surrounding impurity concentration (the impurity concentration measured at a measurement point in an adjacent region). For example, as shown in Figure 1, there is a region P where the impurity concentration profile changes abruptly.
[0036] As described above, the second conductive type cladding layer has a region P where the impurity concentration profile decreases discontinuously. The region P where the concentration profile decreases discontinuously is preferably present in a region of 5 nm to 110 nm from the substrate side of the second conductive type cladding layer. This makes it possible to suppress deterioration of the second conductive type cladding layer without impeding the improvement of the efficiency of carrier injection into the light emitting layer.
[0037] In addition, in the second conductive type cladding layer, a region P where the impurity concentration profile discontinuously decreases is Al e Ga (1-e) It is preferable that the second conductive type cladding layer is formed with N (0.80≦e≦1.0). This makes it possible to suppress deterioration of the second conductive type cladding layer without impeding the improvement of the efficiency of carrier injection into the light emitting layer. The carbon concentration in the second conductive type cladding layer in the region closer to the substrate than the region P where the impurity concentration profile discontinuously decreases is 1×10 17 cm -3 More than 1×10 18 cm -3 Similarly, the oxygen concentration in the second conductive type cladding layer in the region closer to the substrate than the region P where the impurity concentration profile discontinuously decreases is preferably 1×10 17 cm -3 More than 1×10 18 cm -3It is preferable that the thickness of the cladding layer is less than 100 nm. This allows a layer that is effective in suppressing deterioration of the second conductive type cladding layer and a layer that is effective in improving the efficiency of carrier injection into the light emitting layer to be formed well. This makes it possible to more effectively achieve both the effect of suppressing deterioration of the second conductive type cladding layer in the laser diode and the effect of improving the efficiency of carrier injection into the light emitting layer.
[0038] As described above, the second conductive cladding layer is made of Al d Ga (1-d) N (0.1≦d≦1), and has a composition gradient in which the Al composition d decreases with increasing distance from the nitride semiconductor substrate. Furthermore, at least a portion of the second conductivity type cladding layer is a composition discontinuous region Q in which the Al composition is discontinuous in the direction away from the substrate, and in the composition discontinuous region Q, the Al composition d increases with increasing distance from the substrate. In this way, the second conductivity type cladding layer has composition discontinuous region Q, and the laser diode can achieve both the effect of suppressing deterioration of the second conductivity type cladding layer and the effect of improving the efficiency of carrier injection into the light emitting layer.
[0039] Compositional discontinuous region Q is preferably present in a region between 5 nm and 110 nm from the nitride semiconductor substrate side of the second conductivity type cladding layer. In other words, the start point of compositional discontinuous region Q preferably coincides with the start point of region P. By having compositional discontinuous region Q on the nitride semiconductor substrate side of the second conductivity type cladding layer, deterioration of the second conductivity type cladding layer can be suppressed without impeding improvement in the efficiency of carrier injection into the light emitting layer. Furthermore, it is preferable that the composition discontinuous region Q has a composition gradient in which the Al composition d increases by 0.2% or more and 5% or less with increasing distance from the substrate. By having the composition discontinuous region Q have such a composition gradient, a layer that is effective in suppressing deterioration of the second conductivity type cladding layer and a layer that is effective in improving the injection efficiency of carriers into the light emitting layer are formed. Therefore, it is possible to more effectively achieve both the effect of suppressing deterioration of the second conductivity type cladding layer in the laser diode and the effect of improving the injection efficiency of carriers into the light emitting layer.
[0040] In addition, the interface of the second conductive cladding layer on the substrate side (i.e., the interface with the second conductive waveguide layer) has a hydrogen concentration of 1×10 17 cm -3 5×10 or more 19 cm -3 It is preferable that hydrogen is contained in at least a portion of the second conductivity type cladding layer at a higher concentration than in other regions of the second conductivity type cladding layer. Although the second conductivity type cladding layer contains a small amount of hydrogen overall, the second conductivity type cladding layer includes a region (the portion) containing a high concentration of hydrogen in part. This allows the laser diode to compensate for point defects and achieve both the effect of suppressing deterioration of the second conductivity type cladding layer and the effect of improving the efficiency of carrier injection into the light emitting layer.
[0041] Moreover, the region containing hydrogen at a higher concentration than other regions of the second conductive type cladding layer is preferably a region of the second conductive type cladding layer that is 5 nm to 110 nm from the substrate side, which makes it possible to compensate for point defects and suppress deterioration of the second conductive type cladding layer without impeding the improvement of the efficiency of carrier injection into the light emitting layer. Furthermore, the half-width of the hydrogen concentration profile in the region of the second conductive type cladding layer that contains hydrogen at a higher concentration than other regions is preferably 5 nm to 10 nm, which makes it possible to effectively compensate for point defects and improve the efficiency of carrier injection into the light emitting layer.
[0042] In addition, the interface of the second conductive type cladding layer on the substrate side has 1×10 silicon. 17 cm -3 5×10 or more 19 cm -3 At least a portion of the second conductive type cladding layer may contain silicon at a higher concentration than other regions of the second conductive type cladding layer. The region of the second conductive type cladding layer that contains silicon at a higher concentration than other regions of the second conductive type cladding layer is preferably a region that is 5 nm or more and 110 nm or less from the substrate side of the second conductive type cladding layer.
[0043] The surface of the second conductive type cladding layer as described above has a step-terrace structure having terraces and steps that are not linear in plan view, as shown in Fig. 2A. For comparison, a step-terrace structure having terraces and steps that are linear in plan view is shown in Fig. 3. This makes it possible to more effectively suppress deterioration of the second conductive type cladding layer in the laser diode and to more effectively improve the efficiency of carrier injection into the light emitting layer. More specifically, the surface of the second conductive type cladding layer preferably has an uneven shape including a plurality of unevennesses. The unevenness of the surface of such a second conductive type cladding layer may be hexagonal or circular in plan view, or may have a spiral step-terrace structure in plan view. Such a second conductive type cladding layer is grown and formed at a lower temperature than conventionally (described in detail later), and thereby the linear step-terrace structure changes to a hexagonal or circular, or spiral, or other non-linear step-terrace structure. Here, FIG. 2A is an atomic force microscope (AFM) photograph showing the spiral step-terrace structure, and FIG. 2B is a scanning electron microscope (SEM) photograph showing the circular step-terrace structure. When a hexagonal or circular, or spiral step-terrace structure is formed on the surface of the second conductive type cladding layer, a higher effect of improving the luminous efficiency of the second conductive type cladding layer can be obtained. This is believed to be because Ga segregates during the growth of the film having a hexagonal, circular, or spiral step-terrace structure, improving the current injection efficiency.
[0044] The height of the spiral step-terrace structure is preferably 0.2 nm or more and 0.4 nm or less. The distribution density of multiple projections is 1×10 7 cm -2 5×10 or more 8 cm -2 It is preferable that: This makes it possible to obtain a further improved effect of suppressing deterioration of the second conductivity type cladding layer and to improve the current injection efficiency.
