Curable resin composition and use thereof

A curable resin composition with a core-shell structure and specific additives improves handling and adhesive strength, addressing issues in conventional compositions for automotive applications.

JP2024143797AInactive Publication Date: 2024-10-11KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023056685
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional curable resin compositions used in structural adhesives for vehicles face issues with handling properties, shower resistance, and adhesive strength, particularly when cured at lower temperatures, leading to poor performance in automotive manufacturing processes.

Method used

A curable resin composition comprising 100 parts by weight of epoxy resin, 5 to 100 parts by weight of polymer particles with a core-shell structure, 5 to 20 parts by weight of dicyandiamide, 1.5 to 10 parts by weight of a curing agent and/or curing accelerator, and 0 to 20 parts by weight of blocked isocyanate, with specific glass transition temperatures and SP values for the shell layer, enhancing handling properties and adhesive strength.

Benefits of technology

The composition provides a cured product with excellent handling properties, shower resistance, and adhesive strength, suitable for use as a structural adhesive in vehicles, even at low temperatures and reduced curing times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143797000001
    Figure 2024143797000001
  • Figure 2024143797000002
    Figure 2024143797000002
  • Figure 2024143797000003
    Figure 2024143797000003
Patent Text Reader

Abstract

To provide a curable resin composition that yields a cured product with superior handleability and shower resistance as well as superior adhesive strength.SOLUTION: A curable resin composition includes a specific amount of epoxy resin (A), a polymer particle with a core-shell structure including a shell layer with specific physical properties (B), dicyandiamide (C), a curing agent and / or a curing accelerator (D), and a blocked isocyanate (E).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition and its use. [Background technology]

[0002] Curable resin compositions containing epoxy resins are excellent in many respects, such as dimensional stability, mechanical strength, electrical insulation properties, heat resistance, water resistance, and chemical resistance, and are used in a variety of applications.

[0003] One known application of such a curable resin composition containing an epoxy resin is as a structural adhesive for automobiles.Patent Documents 1 to 4 disclose techniques relating to a curable resin composition containing an epoxy resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-194316 A [Patent Document 2] International Publication No. WO2019 / 208569 [Patent Document 3] International Publication No. WO2020 / 218552 [Patent Document 4] Patent Publication No. 2022-092250 Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional curable resin compositions such as those described in Patent Documents 1 to 4 have room for further improvement in terms of handleability and shower resistance, as well as the adhesive strength of a cured product obtained by curing the curable resin composition.

[0006] In view of the above-mentioned current situation, an object of one aspect of the present invention is to provide a curable resin composition that can provide a cured product that has excellent handleability and shower resistance, and also has excellent adhesive strength. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.

[0008] That is, one embodiment of the present invention includes the following configuration. [1] An epoxy resin composition comprising: 100 parts by weight of an epoxy resin (A); 5 to 100 parts by weight of polymer particles (B) having a core-shell structure including a core layer and a shell layer; 5 to 20 parts by weight of dicyandiamide (C); 1.5 to 10 parts by weight of a curing agent and / or a curing accelerator (D); and 0 to 20 parts by weight of a blocked isocyanate (E); wherein the glass transition temperature of the shell layer is −25° C. to 18° C., and the SP value of the shell layer is 10.00 to 10.65 (cal / cm 3 ) 1 / 2 the shell layer contains 30% by mass to 90% by weight of structural units derived from an alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms, relative to 100% by mass of all structural units constituting the shell layer; Curable resin composition. [2] The curable resin composition according to [1], having an exothermic peak temperature of less than 156°C in DSC measurement. [3] The curable resin composition according to [1] or [2], wherein the curable composition contains an aromatic urea-based curing accelerator as the curing agent and / or the curing accelerator (D), and the blocked isocyanate (E) does not contain a structure derived from an aromatic polyisocyanate. [4] The curable resin composition according to any one of [1] to [3], wherein the shell layer has a glass transition temperature of -14°C to 18°C. [5] The curable resin composition according to any one of [1] to [4], wherein the core layer contains at least one selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and organosiloxane-based rubbers. [6] The curable composition according to any one of [1] to [5], wherein the core layer is made of butadiene rubber and the shell layer does not contain a structural unit derived from a vinylcyan monomer. [7] A vehicle structural adhesive comprising the curable composition according to any one of [1] to [6]. [8] A cured product obtained by curing the curable composition according to any one of [1] to [6]. [9] A laminate comprising a plurality of substrates bonded together with the cured product according to [8]. Effect of the Invention

[0009] According to one embodiment of the present invention, it is possible to provide a curable resin composition that can provide a cured product that has excellent handleability and shower resistance, as well as excellent adhesive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims, and embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. In addition, all academic literature and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."

[0011] 1. Technical Concept of the Present Invention In general, when an adhesive containing a curable resin composition mainly composed of epoxy is used as a structural adhesive in the manufacture of vehicles, etc., a washing step (e.g., a shower step with warm water) is present between the step of applying the adhesive to the object to be adhered and the step of curing the adhesive. However, conventional curable resin compositions have problems with shower resistance, such as the uncured adhesive being partially scattered or deformed by the water pressure of the shower during the washing step, and a curable resin composition with excellent shower resistance is required. In order to solve this problem, studies are being made to increase the viscosity of the adhesive in the low shear rate range at high temperatures (e.g., 50°C).

[0012] It is also known that adhesive strength, such as shear adhesion, can be improved by reducing the thickness of the adhesive layer of an adhesive containing a resin composition mainly composed of an epoxy resin. For this reason, when using such an adhesive, the adhesive is applied to one of the adherends, and then the adhesive is thinly spread using a spatula or the like. From the viewpoint of performing this operation efficiently, the curable resin composition is also required to have excellent handleability at low temperatures (e.g., 25°C).

[0013] Incidentally, in the field of structural adhesives, due to the recent trend towards carbon neutrality, there is currently a need to lower the baking temperature of baking furnaces for electrodeposition painting (anti-rust undercoat paint for automobiles) from the conventional 170-190° C. to around 120-140° C. There is also a demand to shorten the baking time (to within 60 minutes).

[0014] In the automobile manufacturing process, automotive structural adhesives are usually cured simultaneously with electrodeposition paints in the above-mentioned baking ovens. For this reason, curable resin compositions for structural adhesives are also required to cure at low temperatures (140°C or less) and in a short time (to have low-temperature curing properties).

[0015] Various techniques have been disclosed to address the above-mentioned problems. For example, Patent Documents 1 and 2 disclose a technique in which a curable resin composition mainly composed of an epoxy resin is combined with polymer particles having a core-shell structure and blocked urethane as a reinforcing agent other than the core-shell polymer particles. Patent Document 3 discloses a technique in which a curable resin composition mainly composed of an epoxy resin is combined with polymer particles having a core-shell structure and fumed silica, and Patent Document 4 discloses a technique in which blocked urethane is combined with a specific metal catalyst or the like. On the other hand, the present inventors have found that when the curable resin compositions described in Patent Documents 1 and 2 are cured at a lower temperature (140° C. or lower), the reaction of the blocked urethane does not proceed sufficiently during curing, and the resulting cured product is insufficiently cured, resulting in a problem of poor adhesive strength. In addition, the present inventors have also found that the curable resin compositions described in Patent Documents 1 to 4 have room for improvement in terms of shower resistance and handling.

[0016] As described above, although handleability, shower resistance, and adhesive strength are all important physical properties in a curable resin composition, particularly in a curable resin composition for structural adhesive applications, a curable resin composition that combines these physical properties has not been known in the past. In this situation, the present inventors have conducted extensive research with the aim of providing a curable composition that can provide a cured product that is excellent in handleability and shower resistance and has excellent adhesive strength. In the course of the research, the present inventors have found that (1) the handleability and shower resistance of the curable resin composition can be improved by blending polymer particles having a core-shell structure with a specific shell layer glass transition temperature and SP value, and (2) the adhesive strength of the resulting cured product can be improved by adjusting the amount of blocked isocyanate in the curable resin composition to a specific amount, and have completed the present invention.

[0017] A curable resin composition having excellent handling properties, shower resistance, and adhesive strength at the same time has not been known and is a surprising discovery. Furthermore, such a curable resin composition is extremely useful as a vehicle structural adhesive used in the manufacture of automobile body structures.

[0018] [2. Curable resin composition] A curable resin composition according to one embodiment of the present invention comprises 100 parts by weight of an epoxy resin (A), 5 to 100 parts by weight of polymer particles (B) having a core-shell structure including a core layer and a shell layer, 5 to 20 parts by weight of dicyandiamide (C), 1.5 to 10 parts by weight of a curing agent and / or a curing accelerator (D), and 0 to 20 parts by weight of a blocked isocyanate (E), wherein the shell layer has a glass transition temperature of −25° C. to 18° C. and an SP value of the shell layer of 10.00 to 10.65 (cal / cm 3 ) 1 / 2 and the shell layer contains 30% by mass to 90% by weight of structural units derived from an alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms, relative to 100% by mass of all structural units constituting the shell layer. Hereinafter, "a curable resin composition according to one embodiment of the present invention" may be referred to as "the present curable resin composition", "epoxy resin (A)" as "component (A)", "polymer particles having a core-shell structure (B)" as "component (B)", "dicyandiamide (C)" as "component (C)", "curing agent and / or curing accelerator (D)" as "component (D)", and "blocked isocyanate (E)" as "component (E)".

[0019] Since the present curable resin composition has the above-mentioned constitution, it has excellent handleability and shower resistance, and the adhesive strength of the obtained cured product is excellent. The present curable resin composition can be cured by a known method to obtain a cured product.

[0020] Each component that the present curable resin composition may contain will be described in detail below.

[0021] <Epoxy resin (A)> The present curable resin composition contains an epoxy resin (A) (component (A)). As component (A) contained in the present curable resin composition, various epoxy resins can be used.

[0022] Examples of the epoxy resin as component (A) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol S type epoxy resins, glycidyl ester type epoxy resins, glycidylamine type epoxy resins, novolac type epoxy resins, glycidyl ether type epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F) type epoxy resins, fluorinated epoxy resins, flame retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ester type epoxy resins, m-amino Examples of such epoxy resins include phenol-type epoxy resins, diaminodiphenylmethane-based epoxy resins, various alicyclic epoxy resins, N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, triglycidyl isocyanurate, divinylbenzene dioxide, resorcinol diglycidyl ether, chelate-modified epoxy resins, rubber-modified epoxy resins, urethane-modified epoxy resins, hydantoin-type epoxy resins, epoxidized products of unsaturated polymers such as petroleum resins, aminoglycidyl ether resins, and epoxy compounds obtained by addition reaction of the above-mentioned epoxy resins with bisphenol A (or F) or polybasic acids.

[0023] Examples of epoxy compounds obtained by subjecting an epoxy resin to an addition reaction with a polybasic acid or the like include an addition reaction product of a dimer of tall oil fatty acid (dimer acid) with a bisphenol A-type epoxy resin, as described in International Publication No. 2010-098950.

