Stretched porous film, roll, sanitary goods and method for producing stretched porous film

A stretched porous film with a polyester resin, inorganic filler, and OH or COOR groups addresses the moisture permeability issue, achieving high moisture transmission and strength through enhanced micropore formation.

JP2024144193APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024034098
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional stretched porous films containing polyester resins do not have sufficient moisture permeability.

Method used

A stretched porous film comprising a polyester resin, an inorganic filler, and a compound with OH or COOR groups, which enhances moisture permeability by improving dispersibility and forming a large number of connected micropores.

Benefits of technology

The film achieves moisture permeability of 5000g/m²·24hrs or more, with improved tear strength and elongation, making it suitable for applications requiring breathability and moisture transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144193000001
    Figure 2024144193000001
Patent Text Reader

Abstract

To provide a stretched porous film with superior moisture permeability.SOLUTION: A stretched porous film includes polyester, an inorganic filler, and a compound with at least one selected from an OH group and a COOR group (where, R is a hydrogen atom or an alkyl group), with the content of the compound being 250-30000 ppm. Also provided are a method for producing a stretched porous film, a roll formed by winding the stretched porous film, and sanitary goods including the stretched porous film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretched porous film, a roll, a sanitary product, and a method for producing a stretched porous film. [Background technology]

[0002] Conventionally, a porous film is known in which a resin composition containing a polyolefin and an inorganic filler is stretched to cause interfacial peeling between the polyolefin and the inorganic filler, forming a large number of voids (micropores). In particular, a stretched porous film made of a resin composition containing a polyolefin and an inorganic filler has internal micropores that form interconnected pores, and is therefore used as a moisture-permeable, waterproof film that has high air permeability and moisture permeability while suppressing the permeation of liquids. Such stretched porous films are widely used in applications requiring breathability, moisture permeability, and waterproofness, such as sanitary products such as paper diapers and feminine hygiene products, clothing such as work clothes, jumpers, jackets, medical clothing, and chemical protective clothing, masks, covers, drapes, sheets, and wraps.

[0003] For example, Patent Document 1 discloses a porous film obtained by stretching a film containing 50 to 200 parts by mass of an inorganic filler per 100 parts by mass of a polyethylene resin at least in the machine direction of the film to make it porous, in which the polyethylene resin has a Z-average molecular weight (Mz) of 300,000 or more and contains linear low-density polyethylene made of a copolymer of ethylene and an α-olefin having 6 or more carbon atoms.

[0004] Meanwhile, in recent years, research has been actively conducted on replacing conventional plastic products with biodegradable resins or biomass resins (raw materials derived from plants) from the viewpoint of environmental conservation. For example, Patent Document 2 discloses a film that contains a thermoplastic resin (A), contains 1 to 70 mass% of a filler (B) in 100 mass% of all components of the film, has a porosity of 80% or less, has a tear strength in any direction of 200 mN or less, and has a tensile strength in any direction of less than 15 MPa. Patent Document 3 also discloses a porous sheet obtained by melt-molding a resin composition containing an aliphatic polyester resin, a filler, and a plasticizer into a raw sheet, and stretching the raw sheet at least uniaxially, characterized in that the blending amount of the filler is 20 to 300 parts by weight relative to 100 parts by weight of the aliphatic polyester resin, the plasticizer is a trimellitic acid ester, and the blending amount of the plasticizer is 0.5 to 100 parts by weight relative to 100 parts by weight of the aliphatic polyester resin. In these documents, the use of polylactic acid resin as the thermoplastic resin is specifically considered. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-161787 A [Patent Document 2] International Publication No. 2014 / 156952 [Patent Document 3] JP 2007-119537 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, in the case of a stretched porous film, the constituent resin has been replaced from a polyolefin resin to a polyester resin such as polylactic acid. However, the moisture permeability of the conventional stretched porous film containing a polyester resin is not sufficient, and improvement is required.

[0007] Therefore, in order to solve such problems of the conventional technology, the present inventors have carried out studies with the aim of providing a stretched porous film containing a polyester resin and having excellent moisture permeability. [Means for solving the problem]

[0008] Examples of specific embodiments of the present invention are given below.

[0009] [1] A composition comprising a polyester, an inorganic filler, and a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group), A stretched porous film having a compound content of 250 to 30,000 ppm. [2] Moisture permeability of 5000g / m2 based on a film thickness of 20μm 2 The stretched porous film according to [1], wherein the duration is 24 hours or longer. [3] The stretched porous film according to [1] or [2], wherein the compound is a fatty acid. [4] The stretched porous film according to [3], wherein the fatty acid is stearic acid. [5] The stretched porous film according to any one of [1] to [4], wherein the compound is a glycol. [6] The stretched porous film according to [5], wherein the glycol is ethylene glycol. [7] The stretched porous film according to any one of [1] to [6], wherein the inorganic filler has an average particle size of 0.1 to 10 μm. [8] The stretched porous film according to any one of [1] to [7], wherein the inorganic filler is calcium carbonate. [9] The stretched porous film according to any one of [1] to [8], wherein the polyester is polybutylene adipate terephthalate.

[10] The stretched porous film according to any one of [1] to [9], which has a thickness of 10 to 150 μm.

[11] A roll obtained by rolling up the stretched porous film according to any one of [1] to

[10] .

[12] A sanitary product comprising a stretched porous film according to any one of [1] to

[10] .

[13] A process for obtaining a resin composition by mixing a polyester with an inorganic filler coated with a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group); A step of forming the resin composition into a sheet to obtain a sheet; and stretching the sheet.