[0045] In addition, when a nitride semiconductor layer having a step-terrace structure is formed and then a nitride semiconductor layer is formed by a conventional method to form a second-conductivity-type cladding layer, the step-terrace structure also appears on the surface of the second-conductivity-type cladding layer. Therefore, by observing the surface shape of the second-conductivity-type cladding layer, the step-terrace structure on the surface of the second-conductivity-type cladding layer can be confirmed. In addition, when a second-conductivity-type contact layer, which will be described later, is formed on the second-conductivity-type cladding layer, the step-terrace structure does not appear on the surface of the second-conductivity-type contact layer. However, by removing only the second-conductivity-type contact layer using sulfur hexafluoride (SF6) gas or the like to expose the second-conductivity-type contact layer and observing it with an SEM or the like, the step-terrace structure on the surface of the second-conductivity-type cladding layer can be confirmed.
[0046] <Composition gradient layer> In the laser diode according to this embodiment, an Al g Ga (1-g) The nitride semiconductor substrate may have a composition gradient layer containing N (0.1≦g≦1) and having an Al composition g that increases with increasing distance from the nitride semiconductor substrate. By providing the composition gradient layer as in the present embodiment, the electrolysis is mitigated, and the degradation suppression effect is improved. The thickness of the composition gradient layer is preferably 2 nm to 5 nm, more preferably 2 nm to 3 nm, in which case the degradation suppression effect is further improved.
[0047] <Second Conductive Type Contact Layer> The semiconductor laminate of the laser diode of this embodiment may further include a second conductive type contact layer disposed on the second conductive type cladding layer. The nitride semiconductor constituting the second conductive type contact layer is preferably formed of, for example, GaN, AlN, or InN, or a mixed crystal containing these, and more preferably is a nitride semiconductor containing GaN.
[0048] In the case of a p-type contact layer, the second conductive type contact layer may contain impurities such as P, As, Sb, and other V group elements other than N, C, H, F, O, Mg, Si, and Be. In view of the versatility of the source gas, the impurity contained in the second conductive type contact layer is preferably Mg. In view of reducing the contact resistance, the concentration of Mg is preferably 8×10 19 cm -3 5×10 or more 21 cm -3 Preferably, it is 5×10 or less. 20 cm -3 5×10 or more 21 cm -3 It is more preferable that:
[0049] The thickness of the second conductive contact layer is preferably 1 nm or more and 20 nm or less. The thinner the second conductive contact layer is, the higher the carrier injection efficiency of the light emitting layer is, and the thicker the second conductive contact layer is, the lower the carrier injection efficiency is.
[0050] <Electron Block Layer> The semiconductor laminate of the laser diode of this embodiment may further include an electron blocking layer above the light emitting layer, the electron blocking layer having a band gap larger than that of the light emitting layer. The electron blocking layer may be provided, for example, on the light emitting layer, or may be provided inside the second conductive type waveguide layer, between the second conductive type waveguide layer and the light emitting layer, or between the second conductive type waveguide layer and the second conductive type cladding layer. The thickness of the electron blocking layer is preferably 30 nm or less, and more preferably 20 nm or less, so that carriers (holes) can easily quantum-transport through the electron blocking layer.
[0051] <Electrode> The laser diode can emit light or oscillate by injecting a current through a second electrode disposed on the second conductive type cladding layer and a first electrode disposed on the first conductive type cladding layer, where the first electrode is formed so as to be in electrical contact with the first conductive type cladding layer, and the second electrode is formed so as to be in electrical contact with the second conductive type cladding layer.
[0052] The first electrode can be disposed, for example, on the back side of the substrate. The first electrode is disposed on the first conductive clad layer exposed by removing the layers above the first conductive clad layer of the semiconductor laminate by, for example, chemical etching or dry etching. In other words, the first electrode is disposed on a region of the first conductive clad layer that does not form a mesa structure.
[0053] When the first conductive type cladding layer is an n-type cladding layer, the first electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the first conductive type cladding layer is a p-type cladding layer, the first electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.
[0054] When the second conductive type cladding layer is an n-type cladding layer, the second electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the second conductive type cladding layer is a p-type cladding layer, the second electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.
[0055] The arrangement area and shape of the first electrode and the second electrode are not limited as long as electrical contact is obtained with each of the first conductivity type cladding layer and the second conductivity type cladding layer (the second conductivity type contact layer if a second conductivity type contact layer is provided).
[0056] (1.2) Method for manufacturing nitride semiconductor device The laser diode, which is the nitride semiconductor device of this embodiment, is manufactured through the steps of forming each layer on a substrate. A method for manufacturing the laser diode will be described below.
[0057] (1.2.1) Laser Diode Manufacturing Method (Formation of the substrate) The substrate is formed by a general substrate growth method such as a vapor phase growth method, such as a sublimation method or a hydride vapor phase epitaxy (HVPE) method, or a liquid phase growth method.
[0058] (Formation of semiconductor laminate) Each layer of the semiconductor laminate formed on the substrate can be formed by, for example, molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), or metal organic chemical vapor deposition (MOCVD). Here, among the layers formed on the substrate, the nitride semiconductor layer can be formed using, for example, an Al source containing trimethylaluminum (TMAl), a Ga source containing trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing ammonia (NH3).
[0059] A semiconductor laminate is formed on a substrate. At this time, an organometallic gas is flowed into a space for forming the semiconductor laminate. First, a first conductivity type cladding layer including a first conductivity type nitride semiconductor is formed on a substrate.
[0060] Next, a first conductivity type waveguide layer made of a nitride semiconductor such as AlGaN is formed on the first conductivity type cladding layer, and then a light emitting layer is formed of a nitride semiconductor (such as AlGaN) including one or more quantum wells. Next, a second conductivity type waveguide layer made of a nitride semiconductor such as AlGaN is formed on the light emitting layer.
[0061] At this time, the formation of the first conductivity type waveguide layer, the light-emitting layer, and the second conductivity type waveguide layer is preferably performed under the condition that -2Tw + 2050 < Vw < -2Tw + 2350 (850 °C < Tw < 970 °C), where Tw is the wafer temperature and Vw is the reactor pressure. Thereby, a light-emitting layer in which Ga is unevenly distributed in the nitride semiconductor layer plane direction can be formed. Similarly, a first conductivity type waveguide and a second conductivity type waveguide in which Ga is unevenly distributed in the nitride semiconductor layer plane direction can be formed. By localizing carriers in this way, the recombination rate can be increased and the light emission efficiency can be improved.
[0062] Subsequently, a second conductivity type clad layer is formed on the second conductivity type waveguide layer. First, before forming a part of the second conductivity type clad layer, the inflow of the organometallic gas is temporarily stopped to interrupt the growth of the nitride semiconductor layer, and the film formation conditions are changed. Subsequently, it is preferable to change the conditions to a wafer temperature of 900 °C or higher and 1000 °C or lower and a reactor pressure of 15 mbar or higher and 350 mbar or lower, resume the inflow of the organometallic gas, and form a part of the second conductivity type clad layer with a second conductivity type nitride semiconductor.
[0063] After forming a part of the second conductivity type clad layer, before forming the remaining part of the second conductivity type clad layer, the inflow of the organometallic gas is temporarily stopped again to interrupt the growth of the nitride semiconductor layer, and the film formation conditions are changed. Subsequently, it is changed to conditions of a wafer temperature of 1030 °C or higher and 1100 °C or lower and a reactor pressure of 15 mbar or higher and 350 mbar or lower, the inflow of the organometallic gas is resumed, and the remaining part of the second conductivity type clad layer is formed.