[0024] Component (A) is not limited to these, and any commonly used epoxy resin can be used. These epoxy resins (A) may be used alone or in combination of two or more.

[0025] Here, in this specification, polyalkylene glycol diglycidyl ethers, glycol diglycidyl ethers, diglycidyl esters of aliphatic polybasic acids, glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols, and monoepoxides are not included in the epoxy resin (A). These polyalkylene glycol diglycidyl ethers, glycol diglycidyl ethers, diglycidyl esters of aliphatic polybasic acids, glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols, and monoepoxides have relatively low viscosities (for example, 500 mPa·s or less at 25°C) compared with the above-mentioned epoxy resins. In other words, in this specification, epoxy group-containing compounds having a viscosity of 500 mPa·s or less at 25°C are not included in the component (A).

[0026] As the chelate-modified epoxy resin, for example, the resins described in paragraphs

[0018] to

[0019] of WO2016-163491 can be used.

[0027] As the urethane-modified epoxy resin, for example, the resins described in paragraphs

[0133] to

[0135] of WO2016-163491 can be used.

[0028] Among these epoxy resins, those having at least two epoxy groups in one molecule are preferred because they have high curability, the cured product has high flexibility, and the incorporation of polymer particles (B) is effective in improving the impact peel resistance of the cured product, etc. In particular, compounds having two epoxy groups in one molecule are preferred.

[0029] The epoxy equivalent of component (A) is preferably less than 220 g / eq, more preferably from 90 g / eq to less than 210 g / eq, and even more preferably from 135 g / eq to less than 200 g / eq. This configuration has the advantage that a cured product with high elastic modulus and heat resistance can be obtained.

[0030] In this specification, the epoxy equivalent refers to the molecular weight per epoxy group contained in a compound having an epoxy group, and specifically, is a value calculated based on the following formula: Epoxy equivalent (g / eq) = mass average molecular weight (Mw) of a compound / number of epoxy groups (average number) per molecule of the compound. The epoxy equivalent can also be measured in accordance with JIS K7236.

[0031] (Unmodified bisphenol A type epoxy resin and / or unmodified bisphenol F type epoxy resin) The present curable resin composition preferably contains, as component (A), an unmodified bisphenol A type epoxy resin and / or an unmodified bisphenol F type epoxy resin.

[0032] When the present curable resin composition contains an unmodified bisphenol A type epoxy resin and / or an unmodified bisphenol F type epoxy resin as component (A), the present curable resin composition particularly preferably contains an unmodified bisphenol A type epoxy resin having an epoxy equivalent of less than 220 g / eq and / or an unmodified bisphenol F type epoxy resin having an epoxy equivalent of less than 220 g / eq as the epoxy resin (A). Both the unmodified bisphenol A type epoxy resin having an epoxy equivalent of less than 220 g / eq and the unmodified bisphenol F type epoxy resin having an epoxy equivalent of less than 220 g / eq are liquid at room temperature and have excellent handleability. Therefore, it is particularly preferable that the present curable resin composition contains an unmodified bisphenol A type epoxy resin having an epoxy equivalent of less than 220 g / eq and / or an unmodified bisphenol F type epoxy resin having an epoxy equivalent of less than 220 g / eq as the epoxy resin (A). In this case, there is an advantage that the handleability of the curable resin composition is further improved.

[0033] The total content of the unmodified bisphenol A type epoxy resin and the unmodified bisphenol F type epoxy resin in component (A) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on 100% by mass of component (A). This configuration has the advantage that the cured product obtained has better impact resistance. The total content of the unmodified bisphenol A type epoxy resin and the unmodified bisphenol F type epoxy resin in component (A) may be 100% by mass, based on 100% by mass of epoxy resin (A). In other words, epoxy resin (A) may be (or may consist of) unmodified bisphenol A type epoxy resin and / or unmodified bisphenol F type epoxy resin.

[0034] (rubber modified epoxy resin) The present curable resin composition may contain a rubber-modified epoxy resin as the epoxy resin (A).

[0035] In this specification, the rubber-modified epoxy resin refers to a reaction product having 1.1 or more epoxy groups, preferably 2 or more, on average per molecule, which is obtained by reacting rubber with an epoxy group-containing compound. Examples of the rubber include rubber-based polymers such as acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), hydrogenated nitrile rubber (HNBR), ethylene propylene rubber (DPDM), acrylic rubber (ACM), butyl rubber (IIR), butadiene rubber, polyoxyalkylene such as polypropylene oxide, polyethylene oxide, and polytetramethylene oxide. The rubber-based polymers also include those having reactive groups such as amino groups, hydroxyl groups, or carboxyl groups at their terminals. Examples of the epoxy group-containing compound that can be reacted with rubber include commonly used epoxy resins, such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and each compound exemplified as other epoxy resins.

[0036] When the present curable resin composition contains a rubber-modified epoxy resin as component (A), the content of the rubber-modified epoxy resin in 100% by mass of the total amount of component (A) is preferably 1% by mass to 20% by mass, and more preferably 5% by mass to 15% by mass. When the content of the rubber-modified epoxy resin in component (A) contained in the present curable resin composition is within the above range, it is possible to provide a cured product that is excellent in handleability and has excellent adhesive strength when cured at a low temperature (e.g., 120 to 140°C).

[0037] <Polymer particles having a core-shell structure (B)> The present curable resin composition contains 5 to 100 parts by mass of polymer particles (B) having a core-shell structure (component (B)) based on 100 parts by mass of component (A).

[0038] In this specification, the polymer particles having a core-shell structure (also referred to as polymer particles) are intended to mean particles in which a core layer made of a core polymer and a shell layer made of a shell polymer form a layer structure. The structure of the polymer particles as component (B) is not particularly limited as long as it has at least one core layer and at least one shell layer, and it is also possible to have a structure of three or more layers having an intermediate layer covering the core layer and / or a shell layer further covering this intermediate layer. In addition, in component (B), the core layer and the shell layer do not have to form a complete layer structure. That is, the shell layer only needs to cover at least a part of the core layer, and does not have to cover the entire core layer. In addition, a part of the shell polymer constituting the shell layer may be embedded in the core layer.

[0039] In component (B), it is preferable that the shell polymer and the core polymer are substantially chemically bonded (for example, graft-bonded). Component (B) is more preferably a polymer particle obtained by forming a shell layer by graft polymerizing a graft copolymerizable monomer (shell monomer) onto the core layer (core polymer) in the presence of the core layer. Such a polymerization operation can be carried out, for example, by adding a shell monomer to a latex of a core polymer prepared in an aqueous polymer latex state and polymerizing it. Component (B) obtained by such an operation can have a structure including a core layer present inside and at least one shell layer graft-polymerized onto the surface thereof to surround or cover a part of the core layer.

[0040] Each layer that may contain component (B) will be specifically described below.

[0041] <Core layer> The core layer is preferably an elastic core layer having rubber properties in order to enhance the toughness of the cured product of the composition.

[0042] The core layer preferably contains a diene-based rubber because it has a high effect of improving the toughness of the cured product, a high effect of improving the impact peel adhesion of the cured product, and is less likely to cause an increase in viscosity over time due to swelling of the core layer due to its low affinity with component (A). The core layer preferably contains a (meth)acrylate-based rubber because a wide range of polymer compositions can be designed by combining a variety of monomers. In addition, when it is intended to improve the impact resistance at low temperatures without decreasing the heat resistance of the cured product, the core layer preferably contains an organosiloxane-based rubber. In other words, the core layer preferably contains one or more rubbers selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and organosiloxane-based rubbers.

[0043] (Diene rubber) The diene rubber is preferably a polymer containing 50% by mass to 100% by mass of structural units (hereinafter also referred to as conjugated diene units) derived from at least one monomer selected from the group consisting of conjugated diene monomers, and 0% by mass to 50% by mass of structural units derived from a vinyl monomer other than a conjugated diene monomer copolymerizable with the conjugated diene monomer.

[0044] Examples of the conjugated diene monomer include 1,3-butadiene, isoprene (2-methyl / 1,3-butadiene), and 2-chloro-1,3-butadiene.

[0045] These conjugated diene monomers may be used alone or in combination of two or more.

[0046] The content of the conjugated diene unit in the core layer is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, based on 100% by mass of all structural units constituting the core layer. When the content of the conjugated diene unit in the core layer is 50% by mass or more, the impact peel adhesion of the obtained cured product can be improved.

[0047] Examples of vinyl monomers other than conjugated diene monomers copolymerizable with the conjugated diene monomers include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.

[0048] These vinyl monomers may be used alone or in combination of two or more. Styrene is particularly preferred.

[0049] From the viewpoints of a higher toughness improving effect of the obtained cured product, a higher impact peel adhesion improving effect of the obtained cured product, and a lower affinity with component (A) so that the viscosity increase over time due to swelling of the core layer is less likely to occur, the core layer more preferably contains butadiene rubber, which is a homopolymer of 1,3-butadiene, and / or butadiene / styrene rubber, which is a copolymer of 1,3-butadiene and styrene, among diene rubbers, more preferably (consists only of) butadiene rubber and / or butadiene / styrene rubber, even more preferably contains butadiene rubber, and particularly preferably (consists only of) butadiene rubber. Also, butadiene / styrene rubber is preferred because it can increase the transparency of the obtained cured product by adjusting the refractive index.

[0050] ((Meth)acrylate rubber) The (meth)acrylate rubber is preferably a polymer obtained by polymerizing a monomer mixture containing 50% by mass to 100% by mass of structural units (hereinafter also referred to as (meth)acrylate units) derived from at least one monomer selected from the group consisting of (meth)acrylate monomers, and 0% by mass to 50% by mass of structural units derived from vinyl monomers other than (meth)acrylate monomers copolymerizable with the (meth)acrylate monomers. In this specification, "(meth)acrylate" means acrylate and / or methacrylate.

[0051] Examples of the (meth)acrylate monomer include: (i) alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (ii) aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; and (iii) hydroxyalkyl (meth)acrylates. (iv) glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; (v) alkoxyalkyl (meth)acrylates; (vi) allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; (vii) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, etc.

[0052] Examples of hydroxyalkyl (meth)acrylates include hydroxy linear alkyl (meth)acrylates (particularly, hydroxy linear C1-6 alkyl (meth)acrylates) such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates; hydroxy branched alkyl (meth)acrylates such as α-(hydroxymethyl)methyl acrylate and α-(hydroxymethyl)ethyl acrylate; and hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).

[0053] These (meth)acrylate monomers may be used alone or in combination of two or more. As the (meth)acrylate monomers, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred.

[0054] Examples of vinyl monomers other than (meth)acrylate monomers copolymerizable with (meth)acrylate monomers include (i) vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; (ii) vinyl carboxylic acids such as acrylic acid and methacrylic acid; (iii) vinyl cyanides such as acrylonitrile and methacrylonitrile; (iv) vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; (v) vinyl acetate; (vi) alkenes such as ethylene, propylene, butylene, and isobutylene; and (vii) polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.

[0055] The vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer may be used alone or in combination of two or more. Styrene is particularly preferred because it can easily increase the refractive index.

