Recording paper
The recording paper structure with a cationic polymer and silane coupling agent-based antistatic layer, combined with a specific print-receiving layer, addresses antistatic and water resistance issues, enhancing electrostatic discharge and moisture resistance for improved print quality and durability.
Patent Information
- Application Number
- JP2023057044
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electrophotographic recording papers face limitations in antistatic performance and water resistance, despite advancements in other recording papers.
A recording paper structure comprising a base material, an antistatic layer made from a reaction product of a cationic polymer and a silane coupling agent, and a print-receiving layer with specific thickness and components, enhancing both antistatic properties and water resistance.
The proposed structure achieves improved antistatic properties and water resistance, ensuring effective electrostatic discharge and preventing moisture absorption at the surface, thereby maintaining print quality and durability.
Smart Images

Figure 2024144879000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a recording paper. [Background technology]
[0002] In recent years, the progress of copying machines and printers has been remarkable, and they are improving dramatically not only in terms of price but also in terms of performance such as recording quality and recording speed. In addition, the performance of various recording papers such as printing paper, poster paper, label paper, inkjet recording paper, thermal recording paper, thermal transfer receiving paper, pressure-sensitive transfer recording paper, and electrophotographic recording paper has also been improved, and various recording papers with excellent water resistance, weather resistance, and durability have been proposed.
[0003] For example, in the electrophotographic printing method, in addition to the above-mentioned functions such as water resistance, a technology that can improve the antistatic properties of the recording paper is required. This is because in the case of electrophotographic printing, the humidity inside the printing machine decreases due to heating during ink drying, creating an environment in which static electricity is easily generated, and the paper alignment ability of aligning the printed paper into a bundle is significantly reduced. In response to such a demand, for example, Patent Document 1 proposes an electrophotographic recording paper that has antistatic properties by incorporating a polymer antistatic agent in the toner receiving layer for printing. In addition, the invention described in Patent Document 1 aims to provide water resistance in addition to the above-mentioned antistatic properties by using a special liposoluble polymer antistatic agent in the toner receiving layer of the electrophotographic recording paper. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-299017 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, even in the electrophotographic recording paper described in Patent Document 1, the antistatic agent that can be used is limited, so there is room for improvement in antistatic performance. Furthermore, according to the study by the present inventors, it has been found that the recording paper described in Patent Document 1 also has room for improvement in water resistance.
[0006] SUMMARY OF THE PRESENT DISCLOSURE The present invention has been made in consideration of the above circumstances, and has an object to provide a recording paper having good antistatic properties and water resistance. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by a recording paper having a base material, an antistatic layer having antistatic properties, and a print-receiving layer having a predetermined thickness, thereby completing the present invention.
[0008] That is, the above objects can be achieved by the present invention having the following configuration, and the present invention includes the following aspects and configurations.
[0009] One aspect of the present invention is 1. A recording paper having a base layer, an antistatic layer, and a print-receiving layer laminated in this order, wherein the antistatic layer contains a reaction product of a cationic polymer and a silane coupling agent, and an antistatic agent, the print-receiving layer contains pigment particles and a binder resin, and the thickness of the print-receiving layer is 0.1 μm or more and less than 3 μm.
[0010] 2. In the recording paper described in 1 above, it is preferable that the cationic polymer has a primary or secondary amino group, or a primary or secondary ammonium salt structure.
[0011] 3. In the recording paper according to 1. or 2. above, it is preferable that the binder resin is water-insoluble.
[0012] 4. In the recording paper according to any one of the above 1. to 3., the content of the antistatic agent in the antistatic layer is preferably 10 to 50% by mass with respect to the total mass of the antistatic layer.
[0013] 5. In the recording paper according to any one of 1. to 4. above, it is preferable that the antistatic agent contains a diallyldimethylammonium salt.
[0014] 6. In the recording paper according to any one of 1. to 5. above, it is preferred that the antistatic layer contains inorganic particles, and the content of the inorganic particles in the antistatic layer is 9 parts by mass or less per 100 parts by mass of the cationic polymer.
[0015] 7. In the recording paper according to any one of the above items 1. to 6., it is preferable that the antistatic layer does not contain thermoplastic resin particles.
[0016] 8. The recording paper according to any one of 1. to 7. above is preferably used for electrophotographic printing. Effect of the Invention
[0017] According to the present invention, it is possible to provide a recording paper having good antistatic properties and water resistance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic cross-sectional view of a recording paper according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a recording paper according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The configuration of the recording paper will be described below with reference to the drawings. In the description of the drawings, the same elements are given the same reference numerals and duplicated descriptions will be omitted. Also, the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.
[0020] FIG. 1 is a schematic cross-sectional view of a recording paper 1 according to an embodiment of the present invention. As shown in FIG. 1, the recording paper 1 has a configuration in which a base layer 2, an antistatic layer 3, and a print-receiving layer 4 are laminated in this order. When the recording paper 1 is used, printing is performed on the surface of the print-receiving layer 4 opposite to the antistatic layer 3 (not shown). Here, the antistatic layer 3 contains a reaction product of a cationic polymer and a silane coupling agent, and an antistatic agent. The print-receiving layer 4 contains pigment particles and a binder resin, and the thickness of the print-receiving layer 4 is 2 μm (0.1 μm or more and less than 3 μm). In the embodiment shown in FIG. 1, the base layer 2 is a multilayer body in which a synthetic resin film 23, an adhesive layer 22, a paper material 21, an adhesive layer 22, and a synthetic resin film 23 are laminated in this order.
[0021] The present inventors have surprisingly found that the recording paper having the above-mentioned constitution has good antistatic properties and also excellent water resistance. The mechanism by which the constitution of the present invention exerts the above-mentioned effect is presumed to be as follows.
[0022] When providing antistatic performance to recording paper, etc., a layer having antistatic performance is generally placed on the surface of the recording paper, etc. This is because many antistatic agents exhibit antistatic performance by being present near the surface of the recording paper, etc. For example, surfactant-based antistatic agents, which are common antistatic agents, form a film by arranging polar hydrophilic groups on the surface side, and this film adsorbs moisture in the outside air to form a multilayer arrangement of water molecules on the surface, thereby leaking static electricity.