[0064] By forming the first conductivity type clad layer, the first conductivity type waveguide layer, the light-emitting layer, and the second conductivity type waveguide layer as described above, the recombination rate of carriers can be increased, point defects in each layer can be reduced, and deterioration suppression and light emission efficiency can be improved. Furthermore, by setting the wafer temperature when forming a portion of the second-conductivity-type cladding layer lower than the wafer temperature when forming the remaining portion of the second-conductivity-type cladding layer, it is possible to form at least one region in which the carbon or oxygen concentration profile in the portion of the second-conductivity-type cladding layer and the remaining portion of the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the substrate. That is, the portion of the second-conductivity-type cladding layer can be formed to contain more carbon or oxygen than the remaining portion of the second-conductivity-type cladding layer. This makes it possible to simultaneously suppress deterioration and improve injection efficiency in the second-conductivity-type cladding layer. Furthermore, by setting the reactor pressure during formation of a portion of the second conductivity type cladding layer to a lower pressure than the reactor pressure during formation of the remaining portion of the second conductivity type cladding layer, the portion of the second conductivity type cladding layer can be formed to contain more carbon or oxygen as an impurity compared to the remaining portion of the second conductivity type cladding layer.
[0065] Furthermore, by temporarily stopping the flow of the metal-organic gas before forming a part of the second-conductivity-type cladding layer, hydrogen and silicon are localized at the interface of the second-conductivity-type cladding layer on the substrate side. This is because, for example, when hydrogen gas (H2) is used as a carrier gas, hydrogen (H) is likely to be localized in the uppermost layer of the nitride semiconductor layer where the growth is interrupted (for example, the interface between the second-conductivity-type waveguide layer and the second-conductivity-type cladding layer and a part of the second-conductivity-type cladding layer). This allows the laser diode to further improve the effect of suppressing deterioration of the second-conductivity-type cladding layer and the effect of improving the efficiency of carrier injection into the light-emitting layer.
[0066] Conventionally, when the growth of a nitride semiconductor layer is interrupted, some elements (for example, Ga in the case of AlGaN) are lost, so interruption of growth is avoided as much as possible. However, by interrupting growth and actively introducing hydrogen, hydrogen is localized at the interface between the second conductive type waveguide layer and the second conductive type cladding layer and in a part of the second conductive type cladding layer, and point defects at the interface are reduced to V. III By compensating for −H3, the deterioration suppression effect can be improved. Conventionally, when the second conductive type cladding layer is a p-type semiconductor layer, it is preferable that it does not contain silicon, which is an n-type impurity. However, by actively introducing silicon by interrupting growth and localizing silicon derived from the raw material or susceptor at the interface between the second conductive type waveguide layer and the second conductive type cladding layer and in a part of the second conductive type cladding layer, it is possible to compensate for point defects at the interface and improve the degradation suppression effect.
[0067] As described above, in this embodiment, the wafer temperature during the formation of a portion of the second-conductivity-type cladding layer is set lower than the wafer temperature during the formation of the remaining portion of the second-conductivity-type cladding layer, thereby forming at least one region in which the carbon or oxygen concentration profile in the portion of the second-conductivity-type cladding layer and the remaining portion of the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the substrate, but the manufacturing method is not limited to this. For example, the flow rate of the organometallic gas may be intentionally changed during the formation of the second-conductivity-type cladding layer to form a region in which the carbon or oxygen concentration profile discontinuously decreases with increasing distance from the substrate.
[0068] Furthermore, if necessary, an intermediate layer may be formed between the second conductivity type cladding layer and the second conductivity type waveguide layer using a nitride semiconductor such as AlGaN, a second conductivity type contact layer may be provided on the second conductivity type cladding layer using a nitride semiconductor including GaN or the like, and an electron blocking layer may be formed above the light emitting layer.
[0069] Laser diodes are manufactured through a process of removing unnecessary portions of each layer of a semiconductor laminate formed on a substrate by etching (mesa structure formation process). Removal of unnecessary portions of each layer of the semiconductor laminate can be performed by, for example, inductively coupled plasma (ICP) etching. In the mesa structure forming step, unnecessary portions of each layer of the conductor laminate portion are removed by etching, thereby exposing a portion of the first conductivity type cladding layer.
[0070] (Electrode formation) The laser diode may also be manufactured through a process of forming electrodes. The electrodes, such as the first electrode and the second electrode, may be formed by various methods of depositing metal by electron beam deposition (EB) such as resistance heating deposition, electron gun deposition, or sputtering, but are not limited to these methods. Each electrode may be formed as a single layer or may be formed by laminating multiple layers. Each electrode may also be heat-treated in an oxygen, nitrogen, or air atmosphere after the layers are formed. Finally, the substrate on which the layers have been formed through the above-mentioned steps is divided into individual pieces by dicing to manufacture the laser diodes.
[0071] Specifically, a first electrode is formed on the surface of the first conductive cladding layer. A second electrode is formed on the top layer (e.g., the second conductive cladding layer) of a mesa structure that is formed as a part of the semiconductor laminate. The formed electrode is alloyed by heating with a rapid thermal annealing (RTA) device, which is a heating process using an infrared lamp, or by laser annealing, which is a heating process using a laser pulse, and contact with the nitride semiconductor layer can be obtained. In this case, the method of alloying is not particularly limited as long as sufficient contact with the nitride semiconductor layer can be obtained. In this manner, according to the method for manufacturing a laser diode according to the present embodiment, it is possible to improve the carrier injection efficiency and the emission intensity.
[0072] (1.3) Measurement methods for the physical properties of laser diodes The physical properties of the laser diode described above can be measured as follows.
[0073] (Layer thickness measurement method) The thickness of each layer constituting the laser diode can be measured by cutting out a predetermined cross section perpendicular to the substrate, observing this cross section with a transmission electron microscope (TEM), and using the length measurement function of the TEM. As a measurement method, first, a cross section perpendicular to the main surface of the substrate of the laser diode is observed using a TEM. Specifically, for example, in a TEM image showing a cross section perpendicular to the main surface of the substrate of the laser diode, a range of 2 μm or more in a direction parallel to the main surface of the substrate is set as the observation width. Since contrast is observed at the interface between two layers with different compositions within this observation width, the thickness up to this interface is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of each layer included in this 200 nm wide observation region can be calculated from five points arbitrarily extracted from the above-mentioned observation width of 2 μm or more, thereby obtaining the layer thickness of each layer.
[0074] (Measurement of impurity and doping concentrations) The concentration of dopants and impurities contained in each layer constituting a laser diode can be measured by secondary ion mass spectrometry (SIMS). When measuring the concentration of dopants and impurities in each layer by SIMS after processing into a device, the measurement can be performed after removing the electrodes by chemical etching or physical polishing. The concentration of dopants and impurities in each layer can also be measured by sputtering from the substrate side where no electrodes are formed. Specifically, SIMS measurements are performed under the measurement conditions provided by Evans Analytical Group (EAG), Inc. A cesium (Cs) ion beam with an energy of 14.5 keV is used to sputter the sample during the measurements.
[0075] (Method of measuring atomic concentration of each layer) One method for measuring the atomic concentration in each layer that constitutes a laser diode is reciprocal space mapping (RSM) using the X-ray diffraction (XRD) method. Specifically, the lattice relaxation rate and Al composition relative to the substrate can be obtained by analyzing reciprocal space mapping data in the vicinity of the diffraction peak obtained using an asymmetric plane as the diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (20-24) plane.
[0076] In addition, layers and regions that do not provide sufficient reflection intensity by XRD, such as the light-emitting layer, the gradient layer, and hillocks formed in each layer, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS).
