Method for manufacturing honeycomb structure

The method of kneading silicon carbide and metallic silicon with a dopant solution in honeycomb structures addresses non-uniform dopant distribution, ensuring stable EHC performance by managing resistivity and preventing excessive current flow, suitable for use in electrically heated catalysts.

JP2024143854AActive Publication Date: 2024-10-11NGK CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023056767
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing methods for manufacturing honeycomb structures used in electrically heated catalysts (EHCs) face challenges in uniformly distributing dopants, leading to non-uniform volume resistivity and potential excessive current flow, especially at low voltages, which can damage power supply circuits.

Method used

A method involving kneading silicon carbide powder, metallic silicon powder, and an aqueous dopant source solution to create a honeycomb structure with controlled dopant distribution, using Group 13 and Group 15 elements, and applying electrode layers to manage resistivity and current flow.

Benefits of technology

The method achieves high uniformity in dopant distribution, preventing excessive current flow and ensuring stable operation across varying voltage ranges, thereby protecting power supply circuits and enhancing the performance of EHCs as catalyst carriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143854000001_ABST
    Figure 2024143854000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a honeycomb structure having high uniformity of dopant distribution.SOLUTION: A method for manufacturing a honeycomb structure of the present invention includes the steps of: kneading a molding raw material containing silicon carbide powder, metallic silicon powder, and an aqueous solution of a dopant source to prepare a green body; forming the green body to prepare a honeycomb formed body having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells which form a flow path from a first end face to a second end face; and firing the honeycomb formed body to prepare a fired honeycomb body, wherein the dopant source contains one or more dopants selected from Group 13 elements and Group 15 elements of the periodic table, and the number of atoms of at least one of the dopants in the aqueous solution of the dopant source is 1×1016 to 5×1020 atoms / cm3, expressed in terms of the number of dopant atoms relative to the volume of the metallic silicon.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a honeycomb structure, and more particularly to a method for manufacturing a honeycomb structure that can be suitably used as an electrically heated carrier. [Background technology]

[0002] Conventionally, catalysts supported on honeycomb structures made of cordierite or silicon carbide have been used to treat harmful substances in exhaust gases emitted from automobile engines. When treating exhaust gases with a catalyst supported on a honeycomb structure, the catalyst needs to be heated to a specified temperature. However, a problem has existed in the past where exhaust gases are not sufficiently purified at engine start-up because the catalyst temperature is low. To address this problem, a system called an electrically heated catalyst (EHC) has been developed in which electrodes are provided on a honeycomb structure made of conductive ceramics, and the honeycomb structure itself is heated by passing electricity through it, thereby heating the catalyst supported on the honeycomb structure to its activation temperature before or at engine start-up.

[0003] An EHC generally includes an outer peripheral wall, a conductive honeycomb structure having partition walls disposed inside the outer peripheral wall to define a plurality of cells that form a flow path from a first end face to a second end face, and a pair of electrode layers disposed on the outer peripheral wall of the honeycomb structure. When an EHC is mounted on an automobile or the like for use, the power source used for the electrical system of the automobile or the like is shared. For this reason, if an excessive current flows through the EHC, the power supply circuit may be damaged. Since various voltages are used for the power source for the EHC, it is important to adjust the resistance of the honeycomb structure for the EHC for each voltage to be used and control it so that an excessive current does not flow.

[0004] Patent Document 1 describes a honeycomb structure in which the partition walls and the outer peripheral wall contain silicon carbide particles as aggregates and silicon as a binder for binding the silicon carbide particles, and the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400° C. Patent Document 1 describes that the volume electrical resistance of the honeycomb structure at 400° C. can be set to 1 to 40 Ωcm by setting the average particle size of the silicon carbide particles to 3 to 40 μm. It also describes that since the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400° C., even if a current is passed through it using a high-voltage power source, an excessive current does not flow, and the honeycomb structure can be suitably used as a heater.

[0005] However, a very wide range of voltages is used for the power source of the EHC, depending on, for example, the type of vehicle in which it is installed. In particular, when a low voltage of 60 V or less, for example 48 V, is used for the power source of the EHC, the appropriate volume resistivity for suppressing the generation of excess current is around 0.1 Ω cm. Thus, in recent EHCs that use a wide range of voltages, there is a need for research and development of technology that effectively suppresses the generation of excess current even when used at a low voltage.

[0006] Therefore, Patent Documents 2 and 3 specify the range of the amount of dopant contained in the silicon constituting the EHC. In Patent Documents 2 and 3, the concentration of the dopant in the silicon in the ceramic constituting the partition walls and the outer peripheral wall of the honeycomb structure is set to 1×10 16 ~5×10 20 pieces / cm 3 It is stated that:

[0007] Patent Document 2 describes a method for manufacturing a honeycomb structure, which includes the steps of preparing a molding raw material by adding a binder, a surfactant, a pore-forming material, water, etc. to a powder of silicon powder to which a dopant has been added, or a powder obtained by mixing the silicon powder to which the dopant has been added with other ceramic materials, kneading the obtained molding raw material to form a puddle, extruding the puddle to prepare an unfired columnar honeycomb structure, and firing the unfired columnar honeycomb structure.

[0008] Patent Document 3 describes a method for manufacturing a honeycomb structure, which includes the steps of: preparing a molding raw material by adding a binder, a surfactant, water, etc. to a ceramic powder containing silicon carbide powder; kneading the obtained molding raw material to form a puddle; extruding the puddle to prepare an unfired honeycomb molded body; drying and degreasing the obtained honeycomb molded body to prepare a honeycomb degreased body; and impregnating and firing the honeycomb degreased body with silicon (metallic silicon), where the impregnation and firing are performed together with silicon doped with a dopant or a dopant source in the honeycomb degreased body. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5735428 [Patent Document 2] JP 2020-204300 A [Patent Document 3] JP 2022-142543 A Summary of the Invention [Problem to be solved by the invention]

[0010] As proposed in Patent Documents 2 and 3, controlling the concentration of dopant in silicon in the ceramics constituting the partition walls and outer peripheral wall of the honeycomb structure is useful for adjusting the volume resistivity of the honeycomb structure. However, in the conventional manufacturing method of the honeycomb structure, there is still room for improvement in terms of uniform distribution of dopant in the honeycomb structure. Uniform distribution of dopant in the honeycomb structure is desirable from the viewpoint of quality stability of the honeycomb structure.

