Aqueous ink, ink cartridge, and inkjet recording method
The inkjet ink formulation with titanium oxide-coated particles and resin, balanced by a specific solvent ratio, addresses the challenges of fixing, hiding, and scratch resistance, ensuring efficient and stable ink ejection for transparent and non-absorbent media.
Patent Information
- Application Number
- JP2024030008
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-11
AI Technical Summary
Existing aqueous inks containing titanium oxide for inkjet recording methods face challenges in achieving both fixing properties, hiding properties, and scratch resistance, with previous solutions either prolonging drying time or compromising ejection characteristics.
The ink formulation includes titanium oxide particles coated with alumina and silica, resin particles, and a specific ratio of water-soluble organic solvent, adhering to the relationships E/T≧0.50 and 0.30≦S/(T+E)≦0.70, to enhance fixing, hiding, and scratch resistance.
The formulation achieves improved fixing properties, hiding properties, and scratch resistance while maintaining stable ejection performance, suitable for transparent and non-absorbent recording media.
Smart Images

Figure 2024144176000014 
Figure 2024144176000015 
Figure 2024144176000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based ink, an ink cartridge, and an ink-jet recording method. [Background technology]
[0002] In recent years, inkjet recording devices have come to be widely used when printing advertisements and exhibits using recording media such as paper and resin film. For example, in order to express clear color images even on transparent recording media, white ink is used in addition to black and basic color inks (hereinafter, these may be collectively referred to as color inks). Specifically, a recording method is used in which white ink is applied in advance to a location on a transparent recording medium including an area where an image is to be recorded to perform base treatment, and color inks are applied on top of that, or each ink is applied in the reverse order (so-called back printing).
[0003] Titanium oxide is widely used as a coloring material for white ink because it is low cost and has excellent properties required for white ink, such as whiteness and hiding power. On the other hand, titanium oxide, which is a metal oxide, has a higher specific gravity than pigments used in inks of basic colors and black. In order to increase the whiteness and hiding power of a printed image, generally, there are two methods that can be considered: increasing the amount of ink applied, and increasing the content of titanium oxide particles in the ink. The former method requires a long drying time, which leads to a decrease in fixation. On the other hand, the latter method requires adjusting the content of water-soluble organic solvents and dispersants in the ink according to the amount of titanium oxide added in order to stably disperse titanium oxide, which has a high specific gravity, and this creates a trade-off with the ejection characteristics.
[0004] In order to shorten the drying time of an image and improve image quality, it has been proposed to adjust the content of the water-soluble organic solvent in the ink and the air volume during drying (see Patent Document 1). Also, an inkjet recording method has been proposed that uses a first ink and a second ink in which the content of the water-soluble organic solvent and the content of the solid matter have been adjusted (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2021-154547 A [Patent Document 2] JP 2017-109485 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present inventors recorded images using the aqueous inks used in the inkjet recording methods described in Patent Documents 1 and 2, and examined various performances. As a result, it was found that both the aqueous inks described in Patent Documents 1 and 2 had insufficient hiding power and abrasion resistance, and there was room for improvement. When the amount of ink applied was increased, the hiding power improved, but the ink took longer to dry, and the fixability decreased. In addition, even if the content of titanium oxide in the ink was increased, the content of water-soluble organic solvent was increased from the viewpoint of ejection characteristics, and the ink took longer to dry, and the fixability also decreased.
[0007] Therefore, an object of the present inventors is to provide an aqueous inkjet ink containing titanium oxide, which is capable of achieving both fixing property, hiding property, and abrasion resistance, an ink cartridge using the aqueous ink, and an inkjet recording method. [Means for solving the problem]
[0008] The above object can be achieved by the present invention, which is described below. That is, the aqueous ink according to the present invention is an aqueous ink for inkjet recording, which contains titanium oxide particles, resin particles, and a water-soluble organic solvent, and is characterized in that the titanium oxide particles are titanium oxide having at least a portion of their surface covered with alumina and silica, and the content (T (% by mass)) of the titanium oxide particles, the content (E (% by mass)) of the resin particles, and the content (S (% by mass)) of the water-soluble organic solvent in the aqueous ink satisfy the relationships of the following formulas (1) and (2). E / T≧0.50 (1) 0.30≦S / (T+E)≦0.70 (2) Effect of the Invention
[0009] According to the present invention, it is possible to provide an aqueous inkjet ink containing titanium oxide, which is capable of achieving both fixing property, hiding property, and abrasion resistance, an ink cartridge using the aqueous ink, and an inkjet recording method. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view illustrating an embodiment of an ink cartridge of the present invention. [Diagram 2] 1A and 1B are diagrams illustrating an example of an inkjet recording apparatus used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording apparatus, and (b) is a perspective view of a head cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt". Titanium oxide and titanium oxide particles may be simply referred to as "pigment". Furthermore, water-based ink for inkjet printing may be simply referred to as "ink". Physical property values are values at room temperature (25°C) unless otherwise specified. Furthermore, since the ink of the present invention is a water-based ink containing water, its specific gravity is set to 1.00 g / mL for convenience.
[0012] As described above, in order to improve the whiteness and hiding power of an image, it is possible to increase the amount of ink applied or the content of titanium oxide, but both methods have problems. Even when the aqueous ink used in the inkjet recording method described in Patent Document 1 and Patent Document 2 is used, the above problems could not be solved. The present inventors have investigated a method for efficiently improving hiding power by a method other than adjusting the amount of ink applied. As a result, they have found that it is important not only to simply increase the content of titanium oxide in the ink, but also to adjust the ratio of titanium oxide to particulate components such as resin particles.
[0013] That is, the ink of the present invention has the following characteristics. First, titanium oxide particles are used, which are titanium oxide having at least a portion of their surface coated with alumina and silica. The ink further contains resin particles. The content of titanium oxide particles (T (mass %)), the content of resin particles (E (mass %)), and the content of water-soluble organic solvent (S (mass %)) in the ink satisfy the relationships of the following formulas (1) and (2). The present inventors speculate as follows about the mechanism by which the above configuration enables the ink to achieve both fixability, hiding power, and abrasion resistance. E / T≧0.50 (1) 0.30≦S / (T+E)≦0.70 (2)
[0014] The ink contains resin particles in addition to titanium oxide particles. By using an ink containing resin particles, an image with excellent abrasion resistance can be obtained. The above formulas (1) and (2) must be satisfied. Formula (1) means that the content (mass%) of resin particles in the ink is 0.50 or more times the mass ratio of the content (mass%) of titanium oxide particles. Formula (2) means that the content (mass%) of water-soluble organic solvent in the ink is 0.30 or more and 0.70 or less times the mass ratio of the content (mass%) of titanium oxide particles and resin particles.
[0015] By making the content of the resin particles 0.50 times or more as a mass ratio to the content of the titanium oxide particles, the resin particles are likely to enter the gaps during the aggregation of the titanium oxide particles. As a result, light scattering is likely to occur. In order for an image to be recognized as white, sufficient light scattering is required, and the concealing property of the image is improved by making the light scattering more likely to occur. If the mass ratio is less than 0.50 times, the resin particles are too few, the light scattering is insufficient, and the concealing property of the image is not obtained. In addition, the resin particles are unlikely to be uniformly present throughout the pigment layer formed, and the scratch resistance of the image is not obtained.
[0016] Formula (2) is the relationship between the content of the water-soluble organic solvent and the titanium oxide particles or resin particles, that is, the particulate components. By setting it within the above range, fixation, hiding, and abrasion resistance can be achieved simultaneously. If S / (T+E) is less than 0.30 times, the amount of water-soluble organic solvent is too small relative to the particulate components, and the dispersion state of the particulate components is likely to become unstable due to evaporation of the liquid components in the ink in the recording head. As a result, titanium oxide aggregates in the recording head, the ejection performance is reduced, and the titanium oxide particles present in a dispersed state in the ink are reduced. Therefore, the hiding property of the image cannot be obtained. On the other hand, if S / (T+E) is more than 0.70 times, the content of the water-soluble organic solvent is too high, and hiding and fixation properties cannot be obtained.
[0017] <Water-based ink> The ink of the present invention is an aqueous ink for inkjet printing, containing titanium oxide coated with a specific inorganic oxide, resin particles, and a water-soluble organic solvent in a specific ratio. This ink is preferably a white ink, since titanium oxide is a white pigment. The components constituting the ink of the present invention and the physical properties of the ink are described in detail below.