[0023] However, the recording paper according to the present invention has antistatic properties, even though the antistatic agent is contained not in the print-receiving layer, which is the surface layer, but in the layer adjacent to the inside of the print-receiving layer (i.e., the antistatic layer). This is thought to be because the print-receiving layer is less than a certain thickness, and the polarity of the antistatic agent contained in the antistatic layer also acts on the surface of the print-receiving layer, and an appropriate amount of water molecules necessary for leakage of static electricity is adsorbed on the surface of the print-receiving layer. Furthermore, as described above, although an appropriate amount of water molecules is present on the surface of the print-receiving layer, no hydrophilic groups having polarity are present, so the print-receiving layer has excellent water resistance.
[0024] It is speculated that the above mechanism allows the recording paper of the present invention to have good antistatic properties and excellent water resistance. Note that the above mechanism is merely speculation and does not limit the technical scope of the present invention in any way.
[0025] Fig. 2 is a schematic cross-sectional view of a recording paper 1 according to another embodiment of the present application. As shown in Fig. 2, in this other embodiment, an antistatic layer 3 and a print-receiving layer 4 are disposed on both sides of a base layer 2. That is, in the embodiment shown in Fig. 2, the print-receiving layer 4, the antistatic layer 3, the base layer 2, the antistatic layer 3, and the print-receiving layer 4 are disposed in this order.
[0026] The configuration of the recording paper 1 according to this embodiment has been described above. Next, the materials constituting each member of the recording paper 1 will be described.
[0027] In this specification, the range "X to Y" means "X or more and Y or less". In addition, unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity 40 to 50% RH. In addition, "A and / or B" includes each of A and B and all combinations of one or more, specifically, it means at least one of A and B, and it means A, B, and a combination of A and B. In addition, the term "(meth)acrylic" includes both acrylic and methacrylic. Thus, for example, the term "(meth)acrylic acid" includes both acrylic acid and methacrylic acid.
[0028] <Base material layer> The recording paper according to the present invention has a structure in which an antistatic layer and a print-receiving layer are laminated on a base layer in this order from the base layer side. The base layer imparts physical strength such as bending elasticity and tensile elasticity to the recording paper, as well as whiteness and opacity as a recording paper. The base layer may also impart water resistance and durability to the recording paper.
[0029] Examples of the base layer include paper, olefin resin film, synthetic paper, etc., but a water-resistant synthetic resin film laminated on one or both sides of a water-resistant paper is preferable. By adopting a base layer having such a configuration, the water resistance of the recording paper can be significantly improved.
[0030] The lamination of the water-resistant paper material and the water-resistant synthetic resin film can be carried out by a known method such as dry lamination or melt lamination, etc. A more preferred lamination method is the dry lamination method in which an adhesive layer is provided between the base material layer and the synthetic resin film and they are bonded together.
[0031] The thickness of the substrate layer is not particularly limited, but is preferably 40 μm to 500 μm, more preferably 50 μm to 400 μm, and even more preferably 80 μm to 300 μm. By having the substrate thickness within the above range, the recording paper becomes suitable for various printing methods, and furthermore, the physical strength described above becomes more sufficient.
[0032] (Paper material) As a paper material, the water absorption rate according to the Cobb method based on JIS-P-8140:1998 is 0 g / m 2 ~50g / m 2 The paper preferably has a water resistance in the range of 0 g / m 2 ~40g / m 2 More preferably, it is 0 g / m 2 ~30g / m 2 It is particularly preferred that:
[0033] The paper material may be, for example, a pulp base paper coated or impregnated with a coating agent that imparts water resistance, or a pulp base paper coated or fused with a synthetic resin having water resistance. More specifically, processed papers such as diazo-sensitive paper base paper, photographic paper base paper, resin-impregnated paper, resin-coated paper, parchment paper, pseudo-parchment paper, water-resistant paper, grease-resistant paper, and waterproof paper can be used as the paper material.
[0034] The thickness of the paper material is preferably 20 μm to 300 μm, and more preferably 50 μm to 250 μm. The thickness of the paper material can be measured based on JIS-P-8118:1998.
[0035] (Synthetic resin film) By using a synthetic resin film, the recording paper has heat resistance, durability, suitable electrostatic capacity, and the like, which makes it particularly suitable for information recording by electrophotographic recording.
[0036] The synthetic resin film preferably has a thickness of 5 μm to 100 μm, and more preferably 12 μm to 50 μm.
[0037] In addition, the synthetic resin film preferably has water resistance and / or insulation. Examples of synthetic resins that impart water resistance and / or insulation to the synthetic resin film include crystalline ethylene resins such as high density polyethylene, medium density polyethylene, and low density polyethylene, crystalline propylene resins, poly(4-methylpent-1-ene), and crystalline olefin resins such as ethylene-cyclic olefin copolymers; polyamide resins such as nylon-6, nylon-6,6, nylon-6,10, and nylon-6,12; thermoplastic polyester resins such as polyethylene terephthalate and copolymers of the same monomer with other components, polyethylene naphthalate, polylactic acid, and aliphatic polyester; and thermoplastic resins such as polycarbonate, atactic polystyrene, isotactic polystyrene, syndiotactic polystyrene, and polyphenylene sulfide. These synthetic resins can be used alone or in a mixture of two or more.
[0038] Among these thermoplastic resins, from the viewpoint of imparting heat resistance particularly suitable for electrophotographic recording systems, it is preferable to use a resin having a melting point in the range of 180°C to 300°C based on JIS-K-7121:1987 as the main component. Therefore, as thermoplastic resins capable of forming the synthetic resin film of the present invention, polyamide-based resins (about 180 to 270°C), poly(4-methylpent-1-ene) (about 230°C), isotactic polystyrene (about 240°C), polycarbonate (about 250°C), polyester-based resins (about 260°C), syndiotactic polystyrene (about 270°C), polyphenylene sulfide (about 280°C), and the like are preferable. If a resin having a melting point of 180° C. or more is used as the main component of the synthetic resin film, the synthetic resin film is unlikely to deform or melt due to heat in the toner fixing process, and therefore it tends to be easier to prevent the recording paper itself from deforming significantly, sticking to a toner fixing device (such as a heat fusion roll), or damaging the recording device. If a resin having a melting point of 300° C. or less is used, a film with a uniform thickness is easily produced, and homogeneous information recording tends to be easy. In addition, the main component of the present invention is one that occupies 50% to 100% by mass of the entire synthetic resin film. If it is 50% by mass or more, the synthetic resin film tends to easily exhibit the desired performance. In addition, the synthetic resin film may contain other thermoplastic resins, fillers, etc.
