Nitride semiconductor device and method of manufacturing the same
By forming opening regions in the inactive areas of the nitride semiconductor layer and using a conductive layer with high etching selectivity, the device addresses substrate warpage issues, achieving a simpler and cost-effective nitride semiconductor structure.
Patent Information
- Application Number
- JP2023056135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Nitride semiconductor devices face issues with substrate warpage due to differences in thermal expansion coefficients between the substrate and the nitride semiconductor layer, leading to structural complications and increased manufacturing costs.
The device incorporates a nitride semiconductor layer with defined active and inactive regions, where portions of the inactive region are removed to form opening regions, reducing the contact area between the substrate and the semiconductor layer, and employs a conductive layer with high etching selectivity to mitigate warpage.
This approach results in a nitride semiconductor device with a simpler structure that effectively reduces substrate warpage, maintaining device performance while minimizing manufacturing complexity and costs.
Smart Images

Figure 2024143445000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride semiconductor device and a method for manufacturing the same. [Background technology]
[0002] High electron mobility transistors (HEMTs) are widely used as high-speed switching devices and high-frequency amplification devices. In addition, the use of nitride semiconductors with a large band gap in the HEMT structure makes it possible to achieve high-speed operation and high voltage resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-077865 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a nitride semiconductor device that reduces warpage of a substrate with a simple structure, and a manufacturing method thereof. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems, one aspect of the present disclosure is a nitride semiconductor device comprising: a substrate having opposite sides defined by a first side and a second side opposed to each other; and a nitride semiconductor layer provided on the first side of the substrate, the nitride semiconductor layer including an active region and an inactive region, the inactive region having an opening region where at least a portion of the nitride semiconductor layer has been removed to reach the substrate.
[0006] Another aspect of the present disclosure is a method for manufacturing a nitride semiconductor device, comprising: forming a nitride semiconductor layer on a first surface of a substrate having both surfaces defined by a first surface and a second surface opposed to each other; forming an active region and an inactive region in the nitride semiconductor layer; selectively etching a portion of the nitride semiconductor layer to form a through region that penetrates the nitride semiconductor layer in the active region and an opening region that penetrates the nitride semiconductor layer in the inactive region; filling the through region with a conductive layer of a material having a high etching selectivity with respect to the substrate; forming an insulating layer on the nitride semiconductor layer; etching an opening in the insulating layer to form a drain electrode and a source electrode in ohmic contact with the nitride semiconductor layer; etching away the insulating layer to form a gate electrode in Schottky contact with the nitride semiconductor layer; selectively etching a portion of the substrate from a second surface of the substrate to form a through hole reaching the conductive layer; forming a first electrode layer in contact with the conductive layer in the through hole; and forming a second electrode layer in contact with the first electrode layer on the second surface. Effect of the Invention
[0007] According to one aspect and another aspect of the present disclosure, it is possible to provide a nitride semiconductor device that reduces warpage of a substrate with a simple structure and a manufacturing method thereof. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a plan view of a nitride semiconductor device according to an embodiment. [Figure 2A] FIG. 2A is a cross-sectional view taken along line II in FIG. [Figure 2B] FIG. 2B is a cross-sectional view taken along line II-II in FIG. [Figure 2C] FIG. 2C is a cross-sectional view of a laminated structure of a first nitride semiconductor layer and a second nitride semiconductor layer. [Figure 2D] FIG. 2D is a cross-sectional view of an example in which the substrate and the nitride semiconductor region have an upwardly convex warp. [Figure 2E] FIG. 2E is a cross-sectional view of an example in which the substrate and the nitride semiconductor region have a downward convex warp. [Figure 3A]FIG. 3A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 3B] FIG. 3B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 4A] FIG. 4A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 4B] FIG. 4B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 5A] FIG. 5A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 5B] FIG. 5B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 6A] FIG. 6A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 6B] FIG. 6B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 7A] FIG. 7A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 7B] FIG. 7B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 8A] FIG. 8A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 8B] FIG. 8B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 9A] FIG. 9A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 9B]FIG. 9B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 10A] FIG. 10A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 10B] FIG. 10B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 11A] FIG. 11A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 11B] FIG. 11B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing the nitride semiconductor device according to the embodiment. [Figure 12A] FIG. 12A is a cross-sectional view taken along line II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. [Figure 12B] FIG. 12B is a cross-sectional view taken along line II-II in FIG. 1, showing a step of the method for manufacturing a nitride semiconductor device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the nitride semiconductor device of the present disclosure will be described with reference to the accompanying drawings. Note that, for simplicity and clarity of description, components shown in the drawings are not necessarily drawn to scale. Also, hatching lines may be omitted in cross-sectional views to facilitate understanding. The accompanying drawings are merely illustrative of embodiments of the present disclosure and should not be considered as limiting the present disclosure.
[0010] The following detailed description includes apparatus and methods embodying exemplary embodiments of the present disclosure. This detailed description is merely explanatory in nature and is not intended to limit the embodiments of the present disclosure or the application and uses of such embodiments.
[0011] In the following description, the direction perpendicular to the substrate extending on the XY plane is referred to as the Z direction, the direction in which the electrodes extend perpendicular to the Z direction is referred to as the Y direction, and the direction in which the electrodes are arranged perpendicular to the Z direction and the Y direction is referred to as the X direction.
[0012] (Embodiment) (Plane layout of nitride semiconductor device) Fig. 1 is a plan view of a nitride semiconductor device according to an embodiment. The nitride semiconductor device 1 may include an insulating layer 16, and a source electrode 18E and a drain electrode 20E formed on the insulating layer 16. The Z-axis direction of mutually orthogonal XYZ axes shown in Fig. 1 is a direction orthogonal to a first surface 2a (see Figs. 2A to 2C) of a substrate 10 described later. The term "plan view" used in this specification means viewing the nitride semiconductor device 1 from above along the Z direction, unless otherwise specified explicitly.
[0013] The insulating layer 16 can be composed of any insulating material capable of insulating the source electrode 18E from the drain electrode 20E. For example, the insulating layer 16 can include SiO2, SiN, SiON, Al2O3, AlN, AlON, HfO, HfN, HfON, HfSiON, AlON, or any combination thereof.
[0014] The source electrode 18E and the drain electrode 20E can be composed of one or more conductive materials. For example, the source electrode 18E and the drain electrode 20E can each include Au, Ti, TiN, Pt, Cu, Al, AlSiCu, AlCu, or any combination thereof.