[0011] Patent Documents 2 and 3 describe adding a dopant to silicon, but do not describe a specific method. In order to dope silicon with a dopant, a method of melting silicon and then dissolving the dopant is conceivable, but there are the following problems. First, the viscosity of molten silicon is high, making it difficult to uniformly disperse the dopant in the silicon. Second, in order to melt silicon, it is necessary to heat it to about 1400°C, and impurities may be mixed in from the melting furnace, lowering the purity. Furthermore, melting Si requires labor and cost.

[0012] In semiconductor manufacturing, doping is used as a method for controlling dopants in silicon, and methods such as doping partially molten silicon as a gas (FZ method) and doping by ion implantation are known. However, these methods are not suitable for uniformly doping honeycomb structures.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide, in one embodiment, a method for manufacturing a honeycomb structure having a highly uniform distribution of dopants. [Means for solving the problem]

[0014] The present inventors have conducted extensive research to solve the above problems, and have found that a process of preparing a clay by kneading a forming raw material containing silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source adjusted to a predetermined concentration is advantageous in obtaining a honeycomb structure having a highly uniform distribution of the dopant. The present invention has been completed based on this finding, and is exemplified below. [Aspect 1] A step of kneading a forming raw material including silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source to prepare a puddle; forming a honeycomb formed body having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths from a first end surface to a second end surface; A step of firing the honeycomb formed body to produce a honeycomb fired body; Including, The dopant source contains one or more dopants selected from Group 13 elements and Group 15 elements of the periodic table, and the number of atoms of at least one of the dopants in the aqueous solution of the dopant source is 1×10 in terms of the number of atoms of the dopant relative to the volume of the metallic silicon. 16 ~5×10 20 pieces / cm 3 That is, A method for manufacturing a honeycomb structure. [Aspect 2] The method according to embodiment 1, wherein the dopant source comprises one or more selected from an inorganic salt containing the dopant and an organic compound containing the dopant. [Aspect 3] 3. The method for manufacturing a honeycomb structure according to embodiment 1 or 2, wherein the dopant source contains P. [Aspect 4] The method according to any one of aspects 1 to 3, wherein the dopant source includes one or more selected from a P-containing inorganic salt and a P-containing organic compound. [Aspect 5] A method according to any one of aspects 1 to 4, wherein the dopant source comprises an organic phosphate. [Aspect 6] The method according to any one of aspects 1 to 5, wherein the dopant source comprises a compound containing the dopant, and the solubility of the compound in water at 20° C. is 1 g / 100 g H2O or more. [Aspect 7] 7. The manufacturing method according to any one of aspects 1 to 6, wherein the partition walls of the honeycomb structure have a metallic silicon content of 20 mass % or more. [Aspect 8] The average concentration of at least one of the dopants in the metallic silicon in the partition walls of the honeycomb structure is 1×10 16 ~5×10 20 pieces / cm 3 The production method according to any one of aspects 1 to 7, [Aspect 9] A method for manufacturing a honeycomb structure according to any one of aspects 1 to 8, further comprising the step of applying a pair of electrode layer forming pastes to the outer surface of the outer wall so as to extend in a band-like shape in the cell extension direction across the central axis of the honeycomb formed body before firing the honeycomb formed body, thereby producing a honeycomb formed body with electrode layer forming paste. Effect of the Invention

[0015] According to one embodiment of the present invention, a method for manufacturing a honeycomb structure having a highly uniform distribution of dopants can be provided. An electrically heated carrier can be manufactured by joining a metal terminal to the honeycomb structure. The electrically heated carrier can be suitably used, for example, as a catalyst carrier for an exhaust gas purification device. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic diagram of an electrically heated carrier according to an embodiment of the present invention, as viewed from a first end surface. [Diagram 2] FIG. 1 is a schematic perspective view of an electrically heated carrier according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0018] (1. Electrically heated carrier) Fig. 1 is a schematic diagram of an electrically heated support 100 according to an embodiment of the present invention when viewed from a first end surface 116. Fig. 2 is a schematic perspective view of the electrically heated support 100 according to an embodiment of the present invention.

[0019] The electrically heated carrier 100 includes a honeycomb structure 110 and a metal terminal 130. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and include co-catalysts such as ceria and zirconia, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples of the catalyst include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular limitation on the method of supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0020] (1-1. Honeycomb structure) In one embodiment, the honeycomb structure 110 is a honeycomb structure having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and partitioning a plurality of cells 115 that form flow paths from a first end surface 116 to a second end surface 118; a first electrode layer 112a provided on the outer surface of the outer peripheral wall 114 and extending in a strip shape in the extension direction of the cells 115; and A second electrode layer 112b is provided on the outer surface of the outer peripheral wall 114, extends in a strip shape in the extending direction of the cells 115, and is provided so as to face the first electrode layer 112a across the central axis O of the honeycomb structure portion. Equipped with. If not required, the first electrode layer 112a and the second electrode layer 112b may be omitted.

[0021] The outer shape of the honeycomb structure 110 is not particularly limited, and may be, for example, a columnar body whose end faces are round, such as circular, oval, elliptical, racetrack, or oval, a columnar body whose end faces are polygonal, such as triangular or rectangular, or a columnar body whose end faces have other irregular shapes. The illustrated honeycomb structure 110 has a circular end face shape and is cylindrical as a whole.

[0022] There is no particular limit to the height of the honeycomb structure 110 (the length from one end face to the other end face), and it may be set appropriately depending on the application and required performance. There is also no particular limit to the relationship between the height of the honeycomb structure 110 and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the honeycomb structure). Therefore, the height of the honeycomb structure 110 may be longer than the maximum diameter of each end face, or the height of the honeycomb structure 110 may be shorter than the maximum diameter of each end face.

[0023] The size of the honeycomb structure 110 is set to 2,000 to 20,000 mm2 in order to enhance heat resistance (suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm. 2 It is more preferable that:

[0024] <Honeycomb structure> The outer peripheral wall 114 and the partition walls 113 constituting the honeycomb structure part have a higher volume resistivity than the electrode layers 112a and 112b, but are conductive. The volume resistivity of the outer peripheral wall 114 and the partition walls 113 is not particularly limited as long as they can generate heat by Joule heat when current is applied, and may be appropriately set according to the voltage to be applied, and may be, for example, 0.001 to 100 Ω·cm. For a high voltage of more than 60 V, the volume resistivity may be 2 to 100 Ω·cm, typically 5 to 100 Ω·cm. For a low voltage of 60 V or less, such as 48 V, the volume resistivity may be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm. In this specification, the volume resistivity of the electrode layer, the partition walls, and the outer peripheral wall is a value measured at 25° C. by a four-terminal method.