[0056] (Organosiloxane rubber) Examples of the organosiloxane rubber include: (i) polysiloxane polymers composed of alkyl or aryl di-substituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy; and (ii) polysiloxane polymers composed of alkyl or aryl mono-substituted silyloxy units, such as organohydrogensilyloxy in which some of the alkyl groups in the side chains are substituted with hydrogen atoms.

[0057] These polysiloxane-based polymers may be used singly or in combination of two or more kinds. Among them, dimethylsilyloxy, methylphenylsilyloxy and dimethylsilyloxy-diphenylsilyloxy are preferred because they can impart heat resistance to the cured product, and dimethylsilyloxy is most preferred because it is easily available.

[0058] In order to enhance the toughness of the resulting cured product, the core layer preferably has a glass transition temperature of 0° C. or lower, more preferably −20° C. or lower, further preferably −40° C. or lower, and particularly preferably −60° C. or lower.

[0059] The volume average particle diameter of the core layer is not particularly limited, but is preferably 0.03 μm to 2 μm, more preferably 0.05 μm to 1 μm, more preferably 0.12 μm to 0.50 μm, more preferably 0.12 μm to 0.28 μm, and even more preferably 0.14 to 0.25 μm. When the volume average particle diameter of the core layer is within this range, the core layer can be produced stably, and the heat resistance and impact resistance of the cured product can be good. The method for measuring the volume average particle diameter of the core layer will be described in detail in the following examples.

[0060] The core layer may be a single layer structure, or may be a multi-layer structure composed of layers having rubber elasticity. In the case where the core layer is a multi-layer structure, the polymer composition of each layer may be different from each other within the range disclosed above.

[0061] In one embodiment of the present invention, an intermediate layer, for example, as described in paragraphs

[0046] to

[0049] of the pamphlet of WO2016-163491, can be provided between the core layer and the shell layer.

[0062] <Shell layer> The shell layer is a polymer formed by polymerizing a shell monomer (monomer for forming the shell layer). The polymer constituting the shell layer (shell polymer) plays a role of improving the compatibility between component (B) and component (A) and enabling component (B) to be dispersed in the form of primary particles in the present curable resin composition and / or the cured product obtained by curing the present curable resin composition.

[0063] The shell layer of component (B) contains 30% by mass to 90% by weight of structural units derived from an alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms, out of 100% by mass of all structural units constituting the shell layer. In other words, the shell layer of component (B) is a polymer obtained by polymerizing a shell monomer (monomer composition) containing 30% by mass to 90% by weight of an alkyl (meth)acrylate monomer having a linear or branched alkyl group having 1 to 3 carbon atoms, out of 100% by mass of the total amount of shell monomers.

[0064] Examples of (meth)acrylate monomers having a linear or branched alkyl group having 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, methyl ethyl (meth)acrylate, etc. The shell layer of component (B) may contain only a structural unit derived from one of these monomers, or may contain structural units derived from two or more of these monomers.

[0065] Of all the structural units constituting the shell layer of component (B) (100% by mass), the content of structural units derived from an alkyl (meth)acrylate having a linear or branched alkyl group with 1 to 3 carbon atoms is 30% by mass to 90% by weight, preferably 40% by mass to 80% by weight, more preferably 50% by mass to 70% by weight, and even more preferably 55% by mass to 65% by weight. By making the shell layer of component (B) contain 30% by mass to 90% by weight of structural units derived from an alkyl (meth)acrylate having a linear or branched alkyl group with 1 to 3 carbon atoms, it is possible to provide polymer particles equipped with a shell layer having a desired glass transition temperature and SP value.

[0066] As long as the shell layer contains 30% by mass to 90% by weight of a structural unit derived from an alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms, the type and content ratio of other structural units contained in the shell layer are not particularly limited. From the viewpoint of compatibility and dispersibility of component (B) in the present curable resin composition, the shell layer preferably contains a structural unit derived from one or more monomers selected from the group consisting of aromatic vinyl monomers and (meth)acrylate monomers other than alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms (other (meth)acrylate monomers).

[0067] Specific examples of the aromatic vinyl monomer include vinylbenzenes such as styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene. As specific examples of other (meth)acrylate monomers, various monomers described in the section on "Core Layer" above can be used. Therefore, the description therein is incorporated by reference and will not be described here.

[0068] In one embodiment of the present invention, the shell monomer preferably does not contain a vinylcyan monomer. In other words, the shell layer of component (B) preferably does not contain a structural unit derived from a vinylcyan monomer. Since vinylcyan monomers have high glass transition temperatures and SP values, when the shell layer contains structural units derived from a vinylcyan monomer, it tends to be difficult to provide polymer particles having a shell layer with a desired glass transition temperature and / or SP value. By not using such a vinylcyan monomer as the shell monomer, it is possible to efficiently provide polymer particles having a shell layer with a desired glass transition temperature and / or SP value.

[0069] Specific examples of the vinylcyan monomer include acrylonitrile and methacrylonitrile.

[0070] In order to maintain a good dispersion state of component (B) without aggregation in the present curable resin composition and in the cured product obtained by curing the present curable resin composition, from the viewpoint of chemically bonding component (B) and component (A), it is preferable that the shell layer has a constitutional unit derived from a reactive group-containing monomer. In other words, it is preferable that the shell layer contains a reactive group.

[0071] The reactive group is preferably at least one selected from the group consisting of, for example, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group.

[0072] The reactive group is preferably an epoxy group, since the resulting cured product has excellent adhesive strength and impact peel adhesion. In other words, the shell layer preferably has a structural unit derived from a monomer having an epoxy group, i.e., preferably has an epoxy group.

[0073] Specific examples of the monomer having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.

[0074] When the shell layer of component (B) has an epoxy group, the content of the epoxy group in the shell layer relative to the total mass of the shell layer of component (B) is preferably more than 0 mmol / g and not more than 2.0 mmol / g, more preferably 0.1 mmol / g to 2.0 mmol / g or more, and more preferably 0.3 mmol / g to 1.5 mmol / g, from the viewpoints of the adhesive strength and impact peel adhesion of the obtained cured product and the storage stability of the composition. According to this configuration, aggregation of component (B) is suppressed, and component (B) can be dispersed in the cured product in the state of primary particles, and as a result, the adhesive strength and impact peel adhesion of the cured product can be improved.

[0075] The monomer having an epoxy group is preferably used for forming the shell layer, and more preferably used only for forming the shell layer, in other words, the core layer and the intermediate layer preferably do not have an epoxy group.

[0076] On the other hand, from the viewpoint of the storage stability of the present curable resin composition, it is preferable that the shell layer of component (B) does not have an epoxy group.

[0077] Specific examples of the monomer having a hydroxyl group as the reactive group-containing monomer include the above-mentioned hydroxyalkyl (meth)acrylates.

[0078] When the shell layer contains a constitutional unit derived from a polyfunctional monomer having two or more radically polymerizable double bonds, it is possible to prevent swelling of the component (B) in the curable resin composition, and the viscosity of the curable resin composition is reduced, which is preferable because it improves the handleability. On the other hand, from the viewpoint of improving the toughness and impact peel adhesion of the obtained cured product, it is preferable that the shell layer does not contain a constitutional unit derived from a polyfunctional monomer having two or more radically polymerizable double bonds.

[0079] Specific examples of the polyfunctional monomer do not include conjugated diene monomers such as butadiene, and include allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; allyloxyalkyl (meth)acrylates; polyfunctional (meth)acrylates having two or more (meth)acrylic groups such as (poly)ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.

[0080] Of these polyfunctional monomers, allyl methacrylate and triallyl isocyanurate are preferred.

[0081] The shell layer is preferably a polymer consisting of, for example, the following structural units: (a) 0% by mass to 50% by mass (preferably 1% by mass to 50% by mass, more preferably 2% by mass to 48% by mass) of structural units derived from an aromatic vinyl monomer (particularly preferably styrene), (b) 0% by mass to 50% by mass (preferably 0% by mass to 30% by mass, more preferably 10% by mass to 25% by mass) of structural units derived from a vinylcyan monomer (particularly preferably acrylonitrile), (c) 0% by mass to 50% by mass (preferably 0% by mass to 30% by mass, more preferably 10% by mass to 25% by mass) of a (meth)acrylate monomer ((i) preferably Preferably, 0% to 100% by mass (preferably 5% to 100% by mass, more preferably 70% to 95% by mass) of structural units derived from one or more monomers selected from the group consisting of methyl acrylate, butyl acrylate, and methyl methacrylate, (ii) particularly preferably methyl methacrylate), and (d) 1% to 50% by mass (preferably 2% to 35% by mass, more preferably 3% to 20% by mass) of structural units derived from a monomer having an epoxy group (particularly glycidyl methacrylate). However, it is intended that the total of (i) structural units derived from aromatic vinyl monomers, structural units derived from vinylcyan monomers, structural units derived from (meth)acrylate monomers, and structural units derived from monomers having an epoxy group is 100% by mass, and (ii) 0% by mass does not necessarily include such structural units.

[0082] The above-mentioned monomer components may be used alone or in combination of two or more. The shell layer may contain a structural unit derived from a monomer other than the above-mentioned monomers.

[0083] The shell layer may have a single layer structure or a multi-layer structure. When the shell layer has a multi-layer structure, the polymer composition of each layer may be different within the above range.

[0084] <SP value of the shell layer of component (B)> The SP value (solubility parameter) of the shell layer of component (B) is set to 10.00 to 10.65 (cal / cm) from the viewpoints of handling and shower resistance. 3 ) 1 / 2and 10.00 to 10.65 (cal / cm 3 ) 1 / 2 It is preferable that the range is 10.10 to 10.60 (cal / cm 3 ) 1 / 2 More preferably, it is 10.20 to 10.55 (cal / cm 3 ) 1 / 2 More preferably, it is 10.30 to 10.50 (cal / cm 3 ) 1 / 2 More preferably, it is 10.40 to 10.50 (cal / cm 3 ) 1 / 2 It is even more preferred that:

[0085] In the present specification, when the shell layer of a polymer particle having a core layer and a shell layer is a copolymer of m types of known monomers (composed of structural units derived from m types of known monomers), the glass transition temperature SP value (SPc) of the shell layer of the polymer particle is a value calculated by the following formula (1):

[0086]

number

[0087] In formula (1), n ​​is a natural number from 1 to m, and SP n is the SP value of the homopolymer of each monomer from which the structural units constituting the shell layer are derived, and W n is the weight of each monomer from which the structural units constituting the shell layer are derived. The SP value of the homopolymer of each monomer can be calculated, for example, by the Fedors method described in Polymer Engineering and Science, 1974, Vol. 14, pp. 147-154.

[0088] <Glass transition temperature (Tg) of the shell layer of component (B)> The glass transition temperature (hereinafter sometimes simply referred to as "Tg") of the shell layer of component (B) is, from the viewpoints of handleability and shower resistance, -25.0°C to 18.0°C, preferably -14.0°C to 18.0°C, more preferably -13.0°C to 15.0°C, even more preferably -12.0°C to 10.0°C, even more preferably -11.0°C to 5.0°C, and even more preferably -10.5°C to 0.0°C.

[0089] The Tg of the shell layer of the polymer particle can be determined by the composition of the structural units contained in the shell layer. In other words, the Tg of the shell layer of the obtained polymer particle can be adjusted by changing the composition of the shell monomer used when producing (polymerizing) the shell layer.

[0090] In the present specification, when the shell layer of the polymer particle is a copolymer of m types of known monomers (composed of structural units derived from m types of known monomers), the glass transition temperature Tg c is a value calculated by the FOX formula (Formula 2) shown below:

[0091]

number

[0092] In formula (2), n is a natural number from 1 to m, and Wf n is the weight fraction of each monomer from which the structural units constituting the shell layer are derived, and Tg n is the Tg of the homopolymer of each monomer from which the structural units constituting the shell layer are derived. The Tg of the homopolymer of each monomer can be, for example, the numerical value described in Polymer Handbook Fourth Edition (edited by J. Brandup et al., Jphn Wiley & Sons, Inc.). In the case of a new polymer, the peak temperature of the loss tangent (tan δ) in the viscoelasticity measurement method (shear method, measurement frequency: 1 Hz) can be used as the Tg.

[0093] When the composition of the monomer from which the structural unit constituting the shell layer of a polymer particle having a core layer and a shell layer is derived is unknown, the Tg of the shell layer of the polymer particle can also be measured by performing viscoelasticity measurement using a flat plate made of the polymer particle. Specifically, the Tg of the shell layer of the polymer particle can be measured as follows: (1) A dynamic viscoelasticity measurement is performed under tensile conditions on a flat plate made of polymer particles using a dynamic viscoelasticity measuring device (e.g., DVA-200, manufactured by IT Measurement and Control Co., Ltd.) to obtain a tan δ graph; (2) The peak temperature of tan δ on the obtained tan δ graph is taken as the Tg of the shell layer. Here, when multiple peaks are obtained in the tan δ graph, the highest peak temperature is taken as the Tg of the shell layer.

[0094] <Volume average particle size (Mv) of component (B)> The volume average particle diameter (Mv) of component (B) is not particularly limited, but from the viewpoint of industrial productivity and workability of the curable resin composition, it is preferably 0.01 μm to 2.00 μm, more preferably 0.03 μm to 0.60 μm, more preferably 0.05 μm to 0.40 μm, more preferably 0.10 μm to 0.30 μm, more preferably 0.15 μm to 0.30 μm, more preferably 0.16 μm to 0.28 μm, more preferably 0.17 μm to 0.27 μm, and even more preferably 0.18 μm to 0.25 μm. When the volume average particle diameter (Mv) of component (B) is (a) 0.01 μm or more, the viscosity of the curable resin composition is low, so that the workability is good, and when it is (b) 2.00 μm or less, the polymerization time of component (B) is short, so that the industrial productivity is high. The method for measuring the volume average particle size (Mv) of component (B) will be described in detail in the Examples below.

[0095] It is preferable that component (B) is dispersed in the curable resin composition in the form of primary particles. In this specification, "component (B) is dispersed in the form of primary particles" (hereinafter also referred to as primary dispersion) means that a plurality of particles of component (B) are dispersed substantially independently (without contact) with each other, and the dispersion state can be confirmed, for example, by dissolving a part of the curable resin composition in a solvent such as methyl ethyl ketone, and subjecting the solution to a particle size measuring device using laser light scattering to measure the particle size of component (B) in the curable resin composition.

[0096] The term "stable dispersion" of component (B) means a state in which component (B) is dispersed steadily for a long period of time under normal conditions without flocculation, separation, or precipitation in the continuous layer. It is also preferable that the distribution of component (B) in the continuous layer does not change substantially, and that the "stable dispersion" can be maintained even if the composition is heated within a safe range to reduce the viscosity and stirred.

[0097] As the component (B), one type of polymer particles may be used alone, or two or more types of polymer particles may be used in combination.

[0098] <Production method of component (B)> (Method of Manufacturing Core Layer) The core layer constituting component (B) can be formed by polymerizing a core monomer by a known polymerization method, such as emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Specific examples of the emulsion polymerization, suspension polymerization, and microsuspension polymerization methods include those described in WO 2005 / 028546 and WO 2006 / 070664.

[0099] (Method of forming shell layer and intermediate layer) The intermediate layer constituting component (B) can be formed by polymerizing the intermediate layer forming monomer by known radical polymerization. When the rubber elastic material constituting the core layer is obtained as an emulsion, it is preferable to polymerize the intermediate layer forming monomer by emulsion polymerization.

[0100] The shell layer constituting component (B) can be formed by polymerizing the shell monomer by known radical polymerization. When the core layer or the polymer particle precursor constituted by covering the core layer with the intermediate layer is obtained as an emulsion, it is preferable to polymerize the shell monomer by emulsion polymerization. As the emulsion polymerization method, for example, the method described in International Publication No. 2005 / 028546 can be appropriately used.

[0101] In emulsion polymerization, an emulsifier (dispersant) is used. Examples of emulsifiers include (i) (i-1) various acids such as alkyl or aryl sulfonic acids, such as dioctyl sulfosuccinic acid and dodecylbenzene sulfonic acid; alkyl or aryl ether sulfonic acids; alkyl or aryl sulfuric acids, such as dodecyl sulfuric acid; alkyl or aryl ether sulfuric acids; alkyl or aryl substituted phosphoric acids; alkyl or aryl ether substituted phosphoric acids; N-alkyl or aryl sarcosinic acids, such as dodecyl sarcosinic acid; alkyl or aryl carboxylic acids, such as oleic acid and stearic acid; alkyl or aryl ether carboxylic acids; and (i-2) anionic emulsifiers (dispersants), such as alkali metal salts or ammonium salts of these acids; (ii) nonionic emulsifiers (dispersants), such as alkyl or aryl substituted polyethylene glycol; and (iii) dispersants, such as polyvinyl alcohol, alkyl substituted cellulose, polyvinylpyrrolidone, and polyacrylic acid derivatives.

[0102] These emulsifiers (dispersants) may be used alone or in combination of two or more.

[0103] It is preferable to use a small amount of emulsifier (dispersant) within a range that does not impair the dispersion stability of the aqueous latex of the polymer particles. In addition, the higher the water solubility of the emulsifier (dispersant), the more preferable it is. If the water solubility is high, the emulsifier (dispersant) can be easily washed off with water, and adverse effects on the final cured product can be easily prevented.

[0104] When the emulsion polymerization method is employed, a peroxide (for example, an organic peroxide), a chain transfer agent, a surfactant, and the like can be used as necessary.

[0105] The polymerization conditions such as polymerization temperature, pressure, deoxidation, etc., may be within the known ranges.

[0106] In order to achieve an excellent balance between the storage stability of the curable resin composition and the toughness improving effect of the obtained cured product, the content of component (B) in the present curable resin composition is preferably 1 part by mass to 100 parts by mass, more preferably 5 parts by mass to 90 parts by mass, even more preferably 10 parts by mass to 80 parts by mass, even more preferably 20 parts by mass to 70 parts by mass, and particularly preferably 30 parts by mass to 60 parts by mass, relative to 100 parts by mass of component (A).

[0107] <Dicyandiamide (C)> The present curable resin composition contains 5 to 20 parts by mass of dicyandiamide (C) (component (C)) relative to 100 parts by mass of component (A). In the present curable resin composition, dicyandiamide as component (C) can function as a curing agent that cures the curable resin composition. Dicyandiamide does not exert a curing action at a temperature of at least 100°C, or even if it exerts a curing action, it proceeds the curing reaction very slowly. On the other hand, when heated to a temperature of 100°C or higher (preferably 120°C), dicyandiamide exerts a rapid curing action and can rapidly cure the curable resin composition. Because of such physical properties, dicyandiamide is sometimes called a latent curing agent.

[0108] The present curable resin composition contains 5 to 20 parts by mass of component (C) relative to 100 parts by mass of component (A), preferably 5.5 to 15 parts by mass, more preferably 6 to 10 parts by mass, and even more preferably 6 to 8 parts by mass. When the content of component (C) in the present curable resin composition is (1) 5 parts by mass or more relative to 100 parts by mass of component (A), there is an advantage that the cured product obtained by curing the present curable resin composition at low temperature has sufficient adhesive strength, and when it is (b) 20 parts by mass or less, there is an advantage that the storage stability of the present curable resin composition is good.

[0109] <Curing agent and / or curing accelerator (D)> The present curable resin composition contains a curing agent and / or a curing accelerator (D) (component (D)) in an amount of 1.5 to 10.0 parts by mass relative to 100 parts by mass of component (A). In this specification, the curing agent that may be contained as component (D) is intended to mean a compound having a function of curing the curable resin composition containing component (A). In addition, the curing catalyst that may be contained as component (D) is a compound that functions as a catalyst for promoting the reaction (i.e., curing reaction) between the epoxy group of component (A) and the epoxide reactive group of the component other than component (C) and component (A) contained in the curable resin composition. When component (D) is a curing agent (a compound that functions as a curing agent), it is preferable to select a (D) component that rapidly cures the curable resin composition containing component (A) when heated to a temperature of 80° C. or higher, preferably 100° C. or higher, more preferably 120° C. or higher.

[0110] The present curable resin composition may contain, as component (D), only a curing agent, only a curing catalyst, or both a curing agent and a curing catalyst.

[0111] The component (D) is not particularly limited as long as it has the above-mentioned effect, and examples thereof include (a) amine adduct compounds such as amine-epoxy adduct compounds which are reaction products between amine compounds and epoxy compounds, and urea adduct compounds which are reaction products between amine compounds and isocyanate compounds or urea compounds; (b) modified aliphatic polyamines which are modified products of aliphatic polyamines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenediamine, diethylaminopropylamine, and hexamethylenediamine; (c) hydrazides such as adipic acid dihydrazide, stearic acid dihydrazide, isophthalic acid dihydrazide, and semicarbazide; (d) 3-(3,4-dichlorophenyl)-1,1-dimethylurea, p (e) aromatic urea compounds such as N-chlorophenyl-N,N-dimethylurea (trade name: Monuron), 3-phenyl-1,1-dimethylurea (trade name: Fenuron), 3,4-dichlorophenyl-N,N-dimethylurea (trade name: Diuron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea (trade name: Chlortoluron), 1,1-dimethylphenylurea (trade name: Dyhard); (f) tertiary amines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol incorporated in a poly(p-vinylphenol) matrix, triethylenediamine, and N,N-dimethylpiperidine; (g) C1-C 12Examples of the imidazoles include alkylene imidazole, N-arylimidazole, 2-methylimidazole, 2-ethyl-2-methylimidazole, N-butylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and addition products of epoxy resins and imidazole; (g) 6-caprolactam. Among these, aromatic urea compounds are particularly preferred as component (D) because they can provide a curable resin composition with better handling properties and shower resistance. Component (D) may be encapsulated in microcapsules or the like, or may be a latent catalyst that becomes active only when the temperature is increased. As component (D), one of these may be used alone, or two or more may be used in combination.

[0112] The present curable resin composition preferably contains 1.5 to 10.0 parts by mass of component (D) relative to 100 parts by mass of component (A), more preferably 2.0 to 7.5 parts by mass, and even more preferably 4.0 to 6.0 parts by mass. When the content of component (D) is (a) 1.5 parts by mass or more relative to 100 parts by mass of epoxy resin (A), a curable resin composition capable of providing a cured product having excellent adhesive strength can be provided, and when (b) is 10.0 parts by mass or less, the storage stability of the present curable resin composition becomes good.

[0113] (Blocked isocyanate (E)) The present curable resin composition contains 0 to 20 parts by mass of a blocked isocyanate (E) (component (E)) relative to 100 parts by mass of component (A). In other words, the present curable resin composition (i) does not contain component (E), or (ii) contains more than 0 and 20 parts by mass or less of component (E) relative to 100 parts by mass of component (A). By making the content of component (E) in the present curable resin composition 20 parts by mass or less, there is no risk of unreacted component (E) remaining in the obtained cured product even when the curable resin composition is cured at a low temperature, and a cured product having superior adhesive strength can be provided.

[0114] The blocked isocyanate of component (E) is an elastomer type compound containing a urethane group and / or a urea group, and a compound having an isocyanate group at its terminal, in which all or a part of the terminal isocyanate group is capped with various blocking agents having active hydrogen groups. In particular, a compound in which all of the terminal isocyanate groups are capped with a blocking agent is preferred. Such a compound (blocked isocyanate) can be obtained, for example, by the following methods: (i) reacting a polyhydroxy compound with an excess of a polyisocyanate compound to obtain a polymer (prepolymer) having a urethane group and / or a urea group in the main chain skeleton and an isocyanate group at its terminal; (ii) after the above (i) or simultaneously with the above (i), a blocking agent having an active hydrogen group is allowed to act on all or a part of the isocyanate groups of the prepolymer, thereby capping all or a part of the isocyanate groups with the blocking agent. Therefore, a blocked isocyanate can also be expressed as the following (i) or (ii): (i) a compound composed of a prepolymer having an average of one or more isocyanate groups in the molecule and a blocking agent, the prepolymer consisting of a polyhydroxy compound and a polyisocyanate compound, or (ii) a compound containing a structure derived from a polyhydroxy compound, a structure derived from a polyisocyanate compound, and a structure derived from a blocking agent.

[0115] The blocked isocyanate component (E) may be, for example, a compound having a structure represented by the following general formula (3): A-(NR 2 -C(=O)-X) a ···General formula (3); (In the general formula (3), a R 2are each independently a hydrocarbon group having 1 to 20 carbon atoms. a represents the average number of capped isocyanate groups per molecule, and is preferably 1.1 or more, more preferably 1.5 to 8, even more preferably 1.7 to 6, and particularly preferably 2 to 4. X is a residue obtained by removing an active hydrogen atom from the blocking agent. A is a residue obtained by removing a terminal isocyanate group from an isocyanate-terminated prepolymer (for example, a urethane prepolymer having an isocyanate group at its terminal).

[0116] The isocyanate groups capped with the blocking agent in component (E) are regenerated by heating, and the regenerated isocyanate groups react with the active hydrogen-containing compound, etc. in the curable resin composition to improve the toughness of the resulting cured product.

[0117] The raw materials (used in the production) of the blocked isocyanate (E), that is, the "polyhydroxy compound", the "polyisocyanate compound" and the "blocking agent", will be described below.

[0118] (Polyhydroxy Compounds) In this specification, the term "polyhydroxy compound" refers to a polymer obtained by polymerizing a monomer having an active hydrogen-containing group at the end. Examples of the main chain structure constituting the polyhydroxy compound include polyether polymers, polyacrylic polymers, polyester polymers, polydiene polymers, saturated hydrocarbon polymers (polyolefins), and polythioether polymers. The polyhydroxy compound can also be said to be an organic polymer having an active hydrogen-containing group at the end.

[0119] (Active hydrogen group) Examples of the active hydrogen-containing group constituting the polyhydroxy compound include a hydroxyl group, an amino group, an imino group, and a thiol group. Among these, from the viewpoint of availability, a hydroxyl group, an amino group, and an imino group are preferred, and from the viewpoint of ease of handling (viscosity) of the resulting blocked isocyanate, a hydroxyl group is more preferred.

[0120] Examples of polyhydroxy compounds include polyether polymers (polyether polyols) having hydroxyl groups at the terminals, polyether polymers (polyether amines) having amino groups and / or imino groups at the terminals, polyacrylic polyols, polyester polyols, diene polymers (polydiene polyols) having hydroxyl groups at the terminals, saturated hydrocarbon polymers (polyolefin polyols) having hydroxyl groups at the terminals, polythiol compounds, polyamine compounds, etc. Among these, polyether polyols, polyether amines, and polyacrylic polyols are preferred because they have excellent compatibility with component (A), the glass transition temperature of the organic polymer is relatively low, and the adhesive layer obtained has excellent impact resistance at low temperatures. In particular, polyether polyols and polyether amines are more preferred because the viscosity of the organic polymer obtained is low and the workability is good, and polyether polyols are particularly preferred.

[0121] The polyhydroxy compounds used when preparing the urethane prepolymer, which is a precursor of the blocked isocyanate (E), may be used alone or in combination of two or more kinds.

[0122] (Polyether Polymer) The polyether polymer is a polymer having 40% by mass or more of repeating units represented by the following general formula (4) based on 100% by mass of an organic polymer: -R 1 -O- General formula (4) (In general formula (4), R 1 is a straight or branched alkylene group having 1 to 14 carbon atoms.

[0123] R in general formula (4) 1is preferably a linear or branched alkylene group having 1 to 14 carbon atoms, more preferably 2 to 4 carbon atoms. Specific examples of the repeating unit represented by the general formula (4) include -CHO-, -CHCHO-, -CHCH(CH)O-, -CHCH(CH)O-, -CHC(CH)O-, -CHCHCHCHO-, and the like. The main chain skeleton of the polyether polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units. In particular, a polyether polymer composed of a polymer mainly composed of polypropylene glycol having 50% or more by mass of propylene oxide repeating units in 100% by mass of the organic polymer is preferred because the resulting cured product has excellent T-peel adhesive strength. In addition, polytetramethylene glycol (PTMG) obtained by ring-opening polymerization of tetrahydrofuran is preferred because the resulting cured product has excellent dynamic splitting resistance.

[0124] The polyether polymer preferably contains 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more of the repeating unit of general formula (4) based on 100% by mass of the organic polymer.

[0125] The blocked isocyanate (E) is preferably a compound in which a urethane prepolymer containing a polyalkylene glycol structure is capped with a blocking agent, and more preferably a compound in which a urethane prepolymer containing a polypropylene glycol structure is capped with a blocking agent, because the temperature-sensitive characteristic of the viscosity of the resulting curable resin composition is small.

[0126] "The temperature sensitivity of the viscosity is small" means that "the temperature dependency of the viscosity is small."

[0127] (Polyether polyols and polyether amines) The polyether polyol is a polyether polymer having a hydroxyl group at its terminal, and the polyether amine is a polyether polymer having an amino group or an imino group at its terminal.

[0128] (Polyacrylic polyol) The polyacrylic polyol may be a polyol having a (meth)acrylic acid alkyl ester (co)polymer skeleton and having a hydroxyl group in the molecule. As the polyacrylic polyol, a polyacrylic polyol obtained by copolymerizing a hydroxyl group-containing (meth)acrylic acid alkyl ester monomer such as 2-hydroxyethyl methacrylate is particularly preferred.

[0129] The polyester polyol may be a polymer obtained by polycondensing (i) one or more selected from the group consisting of polybasic acids such as maleic acid, fumaric acid, adipic acid, phthalic acid, and their acid anhydrides, and (ii) one or more selected from the group consisting of polyhydric alcohols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, in the presence of an esterification catalyst at a temperature range of 150 to 270° C. Other examples include (a) ring-opening polymers such as ε-caprolactone and valerolactone, and (b) active hydrogen compounds having two or more active hydrogens such as polycarbonate diol and castor oil.

[0130] (Polydiene polyol) Examples of the polydiene polyol include polybutadiene polyol, polyisoprene polyol, polychloroprene polyol, etc. In particular, polybutadiene polyol is preferred.

[0131] (Polyolefin polyol) Examples of the polyolefin polyol include polyisobutylene polyol and hydrogenated polybutadiene polyol.

[0132] (Polyisocyanate compounds) Specific examples of the polyisocyanate compound include (a) aromatic polyisocyanates such as toluene (tolylene) diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, etc.; (b) aliphatic polyisocyanates such as isophorone diisocyanate, hexamethylene diisocyanate, hydrogenated toluene diisocyanate, hydrogenated diphenylmethane diisocyanate, etc. Among these, aliphatic polyisocyanates are preferred from the viewpoint of heat resistance, and isophorone diisocyanate and hexamethylene diisocyanate are more preferred from the viewpoint of availability.

[0133] The present inventors have found that when the present curable resin composition contains an aromatic urea compound as component (D), if a blocked polyisocyanate containing a structure derived from an aromatic polyisocyanate is used as component (E), the exothermic peak temperature of the curable resin composition tends to be high, and as a result, the low-temperature curing property of the curable resin composition may be reduced. Therefore, when the present curable resin composition contains an aromatic urea compound as component (D), it is preferable that component (E) is a blocked polyisocyanate that does not contain a structure derived from an aromatic polyisocyanate (a blocked polyisocyanate that does not contain an aromatic polyisocyanate as a raw material).

[0134] The present inventors speculate that the cause of the above phenomenon is as follows: When the curable resin composition is cured (heated), the aromatic urea compound, which is component (D), is thermally dissociated to generate aromatic isocyanate and amine. At this time, when the curable resin composition contains component (E) containing a structure derived from aromatic isocyanate, two types of aromatic isocyanate (derived from component (D) and component (E)) are present in large amounts in the curable resin composition due to dissociation of the blocking agent. Since dissociation of the blocking agent is a reversible reaction, when a large amount of uncapped aromatic isocyanate is present around it, dissociation of the blocking agent is difficult to proceed, and the dissociated blocking agent caps the aromatic isocyanate again, so the curing reaction is relatively delayed (compared to the case where component (E) containing a structure derived from aromatic isocyanate is not contained).

[0135] (Blocking agent having active hydrogen group) Examples of the blocking agent include primary amine-based blocking agents, secondary amine-based blocking agents, oxime-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, mercaptan-based blocking agents, amide-based blocking agents, imide-based blocking agents, heterocyclic aromatic compound-based blocking agents, hydroxy-functional (meth)acrylate-based blocking agents and phenol-based blocking agents.Among these, oxime-based blocking agents, lactam-based blocking agents, hydroxy-functional (meth)acrylate-based blocking agents and phenol-based blocking agents are preferred, hydroxy-functional (meth)acrylate-based blocking agents and phenol-based blocking agents are more preferred, and phenol-based blocking agents are even more preferred.