[0015] As shown in FIG. 1, a plurality of source electrodes 18E may be arranged. In the illustrated example, the source electrode 18E extends in the Y direction, and the plurality of source electrodes 18E are arranged in the X direction. Similarly, the drain electrode 20E may include a base portion 20A and a plurality of drain fingers 20B connected to the base portion 20A. In the illustrated example, the base portion 20A extends in the X direction, and the plurality of drain fingers 20B extend in the Y direction. In the present disclosure, the X direction and the Y direction are also referred to as the "first direction" and the "second direction", respectively. The plurality of source electrodes 18E and the plurality of drain fingers 20B may be arranged alternately while being spaced apart from each other. In the illustrated example, the plurality of source electrodes 18E and the plurality of drain fingers 20B are arranged alternately in the X direction.
[0016] The nitride semiconductor device 1 may further include a gate wiring 19A and a plurality of gate electrodes 19 connected to the gate wiring 19A. The gate wiring 19A and the plurality of gate electrodes 19 may be disposed in a lower layer than the source electrode 18E and the drain electrode 20E, and may be covered by the insulating layer 16.
[0017] In the illustrated example, the gate wiring 19A extends in the X direction, and the gate electrodes 19 extend in the Y direction. Each gate electrode 19 may be disposed between one of the source electrodes 18 and one of the drain fingers 20B in a plan view. In the illustrated example, each gate electrode 19 is disposed between the source electrode 18 and the drain finger 20B that face each other in the X direction in a plan view. The gate wiring 19A may extend between the source electrodes 18E and the drain fingers 20B in a plan view. Further details of the gate electrodes 19 will be described later with reference to FIGS. 2A to 2C.
[0018] The nitride semiconductor device 1 also includes an active region 300 including a two-dimensional electron gas layer in plan view, and an inactive region 200 not including the two-dimensional electron gas layer. In Fig. 1, the active region 300 is shown surrounded by a dashed line. The nitride semiconductor device 1 includes, in at least a part of the inactive region 200, opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 where the nitride semiconductor layer 12 has been removed and which reach the substrate 10. The opening regions will be described in detail later.
[0019] (Cross-sectional structure of a nitride semiconductor device) Fig. 2A is a cross-sectional view taken along line II in Fig. 1. Fig. 2B is a cross-sectional view taken along line II-II in Fig. 1. Fig. 2C is a cross-sectional view of a laminated structure of a first nitride semiconductor layer and a second nitride semiconductor layer.
[0020] The nitride semiconductor device 1 includes a substrate 10 having both sides defined by a first surface 2a and a second surface 2b opposed to each other, and a nitride semiconductor layer 12 disposed on the first surface 2a of the substrate 10. The substrate 10 is, for example, a hexagonal silicon carbide substrate (SiC substrate). The first surface 2a and the second surface 2b are main surfaces of the substrate 10, and the first surface 2a is also referred to as the front surface of the substrate 10, and the second surface 2b is also referred to as the back surface of the substrate 10. The first surface 2a is a surface of the substrate 10 on which the nitride semiconductor layer 12 is epitaxially grown. The first surface 2a is parallel to a first direction (X direction) and a second direction (Y direction) perpendicular to the first direction in a plan view.
[0021] The substrate 10 is a SiC substrate having an off angle θoff. The first surface 2a is inclined at the off angle θoff in a specific crystal direction with respect to the c-plane. The off angle θoff may be 2° or more and 6° or less. More preferably, the off angle θoff may be 3° or more and 5° or less, and further preferably, 3.5° or more and 4.5° or less. In this disclosure, the term "c-plane" is used to refer to the (0001) plane of a hexagonal SiC crystal.
[0022] In this embodiment, the specific crystal direction may be the [11-20] direction. That is, the first face 2a may be inclined at an off angle θoff of 2° to 6° in the [11-20] direction with respect to the c-plane. In addition, in the indexes representing crystal directions and faces in the present disclosure, a number preceded by a minus sign (for example, "2" in the case of the [11-20] direction) means the number with a bar above it.
[0023] The substrate 10 may be a 4H-SiC substrate. Here, "4H" represents the polytype of SiC crystal. In the following, a case where the substrate 10 is a 4H-SiC substrate will be described as an example. The substrate 10 may be conductive. The resistivity of the substrate 10 may be, for example, 0.01 Ω·cm or more and 0.03 Ω·cm or less. In this embodiment, the resistivity of the substrate 10 may be about 0.02 Ω·cm. In addition, the thickness of the substrate 10 may be, for example, 30 μm or more and 300 μm or less. In this embodiment, the substrate 10 may have a thickness of 150 μm.
[0024] The nitride semiconductor layer 12 is epitaxially grown on the first face 2a of the substrate 10. In this embodiment, the nitride semiconductor layer 12 may include a buffer layer formed on the substrate 10 and a semi-insulating layer formed on the buffer layer.
[0025] The buffer layer may be made of any material capable of suppressing, for example, warping of the substrate 10 caused by mismatching of the thermal expansion coefficient between the substrate 10 and the semi-insulating layer, or occurrence of cracks in the nitride semiconductor device 1. For example, the buffer layer may include at least one of an aluminum nitride (AlN) layer, an aluminum gallium nitride (AlGaN) layer, and a graded AlGaN layer having different aluminum (Al) compositions. The buffer layer may be made of a single AlN layer, a single AlGaN layer, a layer having an AlGaN / GaN superlattice structure, a layer having an AlN / AlGaN superlattice structure, or a layer having an AlN / GaN superlattice structure. In this embodiment, the buffer layer may include a first buffer layer that is an AlN layer formed on the first surface 2a of the substrate 10, and a second buffer layer that is an AlGaN layer formed on the AlN layer. The thickness of the buffer layer may be 5 nm or more and 2 μm or less. In this embodiment, the buffer layer may have a thickness of about 0.8 μm.
[0026] The semi-insulating layer may be a GaN layer doped with an impurity. The semi-insulating layer may be provided to suppress leakage current. The impurity may be, for example, carbon (C) or iron (Fe). Alternatively, the impurity may be both C and Fe. The impurity may be such that the difference between the acceptor concentration Na and the donor concentration Nd (Na-Nd) is 1×10 17 cm -3 The GaN layer may be doped to about 1 μm. The thickness of the semi-insulating layer may be 1 μm or more and 10 μm or less. In this embodiment, the semi-insulating layer may have a thickness of 2 μm.
