Adhesive composition, antistatic surface-protective film, and optical component
An adhesive composition with a biomass-derived acrylic copolymer and antistatic agent addresses the need for environmentally friendly antistatic surface protection films, ensuring low peel-off voltages and circuit safety in optical components.
Patent Information
- Application Number
- JP2024048127
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-11
AI Technical Summary
The challenge is to develop a surface protection film for optical components that provides excellent antistatic performance while reducing the use of petroleum-derived materials, considering environmental concerns and minimizing static electricity-induced failures in electrical control circuits.
An adhesive composition comprising an acrylic copolymer with biomass-derived alkyl groups and an antistatic agent, which includes components like polyether-modified siloxane compounds, is used to create an antistatic surface protection film with a glass transition temperature of 40°C or lower, ensuring effective dispersion and interface existence of the antistatic agent.
The solution achieves a surface protection film with excellent antistatic performance, maintaining low peel-off voltages and preventing circuit damage, enhancing production efficiency and reliability in manufacturing processes.
Smart Images

Figure 2024144284000001 
Figure 2024144284000002 
Figure 2024144284000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, an antistatic surface protection film, and an optical component. [Background technology]
[0002] In the manufacturing process of optical components such as polarizing plates and retardation plates, which are components of displays, a surface protection film is attached to the surface of the optical components. The surface protection film is attached to prevent the surface from being dirty or scratched during the manufacturing process, and is therefore peeled off when the optical components are incorporated into products such as displays.
[0003] In recent years, there have been concerns that peel-off charges generated by static electricity generated when peeling off a surface protection film from an optical component may cause failures in the electrical control circuits of liquid crystal displays, and there is a demand for pressure-sensitive adhesive layers with excellent antistatic properties.
[0004] For example, Patent Document 1 discloses a surface protection film that uses an adhesive layer containing an antistatic agent for keeping the peeling electrification voltage low in order to prevent problems caused by high peeling electrification voltage when the surface protection film is peeled off from an optical component that is an adherend. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-224811 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, carbon dioxide emissions from the combustion of petroleum-derived products have become a problem, and there is a demand for reducing the use of fossil resource-based materials such as petroleum. Accordingly, in the field of adhesives, attempts are being made to save the use of petroleum resources by using biologically derived materials instead of petroleum-derived materials. In other words, there is a demand for surface protection films that have excellent antistatic properties while taking environmental issues into consideration.
[0007] The present invention has been made in consideration of the above circumstances, and aims to provide an adhesive composition that uses biological materials and can be used to produce a surface protection film having excellent antistatic performance, and an antistatic surface protection film and optical component using the same. [Means for solving the problem]
[0008] That is, the present invention employs the following configuration. [1] A pressure-sensitive adhesive composition comprising an acrylic copolymer and an antistatic agent, the acrylic copolymer comprising a component (A1) represented by the following general formula (1): [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 R is an alkyl group having 6 to 18 carbon atoms. 2 The alkyl group represented by the formula (I) is derived from biomass. [2] The pressure-sensitive adhesive composition according to [1], comprising two or more types of the (A1) component. [3] The pressure-sensitive adhesive composition according to [1] or [2], wherein the component (A1) has a glass transition temperature of 40° C. or lower. [4] The pressure-sensitive adhesive composition according to any one of [1] to [3], which contains a polyether-modified siloxane compound. [5] The pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the component (A1) is one or two selected from the group consisting of lauryl methacrylate, lauryl acrylate, normal octyl acrylate, isooctyl acrylate, isooctyl methacrylate, isostearyl acrylate, stearyl acrylate, and stearyl methacrylate. [6] The pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the acrylic copolymer has an (A2) component, and the (A2) component is an alkyl (meth)acrylate having a non-biomass-derived alkyl group at an ester terminal. [7] The pressure-sensitive adhesive composition according to any one of [1] to [6], wherein the acrylic copolymer is a copolymer obtained by further copolymerizing a component (B) with a component (C), the component (B) being a copolymerizable vinyl monomer containing either or both of a hydroxyl group and a carboxyl group, and the component (C) being a polyalkylene glycol mono(meth)acrylic acid ester monomer. [8] An antistatic surface protection film comprising a resin film and a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of [1] to [7] on one or both sides of the resin film. [9] An optical component to which the antistatic surface protective film according to [8] is bonded. Effect of the Invention
[0009] According to the present invention, it is possible to provide a pressure-sensitive adhesive composition which uses a biological material and enables the production of a surface protection film having excellent antistatic performance, and an antistatic surface protection film and an optical component which use the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Adhesive composition> The pressure-sensitive adhesive composition of the present invention contains an acrylic copolymer and an antistatic agent. In the present embodiment, the term "adhesive" refers to a liquid in which an adhesive composition is dissolved in a solvent. In this embodiment, the "adhesive composition" refers to a material that is in a soft solid (viscoelastic) state in a temperature range around room temperature (20°C) and has the property of easily adhering to an adherend by the application of pressure. For example, when a numerical range is described as "1-10 parts by weight" or "1 to 10 parts by weight," it means a range from 1 part by weight to 10 parts by weight, including the lower limit of 1 part by weight and the upper limit of 10 parts by weight.
[0011] Acrylic copolymer The acrylic copolymer is a copolymer containing an alkyl (meth)acrylate as a monomer component. When an alkyl (meth)acrylate is used as a monomer component, a pressure-sensitive adhesive composition having high transparency and good adhesive properties is easily obtained. In this embodiment, the alkyl (meth)acrylate includes an alkyl (meth)acrylate having an alkyl group derived from biomass at the ester end.
[0012] [Component (A)] In this embodiment, the acrylic copolymer contains the component (A). The component (A) contains the component (A1) as a monomer component, and may further contain the component (A2). Each of the monomer components constituting the component (A) will be described below.
[0013] Component (A1) The component (A1) is an alkyl (meth)acrylate having an alkyl group derived from biomass at the ester end. That is, the component (A1) is a monomer component represented by the following general formula (1). 2 The alkyl group represented by the formula (I) is an alkyl group derived from biomass.
[0014] [ka] (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 R is an alkyl group having 6 to 18 carbon atoms. 2The alkyl group represented by the formula (I) is derived from biomass.
[0015] The monomer represented by the general formula (1) is R 1 may be an alkyl acrylate in which R is a hydrogen atom; 1 is a methyl group.
[0016] R in general formula (1) 2 R is an alkyl group having 6 to 18 carbon atoms. 2 The alkyl group of R may be linear or branched. 2 may be a cyclic alkyl group.
[0017] As the linear or branched alkyl group, an alkyl group having 8 to 16 carbon atoms is preferable, and an alkyl group having 8 to 12 carbon atoms is more preferable.
[0018] R 2 When a monomer component having a carbon number of R or more is used, the antistatic performance of the antistatic surface protective film produced is improved. 2 It is presumed that when a monomer component having a carbon number equal to or greater than the above lower limit is used, the antistatic agent is adequately dispersed inside the antistatic surface protective film and is able to exist at the interface of the antistatic surface protective film without excessive bleeding out. R 2 The monomer component having the carbon number not exceeding the above upper limit makes it easy to prepare a pressure-sensitive adhesive composition.
[0019] The glass transition temperature of the component (A1) is preferably 40° C. or lower, and more preferably 35° C. or lower. In one embodiment of the present invention, the glass transition temperature of the component (A1) is, for example, 5° C. or higher, 10° C. or higher. In one embodiment of the present invention, the glass transition temperature of the component (A1) is, for example, 5-40°C, or 10-35°C. When the glass transition temperature of the component (A1) is within the above range, it is liquid at room temperature and the pressure-sensitive adhesive composition can be easily prepared.
[0020] The component (A1) is preferably one or two selected from the group consisting of lauryl methacrylate (Tg: -65°C), lauryl acrylate (Tg: -23°C), normal octyl acrylate (Tg: -65°C), isooctyl acrylate (Tg: -44°C), isooctyl methacrylate (Tg: -25°C), isostearyl acrylate (Tg: -18°C), stearyl acrylate (Tg: 30°C), and stearyl methacrylate (Tg: 38°C).
[0021] As the component (A1), the monomer represented by general formula (1) may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination of monomers is not particularly limited. For example, R 2 The monomers may have the same number of carbon atoms, 2 The number of carbon atoms in R may be different. 2 When combining monomers with different carbon numbers, R 2 There is no limitation on the difference in the number of carbon atoms between the groups, and they can be combined in any desired manner.
[0022] When, for example, two types of monomers represented by general formula (1) are used as the component (A1), the blending ratio of each monomer in the total amount of the component (A1) is not particularly limited and can be appropriately adjusted within the range of 1:99 to 99:1.
[0023] The component (A1) is typically an ester of a biomass-derived alkanol and a biomass-derived or non-biomass-derived (meth)acrylic acid. Examples of biomass-derived alkanols include biomass ethanol, palm oil, palm kernel oil, coconut oil, castor oil, and other alkanols derived from plant materials.
[0024] Whether or not the (A1) component is an alkyl (meth)acrylate having a biomass-derived alkyl group at the ester end can be confirmed by measuring the content of the carbon isotope with mass number 14 using accelerator mass spectrometry (AMS) measured in accordance with ASTM D6866.
[0025] ·(A2) Component In this embodiment, the acrylic copolymer may contain a component (A2). The component (A2) may contain an alkyl (meth)acrylate having a non-biomass-derived alkyl group at the ester end. The alkyl (meth)acrylate has a non-biomass-derived alkyl group at the ester end.
[0026] Examples of the (A2) component include (meth)acrylic acid ester monomers in which the alkyl group has 1 to 10 carbon atoms. Specific examples include ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0027] The acrylic copolymer may have the component (A1) and the component (A2) as the component (A), and R 2 The (A1) component may have two or more different types. In the case where the composition contains the (A1) component and the (A2) component, the amount of the (A1) component relative to the total amount of the (A) component (the combined amount of the (A1) component and the (A2) component) is preferably 65 parts by weight or less, more preferably 60 parts by weight or less, and even more preferably 50 parts by weight or less. Furthermore, the amount of the component (A1) relative to the total amount of the component (A) may be 5 parts by weight or more, 10 parts by weight or more, or 20 parts by weight or more.
[0028] The content of the component (A1) relative to the total amount of the component (A) is, for example, 5 to 65 parts by weight, 10 to 60 parts by weight, or 20 to 50 parts by weight.
[0029] When the content of the component (A1) is at least the above lower limit, the antistatic agent is adequately dispersed inside the antistatic surface protective film and can be present at the interface of the antistatic surface protective film without excessive bleed-out, making it possible to produce an antistatic surface protective film with excellent antistatic performance.
[0030] In one embodiment of the present invention, the acrylic copolymer is preferably a copolymer further comprising a (B) component and a (C) component copolymerized therein.
[0031] [(B) Component] Component (B) is a copolymerizable vinyl monomer containing either or both of a hydroxyl group and a carboxyl group. Although the component (B) is an optional component, by copolymerizing the component (B), crosslinking points can be introduced into the acrylic copolymer. Hereinafter, the copolymerizable vinyl monomer containing a hydroxyl group will be referred to as component (B1), and the copolymerizable vinyl monomer having a carboxyl group will be referred to as component (B2).
[0032] ·(B1) Component Examples of the (B1) component include hydroxyalkyl (meth)acrylates and hydroxyl group-containing (meth)acrylamides. Specifically, the (B1) component is preferably at least one selected from the group consisting of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, N-hydroxy (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. Unlike the (C) component described below, the (B1) component does not have a polyalkylene glycol chain.
[0033] ·(B2) component The (B2) component is preferably at least one selected from the group consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, and 2-(meth)acryloyloxyethyl tetrahydrophthalic acid.
[0034] The component (B) may contain either the above component (B1) or component (B2), but it is preferable that it contains both. The content of the (B1) component relative to the combined amount (100 parts by weight) of the (A) and (C) components is preferably 15 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 7 parts by weight or less. Furthermore, the amount of the component (B1) relative to the total amount of the component (B) may be 0.1 parts by weight or more, 1 part by weight or more, or 3 parts by weight or more.
[0035] The content of the component (B1) relative to the total amount of the component (B) is, for example, 0.1-15 parts by weight, 1-10 parts by weight, or 3-7 parts by weight. The content of the (B2) component relative to the combined amount (100 parts by weight) of the (A) and (C) components is preferably 2 parts by weight or less, more preferably 1 part by weight or less, and even more preferably 0.5 parts by weight or less. Furthermore, the amount of the component (B2) relative to the total amount of the component (B) may be 0.01 part by weight or more, 0.02 part by weight or more, or 0.05 part by weight or more.
[0036] The content of the (B2) component relative to the total amount of the (B) component is, for example, 0.01-2 parts by weight, 0.02-1 part by weight, or 0.05-0.5 parts by weight.
[0037] The content of component (B) relative to the total amount (100 parts by weight) of components (A) and (C) is, for example, 0.1-20 parts by weight, 0.5-15 parts by weight, 2.0-14.0 parts by weight, or 2.5-12.0 parts by weight.
[0038] [(C) component] The component (C) is a polyalkylene glycol mono(meth)acrylate monomer. The component (C) functions as an antistatic auxiliary. The (C) component may be a compound in which one of the multiple hydroxyl groups of a polyalkylene glycol is esterified as a (meth)acrylic acid ester. The (meth)acrylic acid ester group is a polymerizable group, so it can be copolymerized with the above (A) component or (B) component. The other hydroxyl group may remain as OH, or may be an alkyl ether such as methyl ether or ethyl ether, or a saturated carboxylate ester such as acetate ester, or the like.
[0039] Examples of the alkylene group contained in the polyalkylene glycol include, but are not limited to, an ethylene group, a propylene group, a butylene group, etc. The polyalkylene glycol may be a copolymer of two or more kinds of polyalkylene glycols such as polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.
[0040] The component (C) preferably has an average repeat number of alkylene oxide constituting the polyalkylene glycol chain of 3 to 14. The "average repeat number of alkylene oxide" refers to the average number of repeating alkylene oxide units in the "polyalkylene glycol chain" portion contained in the molecular structure of the polyalkylene glycol mono(meth)acrylic acid ester monomer (C).
[0041] The component (C) preferably has a diester content in the monomer of 0.2% or less. The "diester content in the monomer" refers to the content (wt%) of polyalkylene glycol di(meth)acrylic acid ester contained in the component (C).
[0042] The component (C) is preferably at least one selected from the group consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate.
[0043] More specifically, component (C) is polyethylene glycol-mono(meth)acrylate, polypropylene glycol-mono(meth)acrylate, polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-mono(meth)acrylate, polyethylene glycol-polybutylene glycol-mono(meth)acrylate, polypropylene glycol-polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-polybutylene glycol-mono(meth)acrylate; methoxypolyethylene glycol-(meth)acrylate, methoxypolypropylene glycol-(meth)acrylate, methoxypolybutylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polypropylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, methoxy-polypropylene glycol-polybutylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate; ethoxy polyethylene glycol-(meth)acrylate, ethoxy polypropylene glycol-(meth)acrylate, ethoxy polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polypropylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polypropylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate, and the like.
[0044] The content of component (C) relative to the total amount (100 parts by weight) of components (A) and (C) is, for example, 1-50 parts by weight, 1-40 parts by weight, 1-30 parts by weight, or 2-25 parts by weight.
[0045] The acrylic copolymer is preferably a copolymer of components (A), (B) and (C). In this case, the content of component (A) is preferably at least 50 parts by weight, for example 50-90 parts by weight, 60-90 parts by weight, or 70-90 parts by weight, relative to the total amount (100 parts by weight) of components (A) and (C).
[0046] The weight average molecular weight of the acrylic copolymer is not particularly limited, but is preferably 200,000 or more and 5,000,000 or less, more preferably 300,000 or more and 4,000,000 or less, and particularly preferably 500,000 or more and 2,000,000 or less. When the weight average molecular weight of the acrylic copolymer is within this range, the obtained adhesive composition can exhibit excellent adhesive strength. In this specification, the weight average molecular weight means a polystyrene-equivalent molecular weight determined by GPC (gel permeation chromatography) measurement.
[0047] The synthesis of the acrylic copolymer may be carried out by polymerizing each of the monomers described above as the (A) component, the (B) component, and the (C) component by a radical reaction in the presence of a polymerization initiator by a conventionally known method. The specific polymerization method is not particularly limited, and a conventionally known method can be used. For example, solution polymerization is preferred.
[0048] <Antistatic agent> The antistatic agent is preferably an ionic compound having a melting point of 25 to 80° C. The ionic compound is preferably a solid at room temperature. Room temperature is, for example, a temperature below 25° C., and specifically, the antistatic agent is preferably an ionic compound that is a solid at 23° C.
[0049] The pressure-sensitive adhesive composition of the present embodiment preferably contains 0.01 to 10 parts by weight of an ionic compound per 100 parts by weight of the above-mentioned acrylic copolymer.
[0050] The anion of the ionic compound is hexafluorophosphate (PF6 - ), thiocyanate (SCN - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - ), inorganic anions such as carboxylates (RCOO - ), sulfonates (RSO3 - ), alkoxide or phenoxide salts (RO - ), organic imide salts (R - ), methide salt (R3C - ), organic borate salts (R4B - ) and other organic anions.
[0051] R included in each general formula of the organic anion is an organic group that may have a fluorine substitution. The organic group may be at least one of an alkyl group, an alkoxy group, an aromatic group (aryl group, aralkyl group, etc.), an aliphatic or aromatic carbonyl group, an aliphatic or aromatic sulfonyl group, etc. The organic group included in the anion may have some or all of the hydrogen atoms substituted with one or more halogen atoms such as a fluorine atom.
[0052] The cation of the ionic compound may be one selected from the group consisting of pyridinium, imidazolium, phosphonium, sulfonium, pyrrolidinium, guanidinium, ammonium, isouronium, thiouronium, piperidinium, pyrazolium, methylium, and morpholinium. The cation of the ionic compound is preferably pyridinium. The organic group contained in the cation may have some or all of the hydrogen atoms substituted with one or more halogen atoms such as fluorine atoms. When either or both of the anion and cation of the ionic compound contain an organic group such as an alkyl group, an ionic compound having a melting point of 25 to 80°C can be obtained by selecting the chain length of the alkyl group, the position and number of the substituents, etc.
[0053] Specific examples of the ionic compound include 1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium hexafluorophosphate, 2-methyl-1-dodecylpyridinium hexafluorophosphate, 3-methyl-1-dodecylpyridinium hexafluorophosphate, 1-octylpyridinium dodecylbenzenesulfonate, 1-dodecylpyridinium thiocyanate, 1-dodecylpyridinium dodecylbenzenesulfonate, 4- Methyl-1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium 2-iodobenzenesulfonate, 4,5-diiodo-1-butyl-3-methylimidazolium hexafluorophosphate, 2-methyl-1-dodecylpyridinium 2-iodobenzenesulfonate, 4,5-diiodo-1-butyl-3-methylimidazolium 3-iodobenzenesulfonate, 1-octyl-2-methylpyridinium trifluoromethane Sulfonate salts, 1,2,3-trimethylimidazolium pentafluoroethanesulfonate salts, 1-butyl-2,3-dimethylimidazolium trifluoromethanesulfonate salts, 1-hexyl-4-methylpyridinium pentafluoroethanesulfonate salts, 1-octyl-3-methylpyridinium trifluoromethanesulfonate salts, n-octylpyridinium trifluoromethanesulfonate salts, 1-propyl-3-methylpyridinium nonafluorobutanesulfonate salts, 3-methyl-1-octylpyridinium nonafluorobutanesulfonate salts, methyltrioctylammonium tris(pentafluorobenzenesulfonyl)methide salts, 1-ethyl-3-methylimidazolium tetrakispentafluorophenylborate salts, 1-butyl-1-methylpiperidinium bis(pentafluorobenzenesulfonyl)imide salts, and the like.
[0054] <Polyether-modified siloxane compound> The pressure-sensitive adhesive composition of the present embodiment may contain a polyether-modified siloxane compound. A polyether-modified siloxane compound is a siloxane compound having a polyether group, and is a compound having a normal siloxane unit [-SiR 11 2-O-], as well as siloxane units with polyether groups [-SiR 11(R 12 O(R 12 O) n R 14 )-O-], where R 11 is one or more alkyl or aryl groups, R 12 and R 13 is one or more alkylene groups, R 14 indicates one or more alkyl or acyl groups (terminal groups). The polyether group is a polyoxyethylene group [(C2H4O) n 〕 and polyoxypropylene group〔(C3H6O) n In the siloxane unit having a polyether group, the terminal of the polyether group is an OH group (R 14 =H).
[0055] Commercially available polyether-modified siloxane compounds include, for example, KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-642, KF-644, KF-6012, KF-6017P, KF-6020, and KF-6204 (manufactured by Shin-Etsu Chemical Co., Ltd.); SH3746, SH3771, SH3772, SH3773M, SH8400, SH8700, SF8410, FZ-2110, FZ-2123, L-7001, and L-7002. (manufactured by Dow-Toray); TSF-4440, TSF-4441, TSF-4445, TSF-4446, TSF-4450 (manufactured by Momentive Performance Materials); BYK-300, BYK-306, BYK-307, BYK-320, BYK-325, BYK-330 (manufactured by BYK-Chemie), etc.
[0056] The amount of polyether-modified siloxane compound added relative to the total amount of the pressure-sensitive adhesive composition varies depending on the type and the degree of compatibility with the pressure-sensitive adhesive, but may be set in consideration of the peeling electrification voltage when the surface protective film is peeled off from the adherend, the tendency to contaminate the adherend, the adhesive properties, etc. The greater the amount of polyether-modified siloxane compound added, the lower the peeling electrification voltage when the surface protective film is peeled off, but since the adherend is more likely to be contaminated, it is necessary to select an appropriate amount to be added.
[0057] The amount of the polyether-modified siloxane compound added is, for example, preferably 0.005 to 0.5 parts by mass, more preferably 0.01 to 0.2 parts by mass, relative to 100 parts by mass of the acrylic copolymer. By incorporating the polyether-modified siloxane compound in the pressure-sensitive adhesive composition, the antistatic agent can be easily dispersed uniformly.
[0058] The pressure-sensitive adhesive composition of the present embodiment can be produced by mixing the acrylic copolymer with, as required, a solvent, a crosslinking agent, a tackifier, a silane coupling agent, and the like.
[0059] Examples of crosslinking agents that may be contained in the pressure-sensitive adhesive composition of the present embodiment include trifunctional or higher isocyanate compounds. Specifically, diisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, and pentamethylene diisocyanate are preferred, and TMP adducts of tolylene diisocyanate and isocyanurates of pentamethylene diisocyanate are particularly preferred.
[0060] <Antistatic surface protection film> The antistatic surface protection film of the present embodiment includes a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of the present embodiment on one or both sides of a resin film.
[0061] The antistatic surface protective film of the present embodiment can be formed by applying the pressure-sensitive adhesive composition of the present embodiment to a substrate or a release film, and then crosslinking the pressure-sensitive adhesive composition.
[0062] <Optical components> One aspect of the present invention is an optical component to which the antistatic surface protective film of the present embodiment is attached. Examples of the optical components include optical films such as a polarizing plate, a retardation plate, a lens film, a polarizing plate that also serves as a retardation plate, and a polarizing plate that also serves as a lens film. Such optical components are used as components of liquid crystal display devices such as liquid crystal display panels, optical devices of various instruments, etc. Examples of the optical components also include optical films such as anti-reflection films, hard coat films, and transparent conductive films for touch panels.
[0063] According to the optical component of the present invention, when the antistatic surface protective film is peeled off and removed from the optical component to which it is adhered, the peeling electrification voltage can be suppressed to a sufficiently low level, so that there is no risk of damaging circuit components such as driver ICs, TFT elements, and gate line driving circuits, and the production efficiency in the process of manufacturing liquid crystal display panels, etc. can be improved and the reliability of the production process can be maintained. EXAMPLES
[0064] The present invention will be explained more specifically below with reference to examples, but the present invention is not limited to these examples.
[0065] <Preparation of Pressure-Sensitive Adhesive Composition> <Production of acrylic copolymer 1> Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 100 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of 4-hydroxybutyl (meth)acrylate, 0.1 parts by weight of acryloyloxyethyl succinic acid, 15 parts by weight of methoxypolyethylene glycol methacrylate, and a solvent (ethyl acetate) were added to the reactor. Then, 0.1 parts by weight of azobisisobutyronitrile as a polymerization initiator was dropped over 2 hours, and the mixture was reacted at 65°C for 6 hours to obtain an acrylic copolymer 1.
[0066] <Production of acrylic copolymers 2-11> Acrylic Copolymers 2 to 11 were produced in the same manner as Acrylic Copolymer 1, except that the monomers shown in Table 1 were used instead.
[0067] The weight average molecular weight (Mw) and molecular weight dispersity (Mw / Mn) of the acrylic copolymer, calculated as standard polystyrene by GPC measurement, are shown in Table 1.
[0068] [Table 1]
[0069] In Table 1, each symbol represents the following material. 2EHA: 2-ethylhexyl acrylate ·EA: Ethyl acrylate IAA: Isoamyl acrylate ·NOCA: Normal octyl acrylate IOCA: Isooctyl acrylate IOCMA: Isooctyl methacrylate ·LA: Lauryl acrylate · LMA: Lauryl methacrylate SA: Stearyl acrylate SMA: Stearyl methacrylate 4HBA: 4-Hydroxybutyl (meth)acrylate B2-1: Acryloyloxyethyl succinate C-1: Methoxypolyethylene glycol methacrylate
[0070] Example 1 (Production of Pressure-Sensitive Adhesive Composition) To 100 parts by weight of acrylic copolymer 4, 1.0 part by weight of a crosslinking agent (Coronate (registered trademark) HX (manufactured by Tosoh Corporation)), 0.3 part by weight of an antistatic agent (tri-n-butylmethylammonium bistrifluoromethanesulfonimide (FC-4400, manufactured by 3M, melting point 27.5°C)), and 0.08 part by weight of a polyether siloxane compound (Dowsil (registered trademark) L-7002 (manufactured by Dow-Toray Industries, Inc.)) were added and mixed with stirring to obtain a pressure-sensitive adhesive composition of Example 1.
[0071] (Manufacturing of adhesive sheets) The adhesive composition of Example 1 was applied onto a film made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then dried at 100° C. for 3 minutes to remove the solvent, thereby obtaining a surface protection film with an adhesive layer having a thickness of 20 μm. Then, a release film (Diafoil (registered trademark) MRF-25 manufactured by Mitsubishi Chemical Corporation) having a thickness of 25 μm and treated with a silicone-based release agent was attached to the adhesive surface, and aging was performed at 40° C. for 3 days to obtain a surface protection film with a release film.
[0072] Examples 2 to 8 and Comparative Examples 1 to 3 Pressure-sensitive adhesive compositions of Examples 2 to 8 and Comparative Examples 1 to 3 shown in Table 2 below were prepared in the same manner as in Example 1, except that the acrylic copolymer was changed to one shown in Table 2.
[0073] [Measurement of whether or not it is derived from biomass] Whether or not the acrylic copolymers 1 to 11 were derived from biomass was confirmed by the following method. The content of the carbon isotope with mass number 14 in the acrylic copolymer contained in the pressure-sensitive adhesive composition was measured by measuring the content of the carbon isotope with mass number 14 using accelerator mass spectrometry (AMS) in accordance with ASTM D6866. Specifically, the content of carbon isotope with mass number 14 in the pressure-sensitive adhesive sheet obtained above (production of pressure-sensitive adhesive sheet) was measured by accelerator mass spectrometry (AMS) in accordance with ASTM D6866.
[0074] Since the adhesive sheet obtained in the above (production of adhesive sheet) corresponds to the solid content from which the solvent component of the adhesive composition has been removed, the biomass degree of the adhesive sheet can be regarded as the biomass degree of the acrylic copolymer contained in the adhesive composition.
[0075] As a result, it was confirmed that the acrylic copolymers 2 to 11 had a content of carbon isotope with mass number 14 of 16% or more and were derived from biomass. The presence of the carbon isotope with mass number 14 could not be confirmed in acrylic copolymer 1, confirming that it was derived from non-biomass.
[0076] [Adhesive strength measurement] The surface protection film obtained in the above (production of adhesive sheet) was attached to a polarizing plate by a pressure roller, and left for 24 hours under an atmosphere of 23°C x 50% RH. As a method for measuring the adhesive strength when peeling the surface protection film from the surface of the polarizing plate, the peel strength when peeled in a 180° direction at a speed of 30 m / min using a tensile tester was taken as the adhesive strength (N / 25 mm) of the adhesive layer of the adhesive film. The results are shown in Table 2.
[0077] [Peeling voltage measurement] The voltage (charged voltage) generated by the polarizing plate being charged when the sample adhesive film (optical film with adhesive layer) was peeled off at 180° at a pulling speed of 30 m / min was measured using high-precision static electricity sensors SK-050 and SK-1000 (manufactured by Keyence Corporation), and the maximum measured value was taken as the peeling charged voltage. The results are shown in Table 2.
[0078] [Table 2]
[0079] The peel withstand voltage is preferably −0.5 kV to 0.5 kV, and more preferably around 0 kV. As shown in Table 2 above, it was confirmed that Examples 1 to 8, which contain the component (A1) represented by general formula (1), have a peel resistance voltage between -0.5 kV and 0.5 kV, and are closer to 0 kV than Comparative Examples 2 and 3. This is presumably because, when the component (A1) represented by general formula (1) is contained, the antistatic agent is adequately dispersed inside the film and can be present at the interface of the antistatic surface protection film.
[0080] Furthermore, it was confirmed that Examples 1 to 8 had sufficient adhesive strength, which is presumably because the antistatic agent did not bleed out excessively.
[0081] Comparative Example 1, in which acrylic copolymer 1 not having a biomass-derived alkyl group was used, had a peel withstand voltage of more than 0.5 kV.
