Sealant

A crosslinked rubber composition with ethylene/α-olefin/diene rubber and perfluoropolyether skeleton addresses the issue of poor plasma resistance and sealing in plasma devices, providing effective sealing performance at low temperatures.

JP2024144642AInactive Publication Date: 2024-10-11MITSUBISHI CABLE INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024123519
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sealing materials lack excellent plasma resistance and sealing performance at low temperatures, particularly in environments involving plasma devices like semiconductor etching and plasma CVD devices.

Method used

A sealing material formed by crosslinking an uncrosslinked rubber composition containing ethylene/α-olefin/diene rubber and a compound with a perfluoropolyether skeleton, which includes specific components and additives for enhanced plasma resistance and sealing performance.

Benefits of technology

The crosslinked rubber composition exhibits excellent plasma resistance and sealing properties at low temperatures, maintaining integrity in plasma environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144642000001
    Figure 2024144642000001
  • Figure 2024144642000002
    Figure 2024144642000002
  • Figure 2024144642000003
    Figure 2024144642000003
Patent Text Reader

Abstract

To provide a sealant with superior plasma resistance and sealability at low temperatures.SOLUTION: This sealant is formed through the crosslinking of an uncrosslinked rubber composition containing ethylene-α-olefin-diene rubber and a compound having a perfluoropolyether skeleton.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sealing material. [Background technology]

[0002] Sealants made of fluororubber are widely known. For example, Patent Document 1 discloses a sealant formed by crosslinking an uncrosslinked rubber composition containing a crosslinkable fluororubber and a reactive fluorine-based compound. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5189728 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a sealing material having excellent plasma resistance and sealing properties at low temperatures. [Means for solving the problem]

[0005] The present invention relates to a sealing material formed by crosslinking an uncrosslinked rubber composition containing an ethylene-α-olefin-diene rubber and a compound having a perfluoropolyether skeleton. Effect of the Invention

[0006] According to the present invention, an uncrosslinked rubber composition containing an ethylene-alpha-olefin-diene rubber and a compound having a perfluoropolyether skeleton is crosslinked, thereby providing excellent plasma resistance and sealing properties at low temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The embodiments will be described in detail below.

[0008] The sealing material according to the embodiment is an O-ring used in an apparatus that uses plasma, such as a semiconductor etching apparatus or a plasma CVD apparatus.

[0009] The sealing material according to the embodiment is a crosslinked uncrosslinked rubber composition containing an ethylene-alpha-olefin-diene rubber (hereinafter referred to as "Component A") and a compound having a perfluoropolyether skeleton (hereinafter referred to as "Component B").

[0010] According to the sealing material of the embodiment, since the uncrosslinked rubber composition containing the A component and the B component is crosslinked, it is possible to obtain excellent plasma resistance and sealing properties at low temperatures.

[0011] Here, examples of component A include ethylene-propylene-diene terpolymer (hereinafter referred to as "EPDM"), ethylene-butene-diene terpolymer (hereinafter referred to as "EBT"), etc. Component A preferably contains one or both of these, and more preferably contains at least EBT from the viewpoint of obtaining excellent plasma resistance and sealing properties at low temperatures.

[0012] Examples of the α-olefin component in the A component include propylene and butene. The α-olefin component is preferably butene from the viewpoint of obtaining excellent plasma resistance and sealing property at low temperature. Examples of the diene component in the A component include ethylidene norbornene, vinyl norbornene, dicyclopentadiene, 1,4-hexadiene, etc. From the same viewpoint as above, the diene component is preferably ethylidene norbornene.

[0013] From the viewpoint of obtaining excellent plasma resistance and low-temperature sealing property, the ethylene content in component A is preferably 40% by mass or more and 70% by mass or less, more preferably 55% by mass or more and 60% by mass or less when the α-olefin component is propylene, and more preferably 48% by mass or more and 53% by mass or less when the α-olefin component is butene. This ethylene content is measured based on ASTM D 3900.