[0025] In one embodiment, the outer peripheral wall 114 and the partition wall 113 contain a silicon carbide-silicon composite material. From the viewpoint of achieving both heat resistance and electrical conductivity, the outer peripheral wall 114 and the partition wall 113 are preferably mainly composed of a silicon carbide-silicon composite material. When the material of the outer peripheral wall 114 and the partition wall 113 is mainly composed of a silicon carbide-silicon composite material, it means that the outer peripheral wall 114 and the partition wall 113 each contain 80 mass% or more of the silicon carbide-silicon composite material (total mass). Here, the silicon carbide-silicon composite material contains silicon carbide particles as an aggregate and metal silicon as a binder for binding the silicon carbide particles. The outer peripheral wall 114 and the partition wall 113 may contain one or two types of aggregate selected from silicon nitride particles and aluminum nitride particles in addition to silicon carbide particles. They may also contain one or more types of other aggregates. Other aggregates include, for example, oxide ceramics such as alumina, mullite, zirconia, and cordierite.

[0026] However, it is preferable that the main component of the aggregate is silicon carbide, since the thermal conductivity is higher and the difference in thermal expansion coefficient with silicon is smaller. When the main component of the aggregate is silicon carbide, it means that the aggregate contains silicon carbide (total mass) in an amount of 80 mass% or more, more preferably 90 mass% or more.

[0027] The metallic silicon contained in the peripheral wall 114 and the partition walls 113 of the honeycomb structure 110 is preferably present as a continuous layer. With such a configuration, it is easy to control the volume resistivity to a low level. Here, the metallic silicon being present as a continuous layer refers to a matrix-domain structure in which the particles of silicon carbide or the like are domains and silicon is the matrix.

[0028] In order for the metallic silicon in the outer peripheral wall 114 and the partition walls 113 of the honeycomb structure 110 to form a continuous layer, the metallic silicon content in the outer peripheral wall 114 and the partition walls 113 is preferably 20% by mass or more. When the metallic silicon content in the outer peripheral wall 114 and the partition walls 113 is 20% by mass or more, the metallic silicon is easily arranged in series in the microstructure. As a result, the volume resistivity of the honeycomb structure 110 can be effectively reduced, and the generation of excess current can be appropriately suppressed even for low voltage applications of 60V or less, such as 48V. In addition, when the metallic silicon content in the outer peripheral wall 114 and the partition walls 113 is 80% by mass or less, the shape stability of the honeycomb structure 110 can be obtained. Therefore, the metallic silicon content in the outer peripheral wall 114 and the partition walls 113 of the honeycomb structure 110 is preferably 20 to 80% by mass, more preferably 25 to 60% by mass, and even more preferably 25 to 45% by mass.

[0029] The content of metallic silicon in the outer peripheral wall 114 and the partition wall 113 of the honeycomb structure 110 can be measured by the following method. In the following method, a calculation method when metallic silicon and silicon carbide are used as ceramic raw materials will be described. When metallic silicon and silicon carbide are used as ceramic raw materials, the outer peripheral wall 114 and the partition wall 113 are composed of metallic silicon (Si), silicon carbide (SiC) and silicon dioxide (SiO2). The content of Si, SiC and SiO2 in the outer peripheral wall 114 and the partition wall 113 can be measured by measuring the amount of silicon element and the amount of oxygen element by a fluorescent X-ray method, and measuring the amount of carbon element by a resistance heating infrared absorption method. The amount of SiC is calculated by assuming that all carbon elements are SiC and calculating the amount of SiC in the outer peripheral wall 114 and the partition wall 113 by molecular weight calculation. The amount of SiO2 is calculated by assuming that all oxygen elements are SiO2 and calculating the amount of SiO2 in the outer peripheral wall 114 and the partition wall 113 by molecular weight calculation. The amount of Si constituting the metallic silicon can be calculated by subtracting the total amount of Si in SiC and SiO2 from the total amount of silicon element using the amounts of SiC and SiO2 calculated above. When a ceramic raw material other than silicon carbide is used, the composition of the honeycomb structure based on the ceramic raw material is confirmed, and then the amount of elements can be measured by X-ray fluorescence method or resistance heating infrared absorption method, and the amount of elements can be calculated in the same manner.

[0030] The metallic silicon in the outer peripheral wall 114 and the partition walls 113 of the honeycomb structure 110 can contain a dopant. The dopant in the metallic silicon is one or more kinds selected from Group 13 elements and Group 15 elements of the periodic table. The at least one dopant selected from Group 13 elements and Group 15 elements has a volume ratio of 1×10 to the volume of the metallic silicon. 16 ~5×10 20 pieces / cm 3It is preferable that the dopant is contained in the metal silicon at an average concentration of 1×10. Here, the group 13 element refers to boron (B), aluminum (Al), gallium (Ga), indium (In), etc., and the group 15 element refers to nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc. If the dopant in the metal silicon contained in the honeycomb structure 110 is an element of the same group, it can exhibit conductivity without being affected by counter doping, so it may contain multiple types of elements. It is more preferable that the dopant is one or two types selected from B and Al. It is also preferable that the dopant is one or two types selected from N and P. Each of B, Al, N, and P has a concentration of 1×10 16 ~5×10 20 pieces / cm 3 In this range of concentration, P can be easily contained as a dopant in metallic silicon. Since P has an atomic radius close to that of silicon and is easy to handle in practice, it is particularly preferable to contain P as a dopant.