[0082] Example 11 (Production of Pressure-Sensitive Adhesive Composition) To 100 parts by weight of acrylic copolymer 4, 1.0 part by weight of a crosslinking agent (Coronate (registered trademark) HX (manufactured by Tosoh Corporation)) and 0.3 part by weight of an antistatic agent (tri-n-butylmethylammonium bistrifluoromethanesulfonimide (FC-4400, manufactured by 3M, melting point 27.5°C)) were added and mixed with stirring to obtain a pressure-sensitive adhesive composition of Example 11.
[0083] (Manufacturing of adhesive sheets) The adhesive composition of Example 11 was applied onto a film made of a polyethylene terephthalate (PET) film having a thickness of 38 μm, and then the solvent was removed by drying at 100° C. for 3 minutes to obtain a surface protection film with an adhesive layer having a thickness of 20 μm. Then, a release film (Diafoil (registered trademark) MRF-25 manufactured by Mitsubishi Chemical Corporation) having a thickness of 25 μm and treated with a silicone-based release agent was attached to the adhesive surface, and aging was performed at 40° C. for 3 days to obtain a surface protection film with a release film.
[0084] Examples 12 to 18 and Comparative Examples 11 to 13 Pressure-sensitive adhesive compositions of Examples 12 to 18 and Comparative Examples 11 to 13 shown in Table 3 below were prepared in the same manner as in Example 11, except that the acrylic copolymer was changed to one shown in Table 3.
[0085] Furthermore, the adhesive strength and peel voltage resistance were measured in the same manner as in Example 1. The results are shown in Table 3.
[0086] [Table 3]
[0087] As shown in Table 3 above, it was confirmed that Examples 11 to 18, which contain the component (A1) represented by general formula (1), have a peel withstand voltage between −0.5 kV and 0.5 kV, and are closer to 0 kV than Comparative Example 12. The addition of a polyether siloxane compound has the effect of uniformly dispersing the antistatic agent and making it easier for it to bleed out onto the surface of the film. However, it has been confirmed that when the film contains the component (A1) represented by general formula (1), the antistatic agent can be adequately dispersed inside the film and present at the interface of the antistatic surface protective film even without the addition of a polyether siloxane compound.
[0088] Furthermore, it was confirmed that Examples 11 to 18 had sufficient adhesive strength, which is presumably because the antistatic agent did not bleed out excessively.
[0089] Comparative Example 11, in which the acrylic copolymer 1 having no biomass-derived alkyl group was used, had a peel withstand voltage significantly exceeding 0.5 kV.
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic copolymer and an antistatic agent, The pressure-sensitive adhesive composition, wherein the acrylic copolymer contains a component (A1) represented by the following general formula (1): 【Chemistry 1】 (In general formula (1), R 1 is a hydrogen atom or a methyl group. 2 is an alkyl group having 6 to 18 carbon atoms. 2 The alkyl group represented by the formula (I) is derived from biomass.
2. The pressure-sensitive adhesive composition according to claim 1 , comprising two or more types of the component (A1).
3. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the component (A1) has a glass transition temperature of 40° C. or lower.
4. The pressure-sensitive adhesive composition according to claim 1 or 2, comprising a polyether-modified siloxane compound.
5. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the component (A1) is one or two selected from the group consisting of lauryl methacrylate, lauryl acrylate, normal octyl acrylate, isooctyl acrylate, isooctyl methacrylate, isostearyl acrylate, stearyl acrylate, and stearyl methacrylate.
6. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the acrylic copolymer comprises an (A2) component, and the (A2) component is an alkyl (meth)acrylate having a non-biomass-derived alkyl group at an ester terminal.
7. The acrylic copolymer is a copolymer obtained by further copolymerizing a component (B) and a component (C), The component (B) is a copolymerizable vinyl monomer containing either or both of a hydroxyl group and a carboxyl group, The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the component (C) is a polyalkylene glycol mono(meth)acrylic acid ester monomer.
8. An antistatic surface protection film comprising a resin film and a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to claim 1 or 2 on one or both sides thereof.
9. An optical part to which the antistatic surface protective film according to claim 8 is attached.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition and surface protection film
JP2012224811A
Cited By
Removable pressure-sensitive adhesive composition, surface protective film, and pressure-sensitive adhesive layer-carrying optical member
JP2026016138A
Removable pressure-sensitive adhesive composition, surface protection film, and optical member with pressure-sensitive adhesive layer
JP7650551B1