[0027] As shown in FIG. 2C, the nitride semiconductor layer 12 includes an electron traveling layer 120 as a first nitride semiconductor layer and an electron supply layer 122 as a second nitride semiconductor layer that forms a heterojunction with the first nitride semiconductor layer. The first nitride semiconductor layer includes a two-dimensional electron gas layer 121 at the interface with the second nitride semiconductor layer. The active region 300 includes the two-dimensional electron gas layer 121 in plan view. The inactive region 200 does not include the two-dimensional electron gas layer 121 in plan view. In other words, the inactive region 200 is a region where the main current of the nitride semiconductor device 1 does not flow.
[0028] The electron traveling layer 120 may be formed on a semi-insulating layer. The electron traveling layer 120 is composed of a nitride semiconductor. The electron traveling layer 120 can be composed of GaN. In the present embodiment, the electron traveling layer 120 may be an n-type GaN layer doped with donor impurities. In another example, the electron traveling layer 120 may be an undoped GaN layer. The thickness of the electron traveling layer 120 may be 0.05 μm or more and 1 μm or less. In the present embodiment, the electron traveling layer 120 may have a thickness of about 0.2 μm.
[0029] The electron supply layer 122, which is the second nitride semiconductor layer, is composed of a nitride semiconductor having a larger bandgap than the electron traveling layer 120. In the present embodiment, the electron supply layer 122 may be composed of Al x Ga 1-x N, where 0 < x ≤ 1, and more preferably, 0.1 < x < 0.3. Note that as the Al composition increases, the bandgap of AlGaN increases. In the present embodiment, X = 0.2 may be used. The thickness of the electron supply layer 122 may be 1 nm or more and 100 nm or less. In the present embodiment, the electron supply layer 122 may have a thickness of about 20 nm.
[0030] The electron transit layer 120 and the electron supply layer 122 are made of nitride semiconductors having different lattice constants. Therefore, the nitride semiconductor (e.g., GaN) constituting the electron transit layer 120 and the nitride semiconductor (e.g., AlGaN) constituting the electron supply layer 122 form a lattice-mismatched heterojunction. The energy level of the conduction band of the electron transit layer 120 near the heterojunction interface is lower than the Fermi level due to spontaneous polarization of the electron transit layer 120 and the electron supply layer 122 and piezoelectric polarization caused by crystal distortion near the heterojunction interface. As a result, a two-dimensional electron gas layer 121 is formed in the electron transit layer 120 at a position close to the heterojunction interface between the electron transit layer 120 and the electron supply layer 122 (for example, within a range of about several nm from the interface). The two-dimensional electron gas layer 121 in the electron transit layer 120 functions as a channel of the nitride semiconductor device 1. The sheet carrier density of the two-dimensional electron gas layer 121 generated in the electron transit layer 120 can be increased by increasing at least one of the Al composition and the thickness of the electron supply layer 122.
[0031] The nitride semiconductor device 1 may further include an insulating layer 14 formed on the electron supply layer 122. A source contact opening 14S, a drain contact opening 14D, and a gate contact opening 14G exposing the surface of the electron supply layer 122 are formed in the insulating layer 14. The source contact opening 14S and the drain contact opening 14D are spaced apart in the X direction. The gate contact opening 14G is located between the source contact opening 14S and the drain contact opening 14D spaced apart in the X direction. The insulating layer 14 may include SiO2, SiN, SiON, Al2O3, AlN, AlON, HfO, HfN, HfON, HfSiON, AlON, or any combination thereof.
[0032] In this embodiment, the insulating layer 14 may be SiN. The thickness of the insulating layer 14 may be, for example, 10 nm or more and 200 nm or less. In this embodiment, the insulating layer 14 may have a thickness of about 100 nm.
[0033] The nitride semiconductor device 1 includes a gate electrode 19, a source electrode 18, and a drain electrode 20 arranged on a nitride semiconductor layer 12. The source electrode 18 and the drain electrode 20 are spaced apart in a first direction (X direction). The gate electrode 19 is arranged between the source electrode 18 and the drain electrode 20 that are spaced apart in the first direction. The source electrode 18, the drain electrode 20, and the gate electrode 19 are arranged so as to enable electrons to travel in the first direction through a two-dimensional electron gas layer 121. The source electrode 18 is in contact with the electron supply layer 122 through a source contact opening 14S. The drain electrode 20 is in contact with the electron supply layer 122 through a drain contact opening 14D. The gate electrode 19 is in contact with the electron supply layer 122 through a gate contact opening 14G.
[0034] The source electrode 18 and the drain electrode 20 may be made of any material capable of forming an ohmic contact with the nitride semiconductor layer 12. In this embodiment, the source electrode 18 and the drain electrode 20 may include a Ti layer and an Al layer. In this case, the Ti layer may be located between the nitride semiconductor layer 12 and the Al layer. In one example, the Ti layer may have a thickness of about 20 nm, and the Al layer may have a thickness of about 300 nm. In another example, the source electrode 18 and the drain electrode 20 may include a Ta layer and an Al layer. In yet another example, the source electrode 18 and the drain electrode 20 may include a Ti layer, an Al layer, a Ni layer, and an Au layer, in this order from the side closer to the nitride semiconductor layer 12.
[0035] The gate electrode 19 may be made of any material that forms a Schottky contact with the nitride semiconductor layer 12. In this embodiment, the gate electrode 19 may include a Ni layer and an Au layer. In this case, the Ni layer may be located between the nitride semiconductor layer 12 and the Au layer. In one example, the Ni layer may have a thickness of 10 nm, and the Au layer may have a thickness of 600 nm.
[0036] The gate electrode 19 is disposed between the source electrode 18 and the drain electrode 20 that are spaced apart in the first direction (X direction) and extends in the second direction (Y direction) (see FIG. 1). The source electrode 18 and the drain electrode 20 also extend in the second direction (Y direction). That is, the source electrode 18, the gate electrode 19, and the drain electrode 20 that extend in the second direction (Y direction) are arranged in this order in the first direction (X direction). Therefore, between the source electrode 18 and the drain electrode 20, electrons can travel in the first direction (X direction) through the two-dimensional electron gas layer 121 of the electron travel layer 120. The source electrode 18, the gate electrode 19, and the drain electrode 20 are disposed so that the first direction (X direction) (i.e., the electron travel direction) satisfies a predetermined relationship with a specific crystal direction (e.g., [11-20]) of the substrate 10.
[0037] The nitride semiconductor device 1 may further include an insulating layer 16 formed on the insulating layer 14. A first opening 16S exposing the surface of the source electrode 18 and a second opening 16D exposing the surface of the drain electrode 20 are formed in the insulating layer 16. The insulating layer 16 may include SiO2, SiN, SiON, Al2O3, AlN, AlON, HfO, HfN, HfON, HfSiON, AlON, or any combination thereof. In this embodiment, the insulating layer 16 may be SiO2. Also, the insulating layer 16 may have a thickness of about 500 nm.
[0038] The source electrode 18E and the drain electrode 20E are formed on the insulating layer 16. The source electrode 18E is connected to the source electrode 18 through a first opening 16S. The drain electrode 20E is connected to the drain electrode 20 through a second opening 16D.
[0039] The above description with reference to FIGS. 2A to 2C focuses on one source electrode 18, one drain electrode 20, and the gate electrode 19 disposed therebetween. However, the nitride semiconductor device 1 may include a plurality of gate electrodes 19, a plurality of source electrodes 18, and a plurality of drain electrodes 20 disposed on the nitride semiconductor layer 12. Each of the plurality of source electrodes 18 can be connected to one of the plurality of source electrodes 18E (see FIG. 1) through a first opening 16S. Similarly, each of the plurality of drain electrodes 20 can be connected to one of the plurality of drain fingers 20B (see FIG. 1) through a second opening 16D. The plurality of source electrodes 18E and the plurality of drain electrodes 20E can be alternately disposed in a first direction (X direction). Also, each of the plurality of gate electrodes 19 can be disposed between one of the plurality of source electrodes 18E and one of the plurality of drain electrodes 20E.
[0040] As shown in FIG. 1, FIG. 2A, and FIG. 2B, the nitride semiconductor device 1 according to the embodiment includes a substrate 10 having both sides defined by a first surface 2a and a second surface 2b facing each other, and a nitride semiconductor layer 12 provided on the substrate 10 and including an active region 300 and an inactive region 200. The substrate 10 may be a SiC substrate having a 6H-SiC crystal structure in addition to a SiC substrate having a 4H-SiC crystal structure. The 6H-SiC crystal structure is frequently used as a SiC substrate together with the 4H-SiC crystal structure. The substrate 10 may also be a silicon substrate (Si substrate). Since there is a large difference in thermal expansion coefficient between a Si substrate and a nitride semiconductor, when a Si substrate is used for the substrate 10, it is effective in suppressing warpage of the substrate 10, which will be described later.
[0041] As described above, a SiC substrate or a Si substrate is used as the substrate 10. For this reason, due to the difference in lattice constant between the substrate 10 and the nitride semiconductor layer 12, for example, when the substrate 10 is cooled after the nitride semiconductor layer 12 is formed on the substrate 10, warping occurs in the laminate of the substrate 10 and the nitride semiconductor layer 12 (hereinafter also referred to as the "base"). The larger the contact area between the substrate 10 and the nitride semiconductor layer 12, the larger the warping of the base. In the nitride semiconductor device 1, in order to suppress warping of the base, the inactive region 200 is provided with opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110, in which a part of the nitride semiconductor layer 12 is removed and reaches the substrate 10. In the following, when opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 are not limited, they are also referred to as "opening region 100." By forming opening region 100 in nitride semiconductor layer 12, the contact area between substrate 10 and nitride semiconductor layer 12 is reduced, and warping of the base in nitride semiconductor device 1 can be suppressed.
[0042] The opening regions 102, 103, 104, 105, 107, 108, 109, and 110 are arranged in the inactive region 200 located in the second direction (Y direction) in which the drain electrode 20, the source electrode 18, and the gate electrode 19 extend as viewed from the active region 300. Although a plurality of opening regions are arranged in the illustrated example, they may be formed integrally.
[0043] The opening regions 101 and 106 are arranged in the inactive region 200 located in a first direction (X direction) in which the drain electrode 20, the source electrode 18, and the gate electrode 19 are arranged as viewed from the active region 300. In other words, in the nitride semiconductor device 1, the opening regions 101 and 106 are arranged at the ends of the substrate 10 in the X direction in a plan view. The opening regions 101 and 106 have areas relatively larger than the opening regions 102, 103, 104, 105, 107, 108, 109, and 110.
[0044] FIG. 2D is a cross-sectional view of an example in which the substrate 10 and the nitride semiconductor layer 12 have a convex warp on the top. Here, "up" indicating the direction of the warp is the direction toward the nitride semiconductor layer 12 as viewed from the substrate 10. As shown in FIG. 2D, when the substrate 10 and the nitride semiconductor layer 12 have a convex warp on the top, the stress that the nitride semiconductor layer 12 exerts on the substrate 10 is a tensile stress in the direction indicated by the arrow TS. Also, FIG. 2E is a cross-sectional view of an example in which the substrate 10 and the nitride semiconductor layer 12 have a convex warp on the bottom. Here, "down" indicating the direction of the warp is the opposite direction to the direction toward the nitride semiconductor layer 12 as viewed from the substrate 10. As shown in FIG. 2E, when the substrate 10 and the nitride semiconductor layer 12 have a convex warp on the bottom, the stress that the nitride semiconductor layer 12 exerts on the substrate 10 is a compressive stress in the direction indicated by the arrow CS. Note that FIG. 2D shows an example in which a tensile stress acts in the X direction, but there are also cases in which a tensile stress acts in the Y direction. Although FIG. 2E shows an example in which compressive stress acts in the X direction, compressive stress may also act in the Y direction.
[0045] In the nitride semiconductor device 1 according to the embodiment, the warp of the substrate 10 may be 1 μm or less per 100 mm.