[0031] The average concentration of at least one dopant selected from Group 13 elements and Group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and the partition wall 113 of the honeycomb structure 110 is 1×10 16 ~5×10 20 pieces / cm 3In this case, it is advantageous in reducing the volume resistivity of the honeycomb structure 110 so that excessive current does not occur even when used for a low voltage of 60V or less, such as 48V. The concentration of the dopant in the metallic silicon in the outer wall 114 and the partition wall 113 of the honeycomb structure 110 can be appropriately adjusted according to the desired volume resistivity of the honeycomb structure 110. In general, when the concentration of the dopant in the metallic silicon is high, the volume resistivity of the honeycomb structure 110 decreases, and when the concentration of the dopant in the metallic silicon is low, the volume resistivity of the honeycomb structure 110 increases. By doping metallic silicon (silicon element) rather than a compound such as silicon carbide particles that functions as an aggregate, the volume resistivity of the honeycomb structure 110 can be effectively reduced. The average concentration of at least one dopant selected from Group 13 elements and Group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and the partition wall 113 of the honeycomb structure 110 is 5×10 17 ~5×10 20 pieces / cm 3 From the viewpoint of easily controlling the volume resistivity, it is more preferable that the average concentration of one kind of dopant selected from the group 13 elements and the group 15 elements of the periodic table in the metallic silicon in the outer wall 114 and the partition walls 113 of the honeycomb structure 110 is 5×10 17 ~5×10 20 pieces / cm 3 and each of the dopants belonging to Group 13 and Group 15 of the periodic table other than the one dopant is preferably 1×10 18 pieces / cm 3 It is preferable that:

[0032] The average concentration of each dopant in the metallic silicon in the peripheral wall 114 and partition walls 113 of the honeycomb structure 110 can be measured by the following method. For the peripheral wall, a total of five peripheral wall samples, each weighing 10 g, are taken from the peripheral wall of the honeycomb structure without bias, and the concentration of the dopant in the metallic silicon for each is measured by the procedure below to obtain an average value. For the partition walls, a total of five partition wall samples, each weighing 10 g, are taken from near the center in the height direction and radial direction of the honeycomb structure, and the concentration of the dopant in the metallic silicon for each is measured by the procedure below to obtain an average value.

[0033] The method for measuring dopants in metal silicon (Si) in the outer wall or partition wall is as follows. According to the silicon separation ICP emission spectroscopy specified in JIS G 1322-3:2010 "Metal silicon analysis method", the outer wall or partition wall sample is decomposed with nitric acid and hydrofluoric acid, perchloric acid is added, and the sample is heated to generate white smoke of perchloric acid, and silicon is volatilized as silicon tetrafluoride and separated, and then the salts are dissolved in water. Next, the amount of each dopant contained in the solution is measured by ICP emission spectroscopy, and the concentration in Si is calculated.

[0034] The metallic silicon contained in the honeycomb structure 110 may contain impurities of Al and Fe. In this case, the content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is preferably 2 mass% or less, respectively, relative to the metallic silicon. When the content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is 2 mass% or less, respectively, relative to the metallic silicon, variation in the shape of the honeycomb structure 110 during manufacture can be effectively suppressed. The content of the impurities Al and Fe in the metallic silicon contained in the honeycomb structure 110 is more preferably 1 mass% or less, and even more preferably 0.1 mass% or less.

[0035] In the embodiment of the present invention, when the metallic silicon contained in the honeycomb structure 110 contains impurities, the impurities are present in a form attached to the metallic silicon. In contrast, in the embodiment of the present invention, when the metallic silicon contained in the honeycomb structure 110 contains a dopant, the dopant is considered to be present in a state dissolved in the metallic silicon particles, but the value measured by the method for measuring the dopant concentration in this specification does not take into account the presence or absence of dopant dissolution.

[0036] Providing the outer peripheral wall 114 on the honeycomb structure portion is useful in terms of ensuring the structural strength of the honeycomb structure portion and suppressing leakage of the fluid flowing through the cells 115 from the outer peripheral wall 114. In this respect, the thickness of the outer peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 114 is made too thick, the strength becomes too high, and the strength balance with the partition walls 113 is lost, resulting in a decrease in thermal shock resistance. Therefore, the thickness of the outer peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Here, the thickness of the outer peripheral wall 114 is defined as the thickness in the normal direction to the tangent of the outer surface of the outer peripheral wall 114 at the measurement point when the portion of the outer peripheral wall 114 to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cells 115. preferable.

[0037] The thickness of the partition walls 113 that define the cells 115 is preferably 0.1 to 0.3 mm, and more preferably 0.1 to 0.2 mm. When the thickness of the partition walls 113 is 0.1 mm or more, it is possible to suppress a decrease in the strength of the honeycomb structure section. When the thickness of the partition walls 113 is 0.3 mm or less, it is possible to suppress an increase in pressure loss when exhaust gas is passed through the honeycomb structure section when the honeycomb structure section is used as a catalyst carrier to support a catalyst. In the present invention, the thickness of the partition walls 113 is defined as the length of a portion that passes through the partition walls 113, of a line segment that connects the centers of gravity of adjacent cells 115 in a cross section perpendicular to the extension direction of the cells 115.

[0038] The partition walls 113 may be dense, such as in the form of Si-impregnated SiC, but are preferably porous. The porosity of the partition walls 113 is preferably 35 to 60%, and more preferably 35 to 45%. If the porosity is 35% or more, the heat generation rate of the EHC can be increased. If the porosity is 60% or less, the strength of the honeycomb structure portion is sufficiently maintained. The porosity is a value measured by a mercury porosimeter. Note that dense refers to a porosity of 5% or less.

[0039] The honeycomb structure has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the extension direction of the cells 115. 2 Preferably, the cell density is 70 to 100 cells / cm. 2 By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while reducing the pressure loss when exhaust gas flows through the honeycomb structure. 2 If the cell density is 150 cells / cm or more, the catalyst carrying area is sufficiently secured. 2 When the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, the pressure loss caused by the exhaust gas flowing therethrough is prevented from becoming too large if the honeycomb structure 110 is used as a catalyst carrier to support a catalyst, and the cell density is a value obtained by dividing the number of cells by the area of ​​one end face of the honeycomb structure part on the inner peripheral side than the outer peripheral wall 114.

[0040] Although there is no limitation on the shape of the cells in a cross section perpendicular to the extension direction of the cells 115, a rectangle, a hexagon, an octagon, or a combination of these is preferable. Among these, a rectangle and a hexagon are preferable. By using such a cell shape, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is excellent. From the viewpoint of easily achieving both structural strength and heating uniformity, a hexagon is particularly preferable.