[0039] Among these thermoplastic resins, polyester resins are particularly preferred as the main component. Examples of polyester resins include polyesters obtained by polycondensation of at least one bifunctional carboxylic acid, such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, bis-α,β(2-chlorophenoxy)ethane-4,4'-dicarboxylic acid, adipic acid, and sebacic acid, and at least one glycol, such as ethylene glycol, triethylene glycol, tetramethylene glycol, hexamethylene glycol, and decamethylene glycol. Furthermore, examples of polyesters obtained by polycondensation of the above-mentioned bifunctional carboxylic acids and glycols with hydroxycarboxylic acids capable of polycondensation.
[0040] Among these polyester resins, polyethylene terephthalate obtained by polycondensation of terephthalic acid and ethylene glycol is particularly preferred because it can easily give a film of uniform thickness, is easy to process, and can impart an appropriate electrostatic capacitance that is neither excessive nor insufficient.
[0041] (adhesive layer) When the base layer according to one embodiment is formed from the above-mentioned paper material and synthetic resin film, it is preferable to use an adhesive layer for bonding them together and laminate them via this adhesive layer.
[0042] In lamination, an adhesive layer is first provided on a paper material or a synthetic resin film by a method such as coating, spraying, melt extrusion lamination, etc. Then, the paper material and the synthetic resin film can be laminated via the adhesive layer by a normal method such as dry lamination or melt lamination using a heat-sealable film or a melt extrusion film.
[0043] The adhesive is not particularly limited, but a solvent-based adhesive or a hot melt adhesive can be used.
[0044] Examples of the solvent-based adhesive include solution-type and emulsion-type adhesives in which a specific resin component is dissolved, dispersed, emulsified, or diluted using a conventionally known solvent. Examples of the specific resin include acrylic resins, urethane resins, ether resins, ester resins, epoxy resins, rubber resins, silicone resins, and ABS resins. The solvent-based adhesive has the characteristic of being fluid and coatable.
[0045] The solvent-based adhesive is applied by a die coater, a bar coater, a comma coater, a lip coater, a roll coater, a rod coater, a curtain coater, a gravure coater, a spray coater, a blade coater, a reverse coater, an air knife coater, a slide hopper, etc. Thereafter, smoothing is performed as necessary, and a drying process is performed to form an adhesive layer.
[0046] The solvent-based adhesive preferably has a solid content after drying of 0.5 to 25 g / m 2 The adhesive is applied so that the adhesive layer is provided.
[0047] When a solvent-based adhesive is used, the adhesive is applied to the surface of the paper material, then a synthetic resin film is placed on top of it and pressure-bonded with a pressure roll, or the adhesive is applied to the back surface of the synthetic resin film, then the paper material is placed on top of it and pressure-bonded with a pressure roll.
[0048] Examples of hot melt adhesives include polyolefin resins such as low density polyethylene, ethylene-vinyl acetate copolymer, metal salts of ethylene-(meth)acrylic acid copolymer (known as Surlyn), chlorinated polyethylene, chlorinated polypropylene, polyamide resins, polybutyral resins, and urethane resins.
[0049] When using a hot melt adhesive, it can be applied to the surface of the paper material by bead coating, curtain coating, slot coating, or the like, or it can be extruded from a die into a molten film and laminated onto the surface of the paper material, and then a synthetic resin film, which is a synthetic resin film, can be placed on top and pressure-bonded with a pressure roll. The adhesive layer using a hot melt adhesive should have a density of 5 to 50 g / m2. 2 It is preferable that the distance between the electrodes is set so as to be equal to or larger than the distance between the electrodes.
[0050] The thickness of the adhesive layer is not particularly limited, but is preferably 1 μm to 50 μm, more preferably 1.5 μm to 30 μm, and even more preferably 2 μm to 10 μm. When the thickness of the adhesive layer is within the above range, the adhesive layer has more sufficient adhesion.
[0051] The adhesive layer may contain an ultraviolet absorbing agent that absorbs any part of the wavelengths from 280 to 400 nm. By containing an ultraviolet absorbing agent, it is possible to form an adhesive layer with an ultraviolet blocking function. By containing an ultraviolet absorbing agent in the adhesive layer, discoloration (yellowing) of the paper material can be suppressed, and long-term use outdoors is possible. Here, the type and content of the ultraviolet absorbing agent contained in the adhesive layer are the same as those described in the ultraviolet blocking layer described later.
[0052] <Antistatic layer> The antistatic layer is a layer containing a reaction product of a cationic polymer and a silane coupling agent, and an antistatic agent, and is a layer for imparting antistatic properties and water resistance to the recording paper.
[0053] The antistatic layer is a layer that can be formed by applying a coating liquid containing a cationic polymer, a silane coupling agent, and an antistatic agent (hereinafter also referred to as a coating liquid for forming an antistatic layer) to a base layer or the like, and then drying the applied liquid.
[0054] Here, the reaction rate between the cationic polymer and the silane coupling agent does not have to be 100%. That is, the antistatic layer may further contain at least one of an unreacted cationic polymer and an unreacted silane coupling agent in addition to the reactant (reaction product).