[0046] In addition, the substrate 10 may have a convex warp of 10 μm or more in 100 mm conversion, and the stress acting on the substrate 10 by the nitride semiconductor layer 12 may be tensile stress. For example, when the substrate 10 alone has a convex warp of 10 μm or more on the first surface 2a, and when the nitride semiconductor layer 12 acts on the substrate 10 with tensile stress, the warp of the substrate 10 alone and the warp due to the tensile stress are in the same direction. Therefore, the effect of forming the opening region 100 in the nitride semiconductor layer 12 is more effective. Furthermore, when the substrate 10 has a convex warp of 20 μm or more in 100 mm conversion, and the stress acting on the substrate 10 by the nitride semiconductor layer 12 is tensile stress, the effect of forming the opening region 100 in the nitride semiconductor layer 12 is also effective.
[0047] The substrate may have a downwardly convex warp of 10 μm or more in 100 mm conversion, and the stress that the nitride semiconductor layer 12 exerts on the substrate 10 may be compressive stress. For example, when the substrate 10 alone has a convex warp of 10 μm or more on the second surface 2b, and compressive stress acts on the substrate 10 due to the nitride semiconductor layer 12, the warp of the substrate 10 alone and the warp due to compressive stress are in the same direction. Therefore, the effect of forming the opening region 100 in the nitride semiconductor layer 12 is more effective. Furthermore, when the substrate 10 has a downwardly convex warp of 20 μm or more in 100 mm conversion, and the stress that the nitride semiconductor layer 12 exerts on the substrate 10 is compressive stress, the effect of forming the opening region 100 in the nitride semiconductor layer 12 is also effective.
[0048] Materials such as AlGaN and InAlGaN are used for the electron supply layer 122 of the nitride semiconductor layer 12. Semiconductor materials such as silicon (Si) and sapphire (Al2O3) are often used for the substrate 10 for epitaxial growth in addition to SiC. Due to the difference in thermal expansion coefficient between the substrate 10 for epitaxial growth and the nitride semiconductor layer 12, warping occurs in the substrate 10 when the crystal growth apparatus is cooled to room temperature after the formation of the epitaxial film.
[0049] At this time, whether the stress acting on the substrate 10 by the nitride semiconductor layer 12 is compressive or tensile stress depends on the crystal growth conditions and the cooling method of the device. It is generally believed that the performance of a semiconductor device is higher when compressive stress is acting. Compound semiconductor substrates such as SiC may have substrate warpage even when used alone due to thermal gradients and thermal fluctuations during crystal growth. If the direction of the warpage of the substrate alone coincides with the direction of the warpage caused by the stress acting on the substrate 10 by the epitaxial film, the substrate 10 will have a larger warpage. As a method for improving the warpage of the substrate 10, a method is also possible in which stress is intentionally incorporated into the electron transit layer during crystal growth, thereby offsetting the warpage of the substrate 10. For example, a superlattice buffer that forms a multi-period stacked structure of AlN / GaN as a buffer layer of the epitaxial structure, or a graded buffer that combines several layers of AlGaN layers with different compositions is formed. In this way, the stress is intentionally incorporated into the electron transit layer during crystal growth, thereby offsetting the stress applied when the substrate is cooled, and reducing the warpage of the substrate 10. However, the method of intentionally incorporating stress in the electron transport layer by forming a buffer layer or the like complicates the device structure and lengthens the time required for crystal growth, resulting in increased manufacturing costs.
[0050] In the nitride semiconductor device 1 according to the embodiment, the open region formed in the nitride semiconductor layer 12 reduces warping of the substrate 10 due to stress acting on the substrate 10 from the nitride semiconductor layer 12. Therefore, the nitride semiconductor device 1 can reduce warping of the substrate 10 with a simple structure, thereby suppressing an increase in manufacturing costs.
[0051] (Manufacturing method) Figures 3A to 12A are cross-sectional views taken along line II in Figure 1, illustrating a step of a method for manufacturing a nitride semiconductor device according to an embodiment. Figures 3B to 12B are cross-sectional views taken along line II-II in Figure 1, illustrating a step of a method for manufacturing a nitride semiconductor device according to an embodiment.
[0052] The manufacturing method of the nitride semiconductor device 1 according to the embodiment includes the following steps. A nitride semiconductor layer 12 is formed on the first surface 2a of the substrate 10, and an active region 300 and an inactive region 200 are formed in the nitride semiconductor layer 12. The nitride semiconductor layer 12 is etched to form a through region 25E in the active region 300 and an opening region 100 in the inactive region. The through region 25E is filled with a conductive layer 22 made of a material having a high etching selectivity with respect to the substrate 10. An insulating layer 14 is formed on the nitride semiconductor layer 12, and the insulating layer 14 is opened by etching to form a drain electrode 20 and a source electrode 18 in ohmic contact with the nitride semiconductor layer 12, and a gate electrode 19 in Schottky contact with the nitride semiconductor layer 12 is formed. A part of the substrate 10 is selectively etched from the second surface 2b to form a through hole 25A reaching the conductive layer 22. A first electrode layer 24E in contact with conductive layer 22 is formed in through hole 25A, and a second electrode layer 24B in contact with first electrode layer 24E is formed on second surface 2b of substrate 10. Hereinafter, the method for manufacturing the nitride semiconductor device according to the embodiment will be described in detail with reference to the drawings.
[0053] (A) First, as shown in Figures 3A and 3B, a nitride semiconductor layer 12 is formed on a first surface 2a of a substrate 10 by epitaxial growth. In the following description, the substrate 10 is assumed to be a SiC substrate. Since a SiC substrate tends to be significantly warped as a single body, forming an opening region in the nitride semiconductor layer 12 has a significant effect in suppressing the warping of the substrate 10.
[0054] (B) Next, as shown in FIG. 4A and FIG. 4B, an inactive region 200 is formed in a part of the first surface 2a of the nitride semiconductor layer 12 by using an ion implantation technique. Here, for example, argon (Ar) is ion-implanted into the first surface 2a of the nitride semiconductor layer 12 to form a modified layer in the vicinity of the first surface 2a of the nitride semiconductor layer 12, thereby forming the inactive region 200. In addition to argon (Ar), for example, ion implantation of nitrogen, oxygen, etc. may be performed. Also, the inactive region 200 can be formed by removing an upper part of a part of the nitride semiconductor layer 12 to be the inactive region 200 by dry etching such as reactive ion etching (RIE) and forming a mesa structure as the active region 300. By performing mesa etching by a method such as dry etching, the part of the inactive region 200 where the two-dimensional electron gas layer 121 is formed can be removed, and the inactive region 200 and the active region 300 can be formed separately.