[0018] (Colorant) The ink contains titanium oxide particles as a coloring material (pigment) in which titanium oxide has been surface-treated with a specific inorganic oxide. In other words, the ink contains titanium oxide particles, which are titanium oxide whose surfaces are coated with a specific inorganic oxide. The content (mass%) of titanium oxide particles in the ink is preferably 0.10% by mass or more and 20.00% by mass or less, based on the total mass of the ink. The content (mass%) of titanium oxide particles in the ink is more preferably 1.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. In particular, the content (mass%) of titanium oxide particles in the ink is particularly preferably 10.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. If the content of titanium oxide particles is less than 10.00% by mass, the concealment of the image may not be sufficient. On the other hand, if the content of titanium oxide particles is more than 20.00% by mass, it is necessary to increase the amount of resin particles added to impart abrasion resistance, which may affect the ejection properties of the ink. As a result, the image may not be concealed sufficiently.
[0019] Titanium oxide is a white pigment, and has three crystal forms: rutile, anatase, and brookite. Among them, rutile titanium oxide is preferred. Titanium oxide can be industrially produced by the sulfuric acid method and the chlorine method, and the titanium oxide used in the present invention may be produced by either method.
[0020] The volume-based cumulative 50% particle diameter (hereinafter also referred to as the average particle diameter) of the titanium oxide particles is preferably 200 nm or more and 500 nm or less. In particular, the volume-based cumulative 50% particle diameter of the titanium oxide particles is more preferably 200 nm or more and 400 nm or less. The volume-based cumulative 50% particle diameter of the titanium oxide particles (D 50 ) is the diameter of the particle that is 50% of the total volume of the measured particles in the particle size accumulation curve, calculated from the small particle size side. 50 can be measured under the following conditions: SetZero: 30 seconds, number of measurements: 3, measurement time: 180 seconds, shape: aspheric, refractive index: 2.60. A particle size analyzer using a dynamic light scattering method can be used as the particle size distribution measuring device. Of course, the measurement conditions are not limited to those described above.
[0021] Titanium oxide that has been surface-treated with alumina and silica is used. The surface treatment is expected to suppress photocatalytic activity and improve dispersibility. In this specification, "alumina" is a general term for oxides of aluminum such as aluminum oxide. In this specification, "silica" is a general term for silicon dioxide or a substance composed of silicon dioxide. Most of the alumina and silica that coat titanium oxide are present in the form of silicon dioxide and aluminum oxide.
[0022] The proportion (mass%) of titanium oxide in the titanium oxide particles is preferably 90.00 mass% or more based on the total mass of the titanium oxide particles, and the proportion (mass%) of titanium oxide in the titanium oxide particles is preferably 98.50 mass% or less based on the total mass of the titanium oxide particles.
[0023] The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.50 to 1.00 times the ratio (mass%) of silica in terms of mass ratio. The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.50 to 4.00 mass% based on the total mass of the titanium oxide particles. In particular, the ratio (mass%) of alumina in the titanium oxide particles is more preferably 1.00 to 4.00 mass% based on the total mass of the titanium oxide particles.
[0024] The proportion (mass%) of silica in titanium oxide particles is preferably 1.00 mass% or more and 4.00 mass% or less based on the total mass of titanium oxide particles. By setting the proportion of silica in the above range, electrostatic repulsion of negative charges due to surface hydroxyl groups derived from silica can be obtained. Furthermore, even when a silane compound described later is used, the reactivity with the silane compound can be appropriately adjusted, and the aggregation of titanium oxide particles can be further suppressed.
[0025] The ratio of alumina and silica in titanium oxide particles, i.e., the amount of alumina and silica coating, can be measured by, for example, quantitative analysis of aluminum and silicon elements by inductively coupled plasma (ICP) emission spectrometry. In this case, it is assumed that all atoms coated on the surface are oxides, and the obtained values of aluminum and silicon can be calculated by converting them to their oxides, i.e., alumina and silica. The ratio (mass%) of aluminum element in titanium oxide particles obtained by inductively coupled plasma emission spectrometry is preferably 0.57 times or more and 1.13 times or less in mass ratio to the ratio (mass%) of silicon element. When this value is converted to its oxides, i.e., alumina and silica, the ratio (mass%) of alumina in titanium oxide particles is 0.50 times or more and 1.00 times or less in mass ratio to the ratio (mass%) of silica.
[0026] As described above, the titanium oxide particles are surface-treated with alumina and silica. Of these, it is preferable that the titanium oxide particles are dispersed at least by the action of silica. The surface charge state of titanium oxide particles, which are titanium oxide coated with alumina and silica, changes depending on the pH of the ink. In the pH range normally used for ink, the surface hydroxyl groups derived from silica are negatively charged. Therefore, even if titanium oxide particles approach each other, aggregation can be suppressed by electrostatic repulsion, and they can be stably dispersed. In the case of an ink containing 0.01% by mass or more of a water-soluble resin other than polyacrylic acid, which will be described later, the dispersion due to the action of silica is destabilized. As a result, the fixation of the image may not be sufficient.
[0027] Surface treatment methods for titanium oxide include wet treatment and dry treatment. For example, titanium oxide can be dispersed in a liquid medium and then reacted with a surface treatment agent such as sodium aluminate or sodium silicate to perform surface treatment, and the desired characteristics can be achieved by appropriately changing the ratio of these surface treatment agents. In addition to alumina and silica, inorganic oxides such as zinc oxide and zirconia, and organic substances such as polyols can also be used for surface treatment, as long as the effects of the present invention are not impaired.
[0028] As long as the effect of the present invention is not impaired, the ink may contain other pigments besides titanium oxide. In this case, the ink may be of a color other than white ink. The content (mass %) of the other pigments in the ink is preferably 0.10 mass % or more and 5.00 mass % or less, and more preferably 0.10 mass % or more and 1.00 mass % or less, based on the total mass of the ink.
[0029] (Resin particles) The ink contains resin particles. The resin particles refer to particles formed from resin, and are roughly divided into (i) resin particles formed from resins such as acrylic resins, urethane resins, olefin resins, and polyester resins, and (ii) wax particles. Wax particles will be described in detail later, and resin particles other than wax particles will be described here. Resin particles are components that are fixed on a recording medium to form a coating, and can increase the adhesion between the recording medium and the image, as well as impart physical strength such as abrasion resistance to the image. In addition, when the ink contains wax particles as resin particles, the wax particles remain on the surface of the recording medium, and can impart slipperiness, thereby improving the abrasion resistance of the image. The resin particles do not need to contain a coloring material. The term "resin particles" refers to a resin that exists in a state in which it is not dissolved in the aqueous medium in the ink, and more specifically, refers to a resin that can exist in the aqueous medium in a state in which it forms particles whose particle diameter can be measured by a dynamic light scattering method. In contrast, the term "water-soluble resin" refers to a resin that exists in a state in which it is dissolved in the aqueous medium in the ink.
[0030] In this specification, "a resin is water-soluble" means that when the resin is neutralized with an alkali equivalent to the acid value, the resin is present in an aqueous medium in a state in which it does not form particles whose particle size can be measured by a dynamic light scattering method. Whether or not a resin is water-soluble can be determined according to the following method. First, a liquid (resin solid content: 10 mass%) containing a resin neutralized with an alkali (sodium hydroxide, potassium hydroxide, etc.) equivalent to the acid value is prepared. Next, the prepared liquid is diluted 10 times (volume basis) with pure water to prepare a sample solution. Then, when the particle size of the resin in the sample solution is measured by a dynamic light scattering method, if particles having a particle size are not measured, the resin can be determined to be water-soluble. The measurement conditions at this time can be, for example, SetZero: 30 seconds, number of measurements: 3 times, and measurement time: 180 seconds. As a particle size distribution measurement device, a particle size analyzer using a dynamic light scattering method (for example, the product name "UPA-EX150", manufactured by Nikkiso) can be used. Of course, the particle size distribution measurement device and measurement conditions used are not limited to those described above.