[0055] The cationic polymer (unreacted portion), the silane coupling agent (unreacted portion), and the reaction product of the cationic polymer and the silane coupling agent in the antistatic layer and the coating liquid for forming the antistatic layer can be confirmed by time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0056] The thickness of the antistatic layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. The thickness of the antistatic layer is preferably 5 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less. That is, the thickness of the antistatic layer is preferably 0.1 μm to 5 μm, more preferably 0.5 μm to 4 μm, and even more preferably 1 μm to 3 μm. By making the thickness of the antistatic layer 0.1 μm or more, the antistatic layer can be formed uniformly and stably, and the water resistance of the antistatic layer becomes sufficient, and the antistatic agent performance of the recording paper becomes more sufficient. In addition, by making the thickness of the antistatic layer 5 μm or less, there is a tendency that the decrease in adhesion with adjacent layers (for example, a base layer or a print receiving layer) due to cohesive failure of the antistatic layer can be suppressed.
[0057] (cationic polymer) In the antistatic layer, the cationic polymer is contained as a reaction product with the silane coupling agent, however, as described above, the antistatic layer may contain unreacted cationic polymer.
[0058] The cationic polymer is preferably water-soluble. The cationic polymer may have a solubility to such an extent that the cationic polymer is in a solution state in an aqueous medium when preparing a coating liquid for forming an antistatic layer.
[0059] Examples of cationic polymers that can be used include (meth)acrylic polymers or ethyleneimine polymers having an amino group or ammonium salt structure, water-soluble polymers having a phosphonium salt structure, and vinyl polymers obtained by cationizing water-soluble polymers such as polyvinylpyrrolidone and polyvinyl alcohol through modification. One of these can be used alone or two or more can be used in combination. Among these, (meth)acrylic polymers or ethyleneimine polymers having an amino group or ammonium salt structure are preferred from the viewpoint of increasing adhesion to the print-receiving layer, and (meth)acrylic polymers or ethyleneimine polymers having an amino group are more preferred. In this specification, cationic polymers having antistatic properties are classified as antistatic agents as "cationic polymer-type antistatic agents" and are not included in the concept of "cationic polymers". For example, cationic polymer-type antistatic agents having a quaternary ammonium salt structure or a quaternary phosphonium salt structure are excluded from cationic polymers.
[0060] From the viewpoint of safety, the (meth)acrylic polymer or ethyleneimine polymer having an amino group or an ammonium salt structure preferably has a primary to tertiary amino group or a primary to tertiary ammonium salt structure, more preferably has a secondary or tertiary amino group or a secondary or tertiary ammonium salt structure, and even more preferably has a tertiary amino group or a tertiary ammonium salt structure. In addition, from the viewpoint of obtaining a resin with a high degree of crosslinking by reaction with a silane coupling agent and obtaining high adhesion to other layers, the cationic polymer preferably has a primary to tertiary amino group or a primary to tertiary ammonium salt structure, more preferably has a primary or secondary amino group or a primary or secondary ammonium salt structure, and even more preferably has a primary amino group or a primary ammonium salt structure.
[0061] Among them, ethyleneimine-based polymers are preferred. The use of ethyleneimine-based polymers tends to increase adhesion to the print-receiving layer. In addition, ethyleneimine-based polymers tend to easily form a crosslinked structure with a silane coupling agent, and tend to suppress a decrease in adhesion to adjacent layers (e.g., a substrate layer or a print-receiving layer) caused by cohesive failure of the antistatic layer.
[0062] Examples of the ethyleneimine-based polymer include polyethyleneimine, poly(ethyleneimine-urea), ethyleneimine adducts of polyamine polyamides, their alkyl-modified products, cycloalkyl-modified products, aryl-modified products, allyl-modified products, aralkyl-modified products, benzyl-modified products, cyclopentyl-modified products, cyclic aliphatic hydrocarbon-modified products, glycidol-modified products, and hydroxides thereof. Examples of the modifier for obtaining the modified products include methyl chloride, methyl bromide, n-butyl chloride, lauryl chloride, stearyl iodide, oleyl chloride, cyclohexyl chloride, benzyl chloride, allyl chloride, cyclopentyl chloride, and the like.
[0063] Among these, an ethyleneimine-based polymer represented by the following general formula (I) is preferred because it tends to enhance adhesion to the print-receiving layer and can further suppress a decrease in adhesion to adjacent layers (e.g., a base layer or a print-receiving layer) due to cohesive failure of the antistatic layer.
[0064] [ka]
[0065] [In the above formula (I), R 1 and R 2 R each independently represents a hydrogen atom; a linear or branched alkyl group having 1 to 12 carbon atoms; an alkyl group having an alicyclic structure having 6 to 12 carbon atoms, or an aryl group. 3represents a hydrogen atom; an alkyl group or an allyl group having 1 to 18 carbon atoms which may contain a hydroxyl group; or an alkyl group or an aryl group having an alicyclic structure having 6 to 12 carbon atoms which may contain a hydroxyl group. m represents an integer of 2 to 6, and n represents an integer of 20 to 3000.
[0066] Commercially available products can also be used as the (meth)acrylic polymer or ethyleneimine polymer having an amino group or an ammonium salt structure. Commercially available products of the (meth)acrylic polymer having an amino group or an ammonium salt structure include Polyment (Nippon Shokubai Co., Ltd.). Commercially available products of the ethyleneimine polymer include Epomin (Nippon Shokubai Co., Ltd.), Polymin SK (manufactured by BASF), and Saftomer AC-72 (manufactured by Mitsubishi Chemical Corporation).
[0067] The weight average molecular weight of the (meth)acrylic polymer or ethyleneimine polymer having an amino group or an ammonium salt structure is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 25,000 or more, from the viewpoint of improving the adhesion between the antistatic layer and the substrate layer and the print-receiving layer. On the other hand, the weight average molecular weight is preferably 1,000,000 or less, and more preferably 500,000 or less. In the present invention, the weight average molecular weight and number average molecular weight of the resin can be obtained by converting the value measured by GPC (Gel Permeation Chromatography) into polystyrene equivalent.
[0068] The content of the cationic polymer component (total amount of unreacted portion and reacted portion with silane coupling agent) in the antistatic layer is preferably 10% by mass or more, more preferably 20% by mass or more, and more preferably 30% by mass or more, based on the total mass of the antistatic layer. The content of the cationic polymer component (total amount of unreacted portion and reacted portion with silane coupling agent) is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less, based on the total mass of the antistatic layer. By having the content of the cationic polymer in the above range, the water resistance of the antistatic layer is further improved, and the antistatic property of the recording paper is also further improved.
[0069] (Silane coupling agent) In the antistatic layer, the silane coupling agent is contained as a reaction product with the cationic polymer, however, as described above, the antistatic layer may contain unreacted silane coupling agent.
[0070] The silane coupling agent can have the effect of increasing the adhesion between the antistatic layer and other adjacent layers (e.g., a substrate layer or a print-receiving layer). Here, the other layer adjacent to the antistatic layer means other layers in contact with both surfaces of the antistatic layer (e.g., both the substrate layer and the print-receiving layer), or other layers in contact with either surface of the antistatic layer (e.g., either the substrate layer or the print-receiving layer).
[0071] Specifically, it is presumed that the silane coupling agent has a functional group that is highly reactive with organic materials, and that this functional group crosslinks the thermoplastic resin and cationic polymer contained in the adjacent layer to enhance adhesion. In addition, the improved adhesion can also prevent moisture from penetrating between the antistatic layer and the adjacent layer, thereby suppressing peeling between the antistatic layer and the adjacent layer. In addition, it is presumed that the silane coupling agent crosslinks cationic polymers to form a network structure, which enhances the cohesive force of the antistatic layer and suppresses the decrease in adhesion between the antistatic layer and the adjacent layer due to cohesive failure. In addition, it is presumed that the silane coupling agent crosslinks cationic polymers to increase the molecular weight of the hydrophilic component (polar resin component) of the cationic polymer, thereby improving water resistance.
[0072] As the silane coupling agent, a silane coupling agent having a group that reacts with a cationic polymer, for example, various functional groups such as a silanol group, can be used. The group that reacts with a cationic polymer refers to a group that reacts with an atom or atomic group of the cationic polymer to form a bond. The bond formed by the reaction may be any of a covalent bond, an ionic bond, a hydrogen bond, etc.
[0073] For example, as the silane coupling agent, a silane compound having, in its molecule, an alkoxysilyl group or a silanol group generated by hydrolysis of the alkoxysilyl group, and at least one functional group selected from the group consisting of an epoxy group, a vinyl group, a (meth)acrylic group, an amino group, a ureido group, a mercapto group, and an isocyanate group can be preferably used.
[0074] It is presumed that the silane coupling agent performs a crosslinking reaction by condensing the silanol group with the thermoplastic resin contained in the adjacent layer, while the functional group other than the silanol group performs a condensation reaction with the amino group or the (meth)acrylic acid residue in the (meth)acrylic polymer having an ammonium salt structure contained in the antistatic layer, or the amino group in the ethyleneimine polymer. Alternatively, it is presumed that the silane coupling agent performs a condensation reaction with the amino group or the (meth)acrylic acid residue in the (meth)acrylic polymer having an ammonium salt structure contained in the antistatic layer, while the functional group other than the silanol group is bound with the thermoplastic resin contained in the adjacent layer with high affinity, thereby performing a crosslinking reaction.
[0075] The content of alkoxysilyl groups or silanol groups generated by hydrolysis thereof in the silane coupling agent is preferably 25% to 75%, more preferably 50% to 75%, from the viewpoint of strong adhesion between the antistatic layer and other adjacent layers. The content of reactive functional groups other than alkoxysilyl groups or silanol groups generated by hydrolysis of the alkoxysilyl groups in the silane coupling agent is preferably 25% to 75%, more preferably 25% to 50%.
[0076] Examples of silane coupling agents that have the above-mentioned effects include epoxy-based silane coupling agents, vinyl-based silane coupling agents, (meth)acrylic-based silane coupling agents, amino-based silane coupling agents, ureido-based silane coupling agents, mercapto-based silane coupling agents, and isocyanate-based silane coupling agents.
[0077] These silane coupling agents may be used alone or in combination of two or more. When two or more types are used in combination, the content of the silane coupling agents refers to the total amount.
[0078] Among these, from the viewpoint of adhesion to printing inks and toners, it is preferable to use epoxy-based silane coupling agents, amino-based silane coupling agents, mercapto-based silane coupling agents, and isocyanate-based silane coupling agents. It is more preferable to use a blocking agent.
[0079] From the viewpoint of ease of crosslinking reaction with the primary to tertiary amino groups of the cationic polymer, it is preferable to use an epoxy-based silane coupling agent, a ureido-based silane coupling agent, or an isocyanate-based silane coupling agent, and it is more preferable to use an epoxy-based silane coupling agent.
[0080] It is known that the hydrolysis rate of the silane coupling agent can be controlled by the type of alkoxysilyl group, and this property can be utilized to suppress the deterioration of the coating liquid for forming the antistatic layer due to the self-condensation of the silane coupling agent, and to improve the stability over time. From the viewpoints of high solubility in water, easy preparation of the coating liquid for forming the antistatic layer, and high stability over time, epoxy-based silane coupling agents are preferred as the silane coupling agent, and 3-glycidoxypropyltrimethoxysilane is particularly preferred.
[0081] In the antistatic layer, the alkoxysilyl group in the silane coupling agent molecule is converted to a silanol group by hydrolysis. It is presumed that the silanol group forms a chemical bond such as hydrogen bond with a functional group such as a hydroxyl group or a carboxyl group on another layer adjacent to the antistatic layer, particularly on a surface-treated layer, thereby improving the adhesion between the antistatic layer and the other adjacent layer. It is also presumed that the condensation reaction between the silanol groups improves the cohesive force of the antistatic layer itself and improves the physical strength of the antistatic layer.
[0082] From the viewpoint of improving water resistance, the content of the silane coupling agent component (total amount of unreacted and reacted components) in the antistatic layer is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 70 parts by mass or more, per 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted components) in the antistatic layer. The content of the silane coupling agent component (total amount of unreacted and reacted components) in the antistatic layer is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 100 parts by mass or less, per 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted components) in the antistatic layer.
[0083] The content of the silane coupling agent component (total amount of unreacted and reacted) in the antistatic layer is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, based on the total mass of the antistatic layer. The content of the silane coupling agent component (total amount of unreacted and reacted) in the antistatic layer is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less, based on the total mass of the antistatic layer.
[0084] The amount of silane coupling agent contained in the antistatic layer is within the above range, so that the amount of unreacted silane coupling agent remaining in the antistatic layer can be suppressed. This makes the hardness of the antistatic layer appropriate, so that it can follow the bending of the recording paper, and can prevent the antistatic layer from cracking. In addition, the amount of silane coupling agent is within the above range, so that the amount of unreacted cationic polymer remaining can be suppressed, so that the water resistance of the antistatic layer is excellent.
[0085] (Antistatic agent) The antistatic agent is used to impart antistatic properties to the antistatic layer.
[0086] The antistatic agent contained in the antistatic layer is not particularly limited, and a conventionally known antistatic agent can be used. Both high molecular weight and low molecular weight antistatic agents can be used, and cationic, anionic, amphoteric or nonionic antistatic agents can also be used. These can be used alone or in combination of two or more. When two or more types are used in combination, the content of the antistatic agent refers to the total amount of them.
[0087] In addition, as the antistatic agent, a compound that reacts with a silane coupling agent or a compound that does not react with a silane coupling agent may be used. However, from the viewpoint of the ease of expressing antistatic performance, a compound that does not react with a silane coupling agent is preferable. Note that the amount of the antistatic agent shown below (mass, mass part, mass %) may include both the antistatic agent that has not reacted with the silane coupling agent and the antistatic agent that has reacted with the silane coupling agent.
[0088] (Polymer-type antistatic agent) Examples of cationic polymeric antistatic agents include those having a quaternary ammonium salt structure, a quaternary phosphonium salt structure, etc. Examples of anionic polymeric antistatic agents include those having an alkali metal salt (lithium salt, sodium salt, potassium salt, etc.) structure of sulfonic acid, phosphoric acid, carboxylic acid, etc. In addition, the anionic polymeric antistatic agent may have an alkali metal salt structure of acrylic acid, methacrylic acid, (anhydrous) maleic acid, etc. in the molecular structure.
[0089] Examples of amphoteric polymeric antistatic agents include those containing both cationic and anionic structures in the same molecule. Examples of amphoteric polymeric antistatic agents include betaine types. Examples of nonionic polymeric antistatic agents include ethylene oxide polymers having an alkylene oxide structure, polymers having ethylene oxide polymerization components in the molecular chain, and the like. Other polymeric antistatic agents include polymeric antistatic agents having boron in the molecular structure.
[0090] Among these, cationic polymer-type antistatic agents are preferred, nitrogen-containing polymer-type antistatic agents are more preferred, polymer-type antistatic agents having a quaternary ammonium salt structure are further preferred, and acrylic resins having a quaternary ammonium salt structure are particularly preferred.
[0091] As the polymer-type antistatic agent, commercially available products can be used. Examples of commercially available polymer-type antistatic agents include Saftomer ST-1000, ST-1100, and ST-3200 (trade names) manufactured by Mitsubishi Chemical Corporation.
[0092] (Low molecular weight antistatic agent) The antistatic agent used in the antistatic layer is preferably a low molecular weight antistatic agent, from the viewpoints of realizing high antistatic performance with a small amount and facilitating control of the water resistance of the antistatic layer.
[0093] Examples of low molecular weight antistatic agents include cationic antistatic agents having a cationic functional group such as quaternary ammonium salts, pyridinium salts, primary, secondary, or tertiary amino groups; anionic antistatic agents having an anionic functional group such as sulfonates, sulfates, phosphonates, and phosphates; and nonionic antistatic agents such as amino alcohols and derivatives thereof, and glycerin and derivatives thereof. Among these, from the viewpoint of enabling stable dispersion in the cationic polymer in the antistatic layer, the antistatic agent preferably contains a low molecular weight cationic antistatic agent, more preferably contains a quaternary ammonium salt, and further preferably contains a quaternary ammonium salt represented by the following chemical formula (2).
[0094] [ka]
[0095] In the above chemical formula (2), R1 and R2 are each independently an alkyl group or a hydroxyalkyl group having 1 to 2 carbon atoms. That is, R1 and R2 are each independently a methyl group, an ethyl group, a hydroxymethyl group, or a hydroxyethyl group. - is the anion (counter anion) that constitutes the quaternary ammonium salt. - There are no particular limitations on the anion, so long as it can form a salt with the quaternary ammonium salt. Examples of such an anion include fluoride ion (F - ), chloride ion (Cl - ), bromide ion (Br - ) and iodide ion (I - ) and other halide ions; hydrogen sulfate ion (HSO4 - ); Sulfite ion (HSO3 - );Alkyl sulfate ion ((Alkyl)SO4 - Alkyl is an alkyl group having 1 to 8 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, preferably ethyl); nitrate ion (NO3 - ); Dihydrogen phosphate ion (H2PO4 - ); Perchlorate ion (ClO4 - ); hydroxide ion (OH - ); carboxylate anions such as acetate ion and lactate ion.
[0096] Among these, R1 and R2 are preferably methyl groups. That is, it is most preferable that the low molecular weight antistatic agent contains a diallyldimethylammonium salt. By containing a diallyldimethylammonium salt in the low molecular weight antistatic agent, high antistatic performance can be imparted to the antistatic layer with a smaller content, and the water resistance of the antistatic layer can be more easily controlled.
[0097] [Diallyldimethylammonium salt] Diallyldimethylammonium salt has the structure represented by the following chemical formula (3):
[0098] [ka]
[0099] In the above chemical formula (3), X2 - is the anion (counter anion) that constitutes the diallyldimethylammonium salt. X2 - As the cation, there is no particular limitation so long as it can form a salt with the diallyldimethylammonium cation. - Among them, the anion (counter anion) is preferably a halide ion, more preferably a chloride ion, a bromide ion or an iodide ion, and particularly preferably a chloride ion. That is, in one embodiment, the diallyldimethylammonium salt is preferably diallyldimethylammonium chloride.
[0100] These diallyldimethylammonium salts may be used alone or in combination of two or more. When two or more types are used in combination, the content of the diallyldimethylammonium salt refers to the total amount.
[0101] In addition, from the viewpoint of further improving the antistatic performance, the content of the antistatic agent in the antistatic layer is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, based on the total mass of the antistatic layer. In addition, from the viewpoint of the water resistance of the antistatic layer, the amount of the antistatic agent contained in the antistatic layer is preferably 50% by mass or less, and more preferably 45% by mass or less, based on the total mass of the antistatic layer. That is, the amount of the antistatic agent contained in the antistatic layer is preferably 10% by mass to 50% by mass, more preferably 15% by mass to 50% by mass, even more preferably 20% by mass to 50% by mass, and particularly preferably 30% by mass to 45% by mass, based on the total mass of the antistatic layer.
[0102] The content of the antistatic agent in the antistatic layer is preferably 15 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and particularly preferably 35 parts by mass or more, relative to 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted components) in the antistatic layer. The content of the antistatic agent in the antistatic layer is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 130 parts by mass or less, relative to 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted components) in the antistatic layer. By the content of the antistatic agent relative to the cationic polymer component being within the above range, the antistatic performance can be further improved, and the water resistance of the antistatic layer can also be made sufficient.
[0103] The content (mass) of the antistatic agent in the antistatic layer can be confirmed by a Fourier transform infrared spectrophotometer (manufactured by JASCO Corporation, product name: FT-IR / 2R-410).
[0104] (Inorganic filler) The antistatic layer may contain an inorganic filler (inorganic particles). Examples of inorganic fillers that may be contained in the antistatic layer include inorganic pigment particles that may be contained in the print-receiving layer described later. However, from the viewpoint of making it easier to obtain antistatic performance and water resistance in some cases for the recording paper, the content of the inorganic filler in the antistatic layer is preferably 9 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the cationic polymer. It is particularly preferable that the antistatic layer does not contain an inorganic filler. Here, the inorganic filler is the same as the inorganic filler contained in the print-receiving layer described later.
[0105] Furthermore, from the viewpoint of improving the antistatic performance of the recording paper, the content of the inorganic filler in the antistatic layer is preferably 5 mass % or less, more preferably 3 mass % or less, and even more preferably 2 mass % or less, relative to the total mass of the antistatic layer, and it is particularly preferable that the antistatic layer does not contain an inorganic filler.
[0106] (thermoplastic resin particles) The antistatic layer may contain thermoplastic resin particles, but it is preferable that the antistatic layer does not contain the thermoplastic resin particles. When the antistatic layer does not contain thermoplastic resin particles, the uniformity of the antistatic layer surface is increased, and a recording paper with excellent appearance can be obtained, and the antistatic performance and water resistance of the recording paper can be more easily obtained. Here, the thermoplastic resin particles can be particles derived from an emulsion of a thermoplastic resin such as an olefin copolymer dispersed in a dispersion medium of a coating liquid for forming an antistatic layer. The fact that the antistatic layer does not contain thermoplastic resin particles and the uniformity of the surface of the antistatic layer can be confirmed by observation with a scanning electron microscope or the like.
[0107] The olefin copolymer emulsion is an emulsion obtained by dispersing or emulsifying an olefin copolymer in the form of fine particles in an aqueous dispersion medium, as disclosed in International Publication WO 2014 / 092142. In this emulsion, a nonionic or cationic surfactant, a nonionic or cationic water-soluble polymer, or the like may be used as a dispersant.
[0108] The olefin copolymer to be dispersed or emulsified in the emulsion may be an olefin copolymer having good emulsifiability and containing a carboxyl group-containing structural unit or a salt thereof as a copolymerization component.
[0109] The olefin copolymer particles in the emulsion usually have a volume average particle size of about 0.2 to 3 μm. The volume average particle size refers to the volume average particle size measured using a laser diffraction type particle size distribution measuring device (SALD-2200, manufactured by Shimadzu Corporation).
[0110] <Print-receiving layer> The print-receiving layer of the recording paper according to this embodiment contains pigment particles and a binder resin, and furthermore, the thickness of the print-receiving layer is 0.1 μm or more and less than 3 μm.
[0111] The thickness of the print-receiving layer is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more. The thickness of the print-receiving layer is preferably 2.8 μm or less, more preferably 2.5 μm or less, and even more preferably 2.0 μm or less. That is, the thickness of the print-receiving layer is preferably 0.5 μm to 2.8 μm, more preferably 1.0 μm to 2.5 μm, and even more preferably 1.5 μm to 2.0 μm. By having the thickness of the print-receiving layer within the above range, the print-receiving layer has functions such as suitability for various printing, and at the same time, the water resistance and antistatic performance become more sufficient.
[0112] (binder resin) The print-receiving layer contains a binder resin to impart toner fixing property and stronger water resistance.
[0113] The binder resin is preferably a water-insoluble binder resin, by which a print-receiving layer having excellent water resistance can be obtained. Here, the term "water-insoluble" binder resin means a binder resin that is completely soluble at 25°C in at least one selected from the group consisting of organic solvents having a solubility parameter (SP value) of 6 to 12, including n-hexane (SP value: 7.3), n-butanol (SP value: 11.4), 2-propanol (SP value: 11.5), toluene (SP value: 8.9), xylene (SP value: 8.8), methyl ethyl ketone (SP value: 9.3), acetone (SP value: 10), methyl isobutyl ketone (SP value: 8.4), cyclohexanone (SP value: 9.9), ethyl acetate (SP value: 9.1), isopropyl acetate (SP value: 8.4), butyl acetate (SP value: 8.5), tetrahydrofuran (SP value: 9.5), ethyl cellosolve (SP value: 9.9), and butyl cellosolve (SP value: 8.9). In addition, the solubility parameter is synonymous with the solubility coefficient, and is a characteristic value of a liquid that is a measure of the miscibility of liquids. If the SP value is δ, the molecular cohesive energy of the liquid is E, and the molecular volume is V, the SP value δ is δ = (E / V) 1 / 2 It is expressed as:
[0114] Examples of the water-insoluble binder resin include urethane resin, terpene resin, petroleum resin, ethylene-vinyl acetate copolymer resin, vinyl chloride resin, vinyl chloride-vinyl acetate copolymer resin, vinylidene chloride resin, vinyl chloride-vinylidene chloride copolymer resin, acrylic acid ester copolymer resin, methacrylic acid ester copolymer resin, chlorinated ethylene resin, chlorinated propylene resin, butyral resin, silicone resin, polyester resin, nitrocellulose resin, styrene-acrylic copolymer resin, styrene-butadiene copolymer resin, etc. These binder resins may be used alone or in combination of two or more. Among these, urethane resins such as polyether urethane, polyester polyurethane, and acrylic urethane or acrylic acid ester copolymer resins are preferred because they have good compatibility (miscibility) with the antistatic agent made of the alkylene oxide compound described above, are stable when mixed together to form a paint, are easy to apply, and have good adhesion to the toner of the resulting print-receiving layer.
[0115] The binder resin content in the print-receiving layer is preferably 10 to 99% by mass, more preferably 15 to 98% by mass, and even more preferably 20 to 97% by mass, based on the total mass of the print-receiving layer. If it is 10% by mass or more, the print-receiving layer can have sufficient cohesive force, so that the image formed by the electrophotographic method tends not to peel off. If it is 99% by mass or less, the antistatic effect tends to be easily obtained.
[0116] (pigment particles) The print-receiving layer contains pigment particles. In this specification, pigment particles is a general term for inorganic pigment particles and organic pigment particles. When the print-receiving layer contains pigment particles, the fixation of ink can be improved.
[0117] The type of inorganic pigment particles that can be used in the print receiving layer is not particularly limited as long as it improves the fixability of the ink described above. Specific examples of inorganic pigment particles include silica, heavy calcium carbonate, light calcium carbonate, calcined clay, talc, diatomaceous earth, barium sulfate, magnesium oxide, zinc oxide, titanium dioxide, silicon dioxide, etc. In addition, surface treatments of these with fatty acids, polymer surfactants, antistatic agents, etc. are also included. Among them, silica is preferably used from the viewpoint of improving the fixability of the toner due to oil absorption. The type of organic pigment particles of the pigment particles that can be used in the print receiving layer is also not particularly limited as long as it improves the fixability of the ink described above. Specific examples of organic pigment particles include acrylic particles, styrene particles, polyethylene particles, polypropylene particles, etc. The pigment particles may be selected from these and used alone, or two or more types may be used in combination.
[0118] The upper limit of the particle size of the pigment particles is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and particularly preferably 5 μm or less. When the upper limit of the particle size of the pigment particles is the above value, the pigment particles are less likely to fall off from the formed print-receiving layer, so that the powdering phenomenon tends to be less likely to occur. The lower limit of the particle size of the pigment particles is not particularly limited, but is preferably 0.1 μm or more.
[0119] The content of pigment particles in the print-receiving layer is preferably 1 to 70% by mass, more preferably 1 to 60% by mass, and even more preferably 1 to 45% by mass, based on the total mass of the print-receiving layer. By having the content of pigment particles in the above range, the print-receiving layer tends to have sufficient cohesive strength, making it easier to prevent peeling of an image formed by an electrophotographic method.
[0120] (UV blocking layer) The recording paper according to one embodiment may have an ultraviolet blocking layer. The ultraviolet blocking layer is preferably provided between the paper material and the synthetic resin film in the above-mentioned base layer. The ultraviolet blocking layer is a layer containing an ultraviolet absorbing agent and / or an ultraviolet reflecting agent. By providing the recording paper with an ultraviolet blocking layer, discoloration (yellowing) of the paper material inside can be suppressed, and long-term use outdoors becomes possible. The ultraviolet blocking layer may be integrated with the above-mentioned adhesive layer, or may be provided separately.
[0121] The ultraviolet absorbing agent that can be used in the ultraviolet blocking layer is one that absorbs a part of light having a wavelength of 280 to 400 nm. For example, it is one of benzotriazole-based, benzophenone-based, salicylate-based, cyanoacrylate-based, nickel-based, or triazine-based, or a mixture thereof, and either low-molecular-weight or high-molecular-weight types can be used.
[0122] Specific examples of benzotriazole-based ultraviolet absorbers include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(1-methyl-1-phenylethyl)-5'-1,1,3,3-tetramethylbutylphenyl)benzotriazole, and 2-(2'-hydroxy-3'-t-butyl-5'-(2-octyloxycarbonyl)ethylphenyl)benzotriazole. Specific examples of benzophenone-based ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'dimethoxybenzophenone, and 2,2',4,4'-tetrahydroxybenzophenone. Specific examples of salicylate-based ultraviolet absorbers include phenyl salicylate, 4-t-butylphenyl salicylate, and 2,4-di-t-butylphenyl-3',5'-di-t-butyl-4'-hydroxybenzoate. Specific examples of cyanoacrylate-based ultraviolet absorbers include ethyl (β,β-diphenyl) cyanoacrylate and 2-ethylhexyl (β,β-diphenyl) cyanoacrylate. Specific examples of nickel-based ultraviolet absorbers include [2,2-thiobis(4-t-octylphenolate)]-n-octylamine nickel salt, [2,2-thiobis(4-t-octylphenolate)]-2-ethylhexylamine nickel salt, nickel dibutyldithiocarbamate, etc. Specific examples of triazine-based ultraviolet absorbers include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol, etc.Among them, benzotriazole-based ultraviolet absorbers are preferred, and 2-(2'-hydroxy-3'-(1-methyl-1-phenylethyl)-5'-1,1,3,3-tetramethylbutylphenyl)benzotriazole (CAS No. 73936-91-1) and 2-(2'-hydroxy-3'-t-butyl-5'-(2-octyloxycarbonyl)ethylphenyl)benzotriazole (CAS No. 127519-17-9) are preferred. The above ultraviolet absorbers can be used alone or in combination of two or more.
[0123] The ultraviolet reflecting agent that can be used in the ultraviolet blocking layer is one that reflects and / or scatters a part of light having a wavelength of 280 to 400 nm. For example, it is any one of zinc oxide, titanium oxide, cerium oxide, tungsten oxide, and strontium titanate, or a mixture thereof. These ultraviolet reflecting agents can be used alone or in combination of two or more.
[0124] As described above, the ultraviolet blocