Ultraviolet curable resin composition for nanoimprint and optical sheet
A UV curable resin composition with a polymerizable component and ultraviolet absorber forms a durable moth-eye structure on optically functional sheets, addressing high reflectance issues and improving their functionality on transparent substrates.
Patent Information
- Application Number
- JP2023056786
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing optically functional sheets exhibit high reflectance on their surfaces, which hinders the desired functionality from being fully demonstrated on transparent substrates such as lenses and windshields, necessitating a solution that reduces reflectance while maintaining durability.
A UV curable resin composition for nanoimprinting is developed, containing a polymerizable component, a polymerization initiator, and an ultraviolet absorber, which forms a coating layer with a fine uneven structure like a moth-eye structure on the substrate, using a manufacturing apparatus to ensure excellent durability.
The UV curable resin composition effectively reduces surface reflectance of optically functional sheets, enhancing their durability and functionality on transparent substrates like lenses and windshields.
Smart Images

Figure 2024143870000006 
Figure 2024143870000007 
Figure 2024143870000008
Abstract
Description
[Technical field]
[0001] The present invention relates to an ultraviolet-curable resin composition for nanoimprinting and an optical sheet. [Background technology]
[0002] In recent years, in order to impart the desired functionality to lenses in eyewear such as spectacles and sunglasses, cover members arranged to cover the windows of storage bodies in head-up display devices used in automobiles, and transparent substrates such as windshields in vehicles such as motorcycles, it has been proposed to affix an optically functional sheet having such functionality to the surface of these items, or to construct these items directly from this optically functional sheet (see, for example, Patent Document 1).
[0003] In this way, by providing transparent substrates such as lenses, cover members, and windshields with optically functional sheets, it is possible to impart the functionality of the optically functional sheets to these transparent substrates.
[0004] However, if the reflectance of the incident light on the surface of this optical functional sheet is too high, a problem occurs in that the functionality to be imparted to the transparent substrate by the attachment of the optical functional sheet cannot be fully exerted. Therefore, it is required that the reflectance of the incident light on the surface of the optical functional sheet can be reduced with excellent durability.
[0005] In addition, such demands are not limited to cases where the optical functional sheet is applied to lenses, head-up display devices, and windshields, but also arise when the optical functional sheet is attached to, for example, display parts of image display devices such as liquid crystal display devices and organic EL display devices, headlights, solar cells, digital signage, light-transmitting parts (window parts) of vehicles such as automobiles, trains, and airplanes, light-transmitting parts (protective glass) such as lenses and windows of touch panels of cash dispensers, ATMs, smartphones, tablet computers, etc., outdoor surveillance cameras (security cameras), motion sensors, etc., window glass of buildings such as houses and buildings, window members such as protective glass, etc.
[0006] In order to satisfy such requirements, for example, it is conceivable to form a coating layer having a moth-eye structure on the surface of a substrate constituting the outer surface of the optical functional sheet, on the surface opposite to the substrate. That is, it is conceivable to form the substrate constituting the outer surface of the optical functional sheet with an optical sheet having a transparent base material and a coating layer having a moth-eye structure on the surface opposite to the base material. Then, it is conceivable to form the coating layer having the moth-eye structure on the base material in this optical sheet by nanoimprinting using a curable resin composition.
[0007] Therefore, if a coating layer having a moth-eye structure can be formed on a substrate with excellent durability using a curable resin composition, it is considered that the requirement that the reflectance of incident light on the surface of an optical functional sheet must be reduced with excellent durability can be satisfied. Therefore, the reality is that there is a demand for the development of a curable resin composition that can form a coating layer having a moth-eye structure on a substrate with excellent durability by nanoimprinting.
[0008] Furthermore, the formation of a coating layer on a substrate by nanoimprinting using such a curable resin composition is not limited to the case of forming a layer having a moth-eye structure on the surface, but is also required to form a layer having excellent durability even in the case of forming a layer having various fine uneven structures such as a wire grid structure, a moth-eye structure, a lotus leaf structure, a honeycomb structure, or a fructal structure. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2009-294445 A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide an ultraviolet-curable resin composition for nanoimprinting which, when used to form by nanoimprinting a coating layer of an optical sheet provided on the surface of a functional optically functional sheet, can form a coating layer having a fine uneven structure on its surface, the coating layer having excellent durability, and an optical sheet having a coating layer having a fine uneven structure on its surface, which is formed using the ultraviolet-curable resin composition for nanoimprinting. [Means for solving the problem]
[0011] Such an object can be achieved by the present invention described in (1) to (9) below. (1) A UV-curable resin composition for nanoimprints, comprising a polymerizable component, a polymerization initiator, and a UV absorber, The ultraviolet absorber has a light absorption peak having a maximum absorptivity peak in a wavelength range of 300 nm or more and 350 nm or less in a light absorption spectrum, The ultraviolet-curable resin composition for nanoimprints, wherein the polymerization initiator has a light absorption peak having a maximum absorptivity within a wavelength range of more than 350 nm and not more than 400 nm in a light absorption spectrum.
[0012] (2) the polymerizable component comprises a radically polymerizable group; The ultraviolet-curable resin composition for nanoimprints according to the above (1), wherein the polymerization initiator is a radical polymerization initiator.
[0013] (3) The ultraviolet-curable resin composition for nanoimprints according to the above (2), wherein the ultraviolet absorber has the radical polymerizable group.
[0014] (4) The ultraviolet-curable resin composition for nanoimprints according to any one of (1) to (3) above, wherein the content of the polymerization initiator is from 1.0% by weight to 8.0% by weight.
[0015] (5) The ultraviolet-curable resin composition for nanoimprints according to any one of (1) to (4) above, wherein the content of the ultraviolet absorbent is from 2.0% by weight to 5.0% by weight.
[0016] (6) The ultraviolet-curable resin composition for nanoimprints according to any one of (1) to (5) above, wherein the polymerizable component contains one having a polymerizable group and an aliphatic chain having 6 to 10 carbon atoms in its skeleton.
[0017] (7) The ultraviolet-curable resin composition for nanoimprints according to any one of (1) to (6) above, wherein the polymerizable component contains one having a polymerizable group and a fluorinated hydrocarbon group in its skeleton.
[0018] (8) The ultraviolet-curable resin composition for nanoimprinting according to any one of (1) to (7) above, which is used for forming, on a substrate containing a resin material as a main material and the ultraviolet absorber, a coating layer having a fine uneven structure provided by nanoimprinting on a surface opposite to the substrate.
[0019] (9) An optical sheet comprising: a substrate; and a coating layer having a fine uneven structure formed on a surface opposite to the substrate by nanoimprinting using the ultraviolet-curable resin composition for nanoimprinting described in any one of (1) to (8) above. Effect of the Invention
[0020] According to the present invention, in an ultraviolet-curable resin composition for nanoimprinting that contains a polymerizable component, a polymerization initiator, and an ultraviolet absorber, the ultraviolet absorber has a light absorption peak having a maximum absorptivity in a wavelength range of 300 nm or more and 350 nm or less in its light absorption spectrum, and the polymerization initiator has a light absorption peak having a maximum absorptivity in a wavelength range of more than 350 nm and 400 nm or less in its light absorption spectrum. Therefore, by using this ultraviolet-curable resin composition for nanoimprinting to form a coating layer having a fine uneven structure on the surface opposite to the substrate by nanoimprinting, a coating layer having a fine uneven structure on the surface composed of a cured product of this ultraviolet-curable resin composition for nanoimprinting and having excellent durability can be formed. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a perspective view showing an embodiment of sunglasses equipped with an optically functional sheet having an optical sheet of the present invention. [Diagram 2] FIG. 2 is a side view of a manufacturing apparatus for manufacturing the optical sheet of the present invention. [Diagram 3] FIG. 1 is a longitudinal sectional view showing a first embodiment of an optical functional sheet having an optical sheet of the present invention. [Figure 4] FIG. 4 is an enlarged vertical cross-sectional view of an area [A] surrounded by a dashed line in FIG. [Diagram 5] FIG. 2 is a longitudinal sectional view showing a second embodiment of an optical functional sheet having an optical sheet of the present invention. [Figure 6] FIG. 1 is a side view showing an embodiment in which an optically functional sheet having an optical sheet of the present invention is applied to a cover member constituting a head-up display of an automobile. [Figure 7] FIG. 7 is an enlarged vertical cross-sectional view of the area [B] surrounded by the dashed line in FIG. 6. [Figure 8] 7 is a schematic diagram showing laser light passing through a cover member constituting the head-up display shown in FIG. 6. [Figure 9] FIG. 1 is a diagram showing an embodiment in which an optically functional sheet having an optical sheet of the present invention is applied to a windshield plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The ultraviolet-curable resin composition for nanoimprints and the optical sheet of the present invention will be described in detail below with reference to preferred embodiments shown in the accompanying drawings.
[0023] The ultraviolet-curable resin composition for nanoimprints of the present invention comprises a polymerizable component, a polymerization initiator, and an ultraviolet absorber. The ultraviolet absorber has a light absorption peak having a maximum absorptance peak in a wavelength range of 300 nm or more and 350 nm or less in its light absorption spectrum, and the polymerization initiator has a light absorption peak having a maximum absorptance peak in a wavelength range of more than 350 nm and 400 nm or less in its light absorption spectrum.
[0024] Therefore, by using this ultraviolet-curable resin composition for nanoimprinting to form a coating layer having a fine uneven structure on the surface opposite to the substrate by nanoimprinting, a coating layer having a fine uneven structure on the surface composed of a cured product of this ultraviolet-curable resin composition for nanoimprinting can be formed that has excellent durability. In other words, an optical sheet (optical sheet of the present invention) comprising a substrate and a coating layer having such a configuration can be made to exhibit excellent durability.
[0025] Therefore, by using this ultraviolet-curable resin composition for nanoimprinting to form a coating layer having a moth-eye structure as a fine uneven structure on a substrate by nanoimprinting, in other words, by forming an antireflection layer having a moth-eye structure as a coating layer on a substrate, the optical sheet can have a reduced reflectance of incident light on its surface with excellent durability.
[0026] The optical sheet (optical sheet of the present invention) having the anti-reflection layer having the moth-eye structure as described above on the substrate as a covering layer is used as a transparent sheet (transparent substrate) covering the surface (front side) of an optical functional sheet (functional substrate) having functionality. Specifically, it is provided to cover the front side of an optical functional sheet (functional substrate) of a lens of eyewear, a cover member provided to cover a window part of a housing of a head-up display, and further a windshield plate of a vehicle, etc., and thus the optical functional sheet of the optical sheet can have a reflectance of incident light on its surface reduced with excellent durability.
[0027] Therefore, before describing the ultraviolet-curable resin composition for nanoimprints and the optical sheet of the present invention, the following description will first describe a case where an optical functional sheet (the optical sheet of the present invention) having an antireflection layer with a moth-eye structure as a coating layer on a substrate is used for the lenses described above, and the lens is applied to sunglasses, which is a type of eyewear.
[0028] <Sunglasses> Fig. 1 is a perspective view showing an embodiment of sunglasses equipped with an optical functional sheet having the optical sheet of the present invention. In Fig. 1, when the sunglasses are worn on the head of a user, the surface of the lens facing the user's eyes is called the back surface, and the opposite surface is called the front surface.
[0029] As shown in FIG. 1, the sunglasses 100 include a frame 20 and a lens 30 (a lens for glasses).
[0030] In this specification, the term "lens (spectacle lens)" includes both lenses having a light-collecting function and lenses having no light-collecting function.
[0031] The frame 20 is fitted to the head of a user so as to position the lenses 30 adjacent to and in front of the user's eyes.
[0032] The frame 20 has a rim portion 21, a bridge portion 22, a temple portion 23, and a nose pad portion 24.
[0033] The rim portions 21 are ring-shaped, one for each of the right and left eyes, and have lenses 30 attached to their insides. This allows the user to view external information through the lenses 30.
[0034] Furthermore, the bridge portion 22 is rod-shaped and is positioned in front of the upper part of the user's nose when the glasses are worn on the user's head, connecting the pair of rim portions 21 together.
[0035] The temple portion 23 is shaped like a temple and is connected to the edge of each rim portion 21 on the opposite side to the position where the bridge portion 22 is connected. The temple portion 23 is hung on the user's ear when the glasses are worn on the user's head.
[0036] The nose pads 24 are provided on the edges of the rims 21 that correspond to the nose of the user when the sunglasses 100 are worn on the head of the user, and come into contact with the nose of the user, forming a shape that corresponds to the contact portion of the nose of the user at this time. This allows the sunglasses 100 to be stably maintained when worn.
[0037] The materials constituting the respective parts of the frame 20 are not particularly limited, and may be, for example, various metal materials, various resin materials, etc. The shape of the frame 20 is not limited to that shown in the figure, so long as it can be worn on the head of the user.
[0038] The lenses 30 are attached to the rim portions 21. The lenses 30 are optically transparent members having a plate-like overall shape curved outward, and have a resin layer (molded layer) and an optical functional sheet 11 (functional substrate).
[0039] The resin layer has optical transparency and is located on the back side of the lens (the side facing the wearer's eye). When the lens 30 is provided with a light collecting function, this resin layer has the light collecting function.
[0040] The material for forming the resin layer is not particularly limited as long as it is a resin material having optical transparency, and examples thereof include various curable resins such as various thermoplastic resins, thermosetting resins, and photocurable resins, and one or more of these may be used in combination.
[0041] Examples of the resin material include polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, polyvinyl chloride, polystyrene, polyamide, polyimide, polycarbonate, poly-(4-methylpentene-1), ionomers, acrylic resins, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymers (ABS resins), acrylonitrile-styrene copolymers (AS resins), butadiene-styrene copolymers, polyesters such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polyethers, polyether ketones (PEK), and polyether ether ketones. Examples of the resin include polyether ether ketone (PEEK), polyetherimide, polyacetal (POM), polyphenylene oxide, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, aromatic polyester (liquid crystal polymer), polytetrafluoroethylene, polyvinylidene fluoride, other fluorine-based resins, epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, polyurethanes, etc., or copolymers, blends, polymer alloys, etc., mainly made of these resins. Among them, it is preferable that the resin material is the same as or the same as the resin material that mainly constitutes the second substrate 112 of the optical functional sheet 11 described later. This can improve the adhesion between the resin layer and the optical functional sheet 11. In addition, since the refractive index difference between the resin layer and the optical functional sheet 11 (second substrate 112) can be set low, diffuse reflection of light between the resin layer and the optical functional sheet 11 can be appropriately suppressed or prevented, and light can be transmitted between the resin layer and the optical functional sheet 11 with excellent light transmittance. The refractive index difference between the resin layer and the optical functional sheet 11 (second substrate 112) is preferably 0.1 or less, and more preferably 0.05 or less, so that the effect obtained by setting the refractive index difference low can be more significantly exhibited.
[0042] The thickness of the resin layer is not particularly limited, and is, for example, preferably 0.5 mm to 5.0 mm, more preferably 1.0 mm to 3.0 mm, which allows the lens 30 to have both a relatively high strength and a light weight.
[0043] The optical functional sheet 11 (functional substrate) is formed into a curved shape having a curved convex surface and a curved concave surface on the outer surface (the side opposite to the wearer's eye) of the resin layer in the lens 30, i.e., on the curved convex surface of the resin layer, in accordance with the shape of the resin layer. In other words, the optical functional sheet 11 is a curved resin substrate to which the curved concave surface of the curved optical functional sheet 11 is bonded as the curved convex surface side of the resin layer, and the lens 30 is provided with this optical functional sheet 11, thereby imparting functionality such as the polarization property and half mirror property of the optical functional sheet 11 to the sunglasses 100. As a result, the sunglasses 100 exhibit the function as sunglasses having the above functionality.
[0044] As described above, the lenses 30 of the sunglasses 100 may or may not have a light-collecting function.
[0045] Furthermore, as described above, the sunglasses 100 may have the frame 20, or may have a frameless configuration from the standpoint of fashionability, lightweightness, and the like.
[0046] Furthermore, in this embodiment, glasses equipped with lenses 30 are applied to sunglasses 100, but this is not limited to this, and the glasses may be, for example, prescription glasses, fashion glasses, goggles that protect the eyes from wind, rain, dust, chemicals, etc.
[0047] In the sunglasses 100 (glasses) configured as described above, the lens 30 of the sunglasses 100 includes a curved optical functional sheet 11 having functionality such as polarization and half-mirror properties. By configuring this optical functional sheet 11 such that an anti-reflection layer 12 is laminated on one surface (upper surface) of a first substrate 111 (base material) included in the optical functional sheet 11, the optical functional sheet 11 can be provided with the anti-reflection layer 12 on its surface, thereby reducing the reflectance of incident light on the surface of the optical functional sheet 11 and therefore the lens 30.
[0048] As described above, in the optical functional sheet 11, the anti-reflection layer 12 is laminated on the first substrate 111 provided in the optical functional sheet 11, and the laminate of the anti-reflection layer 12 and the first substrate 111 (base material) constitutes the optical sheet 10 (the optical sheet of the present invention).
[0049] Such an optically functional sheet 11 can be obtained, for example, by preparing an optical sheet 10, a polarizing film 113, and a second substrate 112 in advance, and then bonding the optical sheet 10 and the polarizing film 113 with a first adhesive layer 114, and further bonding the polarizing film 113 and the second substrate 112 with a second adhesive layer 116. In this optically functional sheet 11, the optical sheet 10 is manufactured, for example, by a manufacturing method for optical sheet 10 to which nanoimprinting is applied using an ultraviolet-curable resin composition (ultraviolet-curable resin composition for nanoimprinting of the present invention) as shown below.
[0050] <Method of manufacturing optical sheets> Fig. 2 is a side view of a manufacturing apparatus for manufacturing the optical sheet of the present invention. For convenience of explanation, the upper side of Fig. 2 will be referred to as "upper" and the lower side as "lower". Also, Fig. 2 shows some parts in an exaggerated manner, and the dimensions are significantly different from the actual dimensions.
[0051] The optical sheet 10 can be obtained by forming an anti-reflection layer 12 composed of a cured product of an ultraviolet-curable resin composition (the ultraviolet-curable resin composition for nanoimprinting of the present invention) containing a polymerizable component, a polymerization initiator, and an ultraviolet absorber on one surface (upper surface) of a first substrate 111 prepared in advance, using a manufacturing apparatus 500 shown in FIG. 2 to which nanoimprinting is applied.
[0052] In this embodiment, the manufacturing apparatus 500 has a paint supply unit (not shown) and a moth-eye structure forming unit 800.
[0053] The paint supply unit (not shown) is disposed upstream of the structure forming unit 800 (conveying plate 810) in the transport direction in which the transport plate 810 provided in the moth-eye structure forming unit 800 described later transports the first substrate 111, and supplies (applies) an ultraviolet-curable resin composition (the ultraviolet-curable resin composition for nanoimprints of the present invention) as paint to the upper surface of a mold 840 placed on the transport plate 810, thereby continuously forming a coating film 600 (film) made of the ultraviolet-curable resin composition between the mold 840 placed on the transport plate 810 provided in the moth-eye structure forming unit 800 described later and the rotating roller 820, based on the rotation of the rotating roller 820 corresponding to the transport direction of the mold 840.
[0054] The moth-eye structure forming unit 800 is disposed downstream of the paint supply unit in the transport direction of the first substrate 111, and adjusts the thickness of a coating film 600 composed of an ultraviolet curable resin composition between the first substrate 111 transported along the transport direction and a mold 840 on a transport plate 810, and forms a moth-eye structure on the surface of the coating film 600, and then cures the ultraviolet curable resin composition constituting the coating film 600 by ultraviolet irradiation to continuously form an antireflection layer 12 on the lower surface of the first substrate 111 along the transport direction. That is, the moth-eye structure forming unit 800 applies nanoimprinting to form an optical sheet 10 in which an antireflection layer 12 (coating layer) having a moth-eye structure is continuously provided on the lower surface of the first substrate 111 along the transport direction on the surface opposite to the lower surface.
[0055] As shown in FIG. 2, the motheye structure forming section 800 has a conveying plate 810, a rotating roller 820 arranged opposite the conveying plate 810, and an ultraviolet irradiation means 830 provided corresponding to the conveying plate 810 downstream of the rotating roller 820.
[0056] The conveying plate 810 provided in the motheye structure forming section 800 is provided, for example, on a belt conveyor having rollers rotatably supported on a frame (not shown) that supports the entire manufacturing apparatus 500, and is thereby configured to be movable along the conveying direction.
[0057] Moreover, the rotating roller 820 is rotatably supported by, for example, a frame (not shown) that supports the entire manufacturing apparatus 500.
[0058] The transport plate 810 and the rotating roller 820 are disposed at a distance from each other such that the rotation axes (central axes) of the rotating rollers 820 face in the same direction in a direction perpendicular to the transport direction of the transport plate 810.
[0059] The rotating roller 820 has a cylindrical outer shape and is positioned opposite the conveying plate 810 on the upstream side of the conveying plate 810, downstream of the paint supply section in the conveying direction.When the coating film 600, which is made of an ultraviolet-curable resin composition, is clamped between the rotating roller 820 and the mold 840 on the conveying plate 810, via the first substrate 111, the roller comes into contact with the first substrate 111 (the side opposite the coating film 600) midway in the longitudinal direction.
[0060] The rotating roller 820 is provided with a moving means such as an air cylinder (not shown) located on the opposite side (upper side) of the conveying plate 810. The air cylinder rotatably supports the rotating roller 820 with respect to the rotating roller 820, and is configured to be able to move the rotating roller 820 so that the distance between the mold 840 and the rotating roller 820 at the opposing position where the mold 840 and the rotating roller 820 on the conveying plate 810 are opposed to each other by the operation of the air cylinder. This makes it possible to move the rotating roller 820 with respect to the mold 840 on the conveying plate 810 by the operation of the air cylinder (moving means). Therefore, the distance between the mold 840 and the rotating roller 820 can be set to a desired size.
[0061] Therefore, the distance is set to a size that allows the mold 840 and the rotating roller 820 on the conveying plate 810 to sandwich the coating film 600 and the first substrate 111 located between the mold 840 and the rotating roller 820, that is, by setting the distance according to the supply amount of the ultraviolet curable resin composition (coating film 600) supplied to the upper surface of the first substrate 111 by the paint supply unit, the mold 840 and the rotating roller 820 can compress the coating film 600 composed of the ultraviolet curable resin composition and the first substrate 111. Therefore, the shape of the recesses provided on the surface of the mold 840 on the rotating roller 820 side can be transferred to the surface of the coating film 600. In other words, by compressing the coating film 600 through the first substrate 111, the rotating roller 820 can function as a compression roller (nip roll) that makes the surface of the coating film 600 follow the shape of the recesses of the mold 840.
[0062] The conveying plate 810 has a flat outer shape and is conveyed (moves) along the conveying direction, and is arranged opposite the rotating roller 820 on its upstream side and opposite the ultraviolet ray irradiation means 830 on its downstream side. The ultraviolet ray curable resin composition and the first substrate 111 are supplied in this order upstream of the rotating roller 820, and the coating film 600 formed by the supply of the ultraviolet ray curable resin composition and the first substrate 111 are conveyed in this order, with the first substrate 111 on the upper side, to the rotating roller 820 and the ultraviolet ray irradiation means 830.
[0063] A mold 840 having a flat outer shape similar to that of the conveying plate 810 and a recess on its upper surface (the surface opposite to the conveying plate 810) is placed on the upper surface of the conveying plate 810. That is, the upper surface of the conveying plate 810 is provided with a mold 840 having recesses continuously formed along the conveying direction of the conveying plate 810. In this mold 840, the recesses have a shape symmetrical in the thickness direction of the first substrate 111 with respect to the shape of the moth-eye structure to be formed on the surface of the coating film 600 opposite to the first substrate 111. Therefore, the mold 840 is placed on the conveying plate 810 as a processing plate having recesses for forming a moth-eye structure on the surface of the coating film 600.
[0064] As described above, at the opposing position where the mold 840 and the rotating roller 820 on the conveying plate 810 face each other, the distance between them is set to a size that allows the coating film 600 and the first substrate 111 to be sandwiched and compressed by the mold 840 and the rotating roller 820. Therefore, by conveying (moving) the conveying plate 810 (mold 840) and rotating the rotating roller 820 to send (supply) the coating film 600 and the first substrate 111 to the opposing position, the shape of the recesses of the mold 840, i.e., the inverted moth-eye structure, can be transferred as a convex portion corresponding to the shape, to the surface of the coating film 600 opposite the first substrate 111. That is, at the opposing position, a moth-eye structure composed of convex portions corresponding to the shape of the recesses of the mold 840 can be formed on the surface of the coating film 600 opposite the first substrate 111.
[0065] As described above, the recesses in the mold 840 are symmetrical in the thickness direction of the first substrate 111 with respect to the shape of the moth-eye structure to be formed on the surface of the coating film 600. In this embodiment, the mold 840 is provided to correspond to almost the entire upper surface of the conveying plate 810 so that a moth-eye structure can be formed on the entire surface of the coating film 600 opposite the first substrate 111 when viewed in a plan view of the first substrate 111.
[0066] Furthermore, the microstructure that constitutes the recesses of the mold 840 is symmetrical in the thickness direction of the first substrate 111 with respect to the shape of the moth-eye structure to be formed on the surface of the coating film 600; in other words, it forms an inverted moth-eye structure on the surface opposite the conveying plate 810; in this specification, this inverted moth-eye structure refers to a surface structure of a mold (moth-eye transfer mold) that can form a moth-eye structure on the surface of the coating film 600 opposite the first substrate 111; in other words, that can provide a moth-eye structure on the surface of the anti-reflection layer 12 opposite the first substrate 111.
[0067] The microstructure on the surface of mold 840 that constitutes the inverted moth-eye structure is set according to the size of the moth-eye structure to be formed on the surface of antireflection layer 12. For example, when the recesses are cylindrical or needle-shaped, the average height (H) is preferably set within the range of 30 nm or more and 1000 nm or less, the average pitch (P) is preferably set within the range of 10 nm or more and 500 nm or less, and the average peak-to-peak distance (D) is preferably set within the range of 20 nm or more and 900 nm or less.
[0068] In this embodiment, in order to form the antireflection layer 12 having a moth-eye structure as a coating layer on the first substrate 111 (base material), a mold 840 having a moth-eye structure with a recessed portion having an inverted shape is prepared, but when forming a coating layer on the first substrate 111 (base material) having another fine uneven structure such as a wire grid structure, a moth's eye structure, a lotus leaf structure, a honeycomb structure, or a fructal structure, which is different from the moth-eye structure, a mold having recessed portions having an inverted shape of these fine uneven structures is prepared. This allows the coating layer having another fine uneven structure to be formed on the first substrate 111 (base material) in the same manner as when the antireflection layer 12 (coating layer) having a moth-eye structure is formed using an ultraviolet curable resin composition.
[0069] Moreover, the ultraviolet ray irradiation means 830 is disposed downstream of the rotating rollers 820 of the transport plate 810 so as to correspond to the transport plate 810 .
[0070] The ultraviolet irradiation means 830 is configured to irradiate ultraviolet rays to the upper surface side of the conveying plate 810, i.e., the upper surface of the mold 840, at a position downstream of the opposing position of the conveying plate 810 and the rotating roller 820. As a result, at the opposing position where the mold 840 on the conveying plate 810 and the rotating roller 820 face each other, the shape of the recesses provided in the mold 840 is transferred to the surface opposite the first substrate 111, that is, the coating film 600 in which the moth-eye structure is formed on the surface opposite the first substrate 111, can be irradiated with ultraviolet rays from the ultraviolet irradiation means 830 through the first substrate 111. Therefore, the ultraviolet curable resin composition constituting the coating film 600 is cured by irradiating the ultraviolet ray to the ultraviolet curable resin composition, and as a result, a cured product of the ultraviolet curable resin composition is formed. That is, the coating film 600 is cured. Thus, while placed on the conveying plate 810 (mold 840), the antireflection layer 12 having the moth-eye structure formed on the surface opposite to the first substrate 111 is formed in a state of being bonded to the lower surface of the first substrate 111. That is, the optical sheet 10 including the antireflection layer 12 and the first substrate 111 can be obtained in a state of being placed on the conveying plate 810 (mold 840).
[0071] (Method of manufacturing optical sheet 10 using manufacturing apparatus 500) Using the manufacturing apparatus 500 configured as described above, the optical sheet 10 having the anti-reflection layer 12 laminated on one surface (upper surface) of the first substrate 111 is manufactured by going through each process to obtain the optical sheet 10 as described below.
[0072] [1] First, an ultraviolet-curable resin composition (the ultraviolet-curable resin composition for nanoimprints of the present invention) is applied (supplied) from a paint supply unit onto the upper surface (one surface) of a mold 840 placed on a conveying plate 810, thereby continuously forming a coating film 600 (thin film) composed of this ultraviolet-curable resin composition along the conveying direction of the conveying plate 810.
[0073] (1-1) In this step, the coating of the ultraviolet-curable resin composition onto the upper surface (one side) of the mold 840 by the coating material supply unit is performed upstream of the rotating roller 820 provided in the structure forming unit 800.
[0074] By carrying out this step (1-1), in the next step [2], when the coating film 600 and the first substrate 111 are clamped between the rotating roller 820 and the mold 840 on the conveying plate 810, the first substrate 111 can be clamped between the rotating roller 820 and the mold 840 with the first substrate 111 facing the roller 820, i.e., with the first substrate 111 on the upper side.
[0075] Prior to applying the ultraviolet-curable resin composition to the upper surface (one side) of the mold 840 in the step (1-1), the upper surface of the mold 840, i.e., the microstructure constituting the recesses on the upper surface of the mold 840, is preferably subjected to a release treatment using a fluorine-based surface treatment agent. This makes it possible to easily peel off the optical sheet 10 including the antireflection layer 12 having the moth-eye structure and the first substrate 111 from the mold 840 in the subsequent step (2-4).
[0076] [2] Next, by transporting along the transport direction of the transport plate 810, the coating film 600 applied on the mold 840 placed on the transport plate 810 and the first substrate 111 are supplied, with the first substrate 111 facing up, to the moth-eye structure forming section 800, whereby an optical sheet 10 having the first substrate 111 and an anti-reflection layer 12 having a moth-eye structure formed on the surface opposite the first substrate 111 is continuously formed along the transport direction.
[0077] (2-1) First, a mold 840 having a coating film 600 (thin film) made of an ultraviolet-curable resin composition coated (formed) on its upper surface is supplied between the conveying plate 810 and the rotating roller 820 at a position where the conveying plate 810 and the rotating roller 820 face each other by conveying along the conveying direction of the conveying plate 810. At this time, the first substrate 111 is also supplied between the conveying plate 810 and the rotating roller 820 with the first substrate 111 facing the rotating roller 820 and the coating film 600 facing the conveying plate 810, with the longitudinal direction of the first substrate 111 aligned with the conveying direction.
[0078] When a mold 840 on which a coating film 600 made of an ultraviolet-curable resin composition is formed is supplied to the opposing position where the conveying plate 810 and the rotating roller 820 face each other, the separation distance between the mold 840 on the conveying plate 810 and the rotating roller 820 at the opposing position is preset to a size large enough to clamp the coating film 600 and the first substrate 111 between the mold 840 and the rotating roller 820 by operation of an air cylinder (moving means) provided corresponding to the rotating roller 820.
[0079] Furthermore, in the step (1-1), before the mold 840 is transported (supplied) to the opposing position between the transport plate 810 and the rotating roller 820, the coating film 600 is formed in advance on the upper surface of the mold 840. Therefore, in the step (2-1), the coating film 600 and the first substrate 111 can be easily supplied to the opposing position with the first substrate 111 facing up.
[0080] (2-2) Next, the coating film 600 formed on the mold 840 is transported (moved) along the transport direction by the operation of the transport plate 810 to an opposing position where the transport plate 810 and the rotating roller 820 face each other, and the first substrate 111 supplied from above the coating film 600 at the opposing position is clamped between the mold 840 on the transport plate 810 and the rotating roller 820 at this opposing position.
[0081] At this time, the surface (upper surface) of the mold 840 on the conveying plate 810 is provided with a recess having an inverted moth-eye structure as described above. The mold 840 on which the coating film 600 made of the ultraviolet curable resin composition is formed is supplied to a facing position where the conveying plate 810 and the rotating roller 820 face each other by the operation of the conveying plate 810. At the same time, the first substrate 111 is also supplied to the facing position with the first substrate 111 facing the rotating roller 820 and the coating film 600 facing the conveying plate 810. At this time, in the mold 840 on which the coating film 600 is formed, the coating film 600 made of the ultraviolet curable resin composition is supplied to the facing position in an uncured state.
[0082] Therefore, the coating film 600 composed of the ultraviolet curable resin composition and the first substrate 111 are sandwiched between the mold 840 and the rotating roller 820 on the conveying plate 810 at the opposing position, and the coating film 600 and the first substrate 111 are compressed by the mold 840 and the rotating roller 820. Therefore, the thickness of the coating film 600 is adjusted by this compression, and the shape of the recesses of the mold 840 is transferred to the surface of the coating film 600 as protrusions symmetrical to the shape of the recesses, due to the depressions being pressed against the surface of the coating film 600. That is, a moth-eye structure is formed on the surface of the coating film 600 (thin film) by nanoimprinting.
[0083] (2-3) Next, ultraviolet light is irradiated from ultraviolet light irradiation means 830 through first substrate 111 onto coating film 600 having a moth-eye structure formed thereon, which is obtained at the opposing position, on mold 840 .
[0084] At this time, the coating film 600 is placed on the mold 840 in a state of being sandwiched between the first substrate 111 and the mold 840. The ultraviolet ray irradiation means 830 is disposed on the opposite side to the conveying plate 810, that is, on the outside of the first substrate 111 side. Therefore, when the ultraviolet ray irradiation means 830 irradiates the conveying plate 810 with ultraviolet rays, the ultraviolet ray passes through the first substrate 111 and reaches the coating film 600 made of an ultraviolet curable resin composition.
[0085] In this way, ultraviolet light passes through first substrate 111, whereby coating film 600 made of an ultraviolet-curable resin composition is irradiated with ultraviolet light, and at this time, a moth-eye structure transferred by mold 840 is formed on the surface of coating film 600 opposite first substrate 111. Therefore, by irradiating coating film 600 with ultraviolet light, coating film 600 made of an ultraviolet-curable resin composition can be cured in a state in which a moth-eye structure is formed on its surface, to produce a cured product.
[0086] Therefore, when placed on the conveying plate 810, an optical sheet 10 can be obtained which includes a first substrate 111 and an antireflection layer 12 having a moth-eye structure formed on the surface opposite to the first substrate 111.
[0087] (2-4) Next, the optical sheet 10 comprising the anti-reflection layer 12 with the moth-eye structure formed thereon and the first substrate 111 is transported along the transport direction of the transport plate 810, and then the optical sheet 10 is peeled off from the mold 840 on the transport plate 810 (not shown).
[0088] By carrying out these steps (2-1) to (2-4), the optical sheet 10 including the antireflection layer 12 and the first substrate 111 is produced in the moth-eye structure forming portion 800.
[0089] By carrying out steps [1] and [2] using the manufacturing apparatus 500 as described above, it is possible to obtain an optical sheet 10 in the form of a film, which comprises a first substrate 111 and an anti-reflection layer 12 having a moth-eye structure formed on the surface opposite the first substrate 111 as a laminate of these.
[0090] As described above, by preparing a mold having a moth-eye structure in which the shape of the recesses is inverted, and performing steps [1] and [2] using the manufacturing apparatus 500, it is possible to obtain an optical sheet 10 including a first substrate 111 and an anti-reflection layer 12 (coating layer) having a moth-eye structure formed thereon. However, by preparing a mold having recesses having a configuration in which other fine uneven structures such as a wire grid structure, a moth-eye structure, a lotus leaf structure, a honeycomb structure, or a fructal structure are inverted, and performing steps [1] and [2] using the manufacturing apparatus 500 using an ultraviolet-curable resin composition, it is possible to manufacture an optical sheet 1 having a coating layer having these fine uneven structures on the first substrate 111 (base material).
[0091] Below, we will describe in detail each embodiment of an optical functional sheet 11 having an optical sheet 10 (the optical sheet of the present invention) composed of a laminate having a first substrate 111 and an antireflection layer 12 (coating layer) and an antireflection layer 12 on the surface side.
[0092] <Optical functional sheet> <<First embodiment>> FIG. 3 is a vertical cross-sectional view showing a first embodiment of an optically functional sheet having an optical sheet of the present invention, and FIG. 4 is an enlarged vertical cross-sectional view of an area [A] surrounded by a dashed line in FIG.
[0093] For convenience of explanation, the upper side of Fig. 3 and Fig. 4 will be referred to as "upper" and the lower side as "lower". The x direction in Fig. 3 will be referred to as "left-right direction" or "flow direction (MD)", the y direction will be referred to as "front-rear direction" or "vertical direction (TD)", and the z direction will be referred to as "up-down direction". In Fig. 3 and Fig. 4, the thickness direction of the optical functional sheet 11 is exaggerated, and therefore the actual dimensions are significantly different. Furthermore, in the lens 30, the optical functional sheet 11 is actually curved, but in Fig. 3 and Fig. 4, it is presented as being flat to improve visibility, and the resin layer is omitted in Fig. 3, but is actually formed in close contact with the second substrate 112 below the optical functional sheet 11.
[0094] 3 and 4, in this embodiment, the optical functional sheet 11 (functional substrate) includes a first substrate 111 having optical transparency, a second substrate 112 having optical transparency provided on the other surface side (lower side) of the first substrate 111, a polarizing film 113 provided between the first substrate 111 and the second substrate 112, and an antireflection layer 12 provided as an outermost layer (surface) on the surface (upper surface) of the first substrate 111 opposite to the polarizing film 113. That is, in the optical functional sheet 11, a laminate of the first substrate 111 and the antireflection layer 12 constitutes the optical sheet 10 as described above.
[0095] By setting the positional relationship of the layers in the optical functional sheet 11 as described above, the polarizing film 113 is located between the first substrate 111 and the second substrate 112 with the antireflection layer 12 as the outermost layer on the upper surface side, and is not exposed on the surface of the optical functional sheet 11. That is, the polarizing film 113 does not constitute the outermost layer exposed on the upper or lower surface of the optical functional sheet 11. Therefore, it is possible to reliably prevent the polarizing film 113 from being hit by sand, dust, rain, or the like, or from being worn by other members, etc., as in the case where the outermost layer is constituted. Therefore, it is possible to reliably prevent the polarizing film 113 from being damaged by this collision or wear. Therefore, the optical functional sheet 11 can be one in which the design and optical properties are maintained for a long period of time. In addition, since the optical functional sheet 11 has the antireflection layer 12 having the configuration described below as the outermost layer, it is possible to more reliably prevent the polarizing film 113 from being damaged by collision or wear.
[0096] The optical functional sheet 11 also includes a polarizing film 113 that has a function of extracting linearly polarized light having a polarization plane in a predetermined direction from incident light (unpolarized natural light). This allows the optical functional sheet 11 to have optical transparency, and further exhibits an optical functionality of transmitting the transmitted light as polarized light. That is, in this embodiment, the optical functional sheet 11 exhibits polarization as an optical characteristic.
[0097] Furthermore, the optically functional sheet 11 has an anti-reflection layer 12 on its surface, and the surface of this anti-reflection layer 12 has a moth-eye structure, so that the reflectance of incident light on the surface of the optically functional sheet 11 is reduced.
[0098] Each layer constituting this optically functional sheet 11 will be described below. The first substrate 111 supports the polarizing film 113 (laminate), and by disposing the polarizing film 113 between the first substrate 111 and the second substrate 112, the first substrate 111 has a function as a protective layer that protects the polarizing film 113.
[0099] This first substrate 111 is not particularly limited as long as it is made mainly of a transparent resin material, but it is preferable that it contains a transparent resin (base resin) having thermoplasticity as the main material.
[0100] In this specification, the term "main material" refers to a constituent material that is contained in an amount of 50% by weight or more among the constituent materials that constitute the layer (substrate) that contains this material.
[0101] The transparent resin is not particularly limited, but examples thereof include resins having transparency such as acrylic resins, polystyrene resins, polyethylene resins, polypropylene resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate resins, polyamide resins, cycloolefin resins, vinyl chloride resins, and polyacetal resins, and one or more of these resins may be used in combination. Among these, polycarbonate resins or polyamide resins are preferable. Polycarbonate resins are rich in mechanical strength such as transparency (translucency) and rigidity, and further have high heat resistance, so that the transparency of the first substrate 111 and the impact resistance and heat resistance of the first substrate 111 can be improved by using polycarbonate resin as the transparent resin. Furthermore, polyamide resins can improve chemical resistance, stress resistance, and the like in addition to transparency and impact resistance.
[0102] As the polycarbonate resin, various resins can be used, among which aromatic polycarbonate resin is preferable. Aromatic polycarbonate resin has an aromatic ring in its main chain, which allows the first substrate 111 to have superior strength.
[0103] The aromatic polycarbonate resin is synthesized, for example, by an interfacial polycondensation reaction between bisphenol and phosgene, or an ester exchange reaction between bisphenol and diphenyl carbonate.
[0104] Examples of bisphenols include bisphenol A and bisphenol (modified bisphenol) which is the source of the repeating unit of polycarbonate represented by the following formula (1A).
[0105] [ka] (In formula (1A), X is an alkyl group having 1 to 18 carbon atoms, an aromatic group, or a cyclic aliphatic group; Ra and Rb are each independently an alkyl group having 1 to 12 carbon atoms; m and n are each an integer of 0 to 4; and p is the number of repeating units.)
[0106] Specific examples of bisphenols that are the source of the repeating units of the polycarbonate represented by the formula (1A) include 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 2,2'-bis(4-hydroxy-3-methylphenyl)propane, and any of these may be used alone or in combination of two or more.
[0107] In particular, it is preferable that the polycarbonate resin contains, as a main component, a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol. By using such a bisphenol-type polycarbonate resin, first substrate 111 exhibits even greater strength.
[0108] The polyamide resin is not particularly limited, and various types can be used, such as alicyclic polyamide and semi-aromatic polyamide. Alicyclic polyamide is a material with excellent impact resistance. Therefore, the optical functional sheet 11 can exhibit excellent impact resistance. Semi-aromatic polyamide is a material with a high elastic modulus. Therefore, the optical functional sheet 11 can have excellent resistance to stress such as bending.
[0109] In this specification, semi-aromatic polyamide refers to a polyamide in which one of the dicarboxylic acid and diamine monomers constituting the polyamide is an aromatic compound and the other is an aliphatic compound, and specifically, can be represented by the following formula (1B).
[0110] [ka] (However, R in formula (1B) 1 and R 2 one of which is a divalent aromatic substituent and the other is a divalent aliphatic substituent, and n is an integer of 2 or greater.
[0111] The polyamide may be a copolymer (random copolymer, block copolymer, etc.) containing two or more kinds of monomers of at least one of dicarboxylic acid and diamine.
[0112] In addition, R in the above formula (1B) 1 , R 2 Of these, the aromatic substituent is preferably one represented by the following formula (2B).
[0113] [ka] (In formula (2B), l and m each independently represent an integer of 0 or more and 2 or less.)
[0114] This makes it possible to more suitably protect the polarizing film 113 and also to improve the processability of the optical functional sheet 11 .
[0115] R in the above formula (1B) 1 , R 2 Of these, the aliphatic substituent is preferably one having 4 to 18 carbon atoms, more preferably a hydrocarbon group having 4 to 18 carbon atoms, and even more preferably a saturated hydrocarbon group having 4 to 18 carbon atoms. This can provide the optically functional sheet 11 with better processability.
[0116] Furthermore, the semi-aromatic polyamide preferably contains an aromatic dicarboxylic acid and an aliphatic diamine as constituent monomers, which can more effectively protect the polarizing film 113 and improve the processability of the optical functional sheet 11.
[0117] An alicyclic polyamide has an alicyclic chemical structure in its molecule, and may have an alicyclic chemical structure in its main chain structure or may have an alicyclic chemical structure in its side chain structure.
[0118] Examples of the alicyclic polyamide include compounds in which at least one of the dicarboxylic acid and diamine monomers constituting the polyamide has an alicyclic chemical structure, and specifically, for example, can be represented by the following formula (3B).
[0119] [ka] (In formula (3B), R 3 , R 4are each independently a hydrogen atom or a hydrocarbon group having 4 or less carbon atoms, o is an integer of 2 or more and 14 or less, p is an integer of 0 or more and 6 or less, and n is an integer of 2 or more.
[0120] Moreover, the glass transition temperature (Tg) of the resin material contained as the main material in the first substrate 111 is preferably 100° C. or more and 190° C. or less, and more preferably 105° C. or more and 155° C. or less. This allows the thermal bending process for forming the optical functional sheet 11 into a curved shape to be carried out relatively easily. Furthermore, the optical functional sheet 11 can be made to have excellent durability and reliability.
[0121] Furthermore, as long as first substrate 111 has optical transparency, its color may be any color, such as colorless, red, blue, or yellow.
[0122] These colors can be selected by incorporating a dye or pigment into the first substrate 111. Examples of the dye include acid dyes, direct dyes, reactive dyes, and basic dyes, and one or more types selected from these may be used in combination.
[0123] Specific examples of dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Direct Black 19, 38, 51, 71, 154, 168, 171, 195, and CI Reactive Red. 14, 32, 55, 79, 249, CI Reactive Black 3, 4, 35, etc.
[0124] Moreover, the first substrate 111 preferably further contains an ultraviolet absorbing agent, which can improve the light resistance of the optically functional sheet 11.
[0125] As the ultraviolet absorbing agent, it is preferable to use the same ultraviolet absorbing agent as that described as the ultraviolet absorbing agent contained in the antireflection layer 12 described later, and specifically, it is preferable to have a light absorption peak having a maximum peak of absorptance in the wavelength range of 300 nm or more and 350 nm or less in the light absorption spectrum. As described above, in the manufacturing method of the optical sheet 10 using the manufacturing apparatus 500, the ultraviolet ray emitted from the ultraviolet ray irradiation means 830 is irradiated to the coating film 600 composed of the ultraviolet curable resin composition after passing through the first substrate 111. Therefore, the effect of the present invention obtained by using a radical polymerization initiator having a light absorption peak having a maximum peak of absorptance in the wavelength range of more than 350 nm and 400 nm or less can be more significantly exhibited with respect to the ultraviolet absorbing agent having a light absorption peak having a maximum peak of absorptance in the wavelength range of 300 nm or more and 350 nm or less in the light absorption spectrum contained in the ultraviolet curable resin composition described later.