[0077] In EELS, the composition of a sample is analyzed by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, the energy loss spectrum of the intensity of the transmitted electron beam is measured and analyzed for a thin-sectioned sample used in TEM observation. The position of the peak that appears around 20 eV of energy loss changes depending on the composition of each layer, and the composition can be determined from the peak position.
[0078] In the same manner as in the method for calculating layer thickness by TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0079] In EDX, characteristic X-rays generated by an electron beam in a thin-sectioned sample used in the above-mentioned TEM observation, etc. are measured and analyzed. In the same manner as the method for calculating layer thickness using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0080] In XPS, the evaluation of the depth direction is possible by performing XPS measurement while performing sputter etching using an ion beam. Although Ar+ is generally used as the ion beam, other ion species such as Ar cluster ions can be used as long as they can be irradiated with the etching ion gun mounted on the XPS device. The XPS peak intensities of Al, Ga, and N are measured and analyzed to obtain the depth direction distribution of the Al composition of each layer. Instead of sputter etching, the laser diode may be polished obliquely so that the cross section perpendicular to the main surface of the substrate is enlarged and exposed, and the exposed cross section may be measured by XPS.
[0081] The composition of each layer can be measured not only by XPS but also by Auger Electron Spectroscopy (AES). In this case, the composition can be measured by Auger Electron Spectroscopy on a cross section exposed by sputter etching or oblique polishing. The composition of each layer can also be measured by SEM-EDX measurement of a cross section exposed by oblique polishing.
[0082] (Method of measuring potential fluctuation) α, which indirectly represents the potential fluctuation, is calculated from the formula FWHM(meV)=αx+10meV using the Al composition x of the nitride semiconductor layer and the half-width FWHM at the emission wavelength. Specifically, FWHM is obtained from the emission spectrum obtained by performing photoluminescence measurement on the nitride semiconductor layer. Also, α can be obtained by using the Al composition x of the nitride semiconductor layer. At this time, a light source with a wavelength shorter than the band gap of the nitride semiconductor layer to be excited is used for the photoluminescence measurement. For example, a 213nm YAG triple-frequency laser is used. It is possible to obtain a more accurate value by measuring while cooling the sample to 10K or less. Also, if there is a layer with a smaller band gap than the nitride semiconductor layer to be excited, it can be removed by etching or the like to measure the specific layer. Specifically, if an emission layer exists on the first conductive type waveguide layer, the quantized emission layer is excited by the excitation light, so an accurate value can be obtained by removing the emission layer by etching before measuring the first conductive type waveguide layer.
[0083] (Method of measuring surface shape) Methods for measuring the surface shape of the second conductivity type cladding layer include a scanning electron microscope (SEM) and an atomic force microscope (AFM). Specifically, the uneven shape of the surface of the second conductive cladding layer is observed using a scanning electron microscope SU9000 manufactured by Hitachi High-Tech Corporation at an accelerating voltage of 30 kV. At this time, the surface shape of the second conductive cladding layer can be clearly observed by setting the magnification at 10K to 50K. Under these conditions, the number of hexagonal or circular unevennesses contained within the observation range is counted, and the value obtained by dividing the number by the area is regarded as the unevenness density. At this time, the corners of the hexagons may be rounded, but in such cases, they are still treated as hexagons. The step height of the unevenness on the surface of the second conductive type cladding layer can be measured by AFM. Specifically, observations are made using a scanning probe microscope manufactured by Hitachi High-Tech Corporation. When observing with the scanning probe microscope, the AFM mode is used to observe an area of 2 μm square. The step height can be calculated from the obtained AFM gain.
[0084] (Applications of nitride semiconductor devices) The laser diode according to the present disclosure can be applied to devices in, for example, the medical and life science fields, the environmental field, the industrial and manufacturing fields, the lifestyle and home appliances field, the agricultural field, and other fields. The laser diode can be applied to a drug or chemical synthesis and decomposition device, a liquid, gas, and solid (container, food, medical equipment, etc.) sterilization device, a semiconductor cleaning device, etc., a surface modification device for film, glass, metal, etc., an exposure device for manufacturing semiconductors, FPD (Flat Panel Display), PCB (Printed Wiring Board), and other electronic products, a printing and coating device, an adhesive and sealing device, a transfer and molding device for film, pattern, mockup, etc., and a measurement and inspection device for banknotes, wounds, blood, chemical substances, etc.
[0085] Examples of liquid sterilization equipment include, but are not limited to, automatic ice makers, ice trays and ice storage containers in refrigerators, water tanks for ice makers, freezers, ice makers, humidifiers, dehumidifiers, cold water tanks, hot water tanks and flow piping for water servers, freezer-type water purifiers, portable water purifiers, water supply units, hot water heaters, wastewater treatment equipment, garbage disposers, toilet drain traps, washing machines, water sterilization modules for dialysis, connector sterilizers for peritoneal dialysis, and disaster water storage systems.
[0086] Examples of gas sterilization devices include, but are not limited to, air purifiers, air conditioners, ceiling fans, floor or bedding vacuum cleaners, futon dryers, shoe dryers, washing machines, clothes dryers, indoor germicidal lamps, storage ventilation systems, shoe boxes, chests of drawers, etc. Examples of solid sterilization equipment (including surface sterilization equipment) include, but are not limited to, vacuum packing machines, belt conveyors, hand tool sterilization equipment for medical, dental, barber, and beauty salon use, toothbrushes, toothbrush holders, chopstick cases, cosmetic pouches, drain covers, toilet spot cleaners, and toilet lids.
[0087] 2. Second embodiment A nitride semiconductor device according to a second embodiment of the present disclosure will now be described. The nitride semiconductor device according to this embodiment is, for example, a light emitting device. Hereinafter, a case where the nitride semiconductor device is a light emitting device will be described.
[0088] (2.1) Structure of the light-emitting element The light-emitting device according to this embodiment includes a nitride semiconductor substrate containing Al, and a semiconductor laminate portion disposed on the nitride semiconductor substrate. The semiconductor laminate portion includes a first-conductivity-type cladding layer containing a first-conductivity-type nitride semiconductor, a light-emitting layer disposed on the first-conductivity-type cladding layer and formed of a nitride semiconductor including one or more quantum wells, and a second-conductivity-type cladding layer disposed on the light-emitting layer and formed of a second-conductivity-type nitride semiconductor. The second-conductivity-type cladding layer has at least one region where the concentration profile of carbon or oxygen contained in the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the nitride semiconductor substrate.
[0089] The light emitting device of this embodiment differs from the laser diode of the first embodiment in that it does not include a first conductive type waveguide layer and a second conductive type waveguide layer. In the light emitting device of this embodiment, the second conductive type cladding layer may be used as a barrier layer. Also, the light emitting device of this embodiment has a different configuration from the first conductive type cladding layer of the laser diode of Embodiment 1. Therefore, the first conductive type cladding layer and the second conductive type cladding layer of the light emitting device will be described in detail below. Note that the layers other than the first conductive type cladding layer, ie, the nitride semiconductor substrate, the buffer layer, and the light emitting layer, are similar to the layers described in the first embodiment, and therefore description thereof will be omitted.
