Raw material for composites, and method for producing composites
The composite material with lignocellulose and urethane resin, utilizing a prepolymer with isocyanate and hydrophilic groups, addresses water resistance issues by ensuring uniform mixing and improved durability.
Patent Information
- Application Number
- JP2023056673
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing composite materials require improvement in water resistance.
A composite material comprising lignocellulose and urethane resin, using a prepolymer with isocyanate and hydrophilic groups, and a mixture of polyols with and without nitrogen atoms, along with an amine catalyst, to enhance water resistance and uniform mixing.
The composite material achieves improved water resistance and uniform mixing, resulting in enhanced durability and performance.
Smart Images

Figure 2024143792000001 
Figure 2024143792000002 
Figure 2024143792000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a raw material for a composite material and a method for producing a composite material. [Background technology]
[0002] Conventionally, composite materials have been known that combine an adhesive, which is a mixture of a first part containing a polyol and a second part containing an isocyanate compound, with an inorganic material and / or a lignocellulosic material (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-19120 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the composite material described in the above Patent Document 1, further improvement in water resistance is required.
[0005] An object of the present invention is to provide a raw material for a composite material capable of improving the water resistance of the composite material, and a method for producing the composite material. [Means for solving the problem]
[0006] The present invention [1] is a raw material for a composite material for producing a composite material of lignocellulose and a urethane resin, the raw material for the composite material comprising an isocyanate component containing a prepolymer having an isocyanate group and a hydrophilic group, the prepolymer being a reaction product of an aromatic polyisocyanate, a macropolyol, and a compound containing the hydrophilic group, a polyol component, and an amine catalyst.
[0007] The present invention [2] includes the composite material raw material of the above [1], in which the polyol component contains a first polyol that does not contain nitrogen atoms and a second polyol that contains nitrogen atoms.
[0008] The present invention [3] includes the composite material raw material according to the above [2], in which the second polyol is a polyether polyol containing nitrogen atoms.
[0009] The present invention [4] includes any one of the composite raw materials [1] to [3] above, in which the moisture content of the lignocellulose is 30% or more.
[0010] The present invention [5] includes any one of the composite material raw materials [1] to [4] above, in which the lignocellulose is cedar bark.
[0011] The present invention [6] comprises a composite material raw material according to any one of the above [1] to [5], which comprises a first agent containing the isocyanate component and a second agent containing the polyol component and the amine catalyst.
[0012] The present invention [7] includes a method for producing a composite material using any one of the raw materials for the composite material [1] to [6] above, the method comprising: a mixing step of mixing the lignocellulose, the isocyanate component, the polyol component, the amine catalyst, and water to prepare a composition for the composite material; and a curing step of curing the composition for the composite material.
[0013] The present invention [8] includes the method for producing a composite material according to the above [7], wherein in the curing step, the composite material composition is sprayed onto a construction surface, and the sprayed composite material composition is compressed and cured.
[0014] The present invention [9] includes the method for producing a composite material according to the above [7] or [8], wherein in the composite material composition, the total amount of the isocyanate component, the polyol component and the amine catalyst is 5 parts by mass or more and 70 parts by mass or less per 100 parts by mass of the solid content of the lignocellulose.
[0015] The present invention
[10] includes the method for producing a composite material according to any one of the above [7] to [9], wherein the polyol component contains a first polyol that does not contain nitrogen atoms and a second polyol that contains nitrogen atoms, and the blending ratio of the second polyol per 100 parts by mass of the isocyanate component in the composite material composition is 10 parts by mass or more and 20 parts by mass or less.
[0016] The present invention
[11] includes the method for producing a composite material according to any one of the above [7] to
[10] , wherein in the composition for the composite material, a mixing ratio of the amine catalyst relative to 100 parts by mass of the isocyanate component is 0.01 parts by mass or more and 1.5 parts by mass or less. Effect of the Invention
[0017] According to the composite material raw material of the present invention, the prepolymer is a reaction product of an aromatic polyisocyanate, a macropolyol, and a compound containing a hydrophilic group, and has an isocyanate group and a hydrophilic group.
[0018] Therefore, when the lignocellulose and the prepolymer are mixed, the prepolymer can be dispersed in water, so that the lignocellulose and the prepolymer can be mixed uniformly.