[0041] The cells 115 may penetrate from the first end face 116 to the second end face 118. In this case, the cells 115 may be open at both the first end face 116 and the second end face 118. Alternatively, a first cell having a plugged first end face 116 and an opening at the second end face 118 and a second cell having an opening at the first end face 116 and a plugged second end face 118 may be alternately arranged adjacent to each other with the partition wall 113 in between.

[0042] <Electrode layer> A first electrode layer 112a and a second electrode layer 112b facing the first electrode layer 112a across the central axis O of the honeycomb structure part can be provided on the outer surface of the outer peripheral wall 114. By disposing the electrode layers 112a and 112b having a lower volume resistivity than the outer peripheral wall 114, the current spreads easily in the circumferential direction of the honeycomb structure 110 and in the extending direction of the cells 115, so that the uniform heat generation of the honeycomb structure 110 can be improved. Referring to FIG. 1, in a cross section perpendicular to the extending direction of the cells 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential centers of the pair of electrode layers 112a and 112b to the central axis O (center of gravity) of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0043] Although there is no particular restriction on the formation region of the pair of electrode layers 112a, 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the pair of electrode layers 112a, 112b are each provided in a band shape extending in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 on the outer surface of the outer peripheral wall 114. Specifically, in a cross section perpendicular to the extension direction of the cells 115, the central angle α formed by two line segments connecting both side ends in the circumferential direction of each electrode layer 112a, 112b and the central axis O (center of gravity) is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation (see FIG. 1). However, if the central angle α is too large, the current passing through the inside of the honeycomb structure 110 decreases, and the current passing through the vicinity of the outer peripheral wall 114 increases. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Moreover, it is desirable that each of the electrode layers 112a and 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a and 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are laminated.

[0044] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. By setting the thickness in this range, the uniform heat generation can be improved. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, and the heat can be generated more uniformly. When the thickness of the electrode layers 112a, 112b is 5 mm or less, the risk of breakage during canning is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the normal direction to the tangent of the outer surface of the electrode layers 112a, 112b at the measurement point when the part of the electrode layers 112a, 112b to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cell 115.

[0045] By making the volume resistivity of the electrode layers 112a, 112b lower than that of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and electricity spreads easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115 when electricity is applied. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference in volume resistivity between the two becomes too large, current concentrates between the ends of the opposing electrode layers 112a, 112b, causing uneven heat generation in the honeycomb structure 110, and therefore the volume resistivity of the electrode layers 112a, 112b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the volume resistivity of the partition walls 113 and the outer peripheral wall 114. As described above, in this specification, the volume resistivities of the electrode layers, partition walls, and outer peripheral wall are values ​​measured at 25°C by the four-terminal method.

[0046] The material of the electrode layers 112a and 112b is not limited, but a composite material (cermet) of metal and ceramic (particularly conductive ceramic) can be used. Examples of metals include, for example, a single metal such as Cr, Fe, Co, Ni, Si, or Ti, or an alloy containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). Specific examples of composite materials (cermets) of metal and ceramics include composite materials of metal silicon and silicon carbide, composite materials of metal silicides such as tantalum silicide and chromium silicide, and composite materials in which one or more insulating ceramics such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride are added to one or more of the above metals from the viewpoint of reducing thermal expansion. As the material for the electrode layers 112a, 112b, among the various metals and ceramics mentioned above, a composite material of a metal silicide such as tantalum silicide or chromium silicide, metal silicon, and silicon carbide is preferable because it can be fired simultaneously with the partition wall and the outer peripheral wall, which contributes to simplifying the manufacturing process.

[0047] (1-2. Metal terminal) The metal terminal 130 can be directly or indirectly joined to the outer surfaces of the pair of electrode layers 112a, 112b. When a voltage is applied to the honeycomb structure 110 via the metal terminal 130, electricity is passed through the honeycomb structure 110, and the honeycomb structure 110 can generate heat by Joule heat. For this reason, the honeycomb structure 110 can also be suitably used as a heater. This makes it possible to improve the uniform heat generation of the honeycomb structure 110. The voltage to be applied is preferably 12 to 900 V, more preferably 48 to 600 V, but the voltage to be applied can be changed as appropriate.

[0048] The metal terminal 130 and the electrode layers 112a, 112b may be directly bonded to each other, or may be bonded to each other via one or more base layers 120 in order to reduce the thermal expansion difference between the electrode layers 112a, 112b and the metal terminal 130 and improve the bonding reliability of the metal terminal 130. Therefore, in a preferred embodiment, the honeycomb structure 110 has a first electrode layer 112a and a second electrode layer 112b disposed on the outer peripheral wall 114 so as to face each other across the central axis O (center of gravity) of the honeycomb structure 110, and one or more metal terminals 130 are bonded to each of the electrode layers 112a, 112b via the base layers 120.

[0049] From the viewpoint of improving the bonding reliability, it is preferable that the thermal expansion coefficient gradually decreases in the order of metal terminal 130 → (underlying layer 120) → electrode layers 112a, 112b → outer peripheral wall 114. Note that the "thermal expansion coefficient" here means the linear expansion coefficient measured according to JIS R1618:2002 when the temperature is changed from 25°C to 800°C.

[0050] The material of the metal terminal 130 is not particularly limited as long as it is a metal, and a single metal or an alloy can be adopted, but from the viewpoint of corrosion resistance, volume resistivity, and linear expansion coefficient, for example, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. The number, shape, and size of the metal terminal 130 are not particularly limited, and can be appropriately designed depending on the size and current-carrying performance of the honeycomb structure 110.

[0051] The material of the underlayer 120 is not limited, but may be a composite material (cermet) of metal and ceramics (particularly conductive ceramics). The thermal expansion coefficient of the underlayer 120 can be controlled by adjusting the compounding ratio of the metal and ceramics, for example.

[0052] The underlayer 120 preferably contains, but is not limited to, one or more metals selected from a Ni-based alloy, an Fe-based alloy, a Ti-based alloy, a Co-based alloy, metallic silicon, and Cr.

[0053] The underlayer 120 preferably contains one or more ceramics selected from oxide ceramics such as alumina, mullite, zirconia, glass, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride, although this is not limited thereto.

[0054] The thickness of the underlayer 120 is not particularly limited, but is preferably 0.1 to 1.5 mm, and more preferably 0.3 to 0.5 mm, from the viewpoint of crack suppression. The thickness of the underlayer 120 is defined as the thickness in the normal direction to the tangent of the outer surface of the underlayer 120 at the measurement point when the underlayer 120 whose thickness is to be measured is observed in a cross section perpendicular to the cell extension direction.

[0055] The method for joining the metal terminal 130 to the electrode layers 112a, 112b or the underlayer 120 is not particularly limited, but examples thereof include thermal spraying, welding, and brazing.

[0056] (2. Manufacturing method) Next, a method for manufacturing a honeycomb structure according to one embodiment of the present invention will be described. The honeycomb structure can be manufactured by a manufacturing method including step 1 of preparing a clay, step 2 of forming the clay to obtain a honeycomb molded body, step 3 of applying a pair of electrode layer forming pastes to the outer surface of the outer peripheral wall so as to extend in a band shape in the cell extension direction across the central axis of the honeycomb molded body, thereby preparing a honeycomb molded body with electrode layer forming paste, and step 4 of firing the honeycomb molded body to prepare a honeycomb fired body. If the electrode layer is not required, step 3 may be omitted.

[0057] (Process 1) In step 1, a forming raw material containing silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source is kneaded to prepare a clay. The dopant source may be any substance containing an element that becomes a dopant, and may include an element and a compound. However, since an element has a low solubility in water, it is preferable to provide it as a compound. The suitable types of dopants are as described above. By providing the dopant source in the form of an aqueous solution, when the dopant source is kneaded with the silicon carbide powder and the metal silicon powder, the dopant source is dispersed with high uniformity in the silicon carbide powder and the metal silicon powder. The dopant in the dopant source is mainly dissolved in the metal silicon, but a part of the dopant may be dissolved in the silicon carbide.

[0058] In step 1, the forming raw materials are kneaded to prepare a clay. Any appropriate device or mechanism can be used as the kneading means. Specific examples include a kneader and a vacuum clay kneader.

[0059] By adjusting the number of dopant atoms in the aqueous solution, the concentration of the dopant in the metal silicon in the outer wall and partition walls of the honeycomb structure can be controlled. From the viewpoint of increasing the adjustment range of the number of dopant atoms, the dopant source is preferably provided as a water-soluble compound containing a dopant. In this case, the solubility of the water-soluble compound containing a dopant in water at 20°C is preferably 1g / 100gH2O or more, more preferably 5g / 100gH2O or more, and even more preferably 10g / 100gH2O or more. Although there is no particular upper limit set for the solubility, from the viewpoint of availability, it is generally 50g / 100gH2O or less, typically 30g / 100gH2O or less. Therefore, the solubility of the water-soluble compound containing a dopant in water at 20°C is, for example, preferably 1 to 50g / 100gH2O, more preferably 5 to 30g / 100gH2O. In this specification, the solubility of a water-soluble compound containing a dopant in water at 20°C is measured by adding various concentrations of the water-soluble compound to 100 mL of water (20°C) stored in a measuring flask, stirring (rotation speed: 500 rpm, 20 minutes), and repeatedly checking for the presence or absence of undissolved solids to determine the concentration of the water-soluble compound in a saturated solution.

[0060] The amount of the aqueous solution of the dopant source may be appropriately set depending on the dopant concentration in the target forming raw material or honeycomb structure. For example, the number of at least one dopant atom in the aqueous solution of the dopant source is 1×10 16 ~5×10 20 pieces / cm 3 It is preferable to set it to 5×10 17 ~5×10 20 pieces / cm 3 It is more preferable that the volume of the metallic silicon is determined by calculating the density of the metallic silicon (2.3290 g / cm) from the mass of the metallic silicon powder. 3 For example, when P is the dopant, if the dopant concentration in the forming raw material or honeycomb structure is 1×1016 pieces / cm 3 is the target, the number of dopant atoms in the aqueous solution of the dopant source can be set according to the following formula: It is possible to incorporate substantially all of the dopant in the aqueous solution into the metallic silicon. (a) Calculation of the number of dopants (number of P atoms) to be added 1×10 16 pieces / cm 3 × volume of metallic silicon V (cm 3 )=V×10 16 (pieces) (b) Calculation of the mass of dopant to be added (P mass) V×10 16 pieces ÷ 6.02×10 23 / mol(Avogadro's constant) × 30.97g / mol(P atomic weight) = 5.14 × 10 -7 ×V(g)

[0061] As the water-soluble compound containing a dopant, one or more compounds selected from inorganic salts and organic compounds can be suitably used. When the dopant is P, examples of water-soluble inorganic salts containing P include tetraphosphorus decaoxide, phosphoric acid, ammonium phosphate, etc. Examples of water-soluble organic compounds containing P include phosphine oxides, phosphine alkenes, phosphine alkynes, phosphonic acid esters, phosphoric acid esters, as well as organic phosphates such as phosphonic acid ester salts and phosphoric acid ester salts. When the dopant is N, examples of water-soluble inorganic salts containing N include dinitrogen pentoxide, aqueous ammonia, and nitric acid. When the dopant is B, examples of the water-soluble inorganic salt containing B include boric acid, etc. Examples of the water-soluble organic compound containing B include methylboronic acid, boronic acid esters, etc. When the dopant is Al, examples of the water-soluble inorganic salt containing Al include aluminum chloride, aluminum sulfate, and aluminum nitrate.

[0062] The mass of the metal silicon powder in the forming raw material is preferably 20 to 80 parts by mass, more preferably 25 to 60 parts by mass, and even more preferably 25 to 45 parts by mass, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass. The average particle size of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle size of the metal silicon particles in the metal silicon powder is preferably 2 to 35 μm, more preferably 2 to 25 μm. The average particle size of the silicon carbide particles and the metal silicon particles refers to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by a laser diffraction method. The silicon carbide particles are fine particles of silicon carbide that constitute the silicon carbide powder, and the metal silicon particles are fine particles of metal silicon that constitute the metal silicon powder.

[0063] The forming raw material may be added with water from other than the aqueous solution of the dopant source, but the total content of water in the forming raw material (including water in the aqueous solution of the dopant source and other water if present) is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass, for the reason of uniformly dispersing the dopant source. In addition, the total content of water in the forming raw material (including water in the aqueous solution of the dopant source and other water if present) is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass, for the reason of maintaining the shape of the honeycomb structure. Therefore, the total content of water in the forming raw material (including water in the aqueous solution of the dopant source and other water if present) is, for example, preferably 20 to 60 parts by mass, more preferably 25 to 50 parts by mass, when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass.