[0090] <First-conductivity-type clad layer> The first-conductivity-type clad layer is a layer of a nitride semiconductor containing Al and Ga. The first-conductivity-type clad layer is, for example, Al a Ga (1-a) formed by N(0 < a < 1), for example, Al a Ga (1-a) It is preferably formed by N(0.7 ≤ a ≤ 1). The first-conductivity-type clad layer is preferably formed of an n-type semiconductor. Also, the film thickness T0 of the first-conductivity-type clad layer is preferably (3500a - 2150) nm or more and (26500a - 17850) nm or less (a is the Al composition a of the nitride semiconductor constituting the first-conductivity-type clad layer). Furthermore, the resistivity of the first-conductivity-type clad layer is preferably 1×10 -3 Ωcm or more and 5×10 -3 Ωcm or less. Other configurations have the same configuration as the first-conductivity-type clad layer described in the first embodiment.
[0091] <Second-conductivity-type clad layer> In the light-emitting element, instead of the second-conductivity-type clad layer with a gradient Al composition, an electron blocking layer with a constant Al composition is provided on the light-emitting layer, and a second-conductivity-type contact layer with a gradient Al composition is provided on the electron blocking layer. This second-conductivity-type contact layer with a gradient Al composition serves as a clad layer. In this case, by growing the electron block layer at a lower temperature than in the past, it is possible to obtain an effect of suppressing deterioration of the electron block layer and the second conductive type contact layer and an effect of improving the efficiency of carrier injection into the light emitting layer, similar to the laser diode according to the first embodiment. If the electron block layer and the second conductive type contact layer are regarded as a second conductive type cladding layer, the inflow of the metalorganic gas is temporarily stopped before the growth of the electron block layer to interrupt the growth of the nitride semiconductor layer, and only a part of the electron block layer is grown at a low temperature. As a result, a light emitting device is obtained in which the concentration profile of carbon or oxygen decreases discontinuously, hydrogen is localized at the interface, and the electron block layer contains more impurities than in the past, similar to the second conductive type cladding layer of a laser diode.
[0092] The thickness of the electron blocking layer is preferably 10 nm or more and 15 nm or less. That is, in the light-emitting device, the region where the concentration profile of carbon or oxygen contained in the electron blocking layer discontinuously decreases is preferably present in a region of the electron blocking layer that is 10 nm or more and 15 nm or less from the substrate side.
[0093] Unlike the laser diode according to the first embodiment, the light-emitting device according to this embodiment does not include a first-conductivity type waveguide layer and a second-conductivity type waveguide layer. Therefore, it is difficult to evaluate α, which indirectly represents potential fluctuation. This is because, when an attempt is made to evaluate α, which indirectly represents potential fluctuation, the quantized light-emitting layer is excited, and a correct result cannot be obtained. However, by forming a nitride semiconductor layer under the same conditions as those of the first embodiment, a nitride semiconductor layer having α, which indirectly represents a similar potential fluctuation, can be formed.
[0094] 3. Specific examples of nitride semiconductor devices The nitride semiconductor device of this embodiment will be described more specifically below with reference to each of Figures 4 to 7. The detailed configuration of each layer in each of the following examples is as described above.
[0095] (3.1) First Example Fig. 4 is a schematic cross-sectional view of a laser diode 1 as a first example. As shown in Fig. 4, the laser diode 1 includes a substrate 11, a semiconductor laminate 10 disposed on the substrate, a first electrode 13, and a second electrode 14. The semiconductor laminate 10 includes a first conductivity type cladding layer 101 having an n-type conductivity type, a first conductivity type waveguide layer 102, a light emitting layer 103, a second conductivity type waveguide layer 104, and a second conductivity type cladding layer 105 having a p-type conductivity type.
[0096] (3.2) Second Example Fig. 5 is a schematic cross-sectional view of a laser diode 2 as a second example. As shown in Fig. 5, the laser diode 2 includes a substrate 11, a buffer layer 12, a semiconductor laminate 10 disposed on the substrate 11 (buffer layer 12), a first electrode 13, and a second electrode 14. The semiconductor laminate 10 includes a first conductivity type cladding layer 101 having an n-type conductivity, a first conductivity type waveguide layer 102, a light emitting layer 103, a second conductivity type waveguide layer 104, and a second conductivity type cladding layer 105 having a p-type conductivity. That is, the laser diode 2 differs from the laser diode 1 in that the laser diode 2 includes a buffer layer 12 .
[0097] (3.3) Third Example Fig. 6 is a schematic cross-sectional view of a laser diode 3 as a third example. As shown in Fig. 6, the laser diode 3 includes a substrate 11, a buffer layer 12, a semiconductor laminate 10 disposed on the substrate, a first electrode 13, and a second electrode 14. The semiconductor laminate 10 includes a first conductivity type cladding layer 101 having an n-type conductivity type, a first conductivity type waveguide layer 102, a light emitting layer 103, a second conductivity type waveguide layer 104, a second conductivity type cladding layer 105 having a p-type conductivity type, and a contact layer 106. That is, the laser diode 3 differs from the laser diode 1 in that the laser diode 3 includes a contact layer 106 . The laser diode of the present disclosure may have a configuration including the buffer layer 12 described in the second example and the contact layer 106 described in the third example.
[0098] (3.4) Fourth Example Fig. 7 is a schematic cross-sectional view of a light-emitting element 4 as a first example. As shown in Fig. 7, the light-emitting element 4 includes a substrate 11, a semiconductor laminate 10 disposed on the substrate, a first electrode 13, and a second electrode 14. The semiconductor laminate 10 includes a first conductivity type cladding layer 101 having an n-type conductivity, a light-emitting layer 103, and a second conductivity type cladding layer 105 having a p-type conductivity. In the light-emitting element 4, an electron block layer and a second conductivity type contact layer are provided to play the role of the second conductivity type cladding layer 105. That is, the light-emitting element 4 differs from the laser diode 1 in that it does not include the first-conductivity-type waveguide layer 102 and the second-conductivity-type waveguide layer 104. The light-emitting element 4 also differs from the laser diode 1 in that it is provided with an electron blocking layer and a second-conductivity-type contact layer that serves as the second-conductivity-type cladding layer 105. The light-emitting device of the present disclosure may have a configuration including the buffer layer 12 described in the second example.
[0099] 4.Effects The above-described nitride semiconductor device has the following effects.
[0100] (1) The nitride semiconductor device of the present disclosure includes a nitride semiconductor substrate containing Al, and a semiconductor laminate portion disposed on the nitride semiconductor substrate. The semiconductor laminate portion includes a first-conductivity-type cladding layer containing a first-conductivity-type nitride semiconductor, a light-emitting layer disposed on the first-conductivity-type cladding layer and formed of a nitride semiconductor including one or more quantum wells, and a second-conductivity-type cladding layer disposed on the light-emitting layer and formed of a second-conductivity-type nitride semiconductor. The second-conductivity-type cladding layer has at least one region where the concentration profile of carbon or oxygen contained in the second-conductivity-type cladding layer discontinuously decreases with increasing distance from the nitride semiconductor substrate. As a result, in the second conductivity type cladding layer, the carbon or oxygen concentration profile in the second conductivity type cladding layer has a steep gradient, which improves the effect of improving the efficiency of carrier injection into the light-emitting layer, and it is possible to achieve both the effect of suppressing deterioration of the second conductivity type cladding layer and the effect of improving the efficiency of carrier injection into the light-emitting layer.
[0101] (2) In the nitride semiconductor device of the present disclosure, the region in which the concentration profile discontinuously decreases is preferably present in a region of the second conductivity type cladding layer that is 5 nm or more and 110 nm or less from the substrate side. This makes it possible to suppress deterioration of the second conductivity type cladding layer without impeding the improvement of the efficiency of carrier injection into the light emitting layer.