[14] The method for producing a stretched porous film according to

[13] , wherein the content of the compound relative to the total mass of the inorganic filler coated with the compound is 0.01 mass% or more. Effect of the Invention

[0010] According to the present invention, it is possible to obtain a stretched porous film containing a polyester resin and having excellent moisture permeability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment or a specific example, but the present invention is not limited to such an embodiment. In this specification, when "X to Y" (X and Y are any numbers) is used, it includes "X or more and Y or less" as well as "preferably greater than X" or "preferably smaller than Y" unless otherwise specified. In addition, when "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also includes "preferably greater than X" or "preferably less than Y". In the following description, "film" and "sheet" are not clearly distinguished from each other, and when "film" is used, it includes "sheet", and when "sheet" is used, it includes "film".

[0012] In this specification, the MD direction of the film is the extrusion direction (or take-up direction or flow direction) during film formation and is also called the machine direction, while the TD direction is the direction perpendicular to the MD direction and is also called the transverse direction or width direction.

[0013] (Stretched porous film) The present embodiment relates to a stretched porous film (hereinafter also referred to as the present stretched porous film) that contains a polyester, an inorganic filler, and a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group), and the compound content is 250 to 30,000 ppm. The stretched porous film of the present embodiment has a large number of voids (micropores), and these voids are connected in the thickness direction, so that the film can exhibit high moisture permeability.

[0014] The pore size of the voids (micropores) is preferably 0.05 to 0.5 μm. If the pore size of the voids (micropores) is within the above range, the film can be made liquid-impermeable (waterproof) while allowing water vapor and air to pass through. The pore size can be evaluated as the maximum pore size measured by the bubble point method (JIS K3832:1990 or ASTM F316), and more specifically, the pore size can be measured using a perm porometer.

[0015] The stretched porous film is a uniaxially stretched film. Since the stretched porous film contains an inorganic filler, the resin composition is stretched in the production process to cause interfacial peeling between the polyester and the inorganic filler, thereby forming a film having a large number of voids (micropores) having the above-mentioned pore size.

[0016] In this embodiment, the inorganic filler is preferably coated with a compound having at least one selected from OH group and COOR group (wherein R is a hydrogen atom or an alkyl group), and such an inorganic filler is mixed with polyester and formed into a sheet, so that the film contains 250 to 30,000 ppm of a compound having at least one selected from OH group and COOR group. The compound having at least one selected from OH group and COOR group may be present on the surface of the inorganic filler (fine particle), or may be present in a state of being separated from the inorganic filler. In the manufacturing process of this stretched porous film, by using an inorganic filler coated with a compound having at least one selected from OH group and COOR group, the dispersibility and mixability of the inorganic filler and polyester can be improved, and as a result, a large number of voids (micropores) can be formed uniformly in the film. In such a stretched porous film, the moisture permeability is more effectively improved. In this embodiment, by using a compound having at least one selected from an OH group and a COOR group as a surface treatment agent for the inorganic filler, it is presumed that the affinity with the polyester having a polar ester bond is improved, the dispersibility of the filler in the sheet is improved, and a large number of voids are generated during stretching, making it possible to obtain a film with high moisture permeability.

[0017] The stretched porous film of the present embodiment can exhibit excellent moisture permeability. Here, the moisture permeability can be measured by the following method. First, a measuring cup (inner diameter 60 mm, inner diameter area 28.27×10 -4 m 2 ) was used to seal calcium chloride, and the cup was then sealed with a stretched porous film. The measuring cup was then placed in a constant temperature and humidity environment at a temperature of 40°C and a relative humidity of 90%, and the moisture permeability (g / m2) was calculated from the increase in the mass of the measuring cup after 24 hours. 2 In this embodiment, the moisture permeability converted into a film thickness of 20 μm can be calculated using the following formula. Moisture permeability of 20 μm thickness = Moisture permeability (measured value) × film thickness (μm) / 20 (μm)

[0018] The moisture permeability of a film with a thickness of 20 μm is 5000 g / m 2 -24hrs or more is preferable, 5500g / m 2 More preferably, 24hrs or more, 6000g / m 2 More preferably, 24 hours or more, 7000g / m 2 It is particularly preferable that the moisture permeability is 15,000 g / m2 or more based on a film thickness of 20 μm. 2 It is preferable that the moisture permeability is 24 hours or less. Thus, the stretched porous film of the present embodiment has excellent moisture permeability.

[0019] The tear strength in the MD direction of the stretched porous film of this embodiment is preferably 0.5 N / mm or more, more preferably 0.6 N / mm or more. The upper limit of the tear strength in the MD direction of the stretched porous film is not particularly limited, but is preferably, for example, 5 N / mm or less. In this embodiment, the tear strength in the MD direction of the stretched porous film is particularly increased. Usually, when a uniaxially stretched film is produced, the film is stretched in the MD direction (longitudinal direction), so that the tear strength in the MD direction tends to decrease. However, in this embodiment, polyester is used as the resin constituting the stretched porous film, and further, an inorganic filler coated with a compound having at least one selected from polyester and OH groups and COOR groups is mixed, so that the tear strength in the MD direction, where the tear strength tends to decrease significantly, can be effectively increased.