[0019] As a result, the water resistance of the resulting composite material can be improved.
[0020] Furthermore, according to the method for producing a composite material of the present invention, in the mixing step, the prepolymer can be dispersed in water, and the lignocellulose and the prepolymer can be mixed uniformly.
[0021] As a result, the water resistance of the resulting composite material can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] 1. Raw materials for composite materials The composite material raw material is a raw material for producing a composite material of lignocellulose and urethane resin. An example of the composite material is the surface layer of a resin-based mixture pavement.
[0023] (1) Lignocellulose Examples of lignocellulose include ground wood, ground bark, and ground bamboo. Note that "wood" refers to wood and does not include bark, which is bark. Examples of ground wood include wood chips. Examples of ground bark include bark chips. Examples of ground bamboo include bamboo chips. The type of wood is not limited. The tree may be a coniferous tree or a broadleaf tree. Examples of coniferous trees include cedar and cypress. Examples of broadleaf trees include beech and boxwood. Examples of lignocellulose preferably include cedar bark.
[0024] When the lignocellulose is cedar bark, a composite material having antibacterial and herbicidal properties can be produced. The composite material produced can be used, for example, for ground paving, walkways, highway walls, house surrounds, interior wall materials, interior floor materials, etc.
[0025] The moisture content of the lignocellulose is, for example, 30% or more, preferably 40% or more. When the moisture content of the lignocellulose is equal to or more than the above lower limit, a composite material can be produced using lignocellulose with a relatively high moisture content. Therefore, the step of drying the lignocellulose can be omitted or simplified, and the production process of the composite material can be simplified.
[0026] The moisture content of the lignocellulose is, for example, 60% or less, preferably 50% or less. When the moisture content of the lignocellulose is equal to or less than the above upper limit, the molding time (curing time) can be prevented from becoming longer, and production efficiency can be improved.
[0027] (2) Composite materials The composite material raw material includes a first part and a second part.
[0028] (2-1) First agent The first agent contains an isocyanate component. In other words, the composite material raw material contains an isocyanate component.
[0029] The isocyanate component contains a prepolymer. The isocyanate component may contain a residual isocyanate. The residual isocyanate monomer is an isocyanate monomer that remains unreacted among the isocyanate monomers used in the production of the prepolymer. Preferably, the isocyanate component is composed of only the prepolymer.
[0030] The proportion of the prepolymer in the first agent is, for example, 95 mass % or more, or preferably 99 mass % or more.
[0031] The prepolymer has an isocyanate group and a hydrophilic group. Since the prepolymer has a hydrophilic group, when the lignocellulose, the first agent, and the second agent are mixed, water can be added to emulsify the prepolymer in the water. This can reduce the viscosity of the mixture of the lignocellulose, the first agent, and the second agent, and improve the moldability of the composite material.
[0032] The content ratio of isocyanate groups in the prepolymer (isocyanate group content) is, for example, 5 mass% or more, preferably 10 mass% or more, more preferably 15 mass% or more, and for example, 30 mass% or less, preferably 25 mass% or less, more preferably 20 mass% or less.
[0033] The isocyanate group content is determined by a titration method using di-n-butylamine in accordance with the isocyanate group content test described in JIS K7301.
[0034] The hydrophilic group is a hydrophilic group that does not react with an isocyanate group. An example of the hydrophilic group that does not react with an isocyanate group is a polyoxyethylene group.
[0035] The prepolymer is the reaction product of an aromatic polyisocyanate, a macropolyol, and a compound containing hydrophilic groups.
[0036] (2-1-1) Aromatic polyisocyanate Aromatic polyisocyanates include, for example, tolylene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI).
[0037] Examples of tolylene diisocyanate include 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate. The tolylene diisocyanate may be a mixture of 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate.
[0038] Diphenylmethane diisocyanate includes 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 2,2'-diphenylmethane diisocyanate. Diphenylmethane diisocyanate may be a mixture of at least two of 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 2,2'-diphenylmethane diisocyanate. Diphenylmethane diisocyanate may also be polymeric MDI.
[0039] As the aromatic polyisocyanate, preferably, diphenylmethane diisocyanate is used, and more preferably, polymeric MDI is used.
[0040] The above aromatic polyisocyanates may be used alone or in combination of two or more kinds.
[0041] (2-1-2) Macropolyol The macropolyol is a compound having two or more hydroxyl groups and a number average molecular weight of 400 or more and 10000 or less. The number average molecular weight of the macropolyol is preferably 500 or more, more preferably 800 or more. The number average molecular weight of the macropolyol is preferably 5000 or less.
[0042] The number average molecular weight can be calculated from the number of hydroxyl groups of the macropolyol and the average hydroxyl value (hereinafter the same).
[0043] The average hydroxyl value of the macropolyol is, for example, 12 mgKOH / g or more, preferably 25 mgKOH / g or more, more preferably 50 mgKOH / g or more, and for example, 270 mgKOH / g or less, preferably less than 200 mgKOH / g.
[0044] The average hydroxyl value is measured in accordance with JIS K1557-1:2007 (hereinafter the same).
[0045] The macro polyol does not contain a nitrogen atom. Examples of the macro polyol include polyether polyol and polyester polyol. The macro polyol is preferably polyether polyol.
[0046] Examples of the polyether polyol include polyoxyalkylene polyols. Examples of the polyoxyalkylene polyol include polyalkylene polyols and polytetramethylene ether polyols.
[0047] Examples of polyalkylene polyols include polyethylene glycol, polypropylene glycol, and ethylene oxide-propylene oxide copolymers (random and / or block copolymers).
[0048] Specifically, polyalkylene polyols are produced by addition polymerization of an alkylene oxide having 2 to 3 carbon atoms to an initiator not containing a nitrogen atom. Examples of the initiator not containing a nitrogen atom include low molecular weight diols, low molecular weight triols, and polyols having 4 or more valences.
[0049] The low molecular weight diol is a diol having a number average molecular weight of not more than 400. Examples of the low molecular weight diol include ethylene glycol and propylene glycol.
[0050] The low molecular weight triol is a triol having a number average molecular weight of not more than 400. Examples of the low molecular weight triol include glycerin and trimethylolpropane.
[0051] The tetrahydric or higher polyol is an alcohol having four or more hydroxyl groups and a number average molecular weight of not more than 400. Examples of the tetrahydric or higher polyol include pentaerythritol, sorbitol, and sucrose.
[0052] The initiators not containing nitrogen atoms preferably include low molecular weight diols and low molecular weight triols.
[0053] Examples of the alkylene oxide include ethylene oxide and propylene oxide.
[0054] Examples of polytetramethylene ether polyols include ring-opening polymers obtained by cationic polymerization of tetrahydrofuran, such as amorphous polytetramethylene ether glycols in which a diol is copolymerized with a polymerization unit of tetrahydrofuran, and amorphous polytetramethylene ether glycols in which ethylene oxide, propylene oxide, epichlorohydrin, and / or benzyl glycidyl ether are copolymerized with a polymerization unit of tetrahydrofuran.
[0055] The polyether polyol is preferably polypropylene glycol, such as bifunctional polypropylene glycol obtained by adding propylene oxide to propylene glycol, trifunctional polypropylene glycol obtained by adding propylene oxide to glycerin, or trifunctional polypropylene glycol obtained by adding propylene oxide to trimethylolpropane.
[0056] The above macropolyols may be used alone or in combination of two or more kinds.
[0057] (2-1-3) Compounds containing hydrophilic groups The compound containing a hydrophilic group has the above-mentioned hydrophilic group and an active hydrogen group that does not contain a nitrogen atom. Examples of the active hydrogen group that does not contain a nitrogen atom include a hydroxyl group and a carboxyl group. A preferred example of the active hydrogen group is a hydroxyl group.
[0058] Examples of the compound containing a hydrophilic group include the above-mentioned monool having a hydrophilic group and the above-mentioned diol having a hydrophilic group. Examples of the monool include methoxypolyethylene glycol. Examples of the diol include polyethylene glycol.
[0059] As the compound containing a hydrophilic group, preferably, the above-mentioned monool having a hydrophilic group is used, and more preferably, methoxypolyethylene glycol is used.
[0060] When the compound containing a hydrophilic group is methoxypolyethylene glycol, the number average molecular weight of the methoxypolyethylene glycol is, for example, 350 or more, preferably 400 or more. The number average molecular weight of the methoxypolyethylene glycol is, for example, 2000 or less, preferably 650 or less.