[0014] When the diene component is ethylidene norbornene, the ENB content (diene content) in component A is preferably 3% by mass or more and 10% by mass or less from the viewpoint of obtaining excellent plasma resistance and low-temperature sealing properties, more preferably 3.5% by mass or more and 5.5% by mass or less when the α-olefin component is propylene, and more preferably 6.5% by mass or more and 7.5% by mass or less when the α-olefin component is butene. This ENB content is measured based on ASTM D 6047.

[0015] As long as component A is the main rubber component, the uncrosslinked rubber composition may contain a rubber component other than component A. Examples of the rubber component other than component A include ethylene propylene copolymer rubber (EPR), fluororubber, silicone rubber, chloroprene rubber, and hydrogenated nitrile rubber.

[0016] From the viewpoint of obtaining excellent plasma resistance and sealing properties at low temperatures, component B is preferably a liquid material of a compound having a perfluoropolyether skeleton uniformly mixed in component A, and is more preferably a one-component material.

[0017] The B component also functions as a co-crosslinking agent that crosslinks the A component by addition polymerization, and from the viewpoint of obtaining excellent plasma resistance and sealing properties at low temperatures, it is preferable that the B component has multiple alkenyl groups in the molecule. Examples of the alkenyl group include a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, and a heptenyl group. From the same viewpoint as above, the vinyl group is preferable as the alkenyl group. The multiple alkenyl groups in the molecule may be the same or different.

[0018] From the viewpoint of obtaining excellent plasma resistance and sealing properties at low temperatures, the content of component B in the uncrosslinked rubber composition is preferably 5 parts by mass or more and 40 parts by mass or less, more preferably 15 parts by mass or more and 35 parts by mass or less, and even more preferably 20 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of component A.

[0019] An example of a commercially available material for component B is SIFEL manufactured by Shin-Etsu Chemical Co., Ltd., and the SIFEL 3000 series is particularly preferred.

[0020] The uncrosslinked rubber composition may contain a powder filler dispersed in the A component. Examples of the powder filler include PVdF resin filler, carbon black, silica, silicon carbide, boron carbide, silicon nitride, boron nitride, etc. The powder filler preferably contains one or more of these, more preferably contains one or more of PVdF resin filler, carbon black, and silica, and further preferably contains PVdF resin filler from the viewpoint of suppressing particle generation even when used in a plasma atmosphere. Commercially available materials for the PVdF resin filler include, for example, the Kynar series manufactured by Arkema.

[0021] Examples of carbon black include MT (N990), FEF (N550), GPF (N600), FT (N880), etc. Of these, the carbon black preferably includes MT.

[0022] Examples of silica include dry silica such as fumed silica and wet silica such as precipitated silica. The surface of the silica may be hydrophobized with organochlorosilane, organoalkoxysilane, hexaorganodisilazane, organosiloxane oligomer, etc. Among these, the silica preferably includes dry silica, more preferably includes dry silica whose surface has been hydrophobized with organochlorosilane, and even more preferably includes fumed silica whose surface has been hydrophobized with dimethyldichlorosilane.

[0023] From the viewpoint of obtaining excellent mechanical properties after crosslinking, the average particle size of the powder filler is preferably 0.01 μm or more and 20 μm or less, more preferably 0.1 μm or more and 18 μm or less, even more preferably 5 μm or more and 15 μm or less, and still more preferably 8 μm or more and 12 μm or less.

[0024] The content of the powder filler in the uncrosslinked rubber composition is preferably 1 part by mass or more and 30 parts by mass or less, preferably 5 parts by mass or more and 15 parts by mass or less, and more preferably 8 parts by mass or more and 12 parts by mass or less, per 100 parts by mass of Component A, from the viewpoint of obtaining excellent mechanical properties after crosslinking.

[0025] The uncrosslinked rubber composition may contain a crosslinking agent for crosslinking the component A. Examples of the crosslinking agent include organic peroxides, polyols, polyamines, triazines, etc. Of these, the crosslinking agent is preferably an organic peroxide.

[0026] Examples of organic peroxides include dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, etc. The crosslinking agent preferably contains one or more of these, and more preferably contains dicumyl peroxide.

[0027] The content of the organic peroxide as the crosslinking agent in the uncrosslinked rubber composition is preferably 1 part by mass or more and 6 parts by mass or less, more preferably 1.5 parts by mass or more and 5 parts by mass or less, per 100 parts by mass of the A component.

[0028] The uncrosslinked rubber composition may contain a co-crosslinking agent for crosslinking the A component together with the crosslinking agent. Examples of the co-crosslinking agent include liquid polybutadiene, amylphenol disulfide polymer, m-phenylenedimaleimide, triallyl isocyanurate, etc. The co-crosslinking agent preferably contains one or more of these, and more preferably contains a low-viscosity liquid polybutadiene having double bonds that serve as crosslinking points in both the main chain and the side chain, from the viewpoint of excellent kneading processability with the A component and excellent mechanical properties after crosslinking.

[0029] The liquid polybutadiene contains a 1,2 addition polymerization portion and a 1,4 addition polymerization portion. The content of the 1,2 addition polymerization portion (vinyl content) in the liquid polybutadiene is preferably 1% by mass or more and 95% by mass or less, more preferably 5% by mass or more and 70% by mass or less. The number average molecular weight of the liquid polybutadiene is preferably 2000 to 15000, more preferably 8000 to 10000.

[0030] The content of the co-crosslinking agent in the uncrosslinked rubber composition is preferably 0.3 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the A component, more preferably 5 parts by mass or more and 25 parts by mass or less in the case of liquid polybutadiene and m-phenylenedimaleimide, more preferably 0.5 parts by mass or more and 1.5 parts by mass or less in the case of amylphenol disulfide polymer, and more preferably 2 parts by mass or more and 6 parts by mass or less in the case of triallyl isocyanurate.

[0031] The uncrosslinked rubber composition may contain other rubber compounding agents such as a processing aid, an antioxidant, a plasticizer, a vulcanization accelerator, and a vulcanization acceleration assistant, if necessary.

[0032] The sealing material according to the embodiment can be produced by preparing an uncrosslinked rubber composition containing the above-mentioned A component and B component, and crosslinking the uncrosslinked rubber composition, that is, crosslinking the A component of the rubber component. Therefore, the sealing material is formed of a rubber composition obtained by crosslinking the uncrosslinked rubber composition. A typical example of the crosslinking method at this time is a method in which the uncrosslinked rubber composition is crosslinked by a crosslinking agent by heating and pressurizing. In this case, after the primary crosslinking treatment by heating and pressurizing is performed, a secondary crosslinking treatment in which the composition is held in a heating furnace for a predetermined time, or a secondary crosslinking treatment in which radiation is irradiated may be performed.

[0033] The hardness Hs of the rubber composition forming the sealing material is preferably A40 or more and A70 or less, more preferably A50 or more and A60 or less. This hardness Hs is measured with a type A durometer based on JIS K6253-3:2012.

[0034] The tensile strength Tb of the rubber composition X is preferably 2 MPa or more, more preferably 5 MPa or more, and even more preferably 8 MPa or more. The elongation Eb of the rubber composition is preferably 100% or more and 500% or less, more preferably 130% or more and 250% or less, and even more preferably 150% or more and 200% or less. The tensile stress S100 at 100% elongation of the rubber composition is preferably 1 MPa or more and 6 MPa or less, more preferably 2 MPa or more and 5 MPa or less, and even more preferably 3 MPa or more and 4 MPa or less. The tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation are measured based on JIS K6251:2017. EXAMPLES

[0035] (Uncrosslinked rubber composition) The following uncrosslinked rubber compositions were prepared in Examples 1 to 14 and Comparative Examples 1 and 2. The configurations of each are also shown in Table 1.

[0036] <Example 1> EPDM (Mitsui EPT3070, manufactured by Mitsui Chemicals, Inc., ethylene content: 58% by mass, ENB content: 4.7% by mass) was used as component A. 100 parts by mass of component A were mixed with 24 parts by mass of component B (SIFEL3000 series X-71-359, manufactured by Shin-Etsu Chemical Co., Ltd.), 10 parts by mass of PVdF resin filler (Kynar MG 15, manufactured by Arkema, average particle size: 10 μm), 4 parts by mass of organic peroxide (dicumyl peroxide) as a crosslinking agent, and 10 parts by mass of liquid polybutadiene 1 (NISSO-PB B-3000, manufactured by Nippon Soda Co., Ltd., vinyl content: 90% or more, number average molecular weight: 3200) as a co-crosslinking agent to prepare an uncrosslinked fluororubber composition, which was designated as Example 1.

[0037] <Example 2> EBT (Metallocene EBT K-9330M, manufactured by Mitsui Chemicals, Inc., ethylene content: 50% by mass, ENB content: 7.1% by mass) was used as component A. 24 parts by mass of component B, 10 parts by mass of PVdF resin filler, 2 parts by mass of organic peroxide as a crosslinking agent, and 15 parts by mass of liquid polybutadiene 2 (Kuraray LBR-352, manufactured by Kuraray, vinyl content: 5 to 70%, number average molecular weight: 9000) as a co-crosslinking agent were blended and kneaded to prepare an uncrosslinked fluororubber composition, which was designated as Example 2.

[0038] <Example 3> An uncrosslinked fluororubber composition was prepared in the same manner as in Example 2, except that the amount of liquid polybutadiene 2 was 10 parts by mass per 100 parts by mass of component A. This was designated Example 3.

[0039] <Example 4> An uncrosslinked fluororubber composition was prepared in the same manner as in Example 2, except that the amount of liquid polybutadiene 2 was 20 parts by mass per 100 parts by mass of component A. This was designated Example 4.

[0040] <Example 5> Example 5 was prepared by using an uncrosslinked fluororubber composition having the same composition as in Example 3, except that the amount of the organic peroxide crosslinking agent was 3 parts by mass per 100 parts by mass of Component A.

[0041] <Example 6> Example 6 was prepared using an uncrosslinked fluororubber composition having the same composition as in Example 2, except that the amount of the organic peroxide crosslinking agent was 3 parts by mass per 100 parts by mass of Component A.

[0042] <Example 7> Example 7 was prepared by using an uncrosslinked fluororubber composition having the same composition as in Example 3, except that the amount of the organic peroxide crosslinking agent was 4 parts by mass per 100 parts by mass of Component A.

[0043] <Example 8> An uncrosslinked fluororubber composition having the same composition as in Example 7 was prepared, except that 10 parts by mass of carbon black MT (THERMAX N990, manufactured by Cancarb, average particle size: 0.3 μm) was blended with respect to 100 parts by mass of component A instead of the PVdF resin filler, and 1 part by mass of amylphenol disulfide polymer (Suncerer AP, manufactured by Sanshin Chemical Industry Co., Ltd.) was blended with respect to 100 parts by mass of component A instead of the liquid polybutadiene 2 co-crosslinking agent, and this was designated as Example 8.

[0044] <Example 9> An uncrosslinked fluororubber composition was prepared with the same composition as in Example 8, except that 10 parts by mass of hydrophobic dry silica (Aerosil R972, manufactured by Evonik, average particle size: 0.02 μm) surface-treated with dimethyldichlorosilane was blended instead of the MT carbon black, per 100 parts by mass of component A. This composition was designated Example 9.

[0045] <Example 10> An uncrosslinked fluororubber composition was prepared in the same manner as in Example 7, except that 1 part by mass of amylphenol disulfide polymer as a co-crosslinking agent was blended per 100 parts by mass of component A instead of liquid polybutadiene 2 as a co-crosslinking agent, and this was designated as Example 10.

[0046] <Example 11> An uncrosslinked fluororubber composition was prepared in the same manner as in Example 2, except that 10 parts by mass of a co-crosslinking agent m-phenylenedimaleimide (Balnoc PM, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) was used per 100 parts by mass of component A instead of the co-crosslinking agent liquid polybutadiene 2, and this was designated Example 11.

[0047] <Example 12> An uncrosslinked fluororubber composition was prepared in the same manner as in Example 2, except that 4 parts by mass of a co-crosslinking agent, triallyl isocyanurate (TAIC, manufactured by Mitsubishi Chemical Corporation), was used per 100 parts by mass of component A instead of the co-crosslinking agent, liquid polybutadiene 2, and this was designated Example 12.

[0048] <Example 13> An uncrosslinked fluororubber composition was prepared with the same composition as in Example 2, except that the amount of the PVdF resin filler was 12 parts by mass per 100 parts by mass of component A. This was designated Example 13.

[0049] <Example 14> An uncrosslinked fluororubber composition was prepared with the same composition as in Example 2, except that the amount of the PVdF resin filler was 18 parts by mass per 100 parts by mass of component A. This was designated Example 14.

[0050] <Comparative Example 1> An uncrosslinked fluororubber composition was prepared with the same composition as in Example 2 except that component B was not blended, and this composition was designated Comparative Example 1.

[0051] <Comparative Example 2> An uncrosslinked fluororubber composition was prepared with the same composition as in Example 9 except that component B was not blended, and this composition was designated Comparative Example 2.

[0052] [Table 1]

[0053] (Test Method and Results) Test pieces of the rubber composition obtained by crosslinking the above uncrosslinked rubber composition were prepared, and the following tests were carried out using them. The results are shown in Tables 2 and 3.

[0054] <Hardness> Three sheets of rubber composition with a thickness of 2 mm prepared by crosslinking each of the uncrosslinked rubber compositions of Examples 1 to 14 and Comparative Examples 1 and 2 were stacked to form a test piece. Based on JIS K6253-3:2012, using a Type A durometer, the hardness Hs was measured as the instantaneous value when the pressure plate was brought into contact with the test piece.

[0055] <Tensile properties> Dumbbell-shaped No. 3 test pieces were cut out from the sheet-shaped rubber compositions prepared by crosslinking each of the uncrosslinked rubber compositions of Examples 1 to 14 and Comparative Examples 1 and 2. Based on JIS K6251:2017, the tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation were measured.

[0056] <Plasma resistance> AS-214 O-rings prepared by crosslinking each of the uncrosslinked rubber compositions of Examples 1 to 13 and Comparative Examples 1 and 2 were used as test pieces, which were set in a plasma exposure apparatus (manufactured by Shinko Seiki Co., Ltd.). Using a mixed gas of O2 gas and CF4 gas mixed at a volume ratio of 50:1, they were exposed to the plasma generated under the conditions of a frequency of 2.45 GHz, a pressure of 100 Pa, and an output of 1500 W for 30 minutes. Then, the presence or absence of dust generation at that time was visually confirmed. Also, the mass reduction rate was calculated based on the following formula from the mass before and after that. Mass reduction rate (%) = {(mass before exposure - mass after exposure) / mass before exposure} × 100

[0057] <He leak test> The AS-214 O-rings prepared by crosslinking the uncrosslinked rubber compositions of Examples 2, 7, and 10, and the fluororubber and silicone rubber were used as test specimens, which were then set in a He leak detector (manufactured by INFICON) and the amount of He leaked was measured at test temperatures of 23°C and -50°C, a He flow rate of 80 ml / min, and an O-ring crushing rate of 25%.

[0058] [Table 2]

[0059] [Table 3] [Industrial Applicability]

[0060] The present invention is useful in the technical field of sealing materials.

Claims

1. A sealing material formed by crosslinking an uncrosslinked rubber composition containing an ethylene-α-olefin-diene rubber and a compound having a perfluoropolyether skeleton.

2. The sealing material according to claim 1, The sealing material, wherein the ethylene-alpha-olefin-diene rubber comprises an ethylene-butene-diene terpolymer.

3. The sealing material according to claim 1, The sealing material, wherein the compound having a perfluoropolyether skeleton has a plurality of alkenyl groups in the molecule.

4. The sealing material according to claim 1, The sealing material, wherein the uncrosslinked rubber composition further contains a co-crosslinking agent.

5. The sealing material according to claim 4, The sealing material, wherein the co-crosslinking agent comprises liquid polybutadiene.

6. The sealing material according to claim 5, A sealing material, wherein the vinyl content of the liquid polybutadiene of the co-crosslinking agent is 5% by mass or more and 70% by mass or less.