[0020] In addition, the tear strength in the TD direction of the stretched porous film of this embodiment is preferably 5.0 N / mm or more, more preferably 6.0 N / mm or more, and even more preferably 7.0 N / mm or more. The upper limit of the tear strength in the TD direction of the stretched porous film is not particularly limited, but is preferably, for example, 30 N / mm or less. In this embodiment, the polyester and the inorganic filler coated with a compound having at least one selected from an OH group and a COOR group are mixed, so that the tear strength in the TD direction (transverse direction) is also increased. By increasing the tear strength of the stretched porous film, breakage during film formation or printing of the film can be suppressed, and the strength of the stretched porous film when used in absorbent articles such as diapers is sufficient. The tear strength of this stretched porous film is measured in accordance with JIS K7128-1:1998 by cutting a sample to a length of 100 mm and a width of 25 mm in the measurement direction, making a 25 mm cut in the center of the width, and using a tensile tester at 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 25 mm.

[0021] The stretched porous film has a breaking elongation in the TD direction of preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, even more preferably 90% or more, and particularly preferably 100% or more. The stretched porous film has a breaking elongation in the TD direction of preferably 800% or less.

[0022] The MD breaking elongation of the stretched porous film is preferably 30% or more, more preferably 33% or more, and even more preferably 35% or more. The MD breaking elongation of the stretched porous film is preferably 200% or less. The breaking elongation of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measuring direction, and using a tensile tester under the conditions of 23°C, 50% relative humidity, a pulling speed of 200 m / min, and a chuck distance of 20 mm.

[0023] In this embodiment, it is preferable that the breaking elongation in the TD direction is greater than that in the MD direction. In a typical stretched porous film using a polyolefin resin or a polylactic acid resin, the breaking elongation in the MD direction is usually greater than that in the TD direction, but in this embodiment, it is preferable that the breaking elongation in the TD direction is increased and that the breaking elongation in the TD direction is greater than that in the MD direction.

[0024] Here, when the breaking elongation in the TD direction is P and the breaking elongation in the MD direction is Q, the value of P / Q is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, and particularly preferably 1.9 or more. The value of P / Q is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less. By setting the value of P / Q within the above range, the moisture permeability of the stretched porous film can be more effectively increased.

[0025] The tensile strength in the MD direction of the present stretched porous film is preferably 10.0 MPa or more, more preferably 12.0 MPa or more, and even more preferably 14.0 MPa or more. The tensile strength in the MD direction of the present stretched porous film is preferably 50 MPa or less, more preferably 48 MPa or less, and even more preferably 45 MPa or less.

[0026] The tensile strength of the stretched porous film in the TD direction is preferably 1.0 MPa or more, more preferably 1.2 MPa or more, and even more preferably 1.4 MPa or more. The tensile strength of the stretched porous film in the TD direction is preferably 10 MPa or less, more preferably 8 MPa or less, and even more preferably 7 MPa or less. The tensile strength of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measurement direction, and using a tensile tester under the conditions of 23°C, relative humidity of 50%, a pulling speed of 200 m / min, and a chuck distance of 20 mm.

[0027] The thickness of the present stretched porous film is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the present stretched porous film is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less. By making the thickness of the present stretched porous film within the above range, it is possible to make the film thinner while maintaining a balance between moisture permeability and mechanical strength.

[0028] The present embodiment may relate to a rolled body obtained by rolling up a stretched porous film. Since the stretched porous film has appropriate strength and flexibility, it can be stored or distributed in the form of a roll.

[0029] (polyester) The stretched porous film contains polyester. Examples of polyester include polyethylene terephthalate, polyethylene terephthalate copolymer, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene adipate terephthalate, polybutylene adipate, polyethylene adipate, polybutylene adipate terephthalate, polyethylene adipate terephthalate, polyethylene succinate, polybutylene succinate, polybutylene succinate carbonate, polybutylene succinate terephthalate, polypropylene succinate, polybutylene succinate adipate, polybutylene succinate terephthalate, polybutylene succinate adipate terephthalate, polybutylene succinate lactate, polybutylene succinate hydroxycaproate, and polybutylene succinate carbonate. polyhydroxyalkanoates such as polyhydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), polyhydroxybutyrate valerate, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyacyl), and polyhydroxyacyl; polylactic acid, polyglycolic acid, lactic acid-glycolic acid copolymer, polycaprolactone, polycaprolactone butylene succinate, polybutylene adipate caprolactone, polypropiolactone, salts and derivatives thereof, and polyester elastomers. Among them, the polyester is preferably at least one selected from the group consisting of polyethylene succinate, polybutylene succinate, polypropylene succinate, polybutylene succinate adipate, and polybutylene adipate terephthalate, and the polyester is particularly preferably polybutylene adipate terephthalate (PBAT).

[0030] Polybutylene adipate terephthalate is a biodegradable resin, and is preferably a thermoplastic resin. When the stretched porous film contains polybutylene adipate terephthalate as a constituent resin, the stretched porous film has excellent biodegradability. In this specification, biodegradability refers to the property of a film being decomposed by the action of organisms such as microorganisms.

[0031] Polybutylene adipate terephthalate is a copolymer of adipic acid, terephthalic acid, and butanediol. Adipic acid, terephthalic acid, and butanediol may be copolymerized simultaneously or in multiple stages.