[0061] (2-1-4) Method for producing prepolymer To produce the prepolymer, an aromatic polyisocyanate, a macropolyol, and a compound containing a hydrophilic group are mixed so that the isocyanate index (the ratio of the isocyanate group concentration (NCO concentration) of the polyisocyanate to the active hydrogen group concentration of the macropolyol and the compound containing a hydrophilic group multiplied by 100, NCO concentration / active hydrogen group concentration × 100) is, for example, greater than 100, preferably 105 or more, for example, 600 or less, preferably 450 or less, and reacted until a predetermined isocyanate group content is reached.
[0062] In this reaction, a urethanization catalyst can be added, if necessary.
[0063] After the reaction, if necessary, the remaining monomer (specifically, unreacted polyisocyanate) is removed using a known distillation method or the like.
[0064] This makes it possible to obtain a prepolymer having an isocyanate group at the molecular terminal.
[0065] (3) Second agent The second agent contains a polyol component and an amine catalyst. In other words, the raw material for the composite material includes a polyol component and an amine catalyst. The second agent is a mixture of the polyol component and the amine catalyst. The raw material for the composite material does not contain a metal catalyst.
[0066] (3-1) Polyol component The polyol component contains a first polyol and a second polyol.
[0067] (3-1-1) First polyol The first polyol does not contain a nitrogen atom. The first polyol has two or more hydroxyl groups. The number average molecular weight of the first polyol is 62 or more and 1000 or less. The number average molecular weight of the first polyol is preferably less than 800.
[0068] The average hydroxyl value of the first polyol is, for example, 200 mgKOH / g or more, preferably 300 mgKOH / g or more, and for example, 2000 mgKOH / g or less.
[0069] Examples of the first polyol include a low molecular weight diol, a low molecular weight triol, and a polyether polyol.
[0070] Examples of low molecular weight diols as the first polyol include ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol.
[0071] Examples of low molecular weight triols as the first polyol include glycerin and trimethylolpropane.
[0072] Examples of polyether polyols as the first polyol include difunctional polypropylene glycols obtained by adding propylene oxide to propylene glycol, trifunctional polypropylene glycols obtained by adding propylene oxide to glycerin, and trifunctional polypropylene glycols obtained by adding propylene oxide to trimethylolpropane.
[0073] The proportion of the first polyol in the second agent is, for example, 1 mass% or more, preferably 3 mass% or more, more preferably 10 mass% or more, preferably 15 mass% or more, and for example, 35 mass% or less, preferably 30 mass% or less, more preferably 25 mass% or less, preferably 20 mass% or less.
[0074] When the ratio of the first polyol in the second part is equal to or more than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.
[0075] In the second agent, the mixing ratio of the first polyol relative to 100 parts by mass of the second polyol is, for example, 1 part by mass or more, preferably 3 parts by mass or more, more preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and for example, 45 parts by mass or less, preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and more preferably 20 parts by mass or less.
[0076] When the mixing ratio of the first polyol to 100 parts by mass of the second polyol is equal to or more than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.
[0077] (3-1-2) Second polyol The second polyol is a compound that contains a nitrogen atom, has two or more hydroxyl groups, and has a number average molecular weight of 200 or more and 1000 or less. The number average molecular weight of the second polyol is preferably less than 800.
[0078] The average hydroxyl value of the second polyol is, for example, 200 mgKOH / g or more, preferably 250 mgKOH / g or more, and for example, 1000 mgKOH / g or less, preferably 900 mgKOH / g or less.
[0079] More specifically, the second polyol is a polyether polyol containing nitrogen atoms. The polyether polyol containing nitrogen atoms is produced, for example, by addition polymerization of an alkylene oxide to an initiator containing nitrogen atoms. Examples of the initiator containing nitrogen atoms include triethanolamine, ethylenediamine, and diethylenetriamine.
[0080] Examples of the polyether polyol containing a nitrogen atom include trifunctional polypropylene glycol obtained by adding propylene oxide to triethanolamine, and tetrafunctional polypropylene glycol obtained by adding propylene oxide to ethylenediamine.
[0081] The proportion of the second polyol in the second agent is, for example, 65 mass% or more, preferably 69 mass% or more, preferably 75 mass% or more, and for example, 95 mass% or less, preferably 90 mass% or less, preferably 85 mass% or less.
[0082] When the ratio of the second polyol in the second part is equal to or more than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted to an appropriate range, improving workability and ensuring the water resistance and physical strength of the composite material.
[0083] (3-2) Amine catalyst Examples of the amine catalyst include tertiary amines, such as dimethylcyclohexylamine (DMCHA), dimethylethanolamine (DMEA), triethanolamine (TEA), and triethylenediamine.
[0084] The proportion of the amine catalyst in the second agent is, for example, 0.1 mass% or more, preferably 0.5 mass% or more, preferably 1 mass% or more, and for example, 10 mass% or less, preferably 7 mass% or less, more preferably 5 mass% or less.
[0085] When the ratio of the amine catalyst in the second part is equal to or more than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.
[0086] In the second agent, the mixing ratio of the amine catalyst relative to 100 parts by mass of the second polyol is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, and for example, 10 parts by mass or less, preferably 8 parts by mass or less, and more preferably 5 parts by mass or less.
[0087] When the mixing ratio of the amine catalyst to 100 parts by mass of the second polyol is equal to or more than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.
[0088] 2. Manufacturing method of composite materials The method for producing a composite material uses the above-mentioned raw materials for the composite material and includes a mixing step and a curing step.
[0089] (1) Mixing process In the mixing step, lignocellulose, the first agent, the second agent, and water are mixed to prepare a composite material composition. In other words, in the mixing step, lignocellulose, an isocyanate component, a polyol component, an amine catalyst, and water are mixed to prepare a composite material composition. The isocyanate component, the polyol component, and the amine catalyst in the composite material composition are defined as binder components.
[0090] The method of mixing lignocellulose, the first agent, the second agent, and water is not limited. For example, the first agent and water are mixed to prepare a first mixed liquid, the second agent and water are mixed to prepare a second mixed liquid, and the first mixed liquid and the second mixed liquid are mixed with lignocellulose to prepare a composite material composition. Alternatively, for example, the first agent, the second agent, and water may be mixed to prepare a mixed liquid, and the resulting mixed liquid may be mixed with lignocellulose. When the composite material is composed of multiple layers, the composite material compositions for producing each of the multiple layers may be prepared separately.
[0091] In the composite material composition, the ratio of the binder components (total amount of the isocyanate component, the polyol component and the amine catalyst) to 100 parts by mass of the lignocellulose solids is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and for example, 70 parts by mass or less, preferably 60 parts by mass or less.
[0092] In the composite material composition, if the ratio of the binder component to 100 parts by mass of the lignocellulose solid content is equal to or greater than the above lower limit, the hardness of the surface layer of the resin-based mixture pavement can be ensured. Also, in the composite material composition, if the ratio of the binder component to 100 parts by mass of the lignocellulose solid content is equal to or less than the above upper limit, a composite material can be easily obtained by spreading the composite material composition, compressing and curing it.
[0093] In the composite material composition, the mixing ratio of the first polyol relative to 100 parts by mass of the isocyanate component is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more, and for example, 5 parts by mass or less, preferably 4.7 parts by mass or less.
[0094] When the blending ratio of the first polyol to 100 parts by mass of the isocyanate component is within the above range, an increase in the 20° C. water absorption thickness expansion rate can be suppressed.
[0095] In the composite material composition, the mixing ratio of the second polyol per 100 parts by mass of the isocyanate component is, for example, 10 parts by mass or more, preferably 11 parts by mass or more, and for example, 20 parts by mass or less, preferably 15 parts by mass or less.
[0096] When the blending ratio of the second polyol to 100 parts by mass of the isocyanate component is within the above range, an increase in the 20° C. water absorption thickness expansion rate can be suppressed.
[0097] In the composite material composition, the mixing ratio of the amine catalyst relative to 100 parts by mass of the isocyanate component is, for example, 0.01 parts by mass or more, preferably 0.1 parts by mass or more, and for example, 1.5 parts by mass or less, preferably 1 part by mass or less.
[0098] When the blending ratio of the amine catalyst to 100 parts by mass of the isocyanate component is within the above range, an increase in the 20° C. water absorption thickness expansion rate can be suppressed.
[0099] The composite material may be composed of only one layer, or may be composed of multiple layers. When the composite material is composed of multiple layers, the composite material has at least a first layer and a second layer. The first layer may be the outermost layer of the composite material. When the first layer is the outermost layer of the composite material, the first layer is produced from the above-mentioned composite material composition.
[0100] The second layer is disposed between the first layer and the application surface. A composite composition for producing the second layer (second composite composition) is prepared separately from a composite composition for producing the first layer (first composite composition).
[0101] The "ratio of the binder component to 100 parts by mass of the lignocellulose solid content" in the second composite material composition is less than the "ratio of the binder component to 100 parts by mass of the lignocellulose solid content" in the first composite material composition. In the second composite material composition, the ratio of the binder component to 100 parts by mass of the lignocellulose solid content is, for example, 5 parts by mass or more, preferably 15 parts by mass or more, and for example, 25 parts by mass or less, preferably 20 parts by mass or more.
[0102] In the second composite material composition, if the ratio of the binder component to 100 parts by mass of the solid content of lignocellulose is equal to or greater than the lower limit, the second layer of the composite material can be made more flexible than the first layer, and as a result, cushioning properties can be imparted to the resin-based mixture pavement.
[0103] (2) Curing process Next, in the curing step, the composite material composition is cured. In the curing step, the composite material composition is sprayed onto a construction surface, and the sprayed composite material composition is compressed and cured.
[0104] Specifically, the composite material composition is sprayed on the application surface and compressed, for example, at a pressure of 1 MPa to 10 MPa for 1 minute to 10 minutes without heating. The compressed composite material composition is then cured as is to harden the composite material composition. If necessary, the compressed composite material composition may be heated to accelerate hardening.
[0105] This makes it possible to obtain a composite material as a cured product of the composite material composition.
[0106] When the composite material has a first layer and a second layer, the above-mentioned second composite material composition is first sprayed onto the application surface, and the sprayed second composite material composition is compressed and cured.
[0107] Next, the above-mentioned first composite material composition is spread on the compressed second composite material composition, and the spread first composite material composition is compressed and cured.
[0108] 3. Physical properties of composite materials Next, the physical properties of the obtained composite material will be described.
[0109] (1) Thickness of the composite material The thickness of the composite material is not limited. The thickness of the composite material is, for example, 14.5 mm or more, preferably 15.0 mm or more, and for example, 17.0 mm or less, preferably 17.5 mm or less.
[0110] The thickness of the composite material is measured in accordance with the dimensional measurement method specified in JIS A5908:2015 (Particleboard).
[0111] In order to adjust the thickness of the composite material to fall within the above range, for example, the ratio of the binder component to 100 parts by mass of the solid content of lignocellulose is adjusted to be equal to or more than the above lower limit and equal to or less than the above upper limit.
[0112] (2) Density of the composite material The density of the composite material is not limited. The density of the composite material is, for example, 300 kg / m 3 More than 320 kg / m 3 For example, 400 kg / m 3 Less than or equal to 360 kg / m 3 The following is the result.
[0113] The density of the composite material is measured using the density test specified in JIS A5908:2015 (Particleboard).
[0114] In order to adjust the density of the composite material to fall within the above range, for example, the weight of the composite material composition to be sprayed is calculated from the volume of the area to which the composite material composition is applied, and then the density is adjusted.
[0115] (3) Water absorption thickness expansion rate of composite material at 20°C The composite material has a water absorption thickness swelling rate at 20° C. of, for example, 10.0% or less, preferably 9.0% or less, more preferably 7.0% or less, more preferably 5.0% or less, and for example, 1.0% or more.
[0116] The 20°C water absorption thickness expansion rate of the composite material is measured according to the water absorption thickness expansion rate test of JIS A5908:2015 (particleboard).
[0117] To adjust the 20° C. water absorption thickness expansion coefficient of the composite material to fall within the above range, for example, the ratio of the binder component to 100 parts by mass of the solid content of lignocellulose is adjusted to be equal to or higher than the above lower limit and equal to or lower than the above upper limit.
[0118] 4. Effects (1) According to the raw material for composite materials, the prepolymer is a reaction product of an aromatic polyisocyanate, a macropolyol, and a compound containing a hydrophilic group, and has an isocyanate group and a hydrophilic group.
[0119] Therefore, when the lignocellulose and the prepolymer are mixed, the prepolymer can be dispersed in water, so that the lignocellulose and the prepolymer can be mixed uniformly.
[0120] As a result, the water resistance of the resulting composite material can be improved.
[0121] (2) According to the method for producing a composite material, in the mixing step, the prepolymer can be dispersed in water, so that the lignocellulose and the prepolymer can be mixed uniformly.
[0122] As a result, the water resistance of the resulting composite material can be improved. EXAMPLES
[0123] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0124] 1.Composite material raw materials (1) Aromatic isocyanates PH (monomeric MDI, NCO%: 33.6, molecular weight: 250.25) PI (monomeric MDI, NCO%: 33.6, molecular weight: 250.25) M-200 (Polymeric MDI, NCO%: 30.8-31.8) (2) Macropolyol Production Example 1 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 112 mgKOH / g, number average molecular weight: 1000) Production Example 2 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 56 mgKOH / g, number average molecular weight: 2000) Production Example 3 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 168 mg KOH / g, number average molecular weight: 1000) Production Example 4 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 56 mg KOH / g, number average molecular weight: 3000) (3) Compounds containing hydrophilic groups M-400 (Uniox M-400, methoxypolyethylene glycol, number of functional groups: 1, average hydroxyl value: 140.3 mgKOH / g, number average molecular weight: 400, NOF Corporation) MPEG500 (methoxypolyethylene glycol, functional group number: 1, average hydroxyl value: 112 mgKOH / g, number average molecular weight: 500, manufactured by Jiahua Chemical Co., Ltd.) M-550 (Uniox M-550, methoxypolyethylene glycol, functionality: 1, average hydroxyl value: 102 mgKOH / g, number average molecular weight: 550, NOF Corporation) MPEG600 (methoxypolyethylene glycol, functional group number: 1, average hydroxyl value: 93.5 mg KOH / g, number average molecular weight: 600, manufactured by Jiahua Chemical Co., Ltd.) (4) First polyol DPG (Dipropylene glycol, Functional group number: 2, Hydroxyl value: 836.25 mg KOH / g, Molecular weight: 134.17, ADEKA Corporation) Production Example 5 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 400 mgKOH / g, number average molecular weight: 280) Gly (glycerin, functional group number: 3, hydroxyl value: 1827.56 mg KOH / g, molecular weight: 92.09, NOF Corp.) Production Example 6 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 280 mgKOH / g, number average molecular weight: 400) Production Example 7 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 420 mg KOH / g, number average molecular weight: 400) Production Example 8 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 240 mgKOH / g, number average molecular weight: 700) (5) Second polyol Production Example 9 (Polyether polyol obtained by adding propylene oxide to triethanolamine, average hydroxyl value: 350 mgKOH / g, number average molecular weight: 480) Production Example 10 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 305 mgKOH / g, number average molecular weight: 740) Production Example 11 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 820 mgKOH / g, number average molecular weight: 270) Production Example 12 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 450 mgKOH / g, number average molecular weight: 500) (6) Amine catalyst DMCHA (Dimethylcyclohexylamine) DMEA (Dimethylethanolamine) TEA (triethanolamine) (7) Metal catalyst Neostan U-100 (dibutyltin dilaurate, manufactured by Nitto Kasei Co., Ltd.) 2.Prepolymer Production According to the formulations shown in Table 1, prepolymers A to G were obtained.
[0125] Specifically, for prepolymers A to D, F and G, first, PH, which is solid at room temperature, was mixed with M-200 in a container under a nitrogen atmosphere, and PH was dissolved while stirring at 40°C to obtain a mixture of PH and M-200. Next, macropolyol and, if necessary, a hydrophilic group-containing compound were added to the obtained mixture, and the mixture was heated to 80°C while stirring, and then reacted at 80°C for 3 hours to obtain a prepolymer. The obtained prepolymer was then cooled to 40°C or lower.
[0126] For prepolymer E, macropolyol and hydrophilic group-containing compound were added to PI in a container under a nitrogen atmosphere, and the mixture was heated to 80°C while stirring, and then reacted at 80°C for 3 hours to obtain a prepolymer. The obtained prepolymer was then cooled to 40°C or lower.
[0127] [Table 1]
[0128] 3. Manufacturing of composite materials According to the formulations shown in Tables 2 to 6, the first agent was mixed with water to prepare a first mixture, and the second agent was mixed with water to prepare a second mixture.
[0129] Next, the first and second mixed liquids were mixed with lignocellulose to prepare a composite material composition. Tables 2 to 6 show the "ratio of binder components to 100 parts by mass of solid content of lignocellulose."
[0130] Next, the composite material composition was spread into the mold, compressed and cured at 25° C. for 90 minutes.
[0131] In this manner, composite materials of each of the examples and comparative examples were obtained.
[0132] In Comparative Example 2, no prepolymer was used as the first agent, and 18 parts by mass of a mixture of 243.11 parts by mass of PH (monomeric MDI) and 756.89 parts by mass of M-200 (polymeric MDI) was used.
[0133] [Table 2]
[0134] [Table 3]
[0135] [Table 4]
[0136] [Table 5]
[0137] [Table 6]
[0138] 4. Physical properties of composite materials According to JIS A5908:2015 (particleboard), the thickness, density, and water absorption thickness expansion rate at 20° C. of the composite material were measured. The results are shown in Tables 2 to 6.
[0139] In addition, the water resistance conforming to the P type specified in JIS A5908:2015 (particleboard) was evaluated according to the following criteria. ○:Has water resistance that meets the P type specified in JIS A5908:2015 (particle board). △: It has water resistance that meets the P type specified in JIS A5908:2015 (particle board), but the water absorption thickness expansion rate at 20°C exceeds 9.0%. ×:Does not have water resistance that meets the P type specified in JIS A5908:2015 (particle board).
Claims
1. A raw material for a composite material for producing a composite material of lignocellulose and a urethane resin, an isocyanate component containing a prepolymer having an isocyanate group and a hydrophilic group, the prepolymer being a reaction product of an aromatic polyisocyanate, a macropolyol, and a compound containing the hydrophilic group; A polyol component; Amine catalyst Composite materials raw materials, including
2. The polyol component is a first polyol that does not contain nitrogen atoms; 2. The composite material raw material according to claim 1, further comprising a second polyol containing a nitrogen atom.
3. 3. The composite material raw material according to claim 2, wherein the second polyol is a polyether polyol containing nitrogen atoms.
4. The composite material raw material according to claim 1 , wherein the moisture content of the lignocellulose is 30% or more.
5. The composite material raw material according to claim 1 , wherein the lignocellulose is cedar bark.
6. A first agent containing the isocyanate component; a second agent containing the polyol component and the amine catalyst; The composite material feedstock of claim 1 .
7. A method for producing a composite material using the raw material for the composite material according to claim 1, a mixing step of mixing the lignocellulose, the isocyanate component, the polyol component, the amine catalyst, and water to prepare a composite material composition; a curing step of curing the composite material composition; A method for producing a composite material, comprising:
8. The method for producing a composite material according to claim 7 , wherein in the curing step, the composite material composition is sprayed on a construction surface, and the sprayed composite material composition is compressed and cured.
9. The method for producing a composite material according to claim 7, wherein in the composite material composition, the total amount of the isocyanate component, the polyol component and the amine catalyst is 5 parts by mass or more and 70 parts by mass or less per 100 parts by mass of the solid content of the lignocellulose.
10. The polyol component contains a first polyol that does not contain a nitrogen atom and a second polyol that contains a nitrogen atom, 8. The method for producing a composite material according to claim 7, wherein in the composite material composition, a mixing ratio of the second polyol relative to 100 parts by mass of the isocyanate component is 10 parts by mass or more and 20 parts by mass or less.
11. 8. The method for producing a composite material according to claim 7, wherein a mixing ratio of the amine catalyst relative to 100 parts by mass of the isocyanate component in the composition for composite material is 0.01 parts by mass or more and 1.5 parts by mass or less.
Citation Information
Patent Citations
Manufacture of lignocellulose molded plate
JP1998180721A
Paving material
JP2000327905A
Adhesive composition for lignocellulose and thermocompression molded product and method for producing thermocompression molded product using the same
JP2001303017A
Adhesive composition for hot press molded article of lignocellulosic material, and hot press molded article using the same and its manufacturing method
JP2002069417A
Resin for molding high strength lignocellulosic substance
JP2008229878A