[0136] (Primary amine blocking agent) Examples of the primary amine-based blocking agent include various compounds described in paragraph

[0098] of the specification of WO2016-163491.

[0137] (Hydroxy-functional (meth)acrylate blocking agents) The hydroxy-functional (meth)acrylate-based blocking agent is a (meth)acrylate having one or more hydroxyl groups. Specific examples of the hydroxy-functional (meth)acrylate-based blocking agent include various compounds described in paragraph

[0099] of the specification of WO2016-163491.

[0138] (Phenol-based blocking agent) The phenolic blocking agent contains at least one phenolic hydroxyl group. The term "phenolic hydroxyl group" refers to a hydroxyl group directly bonded to a carbon atom of an aromatic ring. The phenolic compound may have two or more phenolic hydroxyl groups. The phenolic compound preferably contains only one phenolic hydroxyl group. The phenolic compound may contain other substituents. Examples of the other substituents include (a) linear, branched, or cycloalkyl alkyl groups; (b) aromatic groups (e.g., phenyl, alkyl-substituted phenyl, alkenyl-substituted phenyl, etc.); (c) aryl-substituted alkyl groups; (d) phenol-substituted alkyl groups, (e) alkenyl groups, and (f) allyl groups. Examples of the other substituents are preferably those that do not react with isocyanate groups under the conditions of the capping reaction, and more preferably alkenyl groups and allyl groups. Specific examples of the phenolic blocking agent include various compounds described in paragraph

[0100] of the specification of WO2016-163491.

[0139] The blocking agent is preferably bonded to the end of the polymer chain of the urethane prepolymer in such a manner that the end to which the blocking agent is bonded no longer has a reactive group. It can also be said that the polymer end obtained by bonding the blocking agent to the end of the polymer chain of the urethane prepolymer preferably does not have a reactive group. These blocking agents may be used alone or in combination of two or more.

[0140] As the component (E), a commercially available blocked isocyanate can also be used. Examples of such commercially available blocked isocyanates include QR-9466 (manufactured by ADEKA, a blocked isocyanate containing a structure derived from an aliphatic polyisocyanate) and TAKENATE B7005 (manufactured by Mitsui Chemicals, a blocked isocyanate containing a structure derived from an aromatic polyisocyanate).

[0141] From the viewpoint of providing a cured product having superior adhesive strength, the curable resin composition preferably contains more than 0 and not more than 17 parts by mass, more preferably 1 to 13 parts by mass, and even more preferably 2 to 7 parts by mass of component (E) per 100 parts by mass of component (A).

[0142] <Inorganic filler> The present curable resin composition preferably contains an inorganic filler. When the present curable resin composition contains an inorganic filler, the obtained cured product has an effect of being superior in rigidity at high temperatures.

[0143] Examples of inorganic fillers include silicic acid and / or silicates such as dry silica, wet silica, aluminum silicate, magnesium silicate, calcium silicate, etc.; reinforcing fillers such as wollastonite, talc, dolomite, and carbon black, or calcium oxide, heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, titanium oxide, ferric oxide, fine aluminum powder, zinc oxide, activated zinc oxide, etc. One of these inorganic fillers may be used alone, or two or more may be used in combination.

[0144] The dry silica is also called fumed silica. Examples of fumed silica include hydrophilic fumed silica with no surface treatment and hydrophobic fumed silica produced by chemically treating the silanol group portion of hydrophilic fumed silica with silane or siloxane. From the viewpoint of dispersibility in component (A), hydrophobic fumed silica is preferred.

[0145] The content of the inorganic filler in the present curable resin composition is preferably 1 to 300 parts by mass, more preferably 5 to 200 parts by mass, and even more preferably 10 to 150 parts by mass, relative to 100 parts by mass of component (A). If the content of the inorganic filler is within the above range, there is an advantage that the obtained cured product has even better rigidity and adhesive strength at high temperatures.

[0146] <Other ingredients> The curable resin composition may contain components (other components) other than the above components as necessary. Examples of the other components include reactive diluents, phenolic compounds, reinforcing agents, calcium oxide, radical curable resins, monoepoxides, photopolymerization initiators, expansion agents such as azo-type chemical foaming agents and thermally expandable microballoons, fiber pulps such as aramid pulp, colorants such as pigments and dyes, extender pigments, ultraviolet absorbers, antioxidants, stabilizers (gelling inhibitors), plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, low-shrinkage agents, organic fillers, thermoplastic resins, desiccants, and dispersants.

[0147] <Physical Properties of Curable Resin Composition> (Exothermic peak temperature) The exothermic peak temperature in the DSC measurement of the present curable resin composition is preferably less than 156 ° C, more preferably 155 ° C or less, and even more preferably 150 ° C or less. The exothermic peak temperature of the curable resin composition being less than 156 ° C means that the curable resin composition has excellent low-temperature curing properties (can be completely cured at a lower temperature). Since a curable resin composition having better low-temperature curing properties can be provided, the lower the exothermic peak temperature of the curable resin composition, the more preferable it is, and the lower limit is not particularly limited, but may be, for example, 120 ° C or more. The specific method for measuring the exothermic peak temperature of the curable resin composition is as described in the examples.

[0148] (Ratio of compounded viscosity (η25 / η50)) This curable resin composition has excellent handling properties and shower resistance. The handling properties and shower resistance of the curable resin composition can be evaluated by the ratio of the compounded viscosity (η50) at 50°C to the compounded viscosity (η25) at 25°C (compounded viscosity ratio (η25 / η50)). The smaller the value of η25 / η50 of the curable resin composition, the more excellent the handling properties and shower resistance of the curable resin composition. The specific method for measuring η50, η25 and η25 / η50 of the curable resin composition is as described in the examples.

[0149] <Method for producing curable resin composition> The method for producing the curable resin composition is not particularly limited, and various methods can be used, but examples of the method include a method in which component (B) obtained in an aqueous latex state is contacted with component (A) and then unnecessary components such as water are removed, and a method in which component (B) is once extracted into an organic solvent and then mixed with component (A) and then the organic solvent is removed. Specifically, as such a production method, it is preferable to use the method described in International Publication No. 2005 / 028546. More specifically, the curable resin composition is preferably prepared by a production method including the following steps 1 to 3 in order. a first step of mixing an aqueous latex containing component (B) (specifically, a reaction mixture obtained after producing component (B) by emulsion polymerization) with an organic solvent having a solubility in water at 20°C of 5% by mass to 40% by mass, and then further mixing the mixture with excess water to coagulate component (B); A second step of separating and recovering the aggregated component (B) from the liquid phase and then mixing it again with an organic solvent to obtain an organic solvent solution of component (B); A third step of mixing the organic solvent solution of component (B) with component (A) and then distilling off the organic solvent.

[0150] The present curable resin composition can be obtained by mixing additional components (A), (C), (D), and, if necessary, component (E), an inorganic filler, and other components with the dispersion in which component (B) is dispersed in component (A) in the form of primary particles, which is obtained through the above-mentioned first to third steps. Furthermore, according to this production method, the present curable resin composition in which component (B) is dispersed in the form of primary particles can be obtained. When the present curable resin composition is a composition in which component (B) is dispersed in component (A) in the form of primary particles, there is an advantage that the obtained cured product has excellent impact peel adhesion strength.

[0151] In addition, the present curable resin composition can be produced by redispersing the powdery component (B) obtained by drying after solidification by a method such as salting out in the component (A) using a dispersing machine having a high mechanical shear force such as a three-roll paint roll, a roll mill, or a kneader. In this case, component (B) can be efficiently dispersed in component (A) by applying a mechanical shear force at a high temperature to components (A) and (B). When the present curable resin composition is produced by applying a mechanical shear force using a dispersing machine, the temperature at which component (B) is dispersed in component (A) (the temperature at which the mechanical shear force is applied) is preferably 50°C to 200°C, more preferably 70°C to 170°C, further preferably 80°C to 150°C, and particularly preferably 90°C to 120°C.

[0152] The curable resin composition of the present invention can be used as a one-component curable resin composition that is prepared by premixing all the components, sealing and storing, applying, and then curing by heating or irradiating light. It can also be prepared as a two-component or multi-component curable resin composition that contains a liquid A containing component (A) as the main component and further component (B), and a liquid C prepared separately from the liquid A, containing components (C), (D), and, if necessary, component (E), an inorganic filler, and other components, and that is mixed with the liquid C before use. The curable resin composition of the present invention is particularly useful when used as a one-component curable resin composition.

[0153] When the present curable resin composition is a two-component or multi-component curable resin composition, component (B) may be contained in at least one of liquid A and liquid C. That is, component (B) may be contained only in liquid A, only in liquid C, or both in liquid A and liquid C.

[0154] 3. Uses of the Curable Resin Composition (Vehicle structural adhesives) In one embodiment of the present invention, a vehicle structural adhesive containing the present curable resin composition is provided. The vehicle structural adhesive containing the present curable resin composition has the advantage of being able to provide a cured product (adhesive layer) that is excellent in handleability and shower resistance and has excellent adhesive strength. In addition, the vehicle structural adhesive containing the present curable resin composition also has excellent low-temperature curing properties, so that The vehicle structural adhesive containing the present curable resin composition may be used as an adhesive containing only the present curable resin composition alone, or may be used as an adhesive containing the present composition mixed with other components as necessary.

[0155] (cured product) In one embodiment of the present invention, a cured product obtained by curing the present curable resin composition is provided. In this specification, the "cured product according to one embodiment of the present invention" may be referred to as the "present cured product". Since the present cured product has the above-mentioned configuration, it has the advantage of having excellent adhesive strength. In particular, since the present curable resin composition has excellent low-temperature curing properties, even when cured at low temperature (for example, under conditions of a curing temperature of 140°C and a curing time of 30 minutes), a cured product having excellent adhesive strength can be provided. Therefore, the present cured product is preferably a cured product obtained by curing the present curable resin composition at low temperature.

[0156] (Laminate) In one embodiment of the present invention, a laminate is provided in which a plurality of substrates are bonded together with a cured product (cured product) made of the curable resin composition of the present invention. In this specification, the "laminate according to one embodiment of the present invention" may be referred to as the "laminate of the present invention".

[0157] Examples of the substrate in the present laminate include steel materials such as cold-rolled steel and hot-dip galvanized steel, aluminum materials such as aluminum and coated aluminum, general-purpose plastics, engineering plastics, composite materials such as CFRP and GFRP, and various other plastic-based substrates. In the present laminate, substrates of the same type may be bonded together, or substrates of different types may be bonded together.

[0158] Applications of the present laminate are not particularly limited, but may include, for example, components for automobile and vehicle (bullet train, train, etc.) bodies, aircraft, spacecraft, space stations, structures, buildings, wind power plants, and the like. EXAMPLES

[0159] The following examples are provided to further illustrate one embodiment of the present invention, but the present invention is not limited to these examples.

[0160] 〔material〕 The substances used in the examples and comparative examples are shown below.

[0161] (Component (A)) (A-1) JER828EL (Mitsubishi Chemical, bisphenol A type epoxy resin, epoxy equivalent 186g / eq, liquid at room temperature) (A-2) (CTBN Adduct) Hypox RA1340 (CVC Thermoset Specialities, rubber modified epoxy resin) (Component (B)) As component (B), polymer particles prepared by the following method were used. As described later, component (B) was used in the form of dispersions ((M-1) to (M-9)) in which the prepared polymer particles were dispersed in component (A) ((A-1)).

[0162] 1. Formation of the core layer Production Example 1-1: Preparation of polybutadiene rubber latex (R-1) Into a pressure-resistant polymerization reactor, 200 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.002 parts by mass of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by mass of ferrous sulfate heptahydrate, and 1.55 parts by mass of sodium dodecylbenzenesulfonate (SDBS) were added, and oxygen was removed by thoroughly replacing with nitrogen while stirring. Then, 100 parts by mass of butadiene (Bd) were added to the pressure-resistant polymerization reactor, and the temperature was raised to 45°C. 0.03 parts by mass of paramenthane hydroperoxide (PHP) was added, followed by 0.10 parts by mass of sodium formaldehyde sulfoxylate (SFS), to start polymerization. 0.025 parts by mass of paramenthane hydroperoxide (PHP) was added at 3, 5, and 7 hours after the start of polymerization. In addition, 0.0006 parts by mass of EDTA and 0.003 parts by mass of ferrous sulfate heptahydrate were added 4, 6, and 8 hours after the start of polymerization. The polymerization was terminated 15 hours after polymerization by removing the remaining monomers under reduced pressure through volatilization, and a polybutadiene rubber latex (R-1) consisting mainly of polybutadiene rubber, which would become the core layer, was obtained. The volume average particle diameter of the polybutadiene rubber particles in the obtained latex was 0.08 μm.

[0163] Production Example 1-2: Preparation of polybutadiene rubber latex (R-2) In a pressure-resistant polymerization reactor, 21 parts by mass of the polybutadiene rubber latex (R-1) obtained in Production Example 1-1 (including 7 parts by mass of polybutadiene rubber), 185 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.002 parts by mass of EDTA, and 0.001 parts by mass of ferrous sulfate heptahydrate were added, and the mixture was thoroughly purged with nitrogen while stirring to remove oxygen. Then, 93 parts by mass of Bd was added to the pressure-resistant polymerization reactor and the temperature was raised to 45°C. 0.02 parts by mass of PHP and then 0.10 parts by mass of SFS were added to start polymerization. 0.025 parts by mass of PHP, 0.0006 parts by mass of EDTA, and 0.003 parts by mass of ferrous sulfate heptahydrate were added to the reaction system every 3 hours until the 24th hour after the start of polymerization. After 30 hours of polymerization, the remaining monomer was removed under reduced pressure by volatilization to terminate the polymerization, and a polybutadiene rubber latex (R-2) containing polybutadiene rubber as the main component for the core layer was obtained. The volume average particle diameter of the polybutadiene rubber particles contained in the obtained latex was 0.20 μm.

[0164] 2. Preparation of polymer particles with a core-shell structure (formation of the shell layer) Production Example 2-1: Preparation of latex (L-1) of polymer particles (B-1) having a core-shell structure In a glass reactor equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device, 262 parts by mass of polybutadiene rubber latex (R-2) containing 87 parts by mass of polybutadiene rubber particles prepared in Production Example 1-2 and 59 parts by mass of deionized water were charged and stirred at 60°C while performing nitrogen replacement. Next, 0.005 parts by mass of EDTA, 0.001 parts by mass of ferrous sulfate heptahydrate, and 0.2 parts by mass of SFS were added, and then a mixture of 13 parts by mass of shell monomer (7.2 parts by mass of methyl acrylate, 4 parts by mass of butyl acrylate, 1.8 parts by mass of glycidyl methacrylate) and 0.035 parts by mass of cumene hydroperoxide was continuously added over 1.3 hours to perform graft polymerization. After the addition was completed, the mixture was stirred for another 2 hours to complete the reaction, and a latex (L-1) of polymer particles (B-1) having a core-shell structure was obtained. The volume average particle size of the polymer particles (B-1) having a core-shell structure contained in the obtained latex was 0.21 μm.

[0165] Production Example 2-2: Preparation of latex (L-2) of polymer particles (B-2) having a core-shell structure A latex (L-2) of polymer particles (B-2) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0166] Production Example 2-3: Preparation of latex (L-3) of polymer particles (B-3) having a core-shell structure A latex (L-3) of polymer particles (B-3) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0167] Production Example 2-4: Preparation of latex (L-4) of polymer particles (B-4) having a core-shell structure A latex (L-4) of polymer particles (B-4) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0168] Production Example 2-5: Preparation of latex (L-5) of polymer particles (B-5) having a core-shell structure In a glass reactor equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device, 223 parts by mass of polybutadiene rubber latex (R-2) containing 74 parts by mass of polybutadiene rubber particles prepared in Production Example 1-2 and 85 parts by mass of deionized water were charged and stirred at 60°C while performing nitrogen replacement. Next, 0.005 parts by mass of EDTA, 0.001 parts by mass of ferrous sulfate heptahydrate, and 0.4 parts by mass of SFS were added, and then a mixture of 26 parts by mass of shell monomer (14 parts by mass of methyl acrylate, 8 parts by mass of butyl acrylate, and 4 parts by mass of glycidyl methacrylate) and 0.07 parts by mass of cumene hydroperoxide was continuously added over 2.6 hours to perform graft polymerization. After the addition was completed, the mixture was stirred for another 2 hours to complete the reaction, and a latex (L-5) of polymer particles (B-5) having a core-shell structure was obtained. The volume average particle size of the polymer particles (B-5) having a core-shell structure contained in the obtained latex was 0.21 μm.

[0169] Production Example 2-6: Preparation of latex (L-6) of polymer particles (B'-1) having a core-shell structure A latex (L-6) of polymer particles (B'-2) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0170] Production Example 2-7: Preparation of latex (L-7) of polymer particles (B'-2) having a core-shell structure A latex (L-7) of polymer particles (B'-2) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0171] Production Example 2-8: Preparation of latex (L-8) of polymer particles (B'-3) having a core-shell structure In a glass reactor equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device, 256 parts by mass of polybutadiene rubber latex (R-2) containing 85 parts by mass of polybutadiene rubber particles prepared in Production Example 1-2 and 63 parts by mass of deionized water were charged and stirred at 60°C while performing nitrogen replacement. Next, 0.005 parts by mass of EDTA, 0.001 parts by mass of ferrous sulfate heptahydrate, and 0.23 parts by mass of SFS were added, and then a mixture of 15 parts by mass of monomers for forming a shell layer (12.75 parts by mass of methyl methacrylate, 0.75 parts by mass of butyl acrylate, 1.5 parts by mass of glycidyl methacrylate) and 0.040 parts by mass of cumene hydroperoxide was continuously added over 1.5 hours to perform graft polymerization. After the addition was completed, the mixture was stirred for another 2 hours to complete the reaction, and a latex (L-8) of polymer particles (B'-3) having a core-shell structure was obtained. The volume average particle size of the polymer particles (B'-3) having a core-shell structure contained in the obtained latex was 0.21 µm.

[0172] Production Example 2-9: Preparation of latex (L-9) of polymer particles (B'-4) having a core-shell structure A latex (L-9) of polymer particles (B'-4) having a core-shell structure was prepared in the same manner as in Production Example 2-1, except that the composition of the shell monomer was changed to the composition shown in Table 1 below.

[0173] Production Example 3-1: Preparation of Dispersion (M-1) in which Polymer Particles (Polymer Particles (B-1)) are Dispersed in Epoxy Resin (Component (A)) 132 g of methyl ethyl ketone (MEK) was introduced into a 1 L mixing tank at 25 ° C. Next, while stirring the MEK, 132 g of the latex (L-1) of the polymer particles (B-1) prepared in Production Example 2-1 (corresponding to 40 g of polymer particles (B-1)) was added into the mixing tank. After the raw materials in the mixing tank were uniformly mixed, 200 g of water was added into the mixing tank at a feed rate of 80 g / min while stirring the raw materials in the mixing tank. After the water supply was completed, the stirring was stopped immediately, and a slurry liquid consisting of aggregates containing polymer particles (B-1) and an aqueous phase containing a small amount of organic solvent was obtained. The aggregates were floating. Next, 360 g of the aqueous phase was discharged from the outlet at the bottom of the mixing tank so that the aggregates containing a part of the aqueous phase were left in the mixing tank. 90 g of MEK was added to the obtained aggregates, and these were mixed uniformly to obtain a dispersion in which the polymer particles (B-1) were uniformly dispersed in MEK. To the obtained dispersion, 60 g of (A-1) which is the component (A) was added and mixed uniformly. MEK was removed from the obtained mixture using a rotary evaporator. By this operation, a dispersion (M-1) in which polymer particles (polymer particles (B-1)) were dispersed in the epoxy resin ((A-1)) was obtained.

[0174] Production Examples 3-2 to 3-9: Preparation of Dispersions (M-2) to (M-9) in which Polymer Particles (Polymer Particles (B-2) to (B-5), (B'-1) to (B'-4)) are Dispersed in Epoxy Resin (Component (A)) Except for using latexes (L-2) to (L-9) instead of latex (L-1), the same procedure as in Production Example 3-1 was repeated to obtain dispersions (M-2) to (M-9) in which polymer particles (polymer particles (B-2) to (B-5), (B'-1) to (B'-4)) were dispersed in epoxy resin ((A-1)).

[0175] The composition and physical properties of each of the prepared polymer particles are shown in Table 1. As is clear from Table 1, the polymer particles (B-1) to (B-5) are polymer particles that satisfy all the requirements of the polymer particles (B) according to one embodiment of the present invention, and correspond to the polymer particles (B) according to one embodiment of the present invention. On the other hand, the polymer particles (B'-1) to (B'-4) do not satisfy all the requirements of the polymer particles (B) according to one embodiment of the present invention. Therefore, they are not considered to be the polymer particles (B) according to one embodiment of the present invention.

[0176] [Table 1]

[0177] The SP value of the shell layer of each polymer particle in Table 1 was calculated based on the above formula (1) using the SP value of the homopolymer of each monomer used in the production of the polymer particle. The SP values ​​of the homopolymers of each monomer used in the calculation were as follows: Polymethyl methacrylate: 9.93 (cal / cm 3 ) 1 / 2 , Polybutyl acrylate: 9.77 (cal / cm 3 ) 1 / 2 , Polystyrene: 10.32 (cal / cm 3 ) 1 / 2 Polyacrylonitrile: 11.21 (cal / cm 3 ) 1 / 2 , Polyglycidyl methacrylate: 11.45 (cal / cm 3 ) 1 / 2 , Polymethyl acrylate: 10.56 (cal / cm 3 ) 1 / 2 .

[0178] The Tg of the shell layer of each polymer particle in Table 1 was calculated from the Fox formula shown in the above formula (2) using the Tg value of the homopolymer of each monomer used in the production of the polymer particle. The Tg values ​​of the homopolymer of each monomer used in the calculation were as follows: Methyl methacrylate (MMA): 105°C, Butyl acrylate (BA): -54°C, Methyl acrylate (MA): 8°C Glycidyl methacrylate (GMA): 46°C Styrene (St): 80°C, Acrylonitrile (AN): 97°C.

[0179] (Dicyandiamide (C)) Dyhard 100S (manufactured by AlzChem) (Curing agent and / or curing accelerator (D)) (D-1) Dyhard UR200 (AlzChem, 3-(3,4-dichlorophenyl)-1,1-dimethylurea) (D-2) Dyhard UR500 (AlzChem, toluyl-bis-1,1-dimethylurea) (D-3) Ajicure MY-24 (Ajinomoto Fine Techno, amine-epoxy adduct) (D-4) Ajicure PN-40 (Ajinomoto Fine Techno, amine-epoxy adduct) (D-5) Ancamine 2014AS (manufactured by Evonik, modified aliphatic polyamine).

[0180] (Blocked isocyanate (E)) (E-1) QR-9466 (ADEKA, blocked isocyanate containing an aliphatic polyisocyanate structure) (E-2) TAKENATE B7005 (manufactured by Mitsui Chemicals, a blocked isocyanate containing an aromatic polyisocyanate structure).

[0181] (Other Ingredients) Reactive diluent: Cardura E10P (Hexion, neodecanoic acid glycidyl ester) Calcium oxide: CML#31 (Omi Chemical Industry Co., Ltd.) Fumed silica: CAB-O-SIL TS720 (Cabot) Heavy calcium carbonate: Whiten SB Red (manufactured by Shiraishi Calcium, untreated heavy calcium carbonate, average particle size: 1.8 μm).

[0182] [Measurement method] The methods for measuring the various physical properties in the examples are shown below.

[0183] (Volume average particle size of core layer and polymer particles) The volume average particle diameter (Mv) of the polymer particles as the core layer prepared in the above manufacturing example and the polymer particles dispersed in the core-shell polymer latex was measured using Microtrac UPA150 (manufactured by Nikkiso Co., Ltd.). In the measurement, a latex containing each particle was diluted with deionized water and used as a measurement sample. The measurement was performed by inputting the refractive index of water and the refractive index of each polymer particle, adjusting the sample concentration so that the measurement time was 600 seconds and the signal level was within the range of 0.6 to 0.8.

[0184] (epoxy equivalent) The epoxy equivalent of component (A) was measured in accordance with JIS K 7236.

[0185] (Measurement of exothermic peak temperature) The method for measuring the exothermic peak temperature of the curable resin composition was as follows: 19 to 21 mg of the curable resin composition was measured using a differential scanning calorimeter at a temperature rise rate of 10°C / min, and the exothermic peak temperature was read from the obtained DSC curve.

[0186] (Measurement of compound viscosity) The compounded viscosity of the curable resin composition was measured as follows: the viscosity of the curable resin composition was measured at 25° C. and 50° C. at a shear rate of 5 s-1 using a rheometer. The obtained viscosity of the curable resin composition at 25° C. and 5 s-1 was designated as the compounded viscosity at 25° C. (η25), and the viscosity of the curable resin composition at 50° C. and 5 s-1 was designated as the compounded viscosity at 50° C. (η50).

[0187] (Ratio of blend viscosity) Based on the compounded viscosity (η25) at 25°C and the compounded viscosity (η50) at 50°C of the curable resin composition calculated by the above method, the compounded viscosity ratio (η25 / η50) of the curable resin composition was calculated by the following formula: The compounding viscosity ratio (η25 / η50) of the curable resin composition = the compounding viscosity (η25) of the curable resin composition at 25°C / the compounding viscosity (η50) of the curable resin composition at 50°C.

[0188] (Adhesive strength measurement) The adhesive strength of the cured product obtained by curing the curable resin composition was measured as follows: The curable resin composition was applied to two cold-rolled steel plates (SPCC steel plates) with dimensions: width 25 mm × length 100 mm × thickness 1.6 mm, and the two cold-rolled steel plates were overlapped so that the thickness of the curable resin composition layer was 0.25 mm. Thereafter, the curable resin composition between the two cold-rolled steel plates was cured under the conditions of a curing temperature of 140 ° C. and a curing time of 20 minutes, thereby obtaining a laminate in which the two cold-rolled steel plates were bonded by the cured product obtained by curing the curable resin composition. Using the obtained laminate as a sample, the shear adhesive strength (MPa) of the cured product was measured according to JIS K6850 using an autograph AG-2000E (manufactured by Shimadzu Corporation), and the obtained value was taken as the adhesive strength of the cured product. The measurement conditions were a measurement temperature of 23 ° C. and a test speed of 1.3 mm / min.

[0189] (Examples 1 to 5, Comparative Examples 1 to 5) A curable resin composition was obtained by weighing and thoroughly mixing each component according to the formulation shown in Table 2. The physical properties of the obtained curable resin composition were measured and evaluated. The results are shown in Table 2.

[0190] [Table 2]

[0191] [Summary 1] A comparison of Examples 1 to 5 with Comparative Examples 1 to 4 reveals that the curable resin compositions of Examples 1 to 5 have low η25 / η50, excellent handleability and shower resistance, and also excellent adhesive strength of the cured product. On the other hand, the curable resin compositions of Comparative Examples 1 to 4, which do not contain polymer particles that satisfy the requirements of component (B) according to one embodiment of the present invention, have high η25 / η50 and are curable resin compositions that are poor in handleability and shower resistance. A comparison of Examples 1 to 5 with Comparative Example 5 reveals that when the content of component (D) is too low, the adhesive strength of the cured product becomes poor.

[0192] (Example 6, Comparative Examples 6 and 7) A curable resin composition was obtained by weighing and thoroughly mixing each component according to the formulation shown in Table 3. The physical properties of the obtained curable resin composition were measured and evaluated. The results are shown in Table 3.

[0193] [Table 3]

[0194] [Summary 2] A comparison of Example 6 with Comparative Examples 6 and 7 reveals that the curable resin composition of Example 6 has a low η25 / η50 and is excellent in handleability and shower resistance. On the other hand, the curable resin compositions of Comparative Examples 6 and 7, which do not contain polymer particles that satisfy the requirements of component (B) according to one embodiment of the present invention, have a high η25 / η50 and are poor in handleability and shower resistance.

[0195] (Examples 7 to 9, Comparative Example 8) A curable resin composition was obtained by weighing and thoroughly mixing each component according to the formulation shown in Table 4. The physical properties of the obtained curable resin composition were measured and evaluated. The results are shown in Table 4.

[0196] [Table 4]

[0197] [Summary 3] A comparison of Examples 7 to 9 with Comparative Example 8 reveals that the curable resin compositions of Examples 7 to 9 have low η25 / η50, excellent handleability and shower resistance, and excellent adhesive strength of the cured product. On the other hand, the results of Comparative Example 8 reveal that when the content of component (E) is excessive, the adhesive strength of the cured product becomes poor.

[0198] (Examples 10 to 12, Comparative Example 9) A curable resin composition was obtained by weighing and thoroughly mixing each component according to the formulation shown in Table 5. The physical properties of the obtained curable resin composition were measured and evaluated. The results are shown in Table 5.

[0199] [Table 5]

[0200] [Summary 4] A comparison of Examples 10 to 12 with Comparative Example 9 reveals that the curable resin compositions of Examples 10 to 12 have low η25 / η50, excellent handleability and shower resistance, and excellent adhesive strength of the cured product. On the other hand, the results of Comparative Example 9 reveal that when the content of component (E) is excessive, the adhesive strength of the cured product becomes poor.

[0201] (Examples 13 to 16, Comparative Examples 10 to 12) The components were weighed and thoroughly mixed to obtain a curable resin composition according to the formula shown in Table 6. The physical properties of the obtained curable resin composition were measured and evaluated. The results are shown in Table 6.

[0202] [Table 6]

[0203] [Summary 5] A comparison of Examples 13 to 16 with Comparative Examples 10 to 12 reveals that the curable resin compositions of Examples 13 to 16 have low η25 / η50, excellent handleability and shower resistance, and also excellent adhesive strength of the cured product. On the other hand, the results of Comparative Example 10 reveal that when the content of component (E) is excessive, the adhesive strength of the cured product becomes poor. In addition, it is revealed that the curable resin compositions of Comparative Examples 11 and 12, which do not contain polymer particles that satisfy the requirements of component (B) according to one embodiment of the present invention, are curable resin compositions with high η25 / η50 and poor handleability and shower resistance. [Industrial Applicability]

[0204] According to one embodiment of the present invention, a curable resin composition can be provided that can provide a cured product having excellent handling properties, shower resistance, and adhesive strength. Such a curable resin composition can be suitably used as an adhesive for bonding steel plates, CFRP, aluminum plates, and concrete. Therefore, one embodiment of the present invention can be suitably used in the fields of vehicles, aircraft, space, machinery, electricity, architecture, and civil engineering.

Claims

1. 100 parts by weight of epoxy resin (A); 5 to 100 parts by weight of polymer particles (B) having a core-shell structure including a core layer and a shell layer; 5 to 20 parts by weight of dicyandiamide (C); 1.5 to 10 parts by weight of a curing agent and / or a curing accelerator (D); and 0 to 20 parts by weight of a blocked isocyanate (E), The glass transition temperature of the shell layer is −25° C. to 18° C., The SP value of the shell layer is 10.00 to 10.65 (cal / cm 3 ) 1/2 is less than the shell layer contains 30% by mass to 90% by weight of a structural unit derived from an alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 3 carbon atoms, based on 100% by mass of all structural units constituting the shell layer; Curable resin composition.

2. The curable resin composition according to claim 1, having an exothermic peak temperature of less than 156°C in DSC measurement.

3. The curable resin composition according to claim 1, wherein the curable composition contains an aromatic urea-based curing accelerator as the curing agent and / or the curing accelerator (D), and the blocked isocyanate (E) does not contain a structure derived from an aromatic polyisocyanate.

4. The curable resin composition according to claim 1, wherein the shell layer has a glass transition temperature of -14°C to 18°C.

5. The curable resin composition according to claim 1 , wherein the core layer comprises at least one rubber selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and organosiloxane-based rubbers.

6. The curable composition according to claim 1 , wherein the core layer is a butadiene rubber, and the shell layer does not contain a constitutional unit derived from a vinylcyan monomer.

7. A vehicle structural adhesive comprising the curable composition according to any one of claims 1 to 6.

8. A cured product obtained by curing the curable composition according to any one of claims 1 to 6.

9. A laminate comprising a plurality of substrates bonded together with the cured product according to claim 8.

Citation Information

Patent Citations

  • Adhesion method using polymer fine particle-containing curable resin composition excellent in workability, and laminate obtained using the adhesion method

    JP2019194316A

  • Epoxy resin composition

    JP2022092250A

  • Adhesion method employing polymer microparticle-containing curable resin composition having excellent workability, and laminate obtained using said adhesion method