[0031] Among the resin particles, the acid value of the resin particles of (i) above is preferably 0 mgKOH / g or more and 50 mgKOH / g or less. The weight average molecular weight of the resin constituting the resin particles is preferably 1,000 or more and 3,000,000 or less, more preferably 100,000 or more and 3,000,000 or less. The weight average molecular weight of the resin is a polystyrene-equivalent value measured by gel permeation chromatography (GPC). Among the resin particles, the cumulative 50% particle size on a volume basis of the resin particles of (i) above is preferably 50 nm or more and 500 nm or less, more preferably 100 nm or more and 300 nm or less.
[0032] The content (mass%) of the resin particles in the ink is preferably 0.10% by mass or more and 30.00% by mass or less, and more preferably 5.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. The content (mass%) of the resin particles in the ink must be 0.50 times or more in mass ratio to the content (mass%) of the titanium oxide particles. The mass ratio is preferably 1.50 times or less.
[0033] As shown in formula (1), the content (mass%) of resin particles in the aqueous ink must be 0.50 or more times the content (mass%) of titanium oxide particles. In particular, the mass ratio is preferably 0.70 or more and more preferably 0.95 or less. As shown in formula (2), the content (mass%) of water-soluble organic solvent in the aqueous ink must be 0.30 or more and 0.70 or less times the content (mass%) of titanium oxide particles and resin particles. In particular, the mass ratio is preferably 0.40 or more and 0.60 or less.
[0034] Examples of the resin constituting the resin particles include acrylic resins, urethane resins, olefin resins, and polyester resins. Among these, acrylic resins are preferred. In other words, the resin particles are preferably resin particles formed of acrylic resins.
[0035] [Acrylic resin] The acrylic resin preferably has a hydrophilic unit and a hydrophobic unit as constituent units. Among them, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one of a monomer having an aromatic ring and a (meth)acrylic acid ester monomer is preferred. In particular, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one of a monomer of styrene and α-methylstyrene is preferred.
[0036] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group. The hydrophilic unit can be formed, for example, by polymerizing a hydrophilic monomer having a hydrophilic group. Specific examples of the hydrophilic monomer having a hydrophilic group include acidic monomers having a carboxylic acid group such as (meth)acrylic acid, itaconic acid, maleic acid, and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. Examples of cations constituting the salts of acidic monomers include ions of lithium, sodium, potassium, ammonium, and organic ammonium.
[0037] The hydrophobic unit is a unit that does not have a hydrophilic group such as an anionic group. The hydrophobic unit can be formed, for example, by polymerizing a hydrophobic monomer that does not have a hydrophilic group such as an anionic group. Specific examples of the hydrophobic monomer include monomers having an aromatic ring such as styrene, α-methylstyrene, and benzyl (meth)acrylate; and (meth)acrylic acid ester monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0038] [Urethane resin] The urethane resin can be obtained, for example, by reacting polyisocyanate with polyol. In addition, it may be obtained by further reacting a chain extender. Examples of the olefin resin include polyethylene and polypropylene. A part of the olefin resin can be used as wax particles. Examples of the olefin resin include polyethylene wax and polypropylene wax having a low molecular weight (a molecular weight of tens of thousands or less).
[0039] [Method of manufacturing resin particles] The resin particles can be produced by a conventional method such as emulsion polymerization, mini-emulsion polymerization, seed polymerization, or phase inversion emulsification. Among these, emulsion polymerization and seed polymerization are preferred because they can produce resin particles with a more uniform particle size. By using resin particles with a more uniform particle size, the ejection properties of the ink by the inkjet method can be further improved.
[0040] (wax particles) The ink may contain particles formed of wax (wax particles) as resin particles. By using an ink containing wax particles, slipperiness is imparted to the surface of a recording medium, and an image with improved abrasion resistance can be recorded. The wax may be a composition containing components other than wax, or may be wax itself. The wax particles may be dispersed by a dispersant such as a surfactant or a water-soluble resin.
[0041] The content (mass%) of wax particles in the ink is preferably 0.80% by mass or more and 5.00% by mass or less, more preferably 0.80% by mass or more and 3.00% by mass or less, based on the total mass of the ink. If the content of wax particles is less than 0.80% by mass, the wax particles are too few, and sufficient abrasion resistance may not be obtained. On the other hand, if the content of wax particles is more than 5.00% by mass, the wax particles are too many, which is thought to suppress the aggregation of resin particles and reduce the strength of the recorded image. As a result, sufficient abrasion resistance may not be obtained. In this specification, the content of wax particles is treated as the total content of wax and dispersant for dispersing wax.
[0042] The ratio (mass%) of wax particles to resin particles in the ink is preferably 0.09 times or more and 0.30 times or less, and more preferably 0.15 times or more and 0.25 times or less. If the ratio of wax particles is less than 0.09 times, the wax particles may be buried in the film of the resin particles, making it difficult to improve the abrasion resistance. As a result, sufficient abrasion resistance may not be obtained. If the ratio of wax particles is more than 0.30 times, the wax particles are likely to be mixed between the resin particles, making it difficult for the resin particles to aggregate. As a result, the strength of the image may decrease, and sufficient abrasion resistance may not be obtained.
[0043] The cumulative 50% particle size of titanium oxide particles based on volume (D T (nm)), and the volume-based cumulative 50% particle size of the resin particles (D E (nm)), and the cumulative 50% particle size of the wax particles based on volume (D W(nm)) preferably satisfies the relationship of the following formulas (3) and (4). As shown in formula (3), by making the cumulative 50% particle diameter based on volume of the wax particles equal to or greater than the cumulative 50% particle diameter based on volume of the resin particles, the wax particles can be easily exposed to the surface of the image. Therefore, the effect of the scratch resistance can be efficiently improved with a small amount of wax particles added. Also, as shown in formula (4), by making the cumulative 50% particle diameter based on volume of the titanium oxide particles equal to or greater than twice the cumulative 50% particle diameter based on volume of the resin particles, the resin particles can fill the spaces between the titanium oxide particles on the surface of the recording medium without any gaps. Therefore, the strength of the recorded image can be improved, and the scratch resistance is further improved. D W ≧D E (3) D T ≧2×D E (4)
[0044] Furthermore, the volume-based cumulative 50% particle diameter of the titanium oxide particles is preferably equal to or larger than the volume-based cumulative 50% particle diameter of the wax particles. T (nm)), and the volume-based cumulative 50% particle size of the resin particles (D E (nm)), and the cumulative 50% particle size of the wax particles based on volume (D W It is preferable that the particle diameter (nm) satisfies the relationship of the above formula (4) and the following formula (5). The volume-based cumulative 50% particle diameter of the wax particles is preferably 100 nm or more and 200 nm or less. D T ≧D W ≧D E (5)
[0045] In the narrow sense, wax is an ester of a water-insoluble higher monohydric or dihydric alcohol and a fatty acid, and includes animal waxes and vegetable waxes, but does not include oils and fats. In the broad sense, wax includes high melting point fats, mineral waxes, petroleum waxes, and blends and modified products of various waxes. In the present invention, any wax in the broad sense can be used without particular restrictions. Wax in the broad sense can be classified into natural waxes, synthetic waxes, blends thereof (blended waxes), and modified products thereof (modified waxes).
[0046] Examples of natural waxes include animal waxes such as beeswax, spermaceti, and wool wax (lanolin); vegetable waxes such as wood wax, carnauba wax, sugarcane wax, palm wax, candelilla wax, and rice wax; mineral waxes such as montan wax; and petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum. Examples of synthetic waxes include hydrocarbon waxes such as Fischer-Tropsch wax and polyolefin wax (e.g., polyethylene wax and polypropylene wax). The blended wax is a mixture of the above-mentioned various waxes. The modified wax is a wax obtained by subjecting the above-mentioned various waxes to a modification treatment such as oxidation, hydrogenation, alcohol modification, acrylic modification, and urethane modification. The wax is preferably at least one selected from the group consisting of microcrystalline wax, Fischer-Tropsch wax, polyolefin wax, paraffin wax, and modified or blended products thereof. Among them, a blend of multiple types of wax is more preferable, and a blend of petroleum wax and synthetic wax is particularly preferable.
[0047] The wax is preferably solid at room temperature (25°C). The melting point (°C) of the wax is preferably 40°C or more and 120°C or less, more preferably 50°C or more and 100°C or less. The melting point of the wax can be measured in accordance with the test method described in 5.3.1 (melting point test method) of JIS K2235:1991 (petroleum wax). In the case of microcrystalline wax, petrolatum, and a mixture of multiple types of wax, the test method described in 5.3.2 can be used to measure more accurately. The melting point of the wax is easily affected by characteristics such as molecular weight (the higher the molecular weight, the higher the melting point), molecular structure (the higher the melting point if it is linear, and the lower the melting point if it is branched), crystallinity (the higher the crystallinity, the higher the melting point), and density (the higher the crystallinity, the higher the melting point). Therefore, by controlling these characteristics, a wax having a desired melting point can be obtained.
[0048] (Compound represented by general formula (1)) The titanium oxide particles in the ink are preferably dispersed at least by the action of silica. Furthermore, the dispersion is also assisted by polyacrylic acid, which can be suitably added to the ink. In addition to these, a component that assists the dispersion of the titanium oxide particles may be contained. Among them, the ink preferably further contains a compound represented by the following general formula (1). By containing the following compound, ejection failure can be further suppressed, and as a result, the concealment of the image can be further improved. The content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.01 mass% or more and 1.00 mass% or less, and more preferably 0.02 mass% or more and 0.50 mass% or less, based on the total mass of the ink. Furthermore, the content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.002 times or more and 0.10 times or less in terms of mass ratio to the content (mass%) of the titanium oxide particles.
[0049] A part of OR1 bonded to silicon atoms in the compound represented by general formula (1) is hydrolyzed in an aqueous medium to form a silanol group. Therefore, it has affinity with the surface hydroxyl groups derived from silica on the titanium oxide particle surface. In addition to the structure capable of forming a silanol group as described above, the compound represented by general formula (1) also has a structure having n alkylene oxide groups having 2 to 4 carbon atoms as repeating units ((OR4) in general formula (1)) via X, which serves as a linking group. n ) Hereinafter, the above structure will also be referred to as an alkylene oxide chain. Since the alkylene oxide chain is hydrophilic, it extends appropriately in an aqueous medium and exhibits a repulsive force due to steric hindrance. Therefore, the compound represented by general formula (1) has the effect of assisting the dispersion of titanium oxide particles.
[0050] [ka]
[0051] (In general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Each R4 is independently an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)
[0052] In the general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, and an n-butyl group. Among them, a methyl group is preferable from the viewpoint of ease of hydrolysis. If R1, R2, and R3 are each an alkyl group having more than 4 carbon atoms, it becomes difficult to form a silanol group by hydrolysis, and affinity with titanium oxide particles is not obtained. Therefore, titanium oxide particles cannot be stably dispersed, and ink ejection properties are not sufficient. As a result, the concealment properties of the image may not be sufficient. a, which represents the number of R1O, is 1 to 3, and b, which represents the number of R2, is 0 to 2, and a+b=3. Among them, it is preferable that a is 3 and b is 0, that is, all three substituents of the silicon atom are R1O.
[0053] In the general formula (1), R4 is independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include an ethylene group, an n-propylene group, an i-propylene group, and an n-butylene group. Among them, an ethylene group is preferable. The number of OR4, that is, n (average value) representing the number of alkylene oxide groups, is 6 to 24. When n is less than 6, the length of the alkylene oxide chain is too short, and the repulsive force due to steric hindrance is not sufficiently obtained, so that the ink ejection property is not sufficiently obtained, and as a result, the concealment property of the image may not be sufficiently obtained. When n is more than 24, the length of the alkylene oxide chain is too long, and the hydrophilicity increases and the compound is easily liberated in the aqueous medium. Therefore, the affinity with the surface hydroxyl group of the titanium oxide particles is not sufficiently obtained, and the aggregation of the titanium oxide particles may be difficult to efficiently suppress. Therefore, the ink ejection property is not sufficiently obtained, and as a result, the concealment property of the image may not be sufficiently obtained.
[0054] In the general formula (1), X is a single bond or an alkylene group having 1 to 6 carbon atoms. When X is a single bond, it means that the silicon atom and OR4 are directly bonded. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an i-propylene group, an n-butylene group, an n-pentylene group, and an n-hexylene group. Among them, an n-propylene group is preferable. When X is an alkylene group having more than 6 carbon atoms, the hydrophobicity of the compound represented by the general formula (1) becomes too high, and the effect of stably dispersing the titanium oxide particles is weak, and the ink ejection property may not be sufficiently obtained. As a result, the concealment property of the image may not be sufficiently obtained.
[0055] The compound represented by general formula (1) is preferably a compound represented by the following general formula (2). The compound represented by general formula (2) has three OR1s bonded to silicon atoms, and therefore a portion of the compound can be hydrolyzed in an aqueous medium to form three hydroxyl groups bonded to silicon atoms, thereby increasing the portion having affinity with titanium oxide particles. In addition, the compound represented by the following general formula (2) has a repeating structure of ethylene oxide groups. Therefore, the ethylene oxide chains can be appropriately extended in an aqueous medium, and a repulsive force due to steric hindrance can be obtained.
[0056] [ka]
[0057] (In general formula (2), R1 and R3 each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. m is an integer of 8 to 24.)
[0058] (Polyacrylic acid) The ink may contain polyacrylic acid. The content (mass%) of polyacrylic acid in the ink is preferably 0.01% by mass or more and 0.50% by mass or less, more preferably 0.01% by mass or more and 0.20% by mass or less, based on the total mass of the ink. Polyacrylic acid can assist the dispersion of titanium oxide particles. Polyacrylic acid is a compound having a repeating unit in which hydrogen atoms of a hydrocarbon chain are replaced with carboxylic acid groups at every other carbon atom constituting the hydrocarbon chain. Some of the carboxylic acid groups in polyacrylic acid are negatively charged due to the promotion of ionization by the presence of monovalent cations in the ink. On the other hand, the surface hydroxyl groups derived from alumina of the titanium oxide particles are positively charged, and polyacrylic acid can be adsorbed to the surface of the titanium oxide particles via the surface hydroxyl groups derived from alumina. The titanium oxide particles to which polyacrylic acid is adsorbed are negatively charged due to the carboxylic acid groups in polyacrylic acid in addition to the surface hydroxyl groups derived from silica, and therefore the electrostatic repulsive force between titanium oxide particles can be further strengthened, and the titanium oxide particles can be stably dispersed. Furthermore, even if the distance between titanium oxide particles becomes closer due to settling or drying on a recording medium, the presence of polyacrylic acid can suppress the particles from approaching each other beyond a certain level, that is, polyacrylic acid functions as a spacer. If the content of polyacrylic acid is less than 0.01% by mass, the amount of polyacrylic acid is too small to obtain the above effects sufficiently, and the dispersion stability is not improved. As a result, the ejection properties are not sufficient, and the concealment properties of the image may not be sufficient. If the content of polyacrylic acid is more than 0.50% by mass, an excess amount of polyacrylic acid that is more than the amount that is adsorbed to the titanium oxide particles and functions as a spacer tends to exist in a free state in the ink. As a result, salting out is likely to occur, and the titanium oxide particles are aggregated, so that the dispersion stability is not sufficient. Therefore, the ejection properties are not sufficient, and the concealment properties of the image may not be sufficient.
[0059] Polyacrylic acid may be suitably used whether it is a commercially available product or a synthesized compound. Any known synthesis method may be used as a method for synthesizing polyacrylic acid. For example, polyacrylic acid can be synthesized by polymerization of acrylic acid. The carboxylic acid group of polyacrylic acid may be in an acid form or a salt form. In the case of a salt form, salts of alkali metals such as lithium, sodium, potassium, and (organic) ammonium can be mentioned. From the viewpoint of storage stability of the ink, it is preferable that polyacrylic acid is in an alkali metal salt form.
[0060] The weight-average molecular weight of polyacrylic acid is preferably 2,000 or more and 6,000 or less. If the weight-average molecular weight of polyacrylic acid is less than 2,000, even if polyacrylic acid is adsorbed to titanium oxide particles, the molecular size is too small to play the role of a spacer that suppresses the approach of titanium oxide particles, and does not lead to improvement of dispersion stability. Therefore, the concealment of the image may not be sufficient. If the weight-average molecular weight of polyacrylic acid is more than 6,000, the molecular size of polyacrylic acid is too large, and the carboxylic acid group is adsorbed to the surface of multiple titanium oxide particles, and multiple titanium oxide particles are crosslinked with polyacrylic acid. As a result, the dispersion stability may not be sufficient, and the concealment of the image may not be sufficient.