[0055] (C) Next, as shown in Figures 5A and 5B, a portion of the nitride semiconductor layer 12 is selectively etched away using an inductively coupled plasma (ICP) etching technique to open the nitride semiconductor layer 12 so as to expose the substrate 10. As an etching gas, for example, a chlorine-based gas such as Cl2 or BCl3 can be used. As a result, a through region 25E is formed in the active region 300, and an opening region 100 is formed in the inactive region 200.
[0056] (D) Next, as shown in FIG. 6A and FIG. 6B, a conductive layer 22, which will become an etching stop layer in a process described later, is embedded in the through region 25E opened in the active region 300. Here, the material of the conductive layer 22 may be any material that has a high etching selectivity with respect to the substrate 10. For example, when the substrate 10 is a SiC substrate, nickel (Ni), aluminum (Al), copper (Cu), indium tin oxide (ITO), etc. can be used as the material of the conductive layer 22. The thickness of the conductive layer 22 is, for example, about 0.3 μm to 3 μm. The conductive layer 22 can be formed by techniques such as sputtering, vacuum deposition, and plating.
[0057] (E) Next, as shown in FIG. 7A and FIG. 7B, an insulating layer 14 is formed on the nitride semiconductor layer 12 by using, for example, a plasma-enhanced chemical vapor deposition (PECVD) method. As the insulating layer 14, for example, a SiN layer is used. The thickness of the SiN layer is about 100 nm. As another insulating layer 14, for example, a material such as SiON, SiO2, Al2O3, AlN, AlON, HfO, HfN, HfON, HfSiON, etc. may be used. As another method for forming the insulating layer 14, a low pressure chemical vapor deposition (LPCVD) method, a sputtering method, an atomic layer deposition (ALD) method, a molecular beam epitaxial growth (MBE) method, etc. may be used. Note that, as shown in FIG. 7A, the insulating layer 14 is also formed on the conductive layer 22 in the active region 300. 7B, the insulating layer 14 is formed on the substrate 10 and the ion-implanted layer 13 in the inactive region 200. In addition, the insulating layer 14 is formed also on the first surface 2a of the substrate 10 and the sidewall of the nitride semiconductor layer 12 in the open region 100.
[0058] (F) Next, as shown in FIG. 8A and FIG. 8B, a window is opened in the insulating layer 14 by RIE or the like, and a drain electrode 20 and a source electrode 18 are formed in ohmic contact with the nitride semiconductor layer 12 in the opened region of the insulating layer 14. The source electrode 18 also extends onto the conductive layer 22 and is electrically connected to the conductive layer 22. The ohmic contact of the drain electrode 20 and the source electrode 18 can be realized by forming Ti / Al on the nitride semiconductor layer 12 by electron beam (EB) deposition and maintaining the temperature at about 500 to 550°C. In this embodiment, the thickness of the Ti layer is about 20 nm, and the thickness of the Al layer is about 300 nm. The drain electrode 20 and the source electrode 18 may be made of, for example, Ta / Al. In addition, a sputtering device or MBE device may be used as a film forming device.
[0059] (G) Next, as shown in Figures 9A and 9B, a window is opened in the insulating layer 14 by RIE or the like, and a gate electrode 19 that makes Schottky contact with the nitride semiconductor layer 12 is formed in the opened region. The material of the gate electrode 19 may be any material that makes Schottky contact with the nitride semiconductor, and here a Ni / Au laminated structure is used. The Ni layer is about 10 nm thick, and the Au layer is about 600 nm thick.
[0060] (H) Next, as shown in FIG. 10A and FIG. 10B, a part of the substrate 10 is etched from the second surface 2b side by dry etching such as RIE to form a through hole 25A penetrating the substrate 10. When the substrate 10 is a SiC substrate, a fluorine-based gas such as a mixed gas of SF6 / O2 may be used as an etching gas. CF4 or CHF3 may be used instead of SF6. To etch the substrate 10 from the second surface 2b side, for example, the first surface 2a side of the drain electrode 20, the gate electrode 19, and the source electrode 18 may be attached to a dummy substrate or the like, and the second surface 2b may be placed on the upper surface. By forming the conductive layer 22 as an etching stop layer, it is possible to prevent the nitride semiconductor layer 12 from being etched from the side or the dummy substrate from being etched. A material having an etching rate lower than that of the substrate 10 is selected for the conductive layer 22.
[0061] (I) Next, as shown in FIG. 11A and FIG. 11B, the through hole 25A opened in the substrate 10 is filled with the first electrode layer 24E to form the through via 24. Here, a Ti / Cu laminated structure is formed by sputtering, and then gold plating is formed to form the through via 24. After the first electrode layer 24E is formed, the second electrode layer 24B is formed on the entire second surface 2b of the substrate 10 by metal deposition. The source electrode 18 and the through via 24 are at the same potential via the conductive layer 22. It is also possible to only cover the inside of the through hole 25A with the through via 24 so that the conductive layer 22, which is an etching stop layer, and the second electrode layer 24B, which is a ground electrode, are connected, without filling the entire through hole 25A with the second electrode layer 24B.
[0062] (J) Next, as shown in Figures 12A and 12B, an insulating layer 16 is formed to cover the surfaces of the source electrode 18, the gate electrode 19, the drain electrode 20 and the insulating layer 14. As shown in Figures 7B to 12B, in the opening region 100 from which the nitride semiconductor layer 12 has been removed, the insulating layer 14 and the insulating layer 16 are disposed on the first surface 2a of the substrate 10, but no other layers are formed.
[0063] 2A and 2B, a window is opened in the insulating layer 16, a source electrode 18E electrically connected to the source electrode 18 is formed, a drain electrode 20E electrically connected to the drain electrode 20 is formed, and a laminated structure for a pad electrode is formed. Note that such an electrode laminated structure is not necessarily required.
[0064] (Other embodiments) As described above, one embodiment has been described, but the descriptions and drawings forming a part of the disclosure are illustrative and should not be understood as limiting. From this disclosure, various alternative embodiments, examples and operating techniques will become apparent to those skilled in the art. Thus, the present embodiment includes various embodiments not described herein.
[0065] [Note] The technical ideas that can be understood from the present disclosure are described below. Note that, for the purpose of aiding understanding, not for the purpose of limitation, the components described in the appendices are given the reference symbols of the corresponding components in the embodiments. The reference symbols are shown as examples for the purpose of aiding understanding, and the components described in each appendix should not be limited to the components indicated by the reference symbols.