[0032] When synthesizing polybutylene adipate terephthalate, in addition to adipic acid, terephthalic acid, and butanediol, a small amount of other copolymerization components may be added. Examples of other copolymerization components include dicarboxylic acids other than terephthalic acid and adipic acid, and modifiers for the purpose of chain extension, terminal blocking, etc. These may be used alone or in combination of two or more. Examples of other dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, etc. These may be used alone or in combination of two or more. Examples of modifiers include polyisocyanate compounds, glycol compounds, etc. Examples of the polyisocyanate compound include diisocyanate compounds, and examples of the diisocyanate compound include hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, 1,5-naphthylene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, carbodiimide-modified MDI, and polymethylene phenyl polyisocyanate. Examples of the glycol compound include diols other than butanediol and polyalkylene glycols. Examples of the other diols include methanediol, ethanediol, propanediol, pentanediol, and hexanediol. Examples of polyalkylene glycols include polymethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol (polytetramethylene glycol), etc. These may be used alone or in combination of two or more kinds.

[0033] In 100 mol % of the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate, the constituent units derived from terephthalic acid are preferably contained at 40 to 60 mol %, and the constituent units derived from adipic acid are preferably contained at 40 to 60 mol %. By setting the ratio of the constituent units derived from terephthalic acid and the constituent units derived from adipic acid among the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate within the above range, a film having a good balance of mechanical strength, biodegradability, and flexibility can be easily obtained.

[0034] The melting point of polybutylene adipate terephthalate is preferably 105°C or higher, more preferably 108°C or higher, and even more preferably 110°C or higher. The melting point of polybutylene adipate terephthalate is preferably 130°C or lower, more preferably 128°C or lower, and even more preferably 125°C or lower. The melting point of polybutylene adipate terephthalate is measured by DSC or the like in accordance with JIS K 7121 (2012). By setting the melting point of polybutylene adipate terephthalate within the above range, a film having a good balance between heat resistance and moldability can be easily obtained.

[0035] Examples of polybutylene adipate terephthalate include biodegradable synthetic polymer compounds listed in the positive list of the Japan Bioplastics Association's GreenPla (biodegradable plastic) classification number A-1. Commercially available products include, for example, F Blend C1200 manufactured by BASF and ECO-A05 manufactured by Taiwan Chang Chun Co., Ltd.

[0036] The weight average molecular weight (Mw) of the polyester is preferably 50,000 or more, more preferably 70,000 or more, and even more preferably 100,000 or more. The weight average molecular weight (Mw) of the polyester is preferably 400,000 or less, more preferably 350,000 or less, and even more preferably 300,000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) or the like. By setting the weight average molecular weight (Mw) of the polyester within the above range, a film having a good balance between extrusion moldability and mechanical strength can be easily obtained.

[0037] The molecular weight distribution (Mw / Mn) of the polyester is preferably 1.5 or more, more preferably 1.7 or more, and even more preferably 1.9 or more. The molecular weight distribution (Mw / Mn) of the polyester is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.0 or less. By setting the molecular weight distribution (Mw / Mn) of the polyester within the above range, a film having a good balance of film formability, film rigidity, and impact resistance can be easily obtained.

[0038] The content of polyester in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of polyester is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of polyester in the stretched porous film within the above range, the moisture permeability of the stretched porous film can be more effectively increased.

[0039] (Inorganic fillers / coating compounds) The stretched porous film contains an inorganic filler. Examples of inorganic fillers include various carbonates such as calcium carbonate, magnesium carbonate, and barium carbonate, various sulfates such as magnesium sulfate, barium sulfate, and calcium sulfate, various oxides such as zinc oxide, silicon oxide (silica), zirconium oxide, magnesium oxide, calcium oxide, titanium oxide, magnesium oxide, iron oxide, and alumina, and other hydroxides such as aluminum hydroxide, silicate minerals, various composite oxides such as hydroxyapatite, mica, talc, kaolin, clay, montmorillonite, and zeolite, various phosphates such as lithium phosphate, calcium phosphate, and magnesium phosphate, and various salts such as lithium chloride and lithium fluoride. Among these, from the viewpoint of improving moisture permeability and strength, the inorganic filler is preferably at least one selected from the group consisting of calcium carbonate, barium carbonate, barium sulfate, silicon oxide (silica), and titanium oxide, more preferably at least one selected from the group consisting of calcium carbonate and barium sulfate, and particularly preferably calcium carbonate.

[0040] The average particle size of the inorganic filler is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. The average particle size of the inorganic filler is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. By setting the average particle size of the inorganic filler to the above lower limit or more, poor dispersion and secondary aggregation of the inorganic filler are suppressed, and it is preferable that the inorganic filler can be uniformly dispersed in the resin composition constituting the stretched porous film. If the average particle size is the above upper limit or less, it is possible to suppress the generation of large voids when the film is thinned, and the film can have sufficient strength and water resistance.

[0041] The average particle size of the inorganic filler is calculated from the specific surface area measured by the constant pressure transmission method using a Shimadzu powder specific surface area measuring instrument SS-100. The measurement conditions are as follows: sample weight 3.0 g, sample thickness 1.35 cm, cross-sectional area of ​​the sample layer 2 cm 2, air pressure is 50cmH2O, and the viscosity coefficient of air is 181×10 -6 Calculate the average particle size as g / (cm sec).

[0042] The inorganic filler is preferably surface-treated, and is preferably coated with a compound having at least one selected from OH and COOR groups (wherein R is a hydrogen atom or an alkyl group). In this way, the inorganic filler coated with a compound having at least one selected from OH and COOR groups is mixed with polyester and formed into a sheet, so that the film contains 250 to 30,000 ppm of the compound having at least one selected from OH and COOR groups. The compound having at least one selected from OH and COOR groups may be present on the surface of the inorganic filler (fine particles), or may be present in a state of being detached from the inorganic filler.

[0043] The compound having at least one selected from OH group and COOR group coats the surface of the inorganic filler, and therefore can also be called a surface treatment agent or a coating agent. That is, the stretched porous film of the present embodiment preferably contains 250 to 30,000 ppm of the inorganic filler surface treatment agent or a compound derived from the surface treatment agent.

[0044] The content of the compound having at least one selected from OH group and COOR group is preferably 250 ppm or more, more preferably 260 ppm or more, even more preferably 270 ppm or more, and particularly preferably 280 ppm or more, based on the total mass of the stretched porous film. The content of the compound having at least one selected from OH group and COOR group is preferably 30000 ppm or less, more preferably 25000 ppm or less, even more preferably 20000 ppm or less, even more preferably 15000 ppm or less, and particularly preferably 10000 ppm or less, based on the total mass of the stretched porous film. By setting the content of the compound having at least one selected from OH group and COOR group in the stretched porous film within the above range, the dispersibility and mixability of the inorganic filler and the polyester can be improved, and as a result, the moisture permeability of the stretched porous film can be more effectively improved.

[0045] The content of the compound having at least one selected from OH group and COOR group (the proportion of the compound in the inorganic filler) is preferably 0.01% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.02% by mass or more, based on the total mass of the inorganic filler coated with the compound. The content of the compound having at least one selected from OH group and COOR group is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the inorganic filler coated with the compound. By setting the content of the compound having at least one selected from OH group and COOR group in the inorganic filler within the above range, the dispersibility and mixability of the inorganic filler and polyester can be improved, and as a result, the moisture permeability of the stretched porous film can be more effectively improved.

[0046] R in the COOR group is a hydrogen atom or an alkyl group. When R is an alkyl group, the number of carbon atoms in the alkyl group is preferably 1 to 20, more preferably 1 to 15, even more preferably 1 to 12, still more preferably 1 to 10, and particularly preferably 1 to 5. For example, the alkyl group may be a methyl group or an ethyl group. The alkyl group may further have a substituent, and examples of such a substituent include an aliphatic hydrocarbon group (e.g., an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group), an aromatic hydrocarbon group (e.g., a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, a biphenyl group), a heterocyclic group, an acyl group, an alkoxy group, an amino group, a hydroxy group, a mercapto group, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom), and the like.

[0047] The compound having at least one selected from OH group and COOR group is preferably a fatty acid. The fatty acid may be a chain hydrocarbon compound having at least one carboxyl group in the molecule. The chain hydrocarbon compound having at least one carboxyl group in the molecule means a compound in which the carbon atom to which the carboxyl group is bonded is a constituent atom of the carbon chain. The carbon chain in the chain hydrocarbon compound having at least one carboxyl group in the molecule may be saturated or unsaturated, and may be linear or branched. Among them, the fatty acid is preferably a chain hydrocarbon compound having one carboxyl group. Specifically, the fatty acid may be stearic acid, palmitic acid, myristic acid, lauric acid, behenic acid, oleic acid, linoleic acid, etc. Among them, the fatty acid is preferably at least one selected from the group consisting of stearic acid, palmitic acid, and myristic acid, and is particularly preferably stearic acid.

[0048] In addition, the compound having at least one selected from OH group and COOR group is also preferably a glycol. Glycol is an alcohol having two hydroxyl groups in one molecule. The glycol is preferably an alkylene glycol, and examples of the alkylene glycol include methylene glycol, ethylene glycol, propylene glycol, and diethylene glycol. Among them, the glycol is particularly preferably ethylene glycol.

[0049] The molecular weight of the compound having at least one selected from an OH group and a COOR group is preferably 50 or more, more preferably 100 or more, and even more preferably 150 or more. The molecular weight of the compound having at least one selected from an OH group and a COOR group is preferably 500 or less, more preferably 450 or less, and even more preferably 400 or less.

[0050] The content of the inorganic filler in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of the inorganic filler is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of the inorganic filler in the stretched porous film within the above range, the moisture permeability of the stretched porous film can be more effectively increased.

[0051] The inorganic filler may be one of the above inorganic fillers, or may be a mixture of two or more different fillers having different materials, average particle sizes, types of surface treatment agents, etc. When the inorganic filler is composed of two or more types, the total amount is preferably within the above range.

[0052] (Other resins) The present stretched porous film may contain other resins in addition to polyester. Examples of the other resins include polyolefin resins, polystyrene resins, acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, ethylene-vinyl alcohol copolymers, ethylene-vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyarylate resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, fluorine-based resins, and polyacetal resins. As the other resin, for example, biodegradable resins such as polyvinyl alcohol, polyamide, polyethylene glycol, etc. These other resins may be used alone or in combination of two or more.

[0053] When the present stretched porous film contains other resins in addition to polyester, the content of the other resins is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less, based on the total mass of the stretched porous film.

[0054] (optional ingredient) The stretched porous film may contain various additives as optional components. Examples of additives include plasticizers, lubricants, compatibilizers, processing aids, antioxidants, heat stabilizers, light stabilizers, UV absorbers, antiblocking agents, antifogging agents, matting agents, antibacterial agents, deodorants, antistatic agents, flame retardants, colorants, and pigments. Examples of plasticizers that can be used include low molecular weight polymers (oligomers) such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, metal soaps, higher alcohols, petrolatum, paraffin wax, glycerin fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, castor oil, hydrogenated castor oil, hardened castor oil, dehydrated castor oil, aromatic esters, aromatic amides, polyesters, and the like. The content of additives is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the stretched porous film. In this embodiment, the amount of plasticizer added may be 1% by mass or less, 0.1% by mass or less, or substantially no plasticizer may be included. In particular, when polybutylene adipate terephthalate is used as the polyester, the stretched porous film can exhibit high flexibility even without the inclusion of a plasticizer.

[0055] (Method of manufacturing the stretched porous film) The method for producing the stretched porous film preferably includes, for example, a step of mixing polyester with an inorganic filler coated with a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group) to obtain a resin composition, a step of forming the resin composition into a sheet to obtain a sheet, and a step of stretching the sheet. The step of stretching the sheet preferably includes a step of stretching the sheet in at least one axial direction.

[0056] The stretched porous film may be either planar or tubular, but is preferably planar from the viewpoints of productivity (several pieces can be produced in the width direction of the raw sheet) and printing on the inner surface. The method for producing a planar film preferably includes, for example, a step of melting a resin composition using an extruder, extruding the resin composition into a film shape from a die, and cooling and solidifying the film with a cooling roll, air cooling, or water cooling to obtain an unstretched film, and a step of stretching the unstretched film in at least one axial direction to obtain a stretched porous film.

[0057] The step of obtaining the resin composition preferably includes a step of mixing polyester and an inorganic filler coated with a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group), followed by melt kneading. Specifically, it is preferable to mix for an appropriate time using a mixer such as a tumbler mixer, mixing roll, Banbury mixer, ribbon blender, or super mixer, and then uniformly disperse the resin composition using an extruder such as a counter-rotating twin-screw extruder or a co-rotating twin-screw extruder.

[0058] The content of the compound having at least one selected from OH group and COOR group (the proportion of the compound in the inorganic filler) is preferably 0.01% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.02% by mass or more, based on the total mass of the inorganic filler coated with the compound. The content of the compound having at least one selected from OH group and COOR group is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the inorganic filler coated with the compound. In the inorganic filler mixed in the step of obtaining the resin composition, by setting the content of the compound having at least one selected from OH group and COOR group within the above range, the dispersibility and mixability of the inorganic filler and the polyester can be improved, and as a result, the moisture permeability of the stretched porous film can be more effectively improved.

[0059] In the process of obtaining a sheet (unstretched sheet), it is preferable to connect a die such as a T-die or a round die to the tip of an extruder and form the obtained resin composition into a film. Alternatively, a strand die may be connected to the tip of a kneader, and the resin composition may be pelletized by a method such as strand cutting or die cutting. The pellets obtained (along with an additional composition in some cases) may then be introduced into a single-screw extruder or the like, and a die such as a T-die or a round die may be connected to the tip of the extruder to form the resin into a film. When forming the resin into a film, it is preferable to employ a film forming method such as inflation molding, tubular molding, or T-die molding.

[0060] In the process of stretching the sheet, the unstretched film is stretched at least uniaxially. For example, the resin is melted using an extruder, extruded from a T-die or a round die, cooled and solidified with a cooling roll, and stretched at least uniaxially by roll stretching in the MD direction (longitudinal direction) or tenter stretching in the transverse direction (perpendicular to the flow direction of the film, TD). Among them, the process of obtaining a stretched porous film preferably includes a process of uniaxially stretching in the MD direction (longitudinal direction), and the stretched porous film is preferably a uniaxially stretched porous film. The process of uniaxially stretching in the MD direction (longitudinal direction) may include a process of stretching two or more times in the same direction. The stretching ratio is preferably 2.5 to 6.0 times, and more preferably 3.0 to 5.5 times. By setting the stretching ratio to be equal to or more than the lower limit above, a stretched porous film having excellent moisture permeability and excellent appearance due to being uniformly stretched can be obtained. Moreover, by setting the stretching ratio to be equal to or less than the above upper limit, the breaking elongation of the film can be increased.

[0061] If necessary, a heat treatment or relaxation treatment may be performed after the stretching. When the stretching is performed by roll stretching, the stretched film can be brought into contact with a heated roll (anneal roll) between the stretching step and the winding step to perform a heat treatment. Alternatively, while heating with the anneal roll, the speed of the next roll to be contacted can be made slower than the anneal roll speed to perform a relaxation treatment. Note that these heat treatments and relaxation treatments can also be performed in a separate step after stretching the unstretched film and winding up the stretched porous film.

[0062] The method for producing the present stretched porous film may, if necessary, include a step of performing a surface treatment or surface processing such as slitting, corona treatment, printing, application of an adhesive, coating, deposition, etc. The present stretched porous film may, for example, be printed, or may be a film having a printed layer.

[0063] (Application) The present stretched porous film can be suitably used in a wide range of applications, such as packaging materials for liquids, powders, and solids for various foods, medicines, and miscellaneous goods, agricultural materials, and construction materials, particularly in disposable applications. Specific applications include, for example, agricultural mulch films, tunnel films, greenhouse films, sunshades, weed control sheets, ridge sheets, germination sheets, forestry fumigation sheets, binding tapes containing flat yarns, backsheets for diapers and sanitary products, packaging sheets, hand warmer sheets, shopping bags, plastic bags, garbage bags, draining bags, compost bags, etc. Among these, the present stretched porous film is preferably used as a backsheet for diapers, sanitary products, etc., since it has excellent moisture permeability.

[0064] The present embodiment may relate to a sanitary product having the above-mentioned stretched porous film. Examples of the sanitary product include absorbent articles (diapers, sanitary products, etc.). EXAMPLES

[0065] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0066] <Thickness> The thickness of the film was measured using a stand-type constant pressure thickness measuring instrument in accordance with JIS K7130:1999, and the average of 36 measured values ​​was calculated.