[0061] The content (mass%) of polyacrylic acid is preferably 0.001 times or more in terms of the mass ratio to the content (mass%) of titanium oxide particles. The content (mass%) of polyacrylic acid is preferably 0.010 times or less in terms of the mass ratio to the content (mass%) of titanium oxide particles. If the mass ratio is less than 0.001 times, the amount of polyacrylic acid is too small relative to the titanium oxide particles, and the function of assisting the dispersion of titanium oxide particles cannot be fully exerted. As a result, the dispersion stability is not sufficiently obtained, and the concealment of the image may not be sufficiently obtained. On the other hand, if the mass ratio is more than 0.010 times, there is more polyacrylic acid than can be adsorbed by the titanium oxide particles, so that a part of the polyacrylic acid is likely to exist in a free state in the ink. As a result, salting out is likely to occur, which causes aggregation of titanium oxide particles and tends to reduce the dispersion stability, and therefore the concealment of the image may not be sufficiently obtained.
[0062] (Other resins) The ink may contain resins other than the resin particles (other resins). Examples of other resins include acrylic resins, urethane resins, and urea resins. Of these, acrylic resins are preferred. The content (mass%) of other resins in the ink is preferably 1.00% by mass or more and 25.00% by mass or less, and more preferably 3.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink. Of these, it is particularly preferred that the content is 5.00% by mass or more and 15.00% by mass or less.
[0063] Other resins can be contained in the ink for the purpose of improving various properties of the recorded image. Examples of the form of the other resin include block copolymers, random copolymers, graft copolymers, and combinations thereof.
[0064] The acid value of the other resin (water-soluble resin) is preferably 80 mgKOH / g or more and 250 mgKOH / g or less, more preferably 100 mgKOH / g or more and 200 mgKOH / g or less. The weight average molecular weight of the other resin is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the other resin is a value measured by gel permeation chromatography (GPC) in terms of polystyrene.
[0065] (aqueous medium) The ink is an aqueous ink containing water and a water-soluble organic solvent as an aqueous medium. As the water, deionized water (ion-exchanged water) is preferably used. The content (mass %) of water in the ink is preferably 50.00 mass % or more and 95.00 mass % or less based on the total mass of the ink.
[0066] The water-soluble organic solvent is not particularly limited as long as it is water-soluble (preferably, dissolves in water at any ratio at 25°C). Specifically, monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds, sulfur-containing polar compounds, etc. can be used. Among them, it is preferable to use alkanediols and alkylene glycols that are liquid at 25°C. The shorter the carbon chain of the water-soluble resin, the easier it is to dry, while the longer the carbon chain, the more preferable it is from the viewpoint of forming a film of the resin particles. Therefore, among alkanediols, 1,2-alkanediol is more preferable, and 1,2-butanediol and 1,2-pentanediol are particularly preferable. Furthermore, among alkylene glycols, ethylene glycol, diethylene glycol, triethylene glycol, and propylene glycol are more preferable, and propylene glycol is particularly preferable. In other words, it is preferable that the water-soluble organic solvent contains at least one selected from the group consisting of 1,2-butanediol, 1,2-pentanediol, and propylene glycol. By using these water-soluble organic solvents, the fixability of the image can be further improved.
[0067] The content (mass%) of the water-soluble organic solvent in the ink is preferably 3.00% by mass or more and 50.00% by mass or less, and more preferably 10.00% by mass or more and 40.00% by mass or less, based on the total mass of the ink. If the content (mass%) of the water-soluble organic solvent is less than 3.00% by mass, the ink may stick inside the inkjet recording device, and sufficient sticking resistance may not be obtained. If the content (mass%) of the water-soluble organic solvent is more than 50.00% by mass, poor ink supply may occur. The water-soluble organic solvent does not include "surfactants."
[0068] (Other additives) In addition to the above additives, the ink may contain various additives such as surfactants, pH adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters, and chelating agents, as necessary. Among these, it is preferable that the ink contains a surfactant. The content (mass%) of the surfactant in the ink is preferably 0.10% by mass or more and 5.00% by mass or less, and more preferably 0.10% by mass or more and 2.00% by mass or less, based on the total mass of the ink. Examples of surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants. Among these, nonionic surfactants are preferable because they have low affinity with titanium oxide particles and are effective in small amounts, since they are used to adjust various physical properties of the ink.
[0069] (Ink properties) Since the ink is applied to the inkjet method, it is preferable to appropriately control the physical properties of the ink. The surface tension of the ink at 25°C is preferably 10 mN / m or more and 60 mN / m or less, and more preferably 20 mN / m or more and 40 mN / m or less. The surface tension of the ink can be adjusted by appropriately determining the type and content of the surfactant in the ink. In addition, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.0 or less. The pH of the ink can be measured with a general pH meter equipped with a glass electrode or the like.
[0070] <Ink cartridges> The ink cartridge of the present invention includes ink and an ink storage section that stores the ink. The ink stored in the ink storage section is the water-based ink (white ink) of the present invention described above. FIG. 1 is a cross-sectional view that shows a schematic diagram of an embodiment of the ink cartridge of the present invention. As shown in FIG. 1, an ink supply port 12 for supplying ink to a recording head is provided on the bottom surface of the ink cartridge. The inside of the ink cartridge serves as an ink storage section for storing ink. The ink storage section is composed of an ink storage chamber 14 and an absorber storage chamber 16, which are communicated with each other via a communication port 18. The absorber storage chamber 16 is also communicated with the ink supply port 12. The ink storage chamber 14 stores liquid ink 20, and the absorber storage chamber 16 stores absorbers 22 and 24 that hold the ink in an impregnated state. The ink storage section may not have an ink storage chamber that stores liquid ink, and may be in a form in which the entire amount of ink stored is held by the absorber. The ink containing section may also be of a type that does not have an absorber and contains the entire amount of ink in a liquid state.Furthermore, the ink cartridge may be of a type that is configured to have an ink containing section and a recording head.
[0071] <Inkjet recording method> The inkjet recording method of the present invention is a method of discharging the above-described aqueous ink of the present invention from an inkjet recording head to record an image on a recording medium. Examples of the method of discharging the ink include a method of imparting mechanical energy to the ink and a method of imparting thermal energy to the ink. In the present invention, it is particularly preferable to adopt a method of discharging the ink by imparting thermal energy to the ink. Other than using the ink of the present invention, the steps of the inkjet recording method may be publicly known. For example, when recording an image using white ink, a general inkjet recording method may be applied as it is. In addition, when using white ink as a base treatment for color inks, an image may be recorded by applying color inks (inks such as black, cyan, magenta, and yellow) so as to overlap at least a part of the area to which the white ink has been applied.
[0072] Furthermore, it can also be used for back printing, in which white ink is applied so as to overlap at least a part of the area where color inks are applied. The recording medium is not particularly limited, but since the water-based ink of the present invention can be used as a white ink, it is preferable to use a transparent or colored recording medium. In addition, the recording medium may be a poorly absorbing medium (non-absorbing medium) that has low absorbency of the liquid medium, such as a resin film.
[0073] FIG. 2 is a diagram showing an example of an inkjet recording device used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording device, and (b) is a perspective view of a head cartridge. The inkjet recording device is provided with a conveying means (not shown) for conveying a recording medium 32, and a carriage shaft 34. A head cartridge 36 can be mounted on the carriage shaft 34. The head cartridge 36 includes recording heads 38 and 40, and is configured so that an ink cartridge 42 is set thereon. While the head cartridge 36 is conveyed in the main scanning direction along the carriage shaft 34, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, an image is recorded on the recording medium 32 by conveying the recording medium 32 in the sub-scanning direction by a conveying means (not shown).
[0074] Multi-pass printing is preferred in which the application of ink to a unit area of a print medium is performed by multiple relative scans of the print head and the print medium. In particular, it is preferred to apply white ink and color ink to a unit area by different relative scans. This increases the time until the inks come into contact with each other, making it easier to suppress mixing. The unit area can be set as any area, such as one pixel or one band.
[0075] From the viewpoint of efficient application to a non-absorbent medium, the inkjet recording method of the present invention preferably further comprises a reaction liquid application step of applying an aqueous reaction liquid containing a reactant that reacts with the aqueous ink to the recording medium. Hereinafter, the aqueous reaction liquid is also simply referred to as the reaction liquid.
[0076] (Reaction solution) The reaction liquid reacts with the ink when it comes into contact with the ink, coagulating the components in the ink (components having anionic groups, such as resins and self-dispersing pigments), and contains a reactant. Examples of the reactant include cationic components such as polyvalent metal ions and cationic resins, and organic acids.
[0077] Examples of polyvalent metal ions include Ca. 2+ , Cu 2+ , Ni 2+ , Mg 2+ , Sr 2+ , B.A. 2+ , and Zn 2+ Divalent metal ions such as Fe 3+ , Cr 3+ , Y 3+ , and Al 3+ In order to add a polyvalent metal ion to the reaction solution, a polyvalent metal salt (which may be a hydrate) formed by combining a polyvalent metal ion with an anion can be used. Examples of the anion include Cl. - , Br - , I - , ClO - , ClO2 - , ClO3 - , ClO4 - , NO2 - , NO3 - , SO4 2- , CO3 2- , HCO3 - , PO4 3- , HPO4 2- , and H2PO4 - Inorganic anions such as HCOO - , (COO - )2, COOH(COO - ), CH3COO - , C2H5COO - , CH3CH(OH)COO - , C2H4(COO - )2, C6H5COO - , C6H4(COO - )2, and CH3SO3 - When a polyvalent metal ion is used as the reactant, the content (mass %) of the polyvalent metal salt in the reaction solution is preferably 1.00 mass % or more and 20.00 mass % or less based on the total mass of the reaction solution.
[0078] The reaction liquid containing an organic acid has a buffering ability in the acidic range (less than pH 7.0, preferably pH 2.0 to 5.0), and thus efficiently converts the anionic groups of the components present in the ink into an acid form and causes them to aggregate. Examples of the organic acid include monocarboxylic acids and salts thereof, such as formic acid, acetic acid, propionic acid, butyric acid, benzoic acid, glycolic acid, lactic acid, salicylic acid, pyrrole carboxylic acid, furan carboxylic acid, picolinic acid, nicotinic acid, thiophene carboxylic acid, levulinic acid, and coumaric acid; dicarboxylic acids and salts and hydrogen salts thereof, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, itaconic acid, sebacic acid, phthalic acid, malic acid, and tartaric acid; tricarboxylic acids and salts and hydrogen salts thereof, such as citric acid and trimellitic acid; and tetracarboxylic acids and salts and hydrogen salts thereof, such as pyromellitic acid. When an organic acid is used as the reactant, the content (mass %) of the organic acid in the reaction liquid is preferably 1.00 mass % or more and 50.00 mass % or less based on the total mass of the reaction liquid.
[0079] Examples of cationic resins include resins having a structure of primary to tertiary amines and resins having a structure of quaternary ammonium salts. Specific examples include resins having a structure of vinylamine, allylamine, vinylimidazole, vinylpyridine, dimethylaminoethyl methacrylate, ethyleneimine, guanidine, diallyldimethylammonium chloride, and alkylamine-epichlorohydrin condensate. In order to increase the solubility in the reaction solution, the cationic resin may be used in combination with an acidic compound or the cationic resin may be subjected to a quaternary treatment. When a cationic resin is used as a reactant, the content (mass%) of the cationic resin in the reaction solution is preferably 0.10 mass% or more and 10.00 mass% or less based on the total mass of the reaction solution. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way as long as it does not deviate from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified. In addition, a dispersion of titanium oxide particles is referred to as a "pigment dispersion."
[0081] <Preparation of reaction mixture> The following components were mixed to prepare a reaction solution. Magnesium sulfate heptahydrate 2.0 parts Poly(diallyldimethylammonium chloride) (product name "Unisense FPA101L", manufactured by Senka, cationic resin content: 35.0%) 7.1 parts 20.0 parts 1,2-butanediol 0.5 parts of fluorine-based nonionic surfactant (product name "Capstone FS3100", manufactured by LEHVOSS Group) Preservative (product name "Proxel GXL(S)", manufactured by Arch Chemicals) 0.2 parts 70.2 parts deionized water
[0082] <Preparation of titanium dioxide> Commercially available titanium oxide particles that had been surface-treated in advance and titanium oxide particles prepared by surface-treating untreated titanium oxide were used. The cumulative 50% particle diameter (D 50 ) was measured using a particle size analyzer using dynamic light scattering (trade name "Nanotrac WaveII-EX150", manufactured by Microtrack Bell). The properties of titanium dioxide particles are shown in Table 1. In Table 1, TITANIX:JR, JR-403, and JR-405 are the trade names of rutile-type titanium dioxide manufactured by Teika.
[0083] (Measurement of the amount of alumina and silica coating) The ratio of alumina and silica in the titanium oxide particles, i.e., the amount of alumina and silica coating, was measured as follows. The prepared titanium oxide particles were added to nitric acid to prepare a liquid, and quantitative analysis of aluminum and silicon elements was performed using an inductively coupled plasma (ICP) emission spectrometer. In this case, it was assumed that all atoms coating the surface were in the form of oxides, and the obtained values of aluminum and silicon were converted to the oxides, i.e., alumina and silica, to calculate the mass ratio.
[0084] (Titanium oxide particles 1) Titanium oxide was surface-treated by a wet method to produce titanium oxide particles 1. In the surface treatment by the wet method, untreated titanium oxide is brought into contact with a surface treatment agent (sodium aluminate, sodium silicate, etc.), and the amount and ratio of the surface treatment agent used are appropriately adjusted to perform the surface treatment at any ratio.
[0085] Specifically, 300 parts of rutile-type titanium oxide (trade name "TITANIX JR", manufactured by Teika Co., Ltd.) that had not been subjected to surface treatment and 700 parts of pure water were mixed with a homogenizer. Then, the mixture was heated to 90°C while stirring, and potassium hydroxide (pH adjuster) was added to adjust the pH to 10.5. Next, sodium silicate was added, and dilute sulfuric acid (pH adjuster) was added over about 1 hour to adjust the pH to 5.0. The reaction was continued for about 1 hour. Thereafter, sodium aluminate was added little by little at 90°C. At this time, in order to maintain the pH, dilute sulfuric acid was used in combination to maintain the pH at 6.0 to 8.0. After the addition of sodium aluminate, the reaction was continued for about 1 hour to obtain a dispersion. The dispersion was cooled to 25°C, and then purified by repeating sedimentation using a centrifuge and redispersion in ion-exchanged water, and dried at 120°C to obtain titanium oxide particles 1 that had been surface-treated with alumina and silica. Table 1 shows the characteristics of titanium oxide particles 1.
[0086] (Titanium oxide particles 2, 4, 5) Commercially available titanium oxide particles (including those previously surface-treated with alumina or silica) were used as titanium oxide particles 2, 4, and 5. Table 1 shows the properties of titanium oxide particles 2, 4, and 5. TITANIX: JR-403 and JR405 are product names of rutile-type titanium oxide manufactured by Teika. Also, Typec CR-80 is the product name of rutile-type titanium oxide manufactured by Ishihara Sangyo Kaisha. Some commercially available titanium oxide particles contain inorganic oxides such as zirconia and zinc oxide, and organic compounds such as polyols, in addition to alumina and silica, but the proportion of these is at most about 1.00%. Therefore, for convenience, the proportion of titanium oxide in the titanium oxide particles is shown as T (%) ("Titanium oxide T (%)" in Table 1).
[0087] (Titanium oxide particles 3) Titanium oxide particles 3 surface-treated with alumina and silica were obtained in the same manner as in the preparation of titanium oxide particles 1, except that commercially available rutile-type titanium oxide surface-treated with alumina (product name "TITANIX JR-405", manufactured by Teika) was used.
[0088] [Table 1]
[0089] <Preparation of the compound represented by general formula (1)> The compound represented by general formula (1) was synthesized by the following procedure. The synthesis conditions and structures of the compound synthesized as the compound represented by general formula (1) and the comparative compound are shown in Tables 2 and 3, respectively. The compound represented by general formula (1) can be synthesized by allylation and hydrosilylation of a raw material (such as a polyalkylene glycol monoalkyl ether).