[0126] Furthermore, the first substrate 111 may contain, as necessary, various additives such as antioxidants, fillers, plasticizers, light stabilizers, heat ray absorbers, and flame retardants in addition to the polycarbonate resins, ultraviolet absorbers, and dyes or pigments described above.
[0127] In this case, the content of the polycarbonate resin in the first substrate 111 is not particularly limited, but is preferably 75% by weight or more, and more preferably 85% by weight or more. By setting the content of the polycarbonate resin within the above range, the optical functional sheet 11 can exhibit excellent strength.
[0128] Moreover, the refractive index of first substrate 111 at a wavelength of 589 nm is preferably 1.3 to 1.8, more preferably 1.4 to 1.65. By setting the refractive index of first substrate 111 within the above numerical range, impairment of the function of polarizing film 113 can be appropriately suppressed or prevented.
[0129] The average thickness of the first substrate 111 is preferably set to 0.1 mm or more and 1.5 mm or less, more preferably 0.2 mm or more and 0.8 mm or less. By setting the average thickness of the first substrate 111 within this range, it is possible to reduce the thickness of the optical functional sheet 11 while accurately suppressing or preventing the occurrence of bending in the optical functional sheet 11.
[0130] The second substrate 112 supports the polarizing film 113 (laminate), and by disposing the polarizing film 113 between the second substrate 112 and the above-mentioned first substrate 111, it also functions as a protective layer that protects the polarizing film 113.
[0131] Like the first substrate 111, the second substrate 112 is not particularly limited as long as it is made primarily of a transparent resin material, but it is preferable that the second substrate 112 contains a transparent resin (base resin) having thermoplastic properties as the main material.
[0132] As this transparent resin, the same materials as those mentioned above for the first substrate 111 can be used, but among them, it is preferable that the main material is a polycarbonate-based resin or a polyamide-based resin.
[0133] The polycarbonate resin or polyamide resin is not particularly limited, but for example, the same resins as those listed for the first substrate 111 described above can be used.
[0134] The glass transition temperature (Tg) of the resin material contained as the main material in the second substrate 112 is preferably 100° C. or more and 190° C. or less, and more preferably 105° C. or more and 155° C. or less. This allows the thermal bending process for forming the optical functional sheet 11 into a curved shape to be carried out relatively easily. In addition, the optical functional sheet 11 can be made to have excellent durability and reliability.
[0135] Moreover, it is preferable that the second substrate 112 further contains an ultraviolet absorbing agent, similar to the first substrate 111. This can improve the light resistance of the optically functional sheet 11.
[0136] As this ultraviolet absorbing agent, the same ones as those explained below as ultraviolet absorbing agents contained in the antireflection layer 12 can be used, and one or a combination of two or more of these can be used.
[0137] Furthermore, the second substrate 112 may contain other components in addition to the resin material and the UV absorber contained as the main material. Such components are not particularly limited, but may include, for example, a resin material other than the main material, a colorant such as a dye or pigment, a filler, an alignment aid, a stabilizer (thermal stabilizer), an antioxidant, a plasticizer, a flame retardant, an antistatic agent, and a viscosity adjuster.
[0138] In this case, the content of the resin material in the second substrate 112 is not particularly limited, but is preferably 75% by weight or more, and more preferably 85% by weight or more, based on 100% by weight of the second substrate 112. By setting the content of the resin material within the above range, the optical functional sheet 11 can exhibit excellent strength.
[0139] Moreover, the refractive index of second substrate 112 at a wavelength of 589 nm is preferably 1.3 to 1.8, more preferably 1.4 to 1.65. By setting the refractive index of second substrate 112 within the above numerical range, impairment of the function of polarizing film 113 can be appropriately suppressed or prevented.
[0140] The average thickness of the second substrate 112 is preferably set to 0.1 mm or more and 1.5 mm or less, more preferably 0.2 mm or more and 0.8 mm or less. By setting the average thickness of the second substrate 112 within this range, it is possible to reduce the thickness of the optical functional sheet 11 while accurately suppressing or preventing the occurrence of bending in the optical functional sheet 11.
[0141] The polarizing film 113 constitutes a polarizer having a function of extracting linearly polarized light having a polarization plane in a predetermined direction from incident light (unpolarized natural light). This imparts polarization to the optical functional sheet 11, and the light passing through the optical functional sheet 11 (transmitted light) becomes polarized.
[0142] The polarization degree of the polarizing film 113 is not particularly limited, but is preferably, for example, 50% to 100%, and more preferably, 80% to 100%. The visible light transmittance of the polarizing film 113 is not particularly limited, but is preferably, for example, 10% to 80%, and more preferably, 20% to 50%.
[0143] The material for forming such polarizing film 113 is not particularly limited as long as it has the above-mentioned function, and examples thereof include a polymer film formed of polyvinyl alcohol (PVA), partially formalized polyvinyl alcohol, polyethylene vinyl alcohol, polyvinyl butyral, polycarbonate, ethylene-vinyl acetate copolymer partially saponified product, etc., which is dyed with a dichroic substance such as iodine or a dichroic dye and uniaxially stretched, a polyene-based oriented film such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride, etc.
[0144] Among these, the polarizing film 113 is preferably a polymer film mainly made of polyvinyl alcohol (PVA), which is dyed with iodine or a dichroic dye and uniaxially stretched. Polyvinyl alcohol (PVA) is a material that is excellent in transparency, heat resistance, affinity with the dyeing agent iodine or a dichroic dye, and orientation when stretched. Therefore, the polarizing film 113 mainly made of PVA has excellent heat resistance and polarizing ability.
[0145] Examples of the dichroic dye include Chloratin Fast Red, Congo Red, Brilliant Blue 6B, Benzopurpurine, Chlorazol Black BH, Direct Blue 2B, Diamine Green, Chrysophenone, Sirius Yellow, Direct Fast Red, and Acid Black.
[0146] The refractive index of the polarizing film 113 at a wavelength of 589 nm is not particularly limited, but is preferably, for example, 1.45 or more and 1.55 or less, and more preferably 1.47 or more and 1.53 or less.
[0147] The thickness of the polarizing film 113 is not particularly limited, and is preferably, for example, from 5 μm to 60 μm, and more preferably from 10 μm to 40 μm.
[0148] The first adhesive layer 114 is provided between the first substrate 111 (one of the substrates) and the polarizing film 113, and has a function of bonding the first substrate 111 and the polarizing film 113. This makes it possible to impart excellent adhesion between the first substrate 111 and the polarizing film 113 via the first adhesive layer 114.
[0149] In addition, the second adhesive layer 116 is provided between the second substrate 112 (the other substrate) and the polarizing film 113, and has a function of bonding the second substrate 112 and the polarizing film 113. This makes it possible to impart excellent adhesion between the second substrate 112 and the polarizing film 113 via the second adhesive layer 116.
[0150] The first adhesive layer 114 and the second adhesive layer 116 are each made of an adhesive having optical transparency. The adhesive is not particularly limited, but examples thereof include silicone-based, silylated urethane resin-based, urethane resin-based, epoxy-based, polyolefin-based, chlorinated polyolefin-based, acrylic-based, cyanoacrylate-based, rubber-based, polyester-based, polyimide-based, and phenol-based adhesives.
[0151] Among these, the first adhesive layer 114 and the second adhesive layer 116 are preferably made of a urethane resin-based adhesive. This allows the optical functional sheet 11 to be given the heat resistance required for the thermal bending process when the optical functional sheet 11 is subjected to the thermal bending process to form the optical functional sheet 11 into a curved shape. Furthermore, it is also preferable that the first adhesive layer 114 and the second adhesive layer 116 are made of a silicone-based adhesive. This allows the generation of gas during the curing of the adhesive to be appropriately suppressed or prevented. Therefore, it is possible to appropriately suppress or prevent air bubbles from remaining in the adhesive layers 114 and 116.
[0152] It should be noted that the first adhesive layer 114 and the second adhesive layer 116 may be the same or of the same type, or may be different from the same or of the same type.
[0153] Furthermore, the refractive index at a wavelength of 589 nm of the first adhesive layer 114 and the second adhesive layer 116 is preferably independently 1.3 or more and 1.7 or less, and more preferably 1.4 or more and 1.65 or less.
[0154] The thickness of the first adhesive layer 114 and the second adhesive layer 116 is preferably, for example, 2 μm or more and 100 μm or less, and more preferably 5 μm or more and 35 μm or less, respectively. The first adhesive layer 114 and the second adhesive layer 116 can reliably bond the first adhesive layer 114 and the second adhesive layer 116 to the polarizing film 113, respectively.
[0155] The antireflection layer 12 is provided so as to cover the first substrate 111 (one surface (upper surface) of the optical functional sheet 11) and constitutes the outermost layer of the optical functional sheet 11. In addition, since this antireflection layer 12 is located on the opposite side of the lens 30 from the resin layer, it also constitutes the outermost layer of the lens 30. Therefore, the antireflection layer 12 functions as a protective layer that protects the polarizing film 113 located as an intermediate layer of the optical functional sheet 11.
[0156] The antireflection layer 12 is manufactured by the manufacturing method using the manufacturing apparatus 500 described above, and is formed as a layered layer on the first substrate 111, that is, as a component of the optical sheet 10. Therefore, the antireflection layer 12 has a moth-eye structure formed on the surface opposite to the first substrate 111. Therefore, the antireflection layer 12 functions as an antireflection layer that suppresses or prevents the reflection of the incident light incident on the lens 30.
[0157] In addition, similar to the formation of the anti-reflection layer 12 on the first substrate 111 (one surface (upper surface) of the optical functional sheet 11), an anti-reflection layer may be formed on the second substrate 112 (the other surface (lower surface) of the optical functional sheet 11). In other words, the second substrate 112 may also be configured with an optical sheet 10 made of a laminate in which the anti-reflection layer 12 and the second substrate 112 are laminated. However, in this embodiment, as shown in FIG. 3, the formation of an anti-reflection layer on the second substrate 112 is omitted. This is because the lens 30 has a resin layer provided in contact with the second substrate 112. However, when the refractive index difference between the lens 30 and the second substrate 112 is large, it is preferable to form an anti-reflection layer on the second substrate 112 (the other surface of the optical functional sheet 11). This can improve the transmittance of the incident light incident on the lens 30 from the optical functional sheet 11 to the resin layer.
[0158] This antireflection layer 12 (coating layer) is a so-called coat layer formed using a resin composition exhibiting curability, and as this resin composition (ultraviolet-curable resin composition), in the present invention, one for nanoimprints is used which contains a polymerizable component (curable resin), a polymerization initiator having a light absorption peak with a maximum absorptance peak in a wavelength range of more than 350 nm and not more than 400 nm in its light absorption spectrum, and an ultraviolet absorber having a light absorption peak with a maximum absorptance peak in a wavelength range of 300 nm or more and 350 nm or less in its light absorption spectrum.
[0159] Here, in the manufacturing method of the optical sheet 10 using the manufacturing apparatus 500 described above, the antireflection layer 12 is formed on the first substrate 111 by irradiating the coating film 600 made of the ultraviolet curable resin composition with ultraviolet rays. More specifically, in the step [2], while the concave portion of the mold 840 is pressed against the surface of the coating film 600 made of the ultraviolet curable resin composition, ultraviolet rays are transmitted through the transparent first substrate 111 from the first substrate 111 side and irradiated onto the ultraviolet curable resin composition to cure the ultraviolet curable resin composition, thereby forming the antireflection layer 12 having a moth-eye structure on the surface opposite to the first substrate 111.
[0160] In this case, in the present invention, a combination of an ultraviolet absorber and a polymerization initiator in the ultraviolet curable resin composition is selected that has a light absorption peak having a maximum absorptance peak in a wavelength range of 300 nm or more and 350 nm or less in the light absorption spectrum, and a combination of an optical absorption peak having a maximum absorptance peak in a wavelength range of more than 350 nm and 400 nm or less.
[0161] Therefore, when the ultraviolet-curable resin composition is irradiated with ultraviolet light in the step [2], the ultraviolet light having a wavelength of more than 350 nm and not more than 400 nm can be appropriately suppressed or prevented from being absorbed by the ultraviolet absorber. Therefore, the polymerization reaction of the polymerizable component can be started by the absorption of the ultraviolet light having a wavelength of more than 350 nm and not more than 400 nm by the polymerization initiator, and a cured product composed of the ultraviolet-curable resin composition can be reliably formed. Therefore, the antireflection layer 12 composed of this cured product and having a moth-eye structure formed on the surface can be formed as one having excellent durability.
[0162] Hereinafter, an ultraviolet-curable resin composition containing a polymerizable component, a polymerization initiator, and an ultraviolet absorber, in which the ultraviolet absorber and the polymerization initiator are combined as described above (ultraviolet-curable resin composition for nanoimprints of the present invention) will be described.
[0163] (Polymerizable component) The polymerizable component has a polymerizable group, and is contained in the ultraviolet-curable resin composition in order to form a network (polymer chains) by reaction between these groups, thereby forming a cured product of the ultraviolet-curable resin composition.
[0164] In this polymerizable component, examples of the polymerizable group include a radically polymerizable group and a cationic polymerizable group, with the radically polymerizable group being preferred.
[0165] Here, if the ultraviolet-curable resin composition contains both a polymerizable component having a radical polymerizable group and a polymerizable component having a cationic polymerizable group, and the curing of these components is started almost simultaneously, the formation of a cured product by the polymerizable component having a radical polymerizable group is faster. That is, the reaction rate of the radical polymerizable group is faster than that of the cationic polymerizable group. In addition, in the above-mentioned step [2], the antireflection layer 12 having a moth-eye structure is formed by forming a cured product of the ultraviolet-curable resin composition while pressing the concave portion of the mold 840 against the surface of the coating film 600 composed of the ultraviolet-curable resin composition, but it is necessary to perform the formation of this cured product before the coating film 600 placed on the conveying plate 810 and the first substrate 111 pass through the area corresponding to the ultraviolet irradiation means 830 by the conveying of the conveying plate 810. Therefore, a radical polymerizable group having a high reaction rate is preferably selected as the polymerizable group.
[0166] In addition, the polymerizable component may be either a monomer component (monomer) or a polymer component (polymer) as long as it has a polymerizable group, but is preferably a monomer component. This can reduce the viscosity of the ultraviolet-curable resin composition. Therefore, in the step [2], when the coating film 600 made of the ultraviolet-curable resin composition is sandwiched between the first substrate 111 and the mold 840, the coating film 600 can be adjusted to have a more uniform film thickness. Furthermore, when the antireflection layer 12 is formed in a state in which the concave portion of the mold 840 is pressed against the surface of the coating film 600 made of the ultraviolet-curable resin composition, the conformability of the coating film 600 made of the ultraviolet-curable resin composition to the concave portion of the mold 840 can be improved. Therefore, even a moth-eye structure having a finer shape can be formed with excellent accuracy on the surface of the antireflection layer 12. Furthermore, an anchor effect can be obtained between the antireflection layer 12 (the cured product of the ultraviolet-curable resin composition) and the recesses of the first substrate 111, so that the antireflection layer 12 can have excellent adhesion to the first substrate 111. Therefore, the optical sheet 10 can be made to satisfy the requirement B described below relatively easily.
[0167] Therefore, in the following, an example will be described in which the polymerizable component is a monomer component having a radically polymerizable group.
[0168] In this monomer component, the radical polymerizable group may be, for example, a (meth)acryloyl group, a vinyl group, etc., and among them, a (meth)acryloyl group is preferable. The (meth)acryloyl group is preferably selected as the radical polymerizable group from the viewpoint of excellent radical polymerizability and easy availability of a compound having a (meth)acryloyl group as a polymerizable group. That is, so-called acrylic monomers are preferably selected as the monomer component.
[0169] In addition, in order to form a network based on the reaction between polymerizable components in the ultraviolet-curable resin composition, the monomer component preferably has a plurality of radically polymerizable groups (two or more), and more preferably includes both a monomer component having two radically polymerizable groups and a monomer component having three or more radically polymerizable groups. This allows the network to be formed more strongly in the cured product of the ultraviolet-curable resin composition, and the optical sheet 10 can relatively easily satisfy requirements A and B described below.
[0170] In addition, when the region of the monomer component that is incorporated into the network by the linkage between the radical polymerizable groups is taken as the main chain of the monomer component, examples of the main chain include a straight or branched chain having a urethane bond, a straight or branched chain having an ester bond, a straight or branched chain having an epoxy bond, a straight or branched chain of glycol, and a straight or branched chain having a repeating unit of siloxane bonds (-Si-O-Si-). Among them, a straight or branched chain having a urethane bond, a straight or branched chain having an ester bond, a straight or branched chain having an epoxy bond, and a straight or branched chain of glycol that is relatively excellent in flexibility is preferably selected, and in particular, a straight or branched chain of glycol is preferably selected. This can reliably make the cured product of the ultraviolet curable resin composition soft. Therefore, the conformability of the coating film 600 made of the ultraviolet curable resin composition to the recesses of the mold 840 is improved, and as a result, even a moth-eye structure having a finer shape can be formed with excellent accuracy on the surface of the antireflection layer 12. In addition, the viscosity of the ultraviolet-curable resin composition can be more reliably reduced.
[0171] From the above, it is preferable that the monomer component is one in which a (meth)acryloyl group as a radical polymerizable group is linked to a straight or branched chain of glycol as a main chain. When the monomer component has two radical polymerizable groups, a straight chain of glycol is selected as the main chain, and when the monomer component has three or more radical polymerizable groups, a branched chain of glycol is selected as the main chain.
[0172] Furthermore, in this case, the main chain (straight or branched) of the glycol preferably contains an aliphatic chain having 6 to 10 carbon atoms. In other words, the polymerizable component preferably has, in its skeleton, a radically polymerizable group and an aliphatic chain having 6 to 10 carbon atoms. This makes it possible to more reliably make the cured product of the ultraviolet-curable resin composition soft (flexible), thereby making it possible to more significantly exhibit the above-mentioned effects.
[0173] In addition, when the region of the monomer component that is not incorporated into the network due to the linkage between the radical polymerizable groups is defined as the side chain of the monomer component, the monomer component preferably contains, in addition to the above, one having a fluorinated hydrocarbon group as the side chain. That is, the polymerization component preferably has a radical polymerizable group and a fluorinated hydrocarbon group in its skeleton. As a result, when the polymerization component (monomer component) is polymerized to form a cured product of the ultraviolet curable resin composition, the ultraviolet curable resin composition is cured with a pendant structure in which the fluorinated hydrocarbon group is exposed on the surface of the cured product. Therefore, the surface of the cured product of the ultraviolet curable resin composition, that is, the surface of the antireflection layer 12 on which the moth-eye structure is formed (the surface of the antireflection layer 12 on the side opposite to the first substrate 111) has a structure in which the fluorinated hydrocarbon group is exposed as the side chain. Therefore, since excellent water repellency can be imparted to the surface of the antireflection layer 12, the optical sheet 10 can relatively easily satisfy the requirement C described below. Furthermore, exposure of the fluorinated hydrocarbon groups in the antireflection layer 12 allows the antireflection layer 12 to exhibit excellent sliding properties.
[0174] The content of the monomer component in the ultraviolet curable resin composition is not particularly limited, but is preferably 40.0 parts by weight or more and 95.0 parts by weight or less, and more preferably 70.0 parts by weight or more and 95.0 parts by weight or less, per 100.0 parts by weight of the ultraviolet curable resin composition. By setting the content of the monomer component in the ultraviolet curable resin composition within the above range, the antireflection layer 12 can be provided with a moth-eye structure formed on its surface with excellent precision.
[0175] When the monomer component contains one having a fluorinated hydrocarbon group as a side chain, the content of this monomer component is preferably 0.1 to 5.0 parts by weight, more preferably 0.3 to 2.5 parts by weight, in 100.0 parts by weight of the ultraviolet-curable resin composition, which allows the ultraviolet-curable resin composition to reliably exhibit the effects obtained by containing a monomer component having a fluorinated hydrocarbon group as a side chain.
[0176] (Polymerization initiator) In addition, in the present invention, the ultraviolet-curable resin composition contains a polymerization initiator for initiating a polymerization reaction for forming a network by the polymerization components, and as described above, when the polymerizable component has a radically polymerizable group as the polymerizable group, the ultraviolet-curable resin composition contains, as the polymerization initiator, a radical polymerization initiator (photoradical polymerization initiator) that generates radicals upon irradiation with ultraviolet rays as energy rays.
[0177] As a result, in the step [2], by irradiating the coating film 600 made of the ultraviolet-curable resin composition with ultraviolet light from the first substrate 111 side while the concave portion of the mold 840 is pressed against the surface of the coating film 600, radicals can be reliably generated from the photoradical polymerization initiator. Therefore, the radicals can initiate a polymerization reaction by the polymerizable component having a radically polymerizable group as the polymerizable group. Therefore, the antireflection layer 12 having the moth-eye structure can be reliably formed.
[0178] In addition, the photoradical polymerization initiator is not particularly limited, but examples thereof include acetophenone-based photoradical polymerization initiators, benzoin-based photoradical polymerization initiators, benzophenone-based photoradical polymerization initiators, thioxanthone-based photoradical polymerization initiators, ketone-based photoradical polymerization initiators, imidazole-based photoradical polymerization initiators, carbazole-based photoradical polymerization initiators, oxime ester-based photoradical polymerization initiators, titanocene-based photoradical polymerization initiators, acylphosphine oxide-based photoradical polymerization initiators, trichloromethyltriazine-based photoradical polymerization initiators, and the like, and one or more of these can be used in combination.
[0179] In the present invention, the photoradical polymerization initiator has a light absorption peak having a maximum absorptance peak in the wavelength range of more than 350 nm and less than 400 nm in the light absorption spectrum. Here, the ultraviolet absorber described later is generally one having a light absorption peak having a maximum absorptance peak in the wavelength range of 300 nm or more and 350 nm or less in the light absorption spectrum for the purpose of reliably suppressing or preventing the deterioration and degradation of the antireflection layer 12 and thus the optical sheet 10 (optical functional sheet 11) due to exposure to sunlight. Therefore, even if the ultraviolet absorber absorbs ultraviolet rays in the wavelength range of 300 nm or more and 350 nm or less during irradiation of ultraviolet rays using the ultraviolet irradiation means 830, the photoradical polymerization initiator has a maximum absorptance peak in the wavelength range of more than 350 nm and less than 400 nm, and therefore can reliably generate radicals by absorbing the ultraviolet rays in this range. Therefore, the curing reaction of the ultraviolet-curable resin composition based on this radical can be reliably initiated, and therefore the antireflection layer 12 composed of the cured product of the ultraviolet-curable resin composition can be reliably formed as one cured with a high degree of cure, and therefore, it can be formed as one having excellent durability.
[0180] In this specification, the term "maximum peak" refers to a steep apex (maximum value) in the light absorption spectrum of a photoradical polymerization initiator or an ultraviolet absorber. In addition, when a gentle peak is formed instead of a steep peak, the "maximum peak" showing the maximum value in the light absorption spectrum of the photoradical polymerization initiator in the wavelength range of 350 nm to 500 nm is treated as the "maximum peak", and the "maximum peak" showing the maximum value in the light absorption spectrum of the ultraviolet absorber in the wavelength range of 300 nm to 500 nm is treated as the "maximum peak".
[0181] In addition, when the photoradical polymerization initiator does not have a "maximum peak" in the light absorption spectrum in the wavelength range of 350 nm or more and 500 nm or less, the photoradical polymerization initiator is considered to have a light absorption spectrum of a bifunctional acrylic monomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "A-HD-N") as a background (transmittance T 0 When the light absorption spectrum (transmittance T [%]) of the photoradical polymerization initiator diluted 10,000 times with this bifunctional acrylic monomer ("A-HD-N" manufactured by Shin-Nakamura Chemical Co., Ltd.) was measured, the light absorption spectrum in the wavelength range of 350 nm to 500 nm had a maximum peak of absorptance within a wavelength range of more than 350 nm and less than or equal to 400 nm, and the absorbance at the maximum peak (= 2-log 10 (T / T 0 )) is more preferably 0.2 or more. This allows the photoradical polymerization initiator to more reliably generate radicals by absorbing ultraviolet light having a wavelength in the range of more than 350 nm and not more than 400 nm.
[0182] The content of the photoradical polymerization initiator in the ultraviolet curable resin composition is not particularly limited, but is preferably 1.0 parts by weight or more and 8.0 parts by weight or less, and more preferably 3.0 parts by weight or more and 6.5 parts by weight or less, in 100.0 parts by weight of the ultraviolet curable resin composition. By setting the content of the photoradical polymerization initiator within the above range, radicals can be reliably generated by the absorption of ultraviolet light by the photoradical polymerization initiator.
[0183] (UV absorber) In the present invention, the ultraviolet-curable resin composition contains an ultraviolet absorber.
[0184] In this way, the ultraviolet curable resin composition contains an ultraviolet absorber, so that ultraviolet rays can be absorbed in the antireflection layer 12. Therefore, it is possible to suppress the alteration and deterioration of other constituent materials contained in the ultraviolet curable resin composition. Therefore, it is possible to improve the ultraviolet irradiation resistance of the antireflection layer 12 and relatively easily satisfy the requirements A and B described below. In addition, it is possible to suppress or prevent the arrival of ultraviolet rays at the first substrate 111, so that it is possible to suppress the alteration and deterioration of the first substrate 111. From this viewpoint, it is also possible to relatively easily satisfy the requirements A and B described below.
[0185] The ultraviolet absorbing agent is not particularly limited, but may be, for example, a triazine-based, benzophenone-based, benzotriazole-based, or cyanoacrylate-based agent, and one or two of these may be used in combination. Among these, a benzotriazole-based ultraviolet absorbing agent is preferably used, and among the benzotriazole-based ultraviolet absorbing agents, a hydroxyphenylbenzotriazole-based ultraviolet absorbing agent is more preferable. This allows the above-mentioned effect obtained by including an ultraviolet absorbing agent in the anti-reflection layer 12 to be more significantly exhibited. In addition, a hydroxyphenylbenzotriazole-based ultraviolet absorbing agent can be obtained relatively easily and inexpensively as a material having a functional group reactive with a radical polymerization component, which will be described later.
[0186] In the present invention, the ultraviolet absorbers used have a light absorption peak with a maximum absorptance peak in the wavelength range of 300 nm or more and 350 nm or less in the light absorption spectrum. This can reliably suppress or prevent the antireflection layer 12 and the optical sheet 10 from being altered or deteriorated due to exposure to sunlight. As described above, the effect obtained by using a photoradical polymerization initiator having a light absorption peak with a maximum absorptance peak in the wavelength range of more than 350 nm and 400 nm or less in the light absorption spectrum can be reliably exhibited. In addition, such an ultraviolet absorber is preferably one that has a maximum peak of absorptivity in the wavelength range of 300 nm to 350 nm in the light absorption spectrum in the wavelength range of 300 nm to 500 nm, and an absorbance at the maximum peak of 0.03 or more, when the light absorption spectrum of the ultraviolet absorber diluted 1,000,000 times with the bifunctional acrylic monomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "A-HD-N") is measured with the light absorption spectrum of the bifunctional acrylic monomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "A-HD-N") as the background. This allows the effect obtained by using the above-mentioned photoradical polymerization initiator to be more significantly exhibited.
[0187] Furthermore, the ultraviolet absorber is preferably one having a functional group reactive with the polymerization component. Specifically, when the polymerizable component is a monomer component having a radical polymerizable group, the ultraviolet absorber is preferably one having a radical polymerizable group as a functional group. This allows the ultraviolet absorber to be incorporated into the network formed by the reaction of the polymerization components. Therefore, it is possible to appropriately suppress or prevent the ultraviolet absorber from leaking, i.e., bleeding out, from the anti-reflection layer 12 composed of the cured product of the ultraviolet curable resin composition. Therefore, the requirements A and B can be more reliably satisfied over a long period of time.
[0188] In addition, when the polymerizable group of the polymerization component is a (meth)acryloyl group, an ultraviolet absorber having a (meth)acryloyl group as a functional group reactive with the polymerization component (radical polymerization component) can form a network by radical polymerization between the (meth)acryloyl groups of both the polymerization component and the polymerization component, and is therefore preferably used as an ultraviolet absorber having a functional group reactive with the radical polymerization component. In addition, an ultraviolet absorber having a (meth)acryloyl group as a functional group can be obtained, for example, as a reaction product between a hydroxyphenylbenzotriazole-based ultraviolet absorber having two or more hydroxyl groups and a (meth)acrylate monomer. In addition, in the hydroxyphenylbenzotriazole-based ultraviolet absorber, one hydroxyl group adjacent to the triazine skeleton exists to exert the function as an ultraviolet absorber. Therefore, in order to give the hydroxyphenylbenzotriazole-based ultraviolet absorber reactivity with the (meth)acrylate monomer, it is required that the hydroxyphenylbenzotriazole-based ultraviolet absorber (benzotriazole-based ultraviolet absorber) has one or more hydroxyl groups different from this hydroxyl group.
[0189] The content of the ultraviolet absorbing agent in the ultraviolet curable resin composition is not particularly limited, but is preferably 2.0 parts by weight or more and 5.0 parts by weight or less, and more preferably 2.5 parts by weight or more and 4.5 parts by weight or less, in 100.0 parts by weight of the ultraviolet curable resin composition. If the content of the ultraviolet absorbing agent in the ultraviolet curable resin composition is less than the lower limit, depending on the type of ultraviolet absorbing agent, the effect obtained by adding the ultraviolet absorbing agent to the antireflection layer 12 may not be sufficiently obtained. Even if the content of the ultraviolet absorbing agent in the ultraviolet curable resin composition exceeds the upper limit, no further improvement in ultraviolet irradiation resistance is observed, and the transparency of the antireflection layer 12 and the adhesion of the antireflection layer 12 to the first substrate 111 may be impaired.
[0190] (Light stabilizer) Moreover, it is preferable that the ultraviolet-curable resin composition further contains a light stabilizer.
[0191] The inclusion of a light stabilizer in the ultraviolet-curable resin composition can improve the stability of the antireflection layer 12 when exposed to sunlight. As a result, the ultraviolet radiation resistance of the antireflection layer 12 and therefore the optical sheet 10 can be improved, that is, the requirements A and B can be reliably satisfied.
[0192] The light stabilizer is not particularly limited, but includes hindered amine-based ones, nickel-based ones, etc., and one or two of these can be used in combination. Among these, hindered amine-based ones are particularly preferably used. This makes it possible to more significantly exhibit the above-mentioned effects. In addition, if the hindered amine-based light stabilizer is one having a functional group (polymerizable group) that is reactive with the polymerization component described later, it can be obtained relatively easily and inexpensively.
[0193] Furthermore, it is preferable that the light stabilizer has a functional group reactive with the polymerization component. This allows the light stabilizer to be incorporated into the network formed by the reaction of the polymerization component. Therefore, it is possible to appropriately suppress or prevent the light stabilizer from leaking, i.e., bleeding out, from the anti-reflection layer 12 made of the ultraviolet-curable resin composition. Therefore, the requirements A and B can be more reliably satisfied over a long period of time.
[0194] In addition, when the polymerizable group of the polymerization component is a (meth)acryloyl group, a light stabilizer having a (meth)acryloyl group as a functional group reactive with the polymerization component (radical polymerization component) is preferably used as a light stabilizer having a functional group reactive with the radical polymerization component, since the (meth)acryloyl groups of both the polymerization component and the (meth)acryloyl groups of the polymerization component and the (meth)acryloyl groups of both the polymerization component and the (meth)acryloyl groups of ...
[0195] The content of the light stabilizer in the ultraviolet curable resin composition is not particularly limited, but is preferably 0.01 parts by weight or more and 3.00 parts by weight or less, and more preferably 0.10 parts by weight or more and 1.00 parts by weight or less, in 100.0 parts by weight of the ultraviolet curable resin composition. If the content of the light stabilizer in the ultraviolet curable resin composition is less than the lower limit, depending on the type of light stabilizer, the effect obtained by adding the light stabilizer to the antireflection layer 12 may not be sufficiently obtained. Even if the content of the light stabilizer in the ultraviolet curable resin composition exceeds the upper limit, no further improvement in ultraviolet irradiation resistance is observed, and the transparency of the antireflection layer 12 and the adhesion of the antireflection layer 12 to the first substrate 111 may be impaired.
[0196] The ultraviolet-curable resin composition may further contain additives other than the above-mentioned materials.
[0197] Examples of other additives include heat ray absorbing agents, plasticizers, colorants, sensitizers, surfactants, antioxidants, reduction inhibitors, antistatic agents, and surface conditioners (leveling agents).
[0198] The ultraviolet-curable resin composition having such a configuration may further contain a solvent as another additive, but is preferably a solvent-free resin composition that does not substantially contain a solvent. This eliminates the need to remove the solvent from the resin composition, and therefore in the step [2], ultraviolet light is transmitted through the transparent first substrate 111 from the first substrate 111 side to harden the ultraviolet-curable resin composition, thereby forming the antireflection layer 12, i.e., forming the convex portions of the moth-eye structure, with better film formation accuracy, while pressing the concave portions of the mold 840 against the surface of the coating film 600 made of the ultraviolet-curable resin composition.
[0199] In addition, when the ultraviolet curable resin composition is a solventless resin composition, as described above, the monomer component is preferably selected as the polymerizable component. This allows the ultraviolet curable resin composition to be adjusted to have a low viscosity even when the ultraviolet curable resin composition is a solventless resin composition, specifically, to have a viscosity of preferably 30 cP or more and 200 cP or less, more preferably 50 cP or more and 120 cP or less.
[0200] The ultraviolet-curable resin composition as described above (ultraviolet-curable resin composition for nanoimprints of the present invention) is prepared by forming a coating film 600 of the ultraviolet-curable resin composition on a polycarbonate substrate as a first substrate 111 using a production apparatus 500, and then using a mold 840 (manufactured by Inox Corporation, "HT-AR-05A", length 100 mm x width 100 mm) having needle-shaped recesses with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm, under conditions of a lamination pressure of the rotating roller 820 of 0.01 MPa and a lamination speed of 10 mm / sec, a light source: UV-LED 365 nm, ultraviolet illuminance: 110 mW / cm 2 , UV irradiation amount: 1000mj / cm 2 When the coating film 600 is irradiated with ultraviolet light by the ultraviolet light irradiation means 830 under the above conditions to form an antireflection layer 12 composed of a cured product having an average thickness of 10 μm, the reaction rate of the polymerizable component in the cured product is preferably 65.0% or more, and more preferably 85.0% or more. This ensures that the ultraviolet-curable resin composition has been cured reliably, and the antireflection layer 12 composed of the cured product of the ultraviolet-curable resin composition can have excellent durability. Note that, for example, when the polymerizable group is a (meth)acryloyl group, the reaction rate of the polymerizable component in the cured product is calculated by measuring the remaining rate of the carbon-carbon double bond in the (meth)acryloyl group before and after curing in the light absorption spectrum at a wavelength of 810 cm. -1 The maximum absorption peak of the double bond near 1150 cm -1It can be determined by calculation from the ratio of carbonyl groups in nearby (meth)acryloyl group structures.
[0201] Furthermore, this ultraviolet-curable resin composition preferably satisfies the following requirement A, and more preferably satisfies requirements B to D.
[0202] Requirement A: Using the manufacturing apparatus 500, a coating film 600 of an ultraviolet-curable resin composition is formed on a polycarbonate substrate as a first substrate 111. Then, using a mold 840 (manufactured by Inox Corporation, "HT-AR-05A", length 100 mm x width 100 mm) having needle-shaped recesses with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm, the coating film 600 and the first substrate 111 are sandwiched between the rotating roller 820 and the mold 840 under the conditions of a lamination pressure of 0.01 MPa and a lamination speed of 10 mm / sec., a light source: UV-LED 365 NM, ultraviolet illuminance: 110 mW / cm 2 , UV irradiation amount: 1000mj / cm 2 Under the above conditions, ultraviolet light is irradiated onto the coating film 600 by the ultraviolet light irradiation means 830 to form an antireflection layer 12 composed of a cured product having an average thickness of 10 μm, and then, after irradiating the antireflection layer 12 with ultraviolet light for 600 hours from the side of the antireflection layer 12 using a xenon weather meter in accordance with Cycle No. 3 of Table 3-A of JIS K 7350-2, the change in YI of this film, as specified by JIS K 7373, is less than 3.0.
[0203] Requirement B: Using the manufacturing apparatus 500, a coating film 600 of an ultraviolet-curable resin composition is formed on a polycarbonate substrate as a first substrate 111. Then, using a mold 840 (manufactured by Inox Corporation, "HT-AR-05A", length 100 mm x width 100 mm) having needle-shaped recesses with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm, the coating film 600 and the first substrate 111 are sandwiched between the rotating roller 820 and the mold 840 under the conditions of a lamination pressure of 0.01 MPa and a lamination speed of 10 mm / sec., a light source: UV-LED 365 NM, ultraviolet illuminance: 110 mW / cm 2 , UV irradiation amount: 1000mj / cm 2 Under the above conditions, ultraviolet rays are irradiated onto the coating film 600 by the ultraviolet irradiation means 830 to form an antireflective layer 12 composed of a cured product having an average thickness of 10 μm, and then, after irradiating the antireflective layer 12 with ultraviolet rays for 600 hours from the antireflective layer 12 side using a xenon weather meter in accordance with Table 3-A method-cycle No. 3 of JIS K 7350-2, the adhesion of the antireflective layer 12 composed of the cured product cut into a lattice shape to the first substrate 111 is 90% or more, according to the cross-cut method specified in JIS K 5600-5-6.
[0204] Thus, by satisfying the requirement A and further satisfying the requirement B, it can be said that the optical sheet 10 is endowed with excellent durability.
[0205] Requirement C: Using the manufacturing apparatus 500, a coating film 600 of an ultraviolet-curable resin composition is formed on a polycarbonate substrate as a first substrate 111. Then, using a mold 840 (manufactured by Inox Corporation, "HT-AR-05A", length 100 mm x width 100 mm) having needle-shaped recesses with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm, the coating film 600 and the first substrate 111 are sandwiched between the rotating roller 820 and the mold 840 under the conditions of a lamination pressure of 0.01 MPa and a lamination speed of 10 mm / sec., a light source: UV-LED 365 NM, ultraviolet illuminance: 110 mW / cm2 , UV irradiation amount: 1000mj / cm 2 Under the above conditions, ultraviolet rays are irradiated onto the coating film 600 by the ultraviolet irradiation means 830 to form an antireflective layer 12 composed of a cured product having an average thickness of 10 μm, and then, in accordance with JIS K 7350-2, Table 3-A method, cycle No. 3, ultraviolet rays are irradiated from the antireflective layer 12 side for 600 hours using a xenon weather meter, where E1 [°] is the contact angle of pure water with the antireflective layer 12 before 600 hours of ultraviolet irradiation, and E2 [°] is the contact angle of pure water with the antireflective layer 12 after 600 hours of ultraviolet irradiation, the following relationships are satisfied: E2≧130°, (E1-E2) / E1×100≦10%.
[0206] Requirement D: Using the manufacturing apparatus 500, a coating film 600 of an ultraviolet-curable resin composition is formed on a polycarbonate substrate as a first substrate 111. Then, using a mold 840 (manufactured by Inox Corporation, "HT-AR-05A", length 100 mm x width 100 mm) having needle-shaped recesses with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm, the coating film 600 and the first substrate 111 are sandwiched between the rotating roller 820 and the mold 840 under the conditions of a lamination pressure of 0.01 MPa and a lamination speed of 10 mm / sec., a light source: UV-LED 365 NM, ultraviolet illuminance: 110 mW / cm 2 , UV irradiation amount: 1000mj / cm 2 Under the above conditions, ultraviolet light is irradiated onto coating film 600 by ultraviolet light irradiation means 830 to form antireflective layer 12 composed of a cured product having an average thickness of 10 μm, and then ultraviolet light is irradiated from this antireflective layer 12 side for 600 hours using a xenon weather meter in accordance with JIS K 7350-2, Table 3-A method, cycle No. 3. The reflectance of incident light at a wavelength of 550 nm on the surface of antireflective layer 12 composed of a moth-eye structure opposite first substrate 111 is less than 1.0%.
[0207] Furthermore, since optical sheet 10 further satisfies requirements C and D, it can be said that in optical sheet 10, antireflection layer 12 is endowed with the function of an antireflection layer having a moth-eye structure formed on the surface, with excellent durability. In addition, in the requirement A, it is preferable that the antireflection layer 12 made of the cured product satisfies that the change in YI as defined by JIS K 7373 is less than 3.0, more preferably that the change in YI is 1.5 or less, and even more preferably that the change in YI is 0.8 or less. This more appropriately suppresses or prevents discoloration of the optical sheet 10, and it can be said that the function of the optical sheet 10 is more reliably maintained over a long period of time. In other words, it can be said that the optical sheet 10 has excellent durability.
[0208] Furthermore, in the requirement B, the antireflection layer 12 made of the cured product preferably satisfies that the adhesion of the film cut into a lattice shape by the cross-cut method specified in JIS K 5600-5-6 to the polycarbonate substrate is 90% or more, more preferably 95% or more, and even more preferably 98% or more. This means that even if the optical sheet 10 is exposed to sunlight, the adhesion of the antireflection layer 12 to the first substrate 111 in the optical sheet 10 is more reliably maintained for a long period of time. In other words, the optical sheet 10 can be said to have excellent durability.
[0209] Furthermore, in requirement C, after optical sheet 10 is irradiated with ultraviolet light for 600 hours from the antireflection layer 12 side in accordance with Table 3-A method-cycle No. 3 of JIS K 7350-2 using a xenon weather meter, when the contact angle of pure water with the surface of antireflection layer 12 on which the moth-eye structure is formed before the ultraviolet light irradiation is E1 [°] and the contact angle of pure water with the surface of antireflection layer 12 on which the moth-eye structure is formed after the ultraviolet light irradiation is E2 [°], it is sufficient for optical sheet 10 to satisfy the relationship of E2≧130°, (E1-E2) / E1×100≦10%, preferably satisfy the relationship of E2≧135°, (E1-E2) / E1×100≦8%, and more preferably satisfy the relationship of E2≧140°, (E1-E2) / E1×100≦6%. As a result, it can be said that the water repellency of the surface on which the moth-eye structure of the antireflection layer 12 is formed is more reliably maintained for a long period of time in the optical sheet 10, even if the optical sheet 10 is exposed to sunlight. That is, it can be said that the antireflection layer 12 in the optical sheet 10 is endowed with a function as an antireflection layer with excellent durability.
[0210] Furthermore, in the above requirement D, after the optical sheet 10 is irradiated with ultraviolet light from the antireflection layer 12 side for 600 hours using a xenon weather meter in accordance with JIS K 7350-2 Table 3-A method-cycle No. 3, the optical sheet 10 may satisfy that the reflectance of incident light with a wavelength of 550 nm on the surface of the antireflection layer 12 opposite to the first substrate 111 (base material) having a moth-eye structure is less than 1.0%, but the reflectance is preferably 0.8% or less, more preferably 0.5% or less. This means that even if the optical functional sheet 11 is exposed to sunlight, the reflectance of the surface of the antireflection layer 12 on which the moth-eye structure is formed is more reliably maintained for a long period of time in the optical functional sheet 11. That is, it can be said that the antireflection layer 12 in the optical functional sheet 11 is endowed with a function as an antireflection layer with excellent durability.
[0211] The reflectance of incident light with a wavelength of 550 nm on the surface of the antireflection layer 12 opposite the first substrate 111 can be obtained, for example, by attaching a black resin sheet (PET sheet (refractive index: 1.63)) that does not reflect light with a wavelength of 550 nm (reflectance = 0%) to almost the entire surface of the second substrate 112 side of the optical functional sheet 11, and then irradiating incident light with a wavelength of 550 nm on the surface of the antireflection layer 12 opposite the first substrate 111, i.e., the surface on which the moth-eye structure of the antireflection layer 12 is formed, and measuring the reflected light of the incident light reflected by this surface, for example, using a spectrophotometer (manufactured by JASCO Corporation, "V-670") and an integrating sphere unit (manufactured by JASCO Corporation, "ISN-723").
[0212] The antireflection layer 12 formed of the cured product of the ultraviolet-curable resin composition as described above has an average thickness that is not particularly limited, but is preferably 1.0 μm or more and 20.0 μm or less, and more preferably 8.0 μm or more and 15.0 μm or less. If the average thickness of each antireflection layer 12 is less than the lower limit, the abrasion resistance, antireflection resistance, and ultraviolet radiation resistance of the optical sheet 10 may decrease. On the other hand, if the thickness of the antireflection layer 12 exceeds the upper limit, cracks may occur in the antireflection layer 12 when the optical sheet 10 is made into a curved optical sheet in a curved state.
[0213] Furthermore, in the case where the size of the multiple convex portions (protrusions) in the moth-eye structure formed on the surface of the antireflection layer 12 is imparted with the function of the antireflection layer 12, the size is usually set to the following size. That is, in the moth-eye structure, the average height of the convex portions is preferably set within a range of about 10 nm to 1600 nm, and the average pitch between the convex portions is preferably set within a range of about 5 nm to 800 nm. In addition, when the convex portions are needle-shaped, the average peak-to-peak distance is preferably set to about 10 nm to 1100 nm. If the antireflection layer 12 has a moth-eye structure formed on the surface that is set within such a size range, the antireflection layer 12 can be reliably formed by going through the step of forming a cured product of the ultraviolet curable resin composition in the step [2] while pressing the concave portions of the mold 840 against the surface of the coating film 600 composed of the ultraviolet curable resin composition. Furthermore, by using a mold 840 (moth-eye transfer mold) placed on a conveying plate 810 provided in the manufacturing apparatus 500, which has a microstructure of the size described above formed as a recess (inverted moth-eye structure) on its surface, an anti-reflection layer 12 having a moth-eye structure set within such size range formed on its surface can be formed with excellent precision.
[0214] The refractive index of the antireflection layer 12 at a wavelength of 589 nm is not particularly limited, and is preferably, for example, from 1.40 to 1.60, and more preferably from 1.450 to 1.595.
[0215] The total thickness of the optical functional sheet 11 is not particularly limited, but is preferably about 0.05 mm to 3.0 mm, and more preferably about 0.10 mm to 0.50 mm, which provides the optical functional sheet 11 with excellent strength and allows each layer of the optical functional sheet 11 to reliably perform its function.
[0216] The optically functional sheet 11 may also include an adhesion layer as an intermediate layer at least between the first adhesive layer 114 and the polarizing film 113 and between the second adhesive layer 116 and the polarizing film 113. This can improve the adhesion between the adhesive layers 114, 116 and the polarizing film 113.
[0217] The adhesive layer is not particularly limited, but may be, for example, SiO 2 and Al 2 O 3 The above-mentioned materials are mainly composed of at least one of them.
[0218] <<Second embodiment>> In addition, the optical functional sheet 11 may have a polarizing property by having the configuration described in the first embodiment, or may have a half-mirror property as described below.
[0219] FIG. 5 is a vertical cross-sectional view showing a second embodiment of an optically functional sheet having an optical sheet of the present invention.
[0220] For convenience of explanation, the upper side of FIG. 5 is referred to as "upper" and the lower side is referred to as "lower". The x direction in FIG. 5 is referred to as "left-right direction", the y direction is referred to as "front-rear direction", and the z direction is referred to as "up-down direction". Furthermore, in FIG. 5, the thickness direction of the optical sheet is exaggerated, so that the actual dimensions are significantly different. Furthermore, in the lens 30, the optical functional sheet 11 is actually curved, but in FIG. 5, it is presented as being flat to improve visibility, and the resin layer is not shown in FIG. 5, but is actually formed in close contact with the second substrate 112 below the optical functional sheet 11.
[0221] Hereinafter, the second embodiment of the optical sheet of the present invention will be described with reference to this figure, but the differences from the above-described embodiment will be mainly described, and a description of the similar points will be omitted.
[0222] The optical functional sheet 11 shown in Figure 5 is similar to the optical functional sheet 11 shown in Figure 3, except that the function imparted to the optical functional sheet 11 is different, specifically, instead of being imparted with polarization properties, the optical functional sheet 11 is imparted with half-mirror properties.
[0223] 5, the optical functional sheet 11 of the second embodiment includes a half mirror layer 117 instead of the polarizing film 113 between the first substrate 111 and the second substrate 112. As a result, the optical functional sheet 11 exhibits an optical functionality (half mirror functionality) of selectively reflecting light in a specific wavelength range from the incident light and transmitting the remaining portion, instead of a function (polarizing functionality) of extracting linearly polarized light having a polarization plane in a predetermined direction from the incident light.
[0224] The half mirror layer 117 selectively reflects light in a specific wavelength region among the incident light and transmits the remaining light, so that when a person is positioned on the back side of the curved optical sheet in which the optical functional sheet 11 is curved, that is, when the person wears the sunglasses 100, the person (wearer) can see the front side of the optical functional sheet 11 through the optical functional sheet 11. In addition, the light in a specific wavelength region (light of a specific color) reflected on the front side of the optical functional sheet 11 is visible to a person (a third person) positioned on the opposite side of the wearer through the optical functional sheet 11, so that the optical functional sheet 11 can be provided with design properties.
[0225] 5, in this embodiment, the half mirror layer 117 is configured as a laminate having a high refractive index layer 119 and a low refractive index layer 118 having an optical refractive index (hereinafter, may be simply referred to as "refractive index") lower than that of the high refractive index layer 119. In the illustrated configuration, the high refractive index layer 119 and the low refractive index layer 118 are laminated in this order from the front side (first substrate 111 side).
[0226] The high refractive index layer 119 and the low refractive index layer 118 are, for example, evaporated films formed by vacuum evaporation such as resistance heating or electron beam heating (EB) method, and the half mirror layer 117 is composed of a laminate of these.
[0227] The high refractive index layer 119 and the low refractive index layer 118 may be made of, for example, SiO 2 , SiO, TiO 2 , TiO, Ti 2 O 3 , Ti 2 O 5 , Al 2 O 3 , TaO 2 , Ta 2 O 5 , NdO 2 , NbO, Nb 2 O 3 , NbO 2 , Nb 2 O 5 , CEO 2 , MgO, Y 2 O 3 , SnO 2 , WO 3 , HfO 2 , ZrO 2 , Sc 2 O 3、 CrO, Cr 2 O 3 , In 2 O 3 , La 2 O 3 , CaF 2 , MgF 2 , Na 3 AlF 6 , AlF 3 , BaF 3 , CeF 3 , LaF 2 , LiF, Na 5 Al 3 F 14 , NdF 3 , Y.F. 3 and metal materials such as In, Cr, Ti, Ni, Au, Cu, Sn, Zr, and Al.
[0228] When the high refractive index layer 119 is made of a metal material among the above, the material is preferably made of Cr or Zr. On the other hand, when the low refractive index layer 118 is made of a metal material among the above, the material is preferably made of In or Al. This allows the refractive index of the high refractive index layer 119 to be higher than the refractive index of the low refractive index layer 118. Therefore, the half mirror layer 117 reliably exhibits the half mirror function.
[0229] When the high refractive index layer 119 is made of a metal oxide, Ta 2 O 5 , HfO 2 , ZrO 2 , Y 2 O 3 , Sc 2 O 3 , CEO 2 Preferably, ZrO 2 , CEO 2 On the other hand, when the low refractive index layer 118 is made of a metal oxide, it is more preferable that the material is SiO, SiO 2 , MgF 2 , CaF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 This allows the refractive index of the high refractive index layer 119 to be higher than the refractive index of the low refractive index layer 118. Therefore, the half mirror layer 117 exhibits a half mirror function.
[0230] By configuring the half mirror layer 117 in this way, a part of the light incident from the upper side (front surface) of the optical functional sheet 11 (optical functional sheet 11) passes through the low refractive index layer 118 and is emitted from the lower side (rear surface) of the optical functional sheet 11. Therefore, a person positioned below (rear surface side) of the optical functional sheet 11 can visually recognize the upper side (front side) of the optical functional sheet 11 through this optical functional sheet 11. In addition, since the remaining part of the incident light is reflected by the low refractive index layer 118, when a third person looks at the optical functional sheet 11 from the upper surface side (front surface side), this low refractive index layer 118 also functions as a mirror layer.
[0231] In addition, the high refractive index layer 119 functions as a mirror layer that selectively reflects light in a specific wavelength region, and thus, of the light incident from the upper side (front surface) of the optical functional sheet 11, the light in the specific wavelength region is selectively reflected at the interface between the low refractive index layer 118 and the high refractive index layer 119, and further at the interface between the first adhesive layer 114 and the high refractive index layer 119. Therefore, on the upper surface side (front surface side) of the optical functional sheet 11, i.e., the first substrate 111 side, the remainder of the light reflected by the low refractive index layer 118 and the light in the specific wavelength region reflected by the high refractive index layer 119 are visually recognized by a third party, and as a result, a color based on the light in the specific wavelength region selectively reflected by the high refractive index layer 119 is visually recognized.
[0232] In addition to being configured as a laminate of the high refractive index layer 119 and the low refractive index layer 118 as described above, the half mirror layer 117 can also be configured as a single layer made of a metal film mainly made of Au, Cu, In, etc. By configuring the half mirror layer 117 as a single layer having such a configuration, the thickness of the half mirror layer 117 can be reduced. However, by configuring the half mirror layer 117 as a laminate, i.e., a multi-layer film as described above, various reflected colors can be reproduced, and the half mirror layer 117 can have excellent design.
[0233] By disposing the half mirror layer 117 having such a configuration between the first substrate 111 and the second substrate 112 as described above, it is possible to prevent a decrease in the reflectance of the half mirror layer 117 and a change in the color tone of the half mirror layer 117.
[0234] Furthermore, the average thickness (physical thickness) of the high refractive index layer 119 and the low refractive index layer 118 may be the same or different, but is preferably 1 nm or more and 200 nm or less, and more preferably 1.5 nm or more and 150 nm or less.
[0235] The thickness (optical thickness: relative to a wavelength of 500 nm) of the high refractive index layer 119 and the low refractive index layer 118 is preferably 0.002 / 4 λnm or more and 0.4 / 4 λnm or less, and more preferably 0.003 / 4 λnm or more and 0.3 / 4 λnm or less.
[0236] By making the high refractive index layer 119 and the low refractive index layer 118 have such thicknesses, it is possible to reliably impart to the half mirror layer 117 the function as a half mirror.
[0237] Moreover, the total thickness of the half mirror layer 117 (the sum of the thicknesses of the high refractive index layer 119 and the low refractive index layer 118) is preferably 5 nm to 500 nm, more preferably 7.5 nm to 450 nm, and even more preferably 10 nm to 400 nm. This ensures that the half mirror layer 117 functions as a half mirror.
[0238] Moreover, the refractive index difference (optical refractive index difference) between the high refractive index layer 119 and the low refractive index layer 118 is preferably 0.3 to 2, and more preferably 0.4 to 1.5, which allows the half mirror layer 117 to reliably exhibit its function as a half mirror layer.
[0239] By providing an optically functional sheet 11 having a half mirror layer 117 of such a configuration with an anti-reflection layer 12 on the surface of the first substrate 111, it is possible to reduce reflections of the wearer's own eyes while maintaining the design of the sunglasses 100 having this optically functional sheet 11 (lens 30), thereby improving visibility for the wearer.
[0240] The optical functional sheet 11 of the second embodiment also provides the same effects as those of the first embodiment.
[0241] In the first embodiment, the optical functional sheet 11 includes the polarizing film 113, which imparts polarizing properties to the optical functional sheet 11, and in the second embodiment, the optical functional sheet 11 includes the half mirror layer 117, which imparts half mirror properties to the optical functional sheet 11. However, the optical functional sheet 11 is not limited to such a configuration, and may include, for example, the optical functional sheet 11 that has the polarizing film 113 and the half mirror layer 117 and exhibits both polarizing properties and half mirror properties, or may simply exhibit light transmittance without forming the polarizing film 113 and the half mirror layer 117. In the case where the optical functional sheet 11 simply exhibits light transmittance, the optical functional sheet 11 is considered to be composed of the optical sheet 10 alone.
[0242] <Head-up display> In addition, in the above, the lens 30 of the sunglasses 100 has been described as being equipped with an optical functional sheet 11 having an optical sheet 10 (the optical sheet of the present invention), but below, a case will be described in which the head-up display 350 is equipped with an optical functional sheet 11 as a cover member arranged to cover the window portion 151 of the storage body 353.
[0243] Fig. 6 is a side view showing an embodiment in which an optically functional sheet having the optical sheet of the present invention is applied to a cover member constituting a head-up display of an automobile, Fig. 7 is an enlarged longitudinal sectional view of the area [B] surrounded by a dashed line in Fig. 6, and Fig. 8 is a schematic diagram showing a laser light passing through a cover member constituting the head-up display shown in Fig. 6. In the following, for convenience of explanation, the upper side in Figs. 6 to 8 will be referred to as "upper" or "upper side", and the lower side will be referred to as "lower" or "lower". Also, the left side in Figs. 6 to 8 will be referred to as "front" or "forward", and the right side will be referred to as "rear" or "rear".
[0244] 6, a head-up display 350 is mounted on an automobile 300. The head-up display 350 is built into an upper portion of a dashboard 301.
[0245] As shown in FIG. 7, the head-up display 350 includes a light source 351, a reflecting member 352, and a housing 353.
[0246] The light source 351 can independently irradiate red (R), green (G), and blue (B) laser light LS. An image can be formed by controlling the irradiation timing of the laser light LS of each color while scanning the light source 351. Examples of the light source 351 include a laser light source and an LCD light source.
[0247] The reflecting member 352 is formed of, for example, a prism, and is capable of reflecting the laser light LS emitted from the light source 351. The laser light LS reflected by the reflecting member 352 is projected onto the rear surface 302a (inner surface) of the windshield 302, using the windshield 302 as a screen. This projected light is recognized by the driver H as the image (see FIGS. 6 and 7).
[0248] 7, the housing 353 is box-shaped and can house the light source 351, the reflecting member 352, and other components that constitute the head-up display 350 inside. The housing 353 also has a window 151 that is an opening that opens toward the windshield 302. The laser light LS is emitted to the outside of the housing 353, i.e., toward the windshield 302, through the window 151.
[0249] Moreover, the optical functional sheet 11 is installed as a cover member on the window portion 151 of the housing 353 so as to cover the window portion 151. This allows the laser light LS to be emitted toward the windshield 302, and prevents foreign matter such as dust and dirt from entering the housing 353 through the window portion 151. This prevents the lens of the light source 351 and the reflecting member 352 from becoming cloudy or dirty due to the foreign matter.
[0250] The optical functional sheet 11 is used as a cover member installed to cover the window portion 151, and at this time, as shown in FIG. 8, the optical functional sheet 11 is arranged in the window portion 151 so that the anti-reflection layer 12 is on the inside of the window portion 151. This makes it possible to obtain the same effect as that obtained when the optical functional sheet 11 provided to cover the front side of the lens 30 of the sunglasses 100 has the optical sheet 10. In addition, since it is possible to suppress the occurrence of ghosts due to the reflection of the laser light LS inside the optical functional sheet 11 when the laser light LS passes through the optical functional sheet 11, it is possible to appropriately suppress or prevent the image viewed by the driver H from becoming a double image (see FIG. 8).
[0251] <Windshield> Furthermore, as an example having an optical functional sheet 11 having an optical sheet 10 (the optical sheet of the present invention), the following describes a case in which the optical functional sheet 11 is used as a windshield (vehicle windshield) equipped on a motorcycle.
[0252] 9A and 9B are diagrams ((a) plan view, (b) side view, (c) cross-sectional view along line BB in FIG. 9A) showing an embodiment in which an optically functional sheet having an optical sheet of the present invention is applied to a windshield plate. In the following, for convenience of explanation, the front side of the paper in FIG. 9A will be referred to as the "front", the back side of the paper will be referred to as the "rear", the left side as the "left", the right side as the "right", the upper side as the "upper", and the lower side as the "lower", the front side of the paper in FIG. 9B will be referred to as the "right", the back side of the paper will be referred to as the "left", the left side as the "front", the right side as the "rear", the upper side as the "upper", and the lower side as the "lower", and the front side of the paper in FIG. 9C will be referred to as the "lower", the back side of the paper will be referred to as the "upper", the left side as the "left", the right side as the "right", the upper side as the "front", and the lower side as the "rear".
[0253] As shown in FIG. 9, the windshield plate 400 has a main body portion (central portion) 451 formed long in the vertical direction, two side portions 452 protruding in the left and right directions below the main body portion 451, and a connecting portion 453 connecting the side portions 452 to the main body portion 451, and its overall shape is a curved shape that is symmetrical on the left and right.
[0254] The main body 451 is located approximately in the center of the windshield 400, has a long shape in the vertical direction (a direction perpendicular to one direction), and is fixed at its underside to the body of a motorcycle or the like, so that a person (pilot) can view things located in front of them through this main body 451.
[0255] In this main body 451, the front surface is configured as a curved convex surface, and the rear surface is configured as a curved concave surface, so that the main body 451 has a curved shape (curved surface shape) that protrudes and curves toward the front side. Also, in the main body 451, this curved shape is formed along the left-right direction (one direction).
[0256] The two side portions 452 are formed below the main body portion 451 so as to protrude in the left and right directions, respectively, and are provided to suppress wind from being drawn in from the sides when riding a motorcycle or the like.
[0257] In this side surface portion 452, the front surface is formed as a curved convex surface, and the rear surface is formed as a curved concave surface, similarly to the main body portion 451, so that the side surface portion 452 has a curved shape (curved surface shape) that protrudes and curves toward the front side. Also, in the side surface portion 452, this curved shape is formed along the left-right direction.
[0258] The two connecting portions 453 are interposed between the main body portion 451 and the two side surface portions 452, respectively, to connect them together.
[0259] In this connecting portion 453, the front surface is configured as a curved concave surface, and the rear surface is configured as a curved convex surface, so that the connecting portion 453 has a curved shape (curved surface shape) that protrudes and curves toward the rear side. In addition, in the connecting portion 453, this curved shape is formed along the left-right direction.
[0260] In the windshield 400 having such a configuration and an overall shape that is a curved shape that is symmetrical on the left and right, each part 451 to 453 that constitutes the windshield 400 is formed integrally, and this windshield 400 is made of an optically functional sheet 11 that is made into a curved shape, and by configuring this optically functional sheet 11 to have an optical sheet 10 and curving the optically functional sheet 11 so that the anti-reflection layer 12 is at the front, it is possible to obtain the same effect as that obtained when the optically functional sheet 11, which is provided to cover the front side of the lens 30 of the sunglasses 100, has the optical sheet 10.
[0261] Although the ultraviolet-curable resin composition for nanoimprinting and the optical sheet of the present invention have been described above with reference to the illustrated embodiments, the present invention is not limited thereto, and for example, each part constituting the optical sheet can be replaced with any other component capable of exerting the same function. Also, any other component may be added.
[0262] Furthermore, the optical sheet of the present invention is not limited to being applied to lenses, head-up display devices, and windshields, and can also be applied to, for example, display sections of image display devices such as liquid crystal display devices and organic EL display devices, headlights, solar cells, digital signage, light-transmitting sections (window sections) of vehicles such as automobiles, trains, and airplanes, light-transmitting sections (protective glass) such as lenses and windows of outdoor surveillance cameras (security cameras) and human motion sensors, and window members such as window glass and protective glass of buildings such as houses and buildings. EXAMPLES
[0263] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.
[0264] 1. Preparation of raw materials First, the raw materials used in manufacturing the optical sheet 10 are shown below.
[0265] (Polycarbonate Resin 1) As polycarbonate resin 1, bisphenol A polycarbonate (manufactured by Mitsubishi Engineering Plastics Corporation, "E2000FN") was prepared.
[0266] (Acrylic Monomer 1) As acrylic monomer 1 (monomer component) having a glycol branched chain (number of carbon atoms in the aliphatic chain = 3) as the main chain and having three acryloyl groups as polymerizable groups, glycerin triacrylic monomer (manufactured by Toa Gosei Co., Ltd., "Aronix M-930") was prepared.
[0267] (Acrylic Monomer 2) As acrylic monomer 2 (monomer component) having a straight chain with an ester bond as the main chain and having two acryloyl groups as polymerizable groups, a bifunctional acrylic monomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "A-BPE-4") was prepared.
[0268] (Acrylic Monomer 3) A bifunctional acrylic monomer ("A-HD-N" manufactured by Shin-Nakamura Chemical Co., Ltd.) was prepared as acrylic monomer 3 (monomer component) having a linear glycol chain (number of carbon atoms in the aliphatic chain = 6) as the main chain and two acryloyl groups as polymerizable groups.
[0269] (Acrylic Monomer 4) A polyfunctional acrylic monomer (manufactured by Shin-Etsu Chemical Co., Ltd., "KY-1203") was prepared as acrylic monomer 4 (monomer component) having a branched chain with repeating siloxane bonds (-Si-O-Si-) as the main chain, a fluorinated hydrocarbon group as the side chain, and two or more acryloyl groups as polymerizable groups.
[0270] (Polymerization initiator 1) As polymerization initiator 1, a photoradical polymerization initiator (manufactured by IGM Resins BV, "Omnirad 819") having a maximum peak of absorbance at a wavelength of about 370 nm in its light absorption spectrum was prepared.
[0271] (Polymerization initiator 2) As the polymerization initiator 2, a photoradical polymerization initiator (manufactured by IGM Resins BV, "Omnirad 754") was prepared, which does not have a maximum peak of absorptivity in the light absorption spectrum within a wavelength range of more than 350 nm and not more than 400 nm.
[0272] (Ultraviolet absorber 1) A hydroxyphenylbenzotriazole-based ultraviolet absorber (manufactured by Otsuka Chemical Co., Ltd., "RUVA-93") having a maximum peak of absorbance at a wavelength of about 330 nm in the light absorption spectrum was prepared as the ultraviolet absorber 1. The ultraviolet absorber 1 has a (meth)acryloyl group as a radical polymerizable group.
[0273] (UV absorber 2) As the ultraviolet absorber 2, a hydroxyphenyltriazine ultraviolet absorber (manufactured by BASF Japan, "Tinuvin 400") was prepared, which has a maximum peak of absorbance at a wavelength of about 320 nm in the light absorption spectrum.
[0274] 2. Preparation of UV-curable resin composition for forming anti-reflection layer An ultraviolet-curable resin composition used for forming an anti-reflection layer was prepared by kneading a mixture of 30.0 parts by weight of acrylic monomer 1, 8.0 parts by weight of acrylic monomer 2, 49.6 parts by weight of acrylic monomer 3, 2.4 parts by weight of acrylic monomer 4, 7.0 parts by weight of polymerization initiator 1, and 3.0 parts by weight of ultraviolet absorber 1.
[0275] 3. Preparation of transparent substrates as functional substrates A 0.3 mm-thick transparent substrate (polycarbonate substrate) was prepared as the first substrate 111 by extrusion molding a mixture obtained by kneading an ultraviolet-curable resin composition consisting of 98.0 parts by weight of polycarbonate resin 1 and 2.0 parts by weight of ultraviolet absorber 1.
[0276] 3. Formation of optical sheets Example 1 By forming an optical sheet using a manufacturing apparatus 500 from the previously prepared ultraviolet-curable resin composition and a first substrate 111 (transparent substrate), an optical sheet 10 of Example 1 was obtained, which is composed of a laminate including the first substrate 111 and an anti-reflection layer 12 formed on the upper surface of the first substrate 111.
[0277] The ultraviolet ray irradiation conditions when the ultraviolet ray curable resin composition is irradiated with ultraviolet rays to cure the ultraviolet ray curable resin composition and form the antireflection layer 12 are as follows: light source: UV-LED 365 nm, ultraviolet ray illuminance: 110 mW / cm 2 , UV irradiation amount: 1000mj / cm 2As the mold 840, a moth-eye layer mold (manufactured by INOX, "HT-AR-05A") having needle-shaped recesses (inverted moth-eye structure) with an average peak-to-peak distance (D) of 290 nm, an average height (H) of 300 nm, and an average pitch (P) of 250 nm was used, and the recesses were previously subjected to a release treatment using a fluorine-based surface treatment agent (manufactured by Fluoro Technology, "Fluorosurf NL-2"). The conditions for holding the coating film 600 made of the ultraviolet-curable resin composition and the first substrate 111 between the rotating roller 820 and the mold 840 on the conveying plate 810 were as follows: the lamination pressure by the rotating roller 820 was 0.01 MPa, and the lamination speed was 10 mm / sec.
[0278] In the obtained optical sheet 10, the average thickness of the antireflection layer 12 was 10.0 μm, the average height of the needle-shaped convex portions in the moth-eye structure formed on the surface of the antireflection layer 12 was 300.0 nm, the average pitch between the convex portions was 250.0 nm, and the average distance between the peaks of the convex portions was 290.0 nm. Furthermore, the reaction rate of the polymerization components in the cured product of the ultraviolet-curable resin composition constituting the antireflection layer 12 was 70.0%.
[0279] (Examples 2 to 6, Comparative Example 1) The optical sheets 10 of Examples 2 to 6 and Comparative Example 1 were obtained in the same manner as in Example 1, except that the antireflection layer 12 was formed using an ultraviolet-curable resin composition for forming the antireflection layer, which contained the constituent materials shown in Table 1 in the amounts shown in Table 1.
[0280] 3. Evaluation The optical sheets 10 of the respective examples and comparative examples were evaluated by the following method.
[0281] <1> Measurement of color change of optical sheets (requirement A) For the optical sheets 10 of each of the examples and comparative examples, after irradiating ultraviolet light for 600 hours from the antireflection layer 12 side using a xenon weather meter in accordance with Table 3-A method-cycle No. 3 of JIS K 7350-2, the change in YI defined by JIS K 7373 for the optical sheets 10 was measured, and the optical sheets 10 were evaluated based on the obtained change (ΔYI) as follows.
[0282] [Evaluation Criteria] ◎: ΔYI is 1.5 or less and no change in appearance is observed. ◯: ΔYI is more than 1.5 and less than 3.0, Although some change in appearance was observed, this did not affect the use of the optical sheet 10. ×: ΔYI is 3.0 or more, The change in appearance was clearly observed, making it difficult to use as the optical sheet 10.
[0283] <2> Cross-cut test for optical sheets (requirement B) For each of the optical sheets 10 in the examples and comparative examples, ultraviolet light was irradiated from the antireflection layer 12 side for 600 hours using a xenon weather meter in accordance with Table 3-A method-cycle No. 3 of JIS K 7350-2, and then the adhesion of 100 pieces of the antireflection layer 12 cut into a lattice pattern to the transparent substrate was observed by the cross-cut method specified in JIS K 5600-5-6.
[0284] [Evaluation Criteria] ◎: After 600 hours of irradiation, 95 or more adhesions out of 100 were observed. ○: After 600 hours of irradiation, adhesions of less than 95 / 90 or more / 100 were observed. ×: After 600 hours of irradiation, less than 90 / 100 adhesions were observed.
[0285] <3> Water repellency test for optical sheets (requirement C) First, for each of the optical sheets 10 of the examples and comparative examples, the contact angle E1 [°] of pure water with respect to the surface of the antireflection layer 12 on which the moth-eye structure was formed before irradiation with ultraviolet light was measured.
[0286] Next, the optical sheets 10 of each of the Examples and Comparative Examples were irradiated with ultraviolet light from the antireflection layer 12 side for 600 hours using a xenon weather meter in accordance with JIS K 7350-2, Table 3-A method, cycle No. 3, and then the contact angle E2 [°] of pure water with the surface of the antireflection layer 12 on which the moth-eye structure was formed after the ultraviolet light irradiation was measured. Then, based on the obtained contact angle E2 [°] and (E1-E2) / E1×100 [%] calculated from the contact angle E1 and the contact angle E2, the following evaluation was performed.
[0287] [Evaluation Criteria] ◎: E2≧135°, (E1-E2) / E1×100≦8% are satisfied. ○: 135>E2≧130°, Satisfy 8%<(E1-E2) / E1×100≦10%. ×: E2≧130°, (E1-E2) / E1×100≦10% is not satisfied.
[0288] <4> Reflectance test for optical sheets (requirement D) For each of the optical sheets 10 in the examples and comparative examples, ultraviolet light was irradiated from the antireflection layer 12 side for 600 hours using a xenon weather meter in accordance with Table 3-A method-cycle No. 3 of JIS K 7350-2, and then the reflectance of incident light with a wavelength of 550 nm was measured on the surface of the antireflection layer opposite the transparent substrate, which has a moth-eye structure, and the optical sheets 10 were evaluated based on the obtained reflectance (%) as follows.
[0289] [Evaluation Criteria] ⊚: Reflectance is less than 0.8. ◯: ΔYI is less than 1.0 and 0.8 or more. ×: The reflectance is 1.0% or more.
[0290] The evaluation results of the optical sheets 10 of the examples and comparative examples obtained as described above are shown in Table 1 below.
[0291] [Table 1]
[0292] As shown in Table 1, the optical sheets formed using the ultraviolet-curable resin composition for nanoimprinting of each Example showed results that could be said to satisfy the above-mentioned requirement A and have excellent durability.
[0293] In contrast, it was found that the optical sheet formed using the ultraviolet-curable resin composition for nanoimprints of the comparative example did not satisfy the requirement A, and could not be said to have excellent durability. [Explanation of symbols]
[0294] 10 Optical Sheet 11 Functional Substrates 12 Anti-reflection layer 20 Frames 21 Rim 22 Bridge section 23 Temple Section 24 Nose pad section 30 Lenses 35 Resin layer 100 Sunglasses 111 First board 112 Second board 113 Polarizing Film 114 First adhesive layer 116 Second adhesive layer 117 Half mirror layer 118 Low refractive index layer 119 High refractive index layer 151 Window 300 Automobiles 301 Dashboard 302 Windshield 302a back side 350 Head-Up Display 351 Light source 352 Reflective material 353 Storage unit 400 Windshield 451 Main body 452 Side part 453 Connection section 500 Manufacturing equipment 600 Extrusion Supply Section 610 Storage section 620 Extruder 700 Board transport section 711 Unwinding roller 712 Winding roller 721 Tensioner 722 Tensioner 723 Tensioner 724 Tensioner 800 Moth eye structure formation part 810 First rotating roller 820 Second rotating roller 830 Ultraviolet irradiation means H Driver LS Laser Light
Claims
1. A UV-curable resin composition for nanoimprints, comprising a polymerizable component, a polymerization initiator, and a UV absorber, The ultraviolet absorber has a light absorption peak having a maximum absorptivity peak in a wavelength range of 300 nm or more and 350 nm or less in a light absorption spectrum, The ultraviolet-curable resin composition for nanoimprints, wherein the polymerization initiator has a light absorption peak having a maximum absorptivity within a wavelength range of more than 350 nm and not more than 400 nm in a light absorption spectrum.
2. The polymerizable component comprises a radically polymerizable group, The ultraviolet-curable resin composition for nanoimprints according to claim 1 , wherein the polymerization initiator is a radical polymerization initiator.
3. The ultraviolet ray curable resin composition for nanoimprints according to claim 2 , wherein the ultraviolet ray absorber comprises the radical polymerizable group.
4. The ultraviolet ray curable resin composition for nanoimprints according to claim 3 , wherein the content of the polymerization initiator is 1.0% by weight or more and 8.0% by weight or less.
5. The ultraviolet-curable resin composition for nanoimprints according to claim 4 , wherein the content of the ultraviolet absorbent is from 2.0% by weight to 5.0% by weight.
6. The ultraviolet-curable resin composition for nanoimprints according to claim 2 , wherein the polymerizable component contains a polymerizable group and an aliphatic chain having 6 to 10 carbon atoms in its skeleton.
7. The ultraviolet-curable resin composition for nanoimprints according to claim 2 , wherein the polymerizable component contains a polymerizable group and a fluorinated hydrocarbon group in its skeleton.
8. 2. The ultraviolet-curable resin composition for nanoimprinting according to claim 1, which is used for forming, on a substrate containing a resin material as a main material and the ultraviolet absorber, a coating layer having a fine uneven structure provided by nanoimprinting on a surface opposite to the substrate.
9. 13. An optical sheet comprising: a substrate; and a coating layer having a fine uneven structure formed on a surface opposite to the substrate by nanoimprinting using the ultraviolet-curable resin composition for nanoimprinting according to claim 1.
Citation Information