[0102] (3) In the nitride semiconductor device of the present disclosure, the region in the second conductive type cladding layer where the concentration profile discontinuously decreases is Al d Ga (1-d) It is preferable that the insulating layer is made of N(0.80≦d≦1.0). This makes it possible to suppress deterioration of the second conductivity type cladding layer without impeding the improvement of the efficiency of carrier injection into the light emitting layer.
[0103] (4) In the nitride semiconductor device of the present disclosure, the carbon concentration in the region closer to the nitride semiconductor substrate than the region where the concentration profile of the second conductive type cladding layer discontinuously decreases is 1×10 17 cm -3 More than 1×10 18 cm -3 It is preferable that: This makes it possible to more effectively suppress the deterioration of the second conductivity type cladding layer in the laser diode and to more effectively improve the efficiency of carrier injection into the light emitting layer.
[0104] (5) In the nitride semiconductor device of the present disclosure, the oxygen concentration in the region closer to the nitride semiconductor substrate than the region where the concentration profile of the second conductive type cladding layer discontinuously decreases is 1×10 17 cm -3 More than 1×10 18 cm -3 It is preferable that: This makes it possible to more effectively suppress the deterioration of the second conductivity type cladding layer in the laser diode and to more effectively improve the efficiency of carrier injection into the light emitting layer.
[0105] (6) The method for manufacturing a nitride semiconductor device disclosed herein includes forming a first conductivity type cladding layer including a first conductivity type nitride semiconductor on a nitride semiconductor substrate including Al, forming a light emitting layer on the first conductivity type cladding layer using a nitride semiconductor including one or more quantum wells, forming a part of a second conductivity type cladding layer including a second conductivity type nitride semiconductor under conditions where the wafer temperature is from 900°C to 1000°C and the reactor pressure is from 15 mbar to 350 mbar, and forming a remaining part of the second conductivity type cladding layer under conditions where the wafer temperature is from 1030°C to 1100°C and the reactor pressure is from 15 mbar to 350 mbar, thereby forming a semiconductor stack on the nitride semiconductor substrate. This allows a portion of the second conductivity type cladding layer to be formed so as to contain more carbon or oxygen than the remaining portion of the second conductivity type cladding layer, thereby making it possible to both suppress deterioration and improve injection efficiency in the second conductivity type cladding layer.
[0106] (7) In the method for manufacturing a nitride semiconductor device according to the present disclosure, the reactor pressure when forming a portion of the second conductivity type cladding layer is preferably 15 mbar or more and 100 mbar or less. This allows a portion of the second conductivity type cladding layer to be formed so as to contain more carbon or oxygen than the remaining portion of the second conductivity type cladding layer, thereby further improving the deterioration suppression effect and injection efficiency in the second conductivity type cladding layer.
[0107] (8) In the method for manufacturing a nitride semiconductor device disclosed herein, it is preferable to flow an organometallic gas during the formation of the first conductivity type cladding layer, the light emitting layer, and the second conductivity type cladding layer, to temporarily stop the flow of the organometallic gas after the light emitting layer is formed and before forming a portion of the second conductivity type cladding layer, and to temporarily stop the flow of the organometallic gas after forming a portion of the second conductivity type cladding layer and before forming the remaining portion of the second conductivity type cladding layer. This temporarily halts the growth of the layer containing the nitride semiconductor, localizing hydrogen and silicon at the interface of the second conductivity type cladding layer on the substrate side, thereby further improving the effect of suppressing deterioration of the second conductivity type cladding layer and the effect of improving the efficiency of carrier injection into the light-emitting layer. EXAMPLES
[0108] <Sample 1> The laser diode of the present disclosure will be described below with reference to examples and comparative examples, but the laser diode of the present disclosure is not limited to these examples. The substrate used was a (0001) AlN single crystal substrate having a thickness of 550 μm. Next, an AlN layer, which is a homoepitaxial layer, was formed on the substrate. The AlN layer was formed to a thickness of 500 nm in an environment at 1200°C. At this time, the ratio of the supply rate of the group III element source gas to the supply rate of the nitrogen source gas (V / III ratio) was set to 50. The growth rate of the AlN layer at this time was 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al source, and ammonia (NH3) was used as the N source.
[0109] A first conductive clad layer was formed on the substrate. The first conductive clad layer was an n-type AlGaN layer (Al: 75%, i.e., Al 0.75 Ga 0.25 The first conductive type cladding layer was formed to a thickness of 400 nm under the conditions of a temperature of 1050°C, a reactor pressure of 50 mbar, and a V / III ratio of 4000. The growth rate of the first conductive type cladding layer was 0.4 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material. Ammonia (NH3) was used as the N raw material. Monosilane (SiH4) was used as the Si raw material.
[0110] Next, an n-type waveguide layer, which is a first waveguide layer, was formed on the first conductive cladding layer. The n-type waveguide layer was an n-type AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 The n-type waveguide layer was formed to a thickness of 40 nm under the conditions of a temperature of 950°C, a reactor pressure of 300 mbar, and a V / III ratio of 4000. The growth rate of the n-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, triethylgallium (TEGa) was used as the Ga raw material, and ammonia (NH3) was used as the N raw material.
[0111] Next, a light emitting layer was formed on the n-type waveguide layer. The light emitting layer was formed to have a multiple quantum well structure in which quantum well layers and barrier layers were laminated in two periods. Here, the quantum well layer was an AlGaN layer (Al: 52%, i.e., Al 0.52 Ga 0.48 The barrier layer having a thickness of 6.0 nm was an AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 N layer). The light-emitting layer was formed at a temperature of 950°C, a reactor pressure of 300 mbar, and a V / III ratio of 4000. The growth rate of the quantum well layer was 0.18 μm / hr, and the growth rate of the barrier layer was 0.15 μm / hr.
[0112] Next, a p-type waveguide layer was formed as a second waveguide layer on the light emitting layer. The p-type waveguide layer was an AlGaN layer containing no dopants (Al: 63%, i.e., Al 0.63 Ga 0.37 The p-type waveguide layer was formed to a thickness of 70 nm under the conditions of a temperature of 950°C, a reactor pressure of 300 mbar, and a V / III ratio of 4000. The growth rate of the p-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, and triethylgallium (TEGa) was used as the Ga raw material.
[0113] Next, a second conductive cladding layer was formed on the p-type waveguide layer. The second conductive cladding layer is a compositionally graded layer with a gradient in the Al composition ratio. The layer is an AlGaN layer with a thickness of 2.5 nm and an Al composition distribution that varies from Al=0.63 to 1.0 in the direction away from the substrate, and a p-type AlGaN layer with a thickness of 330 nm and an Al composition distribution that varies from Al=1.0 to 0.7 in the direction away from the substrate. Before growing the second conductive cladding layer, the inflow of the metalorganic gas was temporarily stopped, and the reactor pressure was set to 50 mbar at a temperature of 950 °C while irradiating only hydrogen and NH3. The first layer (A) with a thickness of 72.5 nm and an Al composition of 0.63 → 1.0 → 0.95 was formed under the condition of a V / III ratio of 4000. The growth rate at this time was 0.3 to 0.5 μm / hr. Next, the inflow of the metalorganic gas was temporarily stopped, and the reactor pressure was set to 50 mbar at a temperature of 1050 °C while irradiating only hydrogen and NH3. The remaining layer (B) with a thickness of 257.5 nm and an Al composition of 0.95 → 0.7 was formed under the condition of a V / III ratio of 4000. The growth rate at this time was 0.3 to 0.5 μm / hr. Throughout the experiment, trimethylaluminum (TMAl) was used as the Al source, and triethylgallium (TEGa) was used as the Ga source. The interface between the above-mentioned layers (A) and (B) corresponds to the region P where the impurity concentration profile changes abruptly, or the composition discontinuous region Q where the Al composition is discontinuous in the direction away from the substrate.