[0090] In a three-neck flask equipped with a stirrer and a nitrogen inlet tube, the raw materials, base, and solvent (sometimes referred to as tetrahydrofuran, THF) shown in Table 2 were placed and stirred at 25°C for 30 minutes. As the "sodium hydride", a paraffin dispersion of 60% sodium hydride was used, and the dispersion was used so that the amount of sodium hydride used was as shown in Table 2. Then, the bromide shown in Table 2 was added dropwise while stirring at 25°C, and stirring was continued for 12 hours after the end of the dropwise addition to obtain a solution containing the reactants. After filtering out the unreacted sodium hydride and neutralized product (sodium bromide), THF was removed under reduced pressure to obtain a concentrate. The concentrate was dissolved in 500 parts of pure water, and this aqueous solution was extracted three times with 200 mL of hexane, and then extracted with 200 mL of dichloromethane. The solvent containing the product was dried by adding magnesium sulfate, and concentrated under reduced pressure to obtain each of the allylated compounds (allylation process).
[0091] The allylated raw materials and silane compounds shown in Table 2 were placed in a dry, passivated round-bottom flask equipped with a stirrer and an argon inlet tube, and stirred at 85°C. Then, 0.54 parts of an aqueous solution of 65 mmol / L chloroplatinic acid monohydrate in isopropyl alcohol was added, and the mixture was heated at 85°C for 5 hours. After the reaction was completed, the mixture was allowed to cool to 25°C, and the excess silane compounds were removed under reduced pressure. The residue was purified by column chromatography using silica gel passivated with triethoxysilane as a carrier to obtain each compound (hydrosilylation step). The eluent used for purification by column chromatography was ethyl acetate / hexane / ethanol = 85 / 15 / 5 (by volume).
[0092] [Table 2]
[0093] [Table 3]
[0094] <Preparation of pigment dispersion> The pigment dispersion was prepared according to the following procedure. The preparation conditions for the pigment dispersion are shown in Table 4.
[0095] (Pigment Dispersion 1-10) 40.00 parts of titanium oxide particles, dispersant, potassium hydroxide, and ion-exchanged water with a total of 100.00 parts of the components shown in Table 4 were mixed, and preliminary dispersion was performed using a homogenizer. The amount of potassium hydroxide used was appropriately adjusted so that the pH of the main dispersion was 10.5. The pH of the main dispersion was measured using a pH meter (trade name "Portable pH Meter D-74", manufactured by Horiba, Ltd.) at the time of starting the main dispersion. Thereafter, dispersion treatment (main dispersion) was performed for 12 hours at 25°C using 0.5 mm zirconia beads with a paint shaker. The zirconia beads were filtered off, and an appropriate amount of ion-exchanged water was added as necessary to prepare each pigment dispersion with a titanium oxide particle content of 40.00%. In Table 4, the "aqueous solution of water-soluble resin" of pigment dispersions 7 and 9 was synthesized by the method described below, and the resin content was 40.00%. The "polyacrylic acid" in the pigment dispersion 10 is polyacrylic acid having a weight average molecular weight of 5000 (product name "Polyacrylic acid 5,000" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0096] [Table 4]
[0097] <Synthesis of resin particles> In a four-neck flask equipped with a stirrer, a reflux condenser, and a nitrogen gas inlet tube, 0.2 parts of potassium persulfate and 74.0 parts of ion-exchanged water were placed, and nitrogen gas was introduced. The monomers shown in Table 5 and 0.3 parts of an emulsifier (trade name "NIKKOL BC15", manufactured by Nikko Chemicals) were mixed to obtain a mixture. The obtained mixture was dropped into the four-neck flask over 1 hour under stirring, and then reacted at a temperature of 80°C for 2 hours. Thereafter, the contents were cooled to 25°C, and potassium hydroxide in an amount equivalent to the acid value of the resin and an appropriate amount of ion-exchanged water were added to prepare an aqueous dispersion of each resin particle with a resin particle content of 40.00%. The acid value and particle size (cumulative 50% particle size based on volume) of the resin particles are shown in Table 5. Details of each component in Table 5 are shown below. ·BMA: Butyl methacrylate ·MAA: Methacrylic acid
[0098] [Table 5]
[0099] In addition, as the aqueous dispersion of resin particles 4, a commercially available self-emulsifying anionic polyether polyurethane emulsion aqueous dispersion (product name "Takelac W-5025", manufactured by Mitsui Chemicals, urethane resin particle content 30.0%, cumulative 50% particle diameter by volume 20.3 nm) was used.
[0100] <Synthesis of water-soluble resin> 81.6 parts of butyl methacrylate and 18.4 parts of methacrylic acid were polymerized by a conventional method to synthesize a water-soluble acrylic resin. After adding ion-exchanged water containing potassium hydroxide in an amount equimolar to the acid value to neutralize the acid group, an appropriate amount of water was further added to obtain an aqueous solution of a water-soluble resin with a resin content of 40.00%. The acid value of this water-soluble resin was 120.0 mgKOH / g.
[0101] <Preparation of aqueous dispersion of wax particles> (Water dispersion of wax particles 1) 25.0 parts of wax, 5.0 parts of nonionic surfactant, 1.0 part of phosphoric acid ester (butoxyethylated), 1.0 part of oleic acid, and 1.0 part of triethanolamine were added to 67.0 parts of ion-exchanged water. Here, Fischer-Tropsch wax (trade name "FT-0165", melting point 73°C, manufactured by Nippon Seiro) was used as the wax, and polyoxyethylene cetyl ether (trade name "NIKKOL BC-15", manufactured by Nikko Chemicals) was used as the nonionic surfactant. This mixture was heated to 100°C, and primary circulation emulsification was performed under a pressure condition of 10 MPa using a homogenizer equipped with a heating circulation line. The volume average particle diameter (D 50 When the volume average particle diameter (D ) drops to about 500 nm, the pressure is increased to 25 MPa and secondary circulation emulsification is continued. 50 The dispersion was then subjected to pressure filtration using a cellulose acetate filter (manufactured by Advantec) having a pore size of 3.0 μm, followed by dilution with ion-exchanged water to obtain an aqueous dispersion of wax particles 1 with a wax particle content of 40.00%.
[0102] Volume average particle size (cumulative 50% particle size D 50 ) is the diameter of the particle that is 50% of the total volume of the measured particles when integrated from the small particle diameter side in the particle diameter integration curve. The volume average particle diameter was measured using the dynamic light scattering particle size analyzer and measurement conditions described above.
[0103] (Water dispersion of wax particles 2) In the secondary circulation emulsification, the volume average particle diameter (D 50 An aqueous dispersion of wax particles 2 having a wax particle content of 40.00% was obtained in the same manner as in the preparation of the aqueous dispersion of wax particles 1, except that the dispersion treatment was performed until the particle diameter reached 130 nm.
[0104] (Water dispersion of wax particles 3) An aqueous dispersion of wax particles 3 having a wax particle content of 40.0% was obtained in the same manner as in the preparation of the aqueous dispersion of wax particles 1, except that the wax was replaced with paraffin wax (product name "Parraffin Wax-155", melting point 69°C, manufactured by Nippon Seiro).
[0105] (Water dispersion of wax particles 4) An aqueous dispersion of wax particles 4 with a wax particle content of 40.0% was obtained in the same manner as in the preparation of the aqueous dispersion of wax particles 1, except that the wax was replaced with polyethylene wax (product name "Sunwax 171-P", melting point 100°C, manufactured by Nippon Seiro).
[0106] <Ink Preparation> The types and amounts of each component shown in the upper rows of Tables 6 to 9 were mixed and stirred. Acetylenol E60 (product name) is a nonionic surfactant manufactured by Kawaken Fine Chemicals. For polyacrylic acid, its weight average molecular weight and salt type are listed together. For example, "polyacrylic acid (Mw: 1,900, Na salt)" indicates that the weight average molecular weight is 1,900 and that it is a sodium salt type polyacrylic acid. After that, pressure filtration was performed using a membrane filter (manufactured by Sartorius) with a pore size of 5.0 μm to prepare each ink.