[0066] (Appendix 1) The nitride semiconductor device 1 includes a substrate 10 having both sides defined by a first surface 2a and a second surface 2b opposed to each other, and a nitride semiconductor layer 12 provided on the first surface 2a and including an active region 300 and an inactive region 200. The inactive region 200 has opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 where at least a portion of the nitride semiconductor layer 12 is removed and reaches the substrate 10. According to the nitride semiconductor device 1 of Appendix 1, the opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 absorb warpage of the substrate 10, and a nitride semiconductor device with reduced warpage of the substrate can be provided.
[0067] (Appendix 2) In the nitride semiconductor device described in Appendix 1, the nitride semiconductor layer 12 includes a first nitride semiconductor layer and a second nitride semiconductor layer forming a heterojunction with the first nitride semiconductor layer. The first nitride semiconductor layer includes a two-dimensional electron gas layer 121 at an interface with the second nitride semiconductor layer, and the active region 300 includes the two-dimensional electron gas layer 121 in a plan view. According to the nitride semiconductor device described in Appendix 2, it is possible to reduce warpage of the substrate in a nitride semiconductor device having a HEMT structure.
[0068] (Appendix 3) In the nitride semiconductor device according to Supplementary Note 1 or 2, the substrate 10 is a silicon carbide substrate (SiC substrate) having a 4H-SiC crystal structure. Since the SiC substrate tends to be significantly warped as a single body, forming an opening region in the nitride semiconductor layer 12 has a significant effect of suppressing the warping of the substrate 10.
[0069] (Appendix 4) In the nitride semiconductor device according to Supplementary Note 1 or 2, the substrate 10 is a silicon carbide substrate (SiC substrate) having a 6H-SiC crystal structure. The 6H-SiC crystal structure is frequently used as a SiC substrate along with the 4H-SiC crystal structure.
[0070] (Appendix 5) In the nitride semiconductor device according to Supplementary Note 1 or 2, the substrate 10 is a silicon substrate (Si substrate). Since there is a large difference in thermal expansion coefficient between a Si substrate and a nitride semiconductor, when a Si substrate is used for the substrate 10, it is very effective in suppressing warpage of the substrate 10.
[0071] (Appendix 6) In the nitride semiconductor device according to any one of Supplementary Notes 1 to 5, the warp of the substrate 10 is 1 μm or less per 100 mm.
[0072] (Appendix 7) In the nitride semiconductor device described in any one of Appendices 1 to 5, substrate 10 has a convex warp of 10 μm or more per 100 mm in a direction toward nitride semiconductor layer 12, and the stress acting on substrate 10 by nitride semiconductor layer 12 is tensile stress.
[0073] (Appendix 8) In the nitride semiconductor device described in any one of Appendices 1 to 5, substrate 10 has a convex warp of 20 μm or more per 100 mm in a direction toward nitride semiconductor layer 12, and the stress acting on substrate 10 by nitride semiconductor layer 12 is tensile stress.
[0074] (Appendix 9) In the nitride semiconductor device described in any one of Appendices 1 to 5, substrate 10 has a convex warp of 10 μm or more per 100 mm in a direction opposite to the direction facing nitride semiconductor layer 12, and the stress acting on substrate 10 by nitride semiconductor layer 12 is compressive stress.
[0075] (Appendix 10) In the nitride semiconductor device described in any one of Appendices 1 to 5, substrate 10 has a convex warp of 20 μm or more per 100 mm in a direction opposite to the direction facing nitride semiconductor layer 12, and the stress acting on substrate 10 by nitride semiconductor layer 12 is compressive stress.
[0076] (Appendix 11) The nitride semiconductor device described in Appendix 2 includes a drain electrode 20, a source electrode 18, and a gate electrode 19 provided on the second nitride semiconductor layer. The source electrode 18 is connected to a second electrode layer 24B serving as a ground electrode formed on the second surface 2b of the substrate 10 via a conductive layer 22 penetrating the substrate 10. According to the nitride semiconductor device described in Appendix 11, the source electrode 18 can be electrically connected to the ground electrode from the second surface 2b, thereby making it possible to reduce the chip area.
[0077] (Appendix 12) In the nitride semiconductor device described in Supplementary Note 11, the gate electrode 19 is disposed between the drain electrode 20 and the source electrode 18 .
[0078] (Appendix 13) In the nitride semiconductor device described in Supplementary Note 11 or 12, the opening regions 101, 106 are at least arranged in the inactive region 200 located in a first direction (X direction) in which the drain electrode 20, the source electrode 18, and the gate electrode 19 are arranged as viewed from the active region 300.
[0079] (Appendix 14) In the nitride semiconductor device according to any one of Supplementary Notes 11 to 13, the opening regions 102, 103, 104, 105, 107, 108, 109, and 110 are at least arranged in the inactive region 200 located in a second direction (Y direction) in which the drain electrode 20, the source electrode 18, and the gate electrode 19 extend, as viewed from the active region 300.
[0080] (Appendix 15) The manufacturing method of the nitride semiconductor device 1 includes the following manufacturing steps. A nitride semiconductor layer 12 is formed on a first surface 2a of a substrate 10, both surfaces of which are defined by a first surface 2a and a second surface 2b opposed to each other. An active region 300 and an inactive region 200 are formed in the nitride semiconductor layer 12, and a portion of the nitride semiconductor layer 12 is selectively etched to form a penetrating region 25E penetrating the nitride semiconductor layer 12 in the active region 300, and opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 penetrating the nitride semiconductor layer 12 in the inactive region 200. The penetrating region 25E is filled with a conductive layer 22 made of a material having a high etching selectivity relative to the substrate 10. An insulating layer 14 is formed on the nitride semiconductor layer 12, and the insulating layer 14 is opened by etching to form a drain electrode 20 and a source electrode 18 in ohmic contact with the nitride semiconductor layer 12, and a gate electrode 19 in Schottky contact with the nitride semiconductor layer 12. A part of the substrate 10 is selectively etched from the second surface 2b to form a through hole 25A reaching the conductive layer 22. A first electrode layer 24E in contact with the conductive layer 22 is formed in the through hole 25A, and a second electrode layer 24B in contact with the first electrode layer 24E is formed on the second surface 2b. According to the method for manufacturing the nitride semiconductor device 1 of Appendix 15, the opening regions 101, 102, 103, 104, 105, 106, 107, 108, 109, and 110 absorb the warpage of the substrate 10, and a method for manufacturing a nitride semiconductor device that reduces the warpage of the substrate can be provided.