[0114] Next, a p-type contact layer, which is a second conductive type contact layer, was formed on the second conductive type cladding layer. Here, the p-type contact layer was formed of an AlGaN layer and a GaN layer. The AlGaN layer was a p-type nitride semiconductor layer with a layer thickness of 30 nm, using Mg as a dopant impurity and with an Al composition distribution in the direction away from the substrate, varying from Al=0.7 to 0.4. The GaN layer was formed of GaN (i.e. Al:0%) with a thickness of 10 nm. The second conductive type contact layer was formed under the conditions of a temperature of 950° C., a reactor pressure of 150 mbar, and a V / III ratio of 3650. The growth rate of the second conductive type contact layer at this time was 0.2 μm / hr.
[0115] Various analyses were performed on the nitride semiconductor stack obtained as described above. As a result, the region in which the Al composition was graded at the interface between the well layer and the barrier layer in the light-emitting layer was 2.5 nm. α, which indirectly represents the potential fluctuation, was 146 meV. Next, a discontinuity in the Al composition was observed at the interface between the second conductive cladding layers (A) and (B), and the starting composition of (B) was 3% higher than that of (A). In addition, hydrogen was 5×10 18 cm -3 , Si is 5 × 10 18 cm -3 The FWHM of the hydrogen peak was 7.5 nm. Similarly, more oxygen and carbon were detected in (A) than in (B), and the concentration profile changed discontinuously at the interface between (A) and (B). The oxygen and carbon concentrations were 3×10 17 cm -3 and 3×10 17 cm -3 The second conductive contact layer was removed using SF6 gas, and the surface was observed. The surface shape had hexagonal irregularities, with a step height of 0.3 nm and a step density of 5 × 10 7 cm -2 It was.
[0116] The semiconductor laminate formed as described above was annealed in an N2 atmosphere at 700°C for 10 minutes or more to further reduce the resistance of the second conductive contact layer. A mesa structure was formed by exposing the first conductive cladding layer through dry etching using a gas containing Cl2 using an ICP. The formed mesa structure had a length of 700 μm in the <1-100> direction and a length of 40 μm in the <11-20> direction, where the length of the mesa structure in the <1-100> direction is the distance between the end faces of the cavity mirror in a plan view, and the length in the <11-20> direction is the distance between the side faces of the mesa structure.
[0117] On the second conductive contact layer of the mesa structure, Ni and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as p-type second electrodes. At this time, the width of the second electrode was 5 μm and the length was 600 μm or more. In addition, in the region where the n-type cladding layer of the mesa structure was exposed, V, Al, Ni, Ti, and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as n-type first electrodes. The first and second electrodes were annealed at 550° C. for 60 seconds in a nitrogen atmosphere using an RTA device. Furthermore, the substrate was divided into stripes by cleaving multiple times parallel to the <11-20> direction within the electrode metal region to form individual laser diodes. The length of the mesa structure in the <1-100> direction after division was 600 μm. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 8 V and the oscillation threshold current was 3 kA / cm. 2 The oscillation time was 100 seconds.
[0118] <Sample 2>~<Sample 5> Laser diodes of Samples 2 to 5 were fabricated in the same manner as Sample 1, except that the Al composition ratio of the n-type AlGaN layer using Si as a dopant impurity that constitutes the first conductivity type cladding layer was changed as shown in Table 1.
[0119] <Sample 6>~<Sample 9> Laser diodes of Samples 6 to 9 were fabricated in the same manner as Sample 1, except that the thickness of the first conductivity type cladding layer was changed as shown in Table 1.
[0120] <Sample 10>~<Sample 28> Laser diodes of Samples 10 to 28 were formed in the same manner as Sample 1, except that the wafer temperature and reactor pressure during the growth of the nitride semiconductor layer when forming the light emitting layer, and the first and second conductive type waveguide layers were changed as shown in Table 1. The growth temperature and growth pressure listed in the item for the light emitting layer in Table 1 are the temperatures during the formation of the light emitting layer, and the first and second waveguide layers. α, which indirectly represents the potential fluctuation of the first waveguide layer at this time, had the values shown in Table 1.
[0121] <Sample 29>~<Sample 32> Laser diodes of Samples 29 to 32 were fabricated in the same manner as Sample 1, except that the wafer temperature during the growth of the nitride semiconductor layer in forming the second conductive type cladding layer was changed as shown in Table 1. The discontinuity at the discontinuous point of the Al composition and the concentration of carbon or oxygen contained in the second conductive type cladding layer at this time were the values shown in Table 1, respectively.
[0122] <Sample 33>~<Sample 35> Laser diodes of Samples 33 to 35 were fabricated in the same manner as Sample 1, except that the reactor pressure during growth of the nitride semiconductor layer during partial formation of the substrate side of the second conductive type cladding layer was changed as shown in Table 2. The discontinuity at the discontinuous point of the Al composition and the concentration of carbon or oxygen contained in the second conductive type cladding layer at this time were the values shown in Table 2, respectively.
[0123] <Sample 36>~<Sample 39> Laser diodes Samples 36 to 39 were fabricated in the same manner as Sample 1, except that the wafer temperature during growth of the nitride semiconductor layer when forming the remaining part of the second conductive type cladding layer was changed as shown in Table 2. The discontinuity at the discontinuous point of the Al composition and the concentration of carbon or oxygen contained in the second conductive type cladding layer at this time were the values shown in Table 2, respectively.
[0124] <Sample 40>~<Sample 42> Laser diodes of Samples 40 to 42 were fabricated in the same manner as Sample 1, except that the reactor pressure during growth of the nitride semiconductor layer when forming the remaining part of the second conductive type cladding layer was changed as shown in Table 2. The discontinuity at the discontinuous point of the Al composition and the concentration of carbon or oxygen contained in the second conductive type cladding layer at this time were the values shown in Table 2, respectively.
[0125] <Sample 43>~<Sample 46> Laser diodes of Samples 43 to 46 were fabricated in the same manner as Sample 1, except that the thickness of the second conductive type cladding layer was changed as shown in Table 2. The discontinuity at the discontinuous point of the Al composition and the concentration of carbon or oxygen contained in the second conductive type cladding layer at this time were the values shown in Table 2, respectively.
[0126] <Sample 47>~<Sample 50> Laser diodes of Samples 47 to 50 were formed in the same manner as Sample 1, except that the thickness of the compositionally graded layer formed between the second conductive type waveguide layer and the second conductive type cladding layer was changed as shown in Table 2.
[0127] <Sample 51>~<Sample 55> Laser diodes of Samples 51 to 55 were fabricated in the same manner as Sample 1, except that the thickness of the portion of the second conductivity type cladding layer on the substrate side was changed as shown in Table 2. Here, the thickness of the portion of the second conductivity type cladding layer on the substrate side corresponds to the distance from the substrate side to a region where the Al composition becomes discontinuous or where the carbon or oxygen concentration profile decreases discontinuously.