[0107] In the case of inks prepared from pigment dispersions using titanium oxide particles at least a portion of whose surface is coated with at least silica, the column "Contribution of silica to dispersion of titanium oxide particles" is marked with "○". However, when the ink contains 0.01 mass% or more of a water-soluble resin other than polyacrylic acid, the dispersion caused by the action of silica is likely to be destabilized. In this case, the column "Contribution of silica to dispersion of titanium oxide particles" is marked with "×". Although the term "resin particles" refers to particles containing wax particles, for convenience, the total content of wax particles is shown in "Content of wax particles W (%)" in Tables 6 to 9, and the total content of resin particles excluding wax particles is shown in "Content of resin particles E (%)" in Tables 6 to 9.
[0108] [Table 6]
[0109] [Table 7]
[0110] [Table 8]
[0111] [Table 9]
[0112] <Evaluation> The inks obtained above were evaluated for the following items. In the present invention, for each of the evaluation criteria for the following items, "A" and "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown in Table 10.
[0113] (Concealment) Each ink obtained above was filled into an ink cartridge, and the ink cartridge was set in an inkjet recording device (trade name "PIXUS PRO-10S", manufactured by Canon) equipped with a recording head that ejects ink by thermal energy. In this embodiment, the recording duty of a solid image recorded under the conditions of applying ink droplets of about 3.8 ng to a unit area of 1 / 600 inch x 1 / 600 inch at a resolution of 1200 dpi so that the dot application positions do not overlap, that is, applying one dot (about 3.8 ng per dot) to each area divided into four of the unit area of 1 / 600 inch x 1 / 600 inch, is defined as 100%. Using the above inkjet recording device, the reaction liquid was applied to the entire surface of a transparent label paper (trade name "Livasta PET50A", manufactured by Lintec) so that the recording duty was 50%. Thereafter, two types of solid images of 16.2 mm x 16.2 mm with ink recording duties of 200% and 350% were recorded. The carriage movement speed at this time was 12.7 cm / s. After the ink was applied, the recording medium was not transported in the sub-scanning direction, and hot air at 80°C was blown from a position 10 mm above the recording medium for 10 seconds, and then the paper was discharged to record an evaluation image. The hot air was generated by a hot air dryer (product name "TSK hot air dryer TSK-18", manufactured by Kansai Electric Net) and blown from a nozzle with a diameter of 4 mm. The air speed was 30.0 m / s.
[0114] The above hot air drying is not intended to completely dry the liquid components of the recorded image. This is a method for determining the time during which no transfer or loss occurs due to contact with the image, such as the paper pressing of the recording medium, when handling the recording medium in the next process after recording, and is a pre-drying condition for this purpose. While this pre-drying makes the recording medium easier to handle, it also affects the fixability. Under these recording conditions, evaluation images were recorded on 10 sheets in succession.
[0115] The ten evaluation images were placed in a thermostatic chamber at 80° C. for six minutes to thoroughly dry the liquid components on the recording medium surfaces. The hiding ratio of the evaluation images was measured using a spectrophotometer (product name "CM-3600A", manufactured by Konica Minolta), and the hiding power of the images was evaluated according to the following evaluation criteria. A: Of the images with an ink printing duty of 200%, at least one had a concealment rate of 60% or more, and of the images with an ink printing duty of 350%, at least one had a concealment rate of 60% or more. B: All of the images with an ink printing duty of 200% had a concealment rate of less than 60%, but of the images with an ink printing duty of 350%, at least one had a concealment rate of 60% or more. C: The concealment rate of all images was less than 60%.
[0116] (Fixation) Under the same conditions as the above-mentioned image for evaluating the hiding power, 10 solid images of 16.2 mm x 200 mm with an ink recording duty of 300% were recorded in succession. During this process, image loss due to the transport mechanism and transfer of white ink to non-recorded areas due to ink adhesion to the transport mechanism were visually checked, and fixation was evaluated according to the evaluation criteria shown below. If image loss or transfer occurs, it means that the image has not dried sufficiently and additional drying time is required, so fixation is poor. AA: No image loss was observed in any of the 10 images, and no transfer marks were observed in at least one image. A: Of the 10 images, at least one image was found to be missing an image, but there were no images in which both an image was missing and there were transfer marks. B: Of the 10 images, at least one image was found to have both missing images and transfer marks. C: Both image loss and transfer marks were confirmed in all 10 images.
[0117] (Abrasion resistance) A 32mm x 200mm solid image with an ink recording duty of 300% was recorded under the same conditions as the above-mentioned image for evaluating the hiding power, except that drying with a hot air dryer was not performed. The obtained solid image was placed in an oven at 80°C for 6 minutes, and the liquid components on the surface of the recording medium were thoroughly dried to obtain an evaluation image. Using a friction fastness tester (trade name "JIS L 0849 Gakushin type II type", manufactured by DJK), a test was performed up to 300 times back and forth with a test load of 500g using a cloth cut to 50 x 50 mm from the trade name "Test attachment white cloth cotton (Kanakin No. 3)" (manufactured by JSA GROUP). The friction speed was 30 times back and forth / minute. The state of scraping of the image was visually confirmed every 100 times, and the abrasion resistance of the image was evaluated according to the evaluation criteria shown below. A: No image wear occurred even after 300 round trips, or image wear occurred after 300 round trips but no image wear occurred after 100 or 200 round trips. B: After 200 reciprocating strokes, the image was scraped off, but after 100 reciprocating strokes, the image was not scraped off. C: After 100 reciprocating strokes, the image was scraped off.
[0118] [Table 10]
[0119] The abrasion resistance of Example 24 was evaluated as "B" like Example 25, but Example 24 was superior. The hiding power of Examples 32 and 35 was evaluated as "B" like Example 31, but Examples 32 and 35 were superior.
Claims
1. A water-based inkjet ink containing titanium oxide particles, resin particles, and a water-soluble organic solvent, the titanium oxide particles are titanium oxide having at least a part of their surfaces coated with alumina and silica, The aqueous ink is characterized in that the content (T (mass %)) of the titanium oxide particles, the content (E (mass %)) of the resin particles, and the content (S (mass %)) of the water-soluble organic solvent in the aqueous ink satisfy the relationship of the following formulas (1) and (2): E / T≧0.50...(1) 0.30≦S / (T+E)≦0.70...(2)
2. 2. The water-based ink according to claim 1, wherein the titanium oxide particles are dispersed at least by the action of the silica.
3. 2. The water-based ink according to claim 1, wherein the resin particles are made of an acrylic resin.
4. the resin particles include wax particles, The aqueous ink according to claim 1 , wherein a ratio (mass %) of the wax particles to the resin particles in the aqueous ink is 0.09 to 0.30 times.
5. The volume-based cumulative 50% particle diameter (D T (nm)), the volume-based cumulative 50% particle diameter of the resin particles (D E (nm)), and the volume-based cumulative 50% particle diameter of the wax particles (D W The water-based ink according to claim 4 , wherein (nm) satisfies the relationships of the following formulas (3) and (4): D W ≧D E ...(3) D T ≧2×D E ...(4)
6. 2. The water-based ink according to claim 1, wherein the content (mass %) of the titanium oxide particles in the water-based ink is 10.00 mass % or more and 20.00 mass % or less based on the total mass of the ink.
7. 2. The aqueous ink according to claim 1, wherein the water-soluble organic solvent comprises at least one selected from the group consisting of 1,2-butanediol, 1,2-pentanediol, and propylene glycol.
8. The water-based ink according to claim 1 , further comprising a compound represented by the following general formula (1): [Formula 1] (In general formula (1), R 1 , R 2 , and R 3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 4 is an alkylene group having 2 to 4 carbon atoms; X is a single bond or an alkylene group having 1 to 6 carbon atoms; n is 6 to 24; a is 1 to 3, b is 0 to 2, and a+b=3.
9. 2. The aqueous ink according to claim 1, further comprising polyacrylic acid having a weight average molecular weight of 2,000 or more and 6,000 or less, and a content (mass %) of the polyacrylic acid is 0.010 or less times the content (mass %) of the titanium oxide particles in terms of a mass ratio.
10. An ink cartridge including an ink and an ink storage section for storing the ink, 10. An ink cartridge, wherein the ink is a water-based ink as claimed in claim 1.
11. An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, comprising:
10. An ink-jet recording method, wherein the ink is a water-based ink according to claim 1.
Citation Information
Patent Citations
Ink set and recording method
JP2017109485A
Recording method and recording apparatus
JP2021154547A