[0067] <Breaking elongation / tensile strength> In accordance with JIS K7127:1999, samples were cut to a length of 100 mm and a width of 10 mm in the measurement direction, and the breaking elongation and tensile strength were measured using a tensile tester under conditions of 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 20 mm, and the average of the measured values ​​for three samples was calculated.

[0068] <Tear strength> In accordance with JIS K7128-1:1998, a sample was cut to a length of 100 mm and a width of 25 mm in the measurement direction, a 25 mm notch was made in the center of the width, and the tear strength was measured using a tensile tester under conditions of 23°C, relative humidity 50%, a tensile speed of 200 m / min, and a chuck distance of 25 mm, and the average of the measured values ​​for three samples was calculated.

[0069] <Moisture permeability (20μm equivalent)> In accordance with JIS Z0208:1976, a measuring cup (inner diameter 60 mm, inner surface area 28.27 × 10 -4 m 2 The measuring cup was placed in a constant temperature and humidity environment of 40°C and 90% relative humidity, and the moisture permeability (g / m2) was calculated from the increase in the mass of the measuring cup after 24 hours. 2 After calculating the average of the three measured values, the moisture permeability per 20 μm of film thickness (moisture permeability converted into a film thickness of 20 μm) was calculated using the following formula. Thickness 20 μm moisture permeability = Moisture permeability (measured value) × Thickness of sample (μm) / 20 (μm)

[0070] <Quantification of at least one compound selected from OH groups and COOR groups 1> <<Quantification of surface treatment agent concentration in inorganic filler (fatty acid-based raw material)>> 5 ml of THF was added to 300 mg of the inorganic filler, stirred for 2 hours, then centrifuged, and the extract obtained by drying the supernatant was dissolved in chloroform. Subsequently, qualitative analysis was performed under the following conditions using a gas chromatograph mass spectrometer (GC / MS). Thereafter, palmitic acid, stearic acid, and methyl stearate selected as standard substances were dissolved in chloroform for gas chromatographic analysis (GC measurement), and the peak areas of the extract of the inorganic filler were compared. <<GC / MS measurement conditions>> · Instrument: GC / MS-QP2020 (manufactured by Shimadzu Corporation) · Column: UA1 (MS / HT)-30M-0.1F · Carrier gas: Helium · Flow rate: 1 mL / min · Injection volume: 1 μL · Injection temperature: 320 °C · Column temperature: Hold at 70 °C for 1 minute → Heat up to 320 °C at 25 °C / min → Hold at 320 °C for 5 minutes · Interface temperature: 320 °C · Ion source temperature: 250 °C · Ionization method: EI (70 eV) · Detection range: 35 - 800 m / z <<GC measurement conditions>> · Instrument: GC-2010Plus (manufactured by Shimadzu Corporation) · Column: UA1 (MS / HT)-30M-0.1F · Carrier gas: Helium · Flow rate: 1 mL / min · Injection volume: 1 μL · Injection temperature: 320 °C · Column temperature: Hold at 70 °C for 1 minute → Heat up to 320 °C at 25 °C / min → Hold at 320 °C for 5 minutes · Detector: FID

[0071] <Quantification of a compound having at least one selected from an OH group and a COOR group 2> <<Quantification of the surface treatment agent concentration in an inorganic filler (glycol-based raw material)>> 1.63 g of chloroform was added to 54 mg of the inorganic filler, and after immersion for several hours, centrifugation was performed, and the supernatant was collected and subjected to 1H-NMR analysis. After identifying the structure of the substance from the peaks, the concentration was quantified from the integration ratio of the signals using 0.05 vol% of tetramethylsilane contained in chloroform as a standard.

[0072] <Quantification of the surface treatment agent concentration in the film 1 (fatty acid-based raw material)> For the obtained stretched porous film, 1.8 g of the sample was dissolved in chloroform, the resin was precipitated with methanol, the filtrate after filtration was dried, water was added to the obtained extract, and the precipitate after centrifugation was dissolved in chloroform. Next, qualitative analysis was performed using a gas chromatograph-mass spectrometer (GC / MS) under the following conditions. Thereafter, palmitic acid, stearic acid, and methyl stearate selected as standard substances were dissolved in chloroform and subjected to gas chromatographic analysis (GC measurement), and the peak areas of the extracts of the inorganic filler were compared.

[0073] <Quantification of the surface treatment agent concentration in the film 2 (glycol-based raw material)> For the obtained stretched porous film, 1.8 g of the sample was dissolved in chloroform, the resin was precipitated with methanol, the filtrate after filtration was dried, water was added to the obtained extract, the supernatant after centrifugation was dried, and then dissolved in chloroform. Next, 1H-NMR analysis was performed, and the concentration was quantified from the integration ratio of the signals using 0.05 vol% of tetramethylsilane contained in chloroform as a standard.

[0074] <Moldability> Five test pieces measuring 500 mm in the longitudinal direction and 200 mm in the transverse direction were cut out from the extruded sheet, the number of defective points of appearance defects such as bumps and holes was counted, and the total number of the five test pieces was evaluated according to the following criteria. A: The number of defective points is less than 5 B: 5 to less than 10 defects C: 10 or more defects

[0075] <Polybutylene adipate terephthalate (A)> A-1: BASF "F Blend C1200" (density 1.270g / cm 3 , MFR 3.8g / 10min, melting point: 116°C, structural units derived from terephthalic acid in 100 mol% of structural units derived from dicarboxylic acid: 48.1 mol%, structural units derived from adipic acid: 51.9 mol%, weight average molecular weight: 150,000, Mw / Mn: 2.4)

[0076] <Inorganic filler (B)> B-1: Calcium carbonate "Ryton BS-0" manufactured by Bihoku Funka Kogyo Co., Ltd. (average particle size 1.0 μm, fatty acid surface treatment product, fatty acid raw material concentration 0.029% by mass) B-2: Calcium carbonate "CSK-5" manufactured by Kalfin Co., Ltd. (average particle size 1.5 μm, fatty acid surface treatment product, fatty acid raw material concentration 0.065% by mass) B-3: Calcium carbonate "Ryton 26A" (average particle size 0.85 μm, fatty acid surface treatment product) manufactured by Bihoku Funka Kogyo Co., Ltd. B-4: Bihoku Powder Industry Co., Ltd., calcium carbonate "Lighton BK" (average particle size 0.85 μm, polyethylene glycol surface treatment product) B-5: Calcium carbonate "Suncut-160" manufactured by Kalfin Co., Ltd. (average particle size 1.5 μm, wax surface treatment product) B-6: Calcium carbonate "Softon 1000" (average particle size 2.2 μm, surface untreated), manufactured by Bihoku Powder Industry Co., Ltd.

[0077] <Example 1> After weighing the raw materials in the composition ratio shown in Table 1, they were put into a Henschel mixer and mixed and dispersed for 5 minutes. Next, the materials were melt-kneaded at a set temperature of 200°C using a co-rotating twin-screw extruder. The resin composition was extruded through a T-die connected to the tip of the co-rotating twin-screw extruder, taken up by a casting roll set at 35°C, and cooled and solidified to obtain an unstretched film with a thickness of 59 μm. The unstretched film obtained was then stretched 3.5 times in the machine direction at a temperature of 63°C using a roll-type stretching machine to obtain a stretched porous film.

[0078] <Examples 2 and 3> A stretched porous film roll was obtained in the same manner as in Example 1, except that the stretching ratio was changed.

[0079] <Example 4> An unstretched film having a thickness of 55 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 3.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.

[0080] <Example 5> A stretched porous film roll was obtained in the same manner as in Example 4, except that the stretching ratio was changed.

[0081] <Example 6> An unstretched film having a thickness of 61 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.

[0082] <Example 7> A stretched porous film roll was obtained in the same manner as in Example 6, except that the stretching ratio was changed.

[0083] <Example 8> An unstretched film having a thickness of 65 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 4.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.

[0084] <Comparative Example 1> An unstretched film having a thickness of 62 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 3.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.

[0085] <Comparative Example 2> A stretched porous film roll was obtained in the same manner as in Comparative Example 1, except that the stretching ratio was changed.

[0086] <Comparative Example 3> The raw materials were changed to have the composition ratio shown in Table 1, and an unstretched film having a thickness of 65 μm was obtained in the same manner as in Example 1.

[0087] <Reference example 1> The moisture permeability of Mitsubishi Chemical's moisture-permeable film KTF, which is made of polyethylene resin and calcium carbonate, was measured and found to be 5965 (g / m 2 24hrs).

[0088] [Table 1]

[0089] In the examples, the moisture permeability is excellent compared to the comparative examples.In the conventional stretched porous film, polypropylene resin is mainly used from the viewpoint of moisture permeability, but the stretched porous film obtained in the examples achieves the same moisture permeability as the stretched porous film using polypropylene resin.If the polypropylene resin can be replaced with a polyester resin, for example, a polyester resin having biodegradability can be used, and it is also possible to obtain a stretched porous film having excellent biodegradability.

Claims

1. The composition comprises a polyester, an inorganic filler, and a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group); A stretched porous film, wherein the content of the compound is 250 to 30,000 ppm.

2. Moisture permeability of 5000g / m2 based on a film thickness of 20μm 2 The stretched porous film according to claim 1, having a stretchability of 24 hours or more.

3. 2. The stretched porous film of claim 1, wherein the compound is a fatty acid.

4. 4. The stretched porous film according to claim 3, wherein the fatty acid is stearic acid.

5. 2. The stretched porous film of claim 1, wherein the compound is a glycol.

6. 6. The stretched porous film of claim 5, wherein the glycol is ethylene glycol.

7. The stretched porous film according to claim 1, wherein the inorganic filler has an average particle size of 0.1 to 10 μm.

8. 2. The stretched porous film according to claim 1, wherein the inorganic filler is calcium carbonate.

9. 2. The stretched porous film of claim 1, wherein the polyester is polybutylene adipate terephthalate.

10. 2. The stretched porous film according to claim 1, having a thickness of 10 to 150 μm.

11. A roll obtained by rolling up the stretched porous film according to any one of claims 1 to 10.

12. A sanitary product comprising the stretched porous film according to any one of claims 1 to 10.

13. A step of mixing a polyester with an inorganic filler coated with a compound having at least one selected from an OH group and a COOR group (wherein R is a hydrogen atom or an alkyl group) to obtain a resin composition; forming the resin composition into a sheet to obtain a sheet; and stretching the sheet.

14. The method for producing a stretched porous film according to claim 13, wherein the content of the compound relative to the total mass of the inorganic filler coated with the compound is 0.01 mass% or more.

Citation Information

Patent Citations

  • Porous sheet

    JP2007119537A

  • Polyethylene porous film

    JP2007161787A

  • film

    WO2014156952A1