[0128] <Sample 56>~<Sample 59> Laser diodes of Samples 56 to 59 were fabricated in the same manner as Sample 1, except that the thickness of the portion of the second conductivity type cladding layer on the substrate side was changed as shown in Table 2. Here, the thickness of the portion of the second conductivity type cladding layer on the substrate side corresponds to the distance from the substrate side to a region where the Al composition becomes discontinuous or where the carbon or oxygen concentration profile decreases discontinuously.
[0129] <Sample 60>~<Sample 61> Laser diodes of Samples 60 and 61 were formed in the same manner as Sample 1, except that the growth of the nitride semiconductor layer was not interrupted before or after forming a portion of the second conductivity type cladding layer on the substrate side.
[0130] <Sample 60> A laser diode of sample 60 was formed in the same manner as sample 1, except that the second conductive type cladding layer was formed so that there was no discontinuity in the Al composition at the interface between the portion of the second conductive type cladding layer on the substrate side and the remaining portion.
[0131] <Sample 61> A laser diode of sample 61 was formed in the same manner as sample 1, except that a second conductivity type cladding layer was formed in which the Al composition at the interface between a portion of the second conductivity type cladding layer on the substrate side and the remaining portion thereof was discontinuously decreased.
[0132] [Table 1]
[0133] [Table 2]
[0134] Laser diodes in which the growth of the nitride semiconductor layer was interrupted before and after forming a portion of the second conductive type cladding layer on the substrate side, and a region in which the concentration profile of carbon or oxygen contained in the second conductive type cladding layer discontinuously decreases at at least one location, such as Samples 1 to 59 in Tables 1 and 2, had lower threshold voltages and oscillation thresholds overall and longer oscillation times than Samples 60 to 63. It was confirmed that this achieved both suppression of cladding layer deterioration and improvement of carrier injection efficiency.
[0135] Although the embodiments of the present disclosure have been described above, the above embodiments are merely examples of devices and methods for embodying the technical ideas of the present disclosure, and the technical ideas of the present disclosure do not specify the materials, shapes, structures, arrangements, etc. of the components. The technical ideas of the present disclosure can be modified in various ways within the technical scope defined by the claims. [Explanation of symbols]
[0136] 1,2,3 Laser Diode 4 Light emitting element 10 Semiconductor laminate 11 Substrate 12 Buffer layer 13 1st electrode 14 2nd electrode 101 First conductive type cladding layer 102 First conductive type waveguide layer 103 Light-emitting layer 104 Second conductive type waveguide layer 105 Second conductive type cladding layer 106 Contact Layer
Claims
1. a nitride semiconductor substrate containing Al; a semiconductor laminate portion disposed on the nitride semiconductor substrate; Equipped with The semiconductor laminate portion is a first conductivity type cladding layer including a first conductivity type nitride semiconductor; a light emitting layer formed of a nitride semiconductor including one or more quantum wells and disposed on the first conductive type cladding layer; a second conductive type cladding layer disposed on the light emitting layer and made of a second conductive type nitride semiconductor containing Al; having The second conductive type cladding layer has at least one region in which a concentration profile of carbon or oxygen contained in the second conductive type cladding layer discontinuously decreases with increasing distance from the nitride semiconductor substrate. Nitride semiconductor element.
2. The region in which the concentration profile discontinuously decreases exists in a region of 5 nm to 110 nm from the nitride semiconductor substrate side of the second conductive type cladding layer. The nitride semiconductor device according to claim 1 .
3. The region of the second conductive type cladding layer where the concentration profile discontinuously decreases is d G (1-d) N (0.80≦d≦1.0) The nitride semiconductor device according to claim 1 or 2.
4. The carbon concentration in the region of the second conductive type cladding layer closer to the nitride semiconductor substrate than the region where the concentration profile of the second conductive type cladding layer discontinuously decreases is 1×10 17 cm -3 Above 1 x 10 18 cm -3 is less than or equal to The nitride semiconductor device according to claim 1 .
5. The second conductive type cladding layer has an oxygen concentration of 1×10 in a region closer to the nitride semiconductor substrate than the region where the concentration profile discontinuously decreases. 17 cm -3 Above 1 x 10 18 cm -3 is less than or equal to The nitride semiconductor device according to claim 1 .
6. The nitride semiconductor substrate is an AlN single crystal substrate. The nitride semiconductor device according to claim 1 .
7. The first conductive type cladding layer is made of Al a G (1-a) N (0.65<a≦0.9) The nitride semiconductor device according to claim 1 .
8. The thickness of the first conductive type cladding layer is 250 nm or more and 800 nm or less. The nitride semiconductor device according to claim 1 .
9. a first conductivity type waveguide layer disposed between the first conductivity type cladding layer and the light emitting layer to confine light to the light emitting layer; a second conductive type waveguide layer disposed between the second conductive type cladding layer and the light emitting layer to confine light to the light emitting layer; Equipped with The nitride semiconductor device according to claim 1 .
10. a second conductive type contact layer disposed on the second conductive type cladding layer and formed of a nitride semiconductor containing GaN; The second conductive type cladding layer is made of Al d G (1-d) N (0.1≦d≦1), has a composition gradient in which the Al composition d decreases with increasing distance from the nitride semiconductor substrate, and has a film thickness of 500 nm or less. The nitride semiconductor device according to claim 1 .
11. The second conductive type cladding layer has a composition gradient in which the Al composition ratio d changes from 1 to 0.7 with increasing distance from the nitride semiconductor substrate side. The nitride semiconductor device according to claim 10.
12. The thickness of the second conductive type cladding layer is 250 nm or more and 500 nm or less. The nitride semiconductor device according to claim 10 or 11.
13. The thickness T0 of the first conductive type cladding layer is 3500a-2150 nm or more and 26500a-17850 nm or less (a is the Al composition a of the nitride semiconductor constituting the first conductive type cladding layer). The nitride semiconductor device according to claim 1 .
14. The resistivity of the first conductive type cladding layer is 1×10 -3 Ωcm or more 5×10 -3 Ωcm or less The nitride semiconductor device according to claim 13.
15. forming a first conductivity type cladding layer containing a first conductivity type nitride semiconductor on a nitride semiconductor substrate containing Al; forming a light emitting layer on the first conductive type cladding layer using a nitride semiconductor including one or more quantum wells; forming a part of a second conductivity type cladding layer including a second conductivity type nitride semiconductor under the conditions of a wafer temperature of 900° C. or more and 1000° C. or less and a reactor pressure of 15 mbar or more and 350 mbar or less; A remaining part of the second conductive type cladding layer is formed under the conditions that the wafer temperature is 1030° C. or more and 1100° C. or less and the reactor pressure is 15 mbar or more and 350 mbar or less to form a semiconductor laminate portion on the nitride semiconductor substrate. A method for manufacturing a nitride semiconductor device.
16. The reactor pressure during the formation of a portion of the second conductive type cladding layer is 15 mbar or more and 100 mbar or less. The method for producing a nitride semiconductor device according to claim 15 .
17. an organometallic gas is introduced during the formation of the first conductive type cladding layer, the light emitting layer, and the second conductive type cladding layer; After forming the light emitting layer, the flow of the metal-organic gas is temporarily stopped before forming a part of the second conductive type cladding layer; After forming a portion of the second conductive type cladding layer, and before forming a remaining portion of the second conductive type cladding layer, the flow of the metal-organic gas is temporarily stopped. The method for manufacturing a nitride semiconductor device according to claim 15 or 16.