[0064] The forming raw material may contain a binder, a surfactant, and a pore former in addition to the silicon carbide powder, the silicon metal powder, and the aqueous solution of the dopant source.

[0065] Examples of the binder include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0066] The surfactant may be ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0067] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metal silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0068] (Process 2) In step 2, the clay produced in step 1 is molded to obtain a honeycomb molded body. Specifically, the clay is extrusion molded to produce a columnar honeycomb molded body having an outer peripheral wall and partition walls. A die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used during extrusion molding. Next, it is preferable to dry the obtained honeycomb molded body. If the length of the honeycomb molded body in the central axis direction is not the desired length, both ends of the honeycomb molded body can be cut to obtain the desired length. The honeycomb molded body after drying is called a dried honeycomb body.

[0069] The honeycomb formed body may be fired once as a modified example of step 1. That is, in this modified example, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 3 is then carried out on the honeycomb fired body.

[0070] (Step 3) Step 3 is a step of applying a pair of electrode layer forming pastes to the outer surface of the outer peripheral wall of the honeycomb molded body so as to extend in a band shape in the extending direction of the cells across the central axis of the honeycomb molded body, thereby producing a honeycomb molded body with the electrode layer forming paste. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, etc.) mixed according to the required characteristics of the electrode layer, and kneading them. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powders refers to the arithmetic mean diameter based on volume when the frequency distribution of particle size is measured by a laser diffraction method.

[0071] Next, the obtained electrode layer forming paste is applied to required locations on the outer surface of the outer peripheral wall of a honeycomb formed body (typically a dried honeycomb body) to obtain a honeycomb formed body with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with a known method for manufacturing a honeycomb structure, but in order to give the electrode layer a lower volume resistivity than the outer peripheral wall and the partition walls, the metal content can be made higher than that of the outer peripheral wall and the partition walls, or the particle size of the metal particles in the raw material powder can be made smaller. After application, it is preferable to dry the electrode layer forming paste.

[0072] (Step 4) Step 4 is a step of firing the honeycomb molded body with the electrode layers to obtain a honeycomb fired body, i.e., the desired honeycomb structure. Before firing, degreasing may be performed to remove binders and the like. The method of degreasing and firing is not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. The firing conditions vary depending on the material of the honeycomb structure, but are preferably heated at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0073] By joining a metal terminal to the electrode layer of the honeycomb structure thus obtained, an electrically heated carrier can be manufactured. The joining method is not particularly limited, and examples thereof include thermal spraying, welding, and brazing. In order to improve the joining property between the electrode layer and the metal terminal, a base layer may be formed by a method such as thermal spraying.

[0074] An appropriate catalyst may be supported on the electrically heated carrier depending on the application. An example of a method for supporting a catalyst on a honeycomb structure is a method in which a catalyst slurry is introduced into cells by a conventionally known suction method or the like, and is attached to the surfaces and pores of the partition walls, and then a high-temperature treatment is performed to bake the catalyst contained in the catalyst slurry onto the partition walls and support the catalyst. EXAMPLES

[0075] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0076] <Test No. 1> (1. Making cylindrical clay pots) 30 g of the phosphate salt was added to 30 kg of pure water and stirred for 20 minutes to obtain an aqueous solution of the dopant source. The solubility of the phosphate salt in water at 20°C was measured by the above-mentioned method and found to be 8.4 g / 100 gH2O. In addition, silicon carbide (SiC) powder and metal silicon (Si) powder were mixed in a mass ratio of 75:25 to prepare a ceramic raw material. Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore former, and an aqueous solution of the dopant source were added to the ceramic raw material to prepare a molding raw material. Next, the molding raw material was kneaded in a vacuum kneader to prepare a cylindrical clay body.

[0077] In the forming raw material, the binder content was 8 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. The pore former content was 3 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. The dopant source aqueous solution content was 30 parts by mass when the total of silicon carbide (SiC) powder and metal silicon (Si) powder was 100 parts by mass. As a result, the atomic concentration of P, which is a dopant, in the forming raw material was 100 parts by mass of metal silicon (1 cm 3 ) for 2.9 × 10 18 pieces / cm 3 The average particle size of the silicon carbide powder was 20 μm, and the average particle size of the metal silicon powder was 6 μm. The average particle size of the pore-forming material was 20 μm. The average particle sizes of the silicon carbide powder, metal silicon powder, and pore-forming material refer to the arithmetic mean diameters based on volume when the particle size frequency distribution is measured by a laser diffraction method.

[0078] (2. Preparation of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine with a specified die structure to obtain a cylindrical honeycomb molded body in which each cell shape in a cross section perpendicular to the cell extension direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried in an air atmosphere at 120°C for 2 hours using a hot air dryer, and both end faces were cut by a specified amount to produce a dried honeycomb body.

[0079] (3. Firing) The obtained honeycomb dried body was degreased in an air atmosphere at 550°C for 3 hours. Next, the degreased honeycomb dried body was fired in an Ar atmosphere at 1450°C for 0.5 hours. Finally, the honeycomb structure was heat-treated in a water vapor atmosphere at 950°C for 50 hours to obtain a cylindrical honeycomb structure. The honeycomb structures were manufactured in the number required for the following tests.

[0080] (4. Specifications of honeycomb structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 0.125 mm, an outer peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm. 2 The porosity of the partition walls was 38%.

[0081] (5. Metallic silicon content) For the honeycomb structure obtained above, the metallic silicon contents in the partition walls and the outer peripheral wall were measured according to the above-mentioned method, and both were 30% by weight.

[0082] (6. Concentration of dopant in metallic silicon) A total of five partition wall samples, each weighing 10 g, were taken from near the center in the height direction and radial direction of the honeycomb structure obtained above, and the concentration of dopant (P) in the metallic silicon for each was measured in accordance with the method described above, and the average value was calculated. In addition, a total of five peripheral wall samples, each weighing 10 g, were taken from the peripheral wall of the honeycomb structure obtained above without bias, and the concentration of dopant (P) in the metallic silicon for each was measured in accordance with the method described above, and the average value was calculated. The ICP (inductively coupled plasma) analyzer used was a model PS3510DD manufactured by Hitachi High-Tech Corporation. As a result, both were 2.8 x 10 18 pieces / cm 3 It was.