[0081] (Appendix 16) In the method for manufacturing a nitride semiconductor device described in Supplementary Note 15, the inactive region 200 is formed by performing ion implantation into the nitride semiconductor layer 12.
[0082] (Appendix 17) In the method for manufacturing a nitride semiconductor device described in Supplementary Note 15, the inactive region 200 is formed by performing mesa etching to remove a part of the upper portion of the nitride semiconductor layer 12.
[0083] (Appendix 18) In the method for manufacturing a nitride semiconductor device according to any one of Supplementary Notes 15 to 17, the source electrode 18 is electrically connected to the conductive layer 22, and is connected to the second electrode layer 24B via the first electrode layer 24E penetrating the substrate 10. According to the method for manufacturing a nitride semiconductor device according to Supplementary Note 18, the source electrode 18 can be electrically connected to the ground electrode from the second surface 2b of the substrate 10, thereby making it possible to reduce the chip area.
[0084] The above description is merely illustrative. Those skilled in the art may recognize that many more possible combinations and permutations are possible other than the components and methods (manufacturing processes) listed for the purpose of describing the technology of the present disclosure. The present disclosure is intended to embrace all alternatives, modifications, and alterations that fall within the scope of the present disclosure, including the scope of the claims. [Explanation of symbols]
[0085] 1...Nitride semiconductor device 2a…Side 1 2b…Second side 10...Substrate 12...Nitride semiconductor layer 13...Ion implantation layer 14, 16…Insulating layer 14S…Source contact opening 14D…Drain contact opening 14G…Gate contact opening 16S…1st opening 16D…Second opening 18, 18E…Source electrode 19...Gate electrode 19A…Gate wiring 20, 20E…Drain electrode 22...Conductive layer 24…Through via 24B…Second electrode layer 24E...First electrode layer 25A...Through hole 25E…Penetration area 101, 102, 103, 104, 105, 106, 107, 108, 109, 110...Aperture area 120...Electron transport layer 121...2-dimensional electron gas layer 122...electron supply layer 200…Inactive area 300...active area
Claims
1. a substrate having opposing first and second surfaces defined thereon; a nitride semiconductor layer provided on the first surface of the substrate, the nitride semiconductor layer including an active region and an inactive region; Equipped with The inactive region has an opening region where at least a portion of the nitride semiconductor layer is removed to reach the substrate.
2. The nitride semiconductor layer is A first nitride semiconductor layer; a second nitride semiconductor layer forming a heterojunction with the first nitride semiconductor layer; the first nitride semiconductor layer has a two-dimensional electron gas layer at an interface with the second nitride semiconductor layer; The nitride semiconductor device according to claim 1 , wherein said active region includes said two-dimensional electron gas layer in a plan view.
3. 2. The nitride semiconductor device according to claim 1, wherein said substrate is a silicon carbide substrate having a 4H-SiC crystal structure.
4. 2. The nitride semiconductor device according to claim 1, wherein said substrate is a silicon carbide substrate having a 6H-SiC crystal structure.
5. The nitride semiconductor device according to claim 1 , wherein said substrate is a silicon substrate.
6. 5. The nitride semiconductor device according to claim 1, wherein the warp of the substrate is 1 μm or less per 100 mm.
7. 5. The nitride semiconductor device according to claim 1, wherein the substrate has a convex warp of 10 μm or more per 100 mm in a direction toward the nitride semiconductor layer, and the stress acting on the substrate by the nitride semiconductor layer is a tensile stress.
8. 5. The nitride semiconductor device according to claim 1, wherein the substrate has a convex warp of 20 μm or more per 100 mm in a direction toward the nitride semiconductor layer, and the stress acting on the substrate by the nitride semiconductor layer is a tensile stress.
9. The nitride semiconductor device according to any one of claims 1 to 4, wherein the substrate has a convex warp of 10 μm or more per 100 mm in a direction opposite to a direction facing the nitride semiconductor layer, and a stress acting on the substrate by the nitride semiconductor layer is a compressive stress.
10. 5. The nitride semiconductor device according to claim 1, wherein the substrate has a convex warp of 20 μm or more per 100 mm in a direction opposite to a direction facing the nitride semiconductor layer, and a stress acting on the substrate by the nitride semiconductor layer is a compressive stress.
11. a drain electrode, a source electrode, and a gate electrode provided on the second nitride semiconductor layer; The nitride semiconductor device according to claim 2 , wherein said source electrode is connected to a ground electrode formed on said second surface of said substrate via a conductive layer penetrating said substrate.
12. The nitride semiconductor device according to claim 11 , wherein said gate electrode is disposed between said drain electrode and said source electrode.
13. 13 . The nitride semiconductor device according to claim 11 , wherein the opening region is disposed at least in the inactive region located in a first direction in which the drain electrode, the source electrode, and the gate electrode are arranged, as viewed from the active region.
14. 13 . The nitride semiconductor device according to claim 11 , wherein the opening region is disposed at least in the inactive region located in a second direction in which the drain electrode, the source electrode, and the gate electrode extend, as viewed from the active region.
15. forming a nitride semiconductor layer on a first surface of a substrate having opposing first and second surfaces; forming an active region and an inactive region in the nitride semiconductor layer; selectively etching a portion of the nitride semiconductor layer to form a penetrating region penetrating the nitride semiconductor layer in the active region and an opening region penetrating the nitride semiconductor layer in the inactive region; filling the through region with a conductive layer of a material having a high etching selectivity with respect to the substrate; forming an insulating layer on the nitride semiconductor layer; the insulating layer is etched to form drain and source electrodes in ohmic contact with the nitride semiconductor layer; removing the insulating layer by etching to form a gate electrode in Schottky contact with the nitride semiconductor layer; selectively etching a portion of the substrate from the second surface of the substrate to form a through hole reaching the conductive layer; forming a first electrode layer in contact with the conductive layer in the through hole; forming a second electrode layer on the second surface in contact with the first electrode layer.
Citation Information
Patent Citations
Semiconductor device
JP2020077865A