[0083] (7. Measurement of dopant concentration distribution in metallic silicon) The standard deviation was calculated based on the dopant (P) concentration in the metallic silicon of the five partition wall samples for which the average dopant (P) concentration was calculated. The standard deviation was 7.0 x 10 16 pieces / cm 3 (σ=2.5% of the average value).

[0084] (8. Volume resistivity measurement) A total of five partition wall samples, each measuring 5 mm x 5 mm x 50 mm (length in the cell extension direction), were taken from the honeycomb structure obtained above, and the volume resistivity of each was measured at 25°C using the four-terminal method. The partition wall samples were taken near the center of the honeycomb structure. The average value was 61 Ω cm, with a standard deviation of 1.9 Ω cm (σ=3.1% of the average value).

[0085] <Test No. 2 (Comparative Example)> (1. Making cylindrical clay pots) A ceramic raw material was prepared by mixing silicon carbide (SiC) powder and P-doped silicon metal (Si) powder in a mass ratio of 65:35. The P-doped silicon metal (Si) powder was prepared by melting Si in a melting furnace, then adding phosphate rock (3Ca3(PO4)2·CaF2) to the melting furnace to dope with P. With this method, the concentration of the dopant P was adjusted to 100% by mass of silicon metal (1 cm3 ) for 3.0×10 18 pieces / cm 3 was adjusted to. Hydroxypropylmethylcellulose as a binder, a water-absorbent resin as a pore former, and pure water were added to the ceramic raw material to prepare a molding raw material. The molding raw material was then kneaded in a vacuum kneader to prepare a cylindrical clay body.

[0086] In the molding raw material, the content of the binder was 7 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. The content of the pore former was 3 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. The content of the pure water was 30 parts by mass when the total of the silicon carbide (SiC) powder and the metal silicon (Si) powder was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm, and the average particle diameter of the metal silicon powder was 6 μm. The average particle diameter of the pore former was 20 μm. The average particle diameters of the silicon carbide powder, the metal silicon powder, and the pore former refer to the arithmetic mean diameter based on the volume when the frequency distribution of the particle size is measured by the laser diffraction method.

[0087] (2. Preparation of honeycomb structure) Using the obtained cylindrical clay, honeycomb structures were obtained in the same manner as in Test No. 1 in the number required for the following tests.

[0088] (3. Specifications of honeycomb structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 125 mm, an outer peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm. 2 The porosity of the partition walls was 38%.

[0089] (4. Metallic silicon content) For the honeycomb structure obtained above, the metallic silicon contents in the partition walls and the outer peripheral wall were measured according to the above-mentioned method, and both were 30% by weight.

[0090] (5. Concentration of dopant in metallic silicon) For the honeycomb structure obtained above, the average concentration of the dopant (P) in the metallic silicon in the partition walls and the outer peripheral wall was measured according to the above-mentioned method. 18 pieces / cm 3 It was.

[0091] (6. Measurement of dopant concentration distribution in metallic silicon) As in Test No. 1, the standard deviation was calculated based on the concentration of dopant (P) in the metallic silicon of the five partition wall samples for which the average concentration of dopant (P) was calculated. The standard deviation was 3.5×10 17 pieces / cm 3 (σ=14% of the average value).

[0092] (7. Volume resistivity measurement) As in Test No. 1, a total of five partition wall samples were taken from near the center of the honeycomb structure, and the volume resistivity was measured at 25°C by the four-probe method. As a result, the average value was 74 Ω cm, and the standard deviation was 11 Ω cm (σ=15% of the average value). [Explanation of symbols]

[0093] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112b: Second electrode layer 113: Bulkhead 114:Outer wall 115: Cell 116: First end surface 118: Second end face 120: Base layer 130: Metal terminal

Claims

1. A step of kneading a forming raw material including silicon carbide powder, metal silicon powder, and an aqueous solution of a dopant source to prepare a puddle; forming a honeycomb formed body having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths from a first end surface to a second end surface; A step of firing the honeycomb formed body to produce a honeycomb fired body; Including, The dopant source contains one or more dopants selected from Group 13 elements and Group 15 elements of the periodic table, and the number of atoms of at least one of the dopants in the aqueous solution of the dopant source is 1×10 in terms of the number of atoms of the dopant relative to the volume of the metallic silicon. 16 ~5×10 20 pieces / cm 3 That is, A method for manufacturing a honeycomb structure.

2. The method according to claim 1 , wherein the dopant source comprises one or more selected from an inorganic salt containing the dopant and an organic compound containing the dopant.

3. The method for manufacturing a honeycomb structure according to claim 1 or 2, wherein the dopant source contains P.

4. 3. The method according to claim 1, wherein the dopant source comprises one or more selected from the group consisting of an inorganic salt containing P and an organic compound containing P.

5. 3. The method of claim 1, wherein the dopant source comprises an organic phosphate.

6. The dopant source includes a compound containing the dopant, and the compound has a solubility in water at 20° C. of 1 g / 100 gH 2 The method according to claim 1 or 2, wherein the molecular weight is O or more.

7. 3. The method according to claim 1, wherein the partition walls of the honeycomb structure have a metallic silicon content of 20 mass % or more.

8. The average concentration of at least one of the dopants in the metallic silicon in the partition walls of the honeycomb structure is 1×10 16 ~5×10 20 pieces / cm 3 The method according to claim 1 or 2, wherein

9. 3. A method for manufacturing a honeycomb structure as described in claim 1 or 2, further comprising a step of applying a pair of electrode layer forming pastes to the outer surface of the outer wall so as to extend in a band-like shape in the cell extension direction, sandwiching the central axis of the honeycomb formed body, before firing the honeycomb formed body, thereby producing a honeycomb formed body with electrode layer forming paste.

Citation Information

Patent Citations

  • Method for producing conductive ceramic sintered compact

    JP2012214306A

  • Honeycomb structure, electric heating-type honeycomb structure, electric heating-type carrier and exhaust emission control device

    JP2020204300A

  • Honey-comb structure and electric heating carrier

    JP2022142543A

  • Honeycomb structure, and electric heating support and exhaust gas treatment device each using the honeycomb structure

    JP2022148668A

  • Honeycomb structure

    JP5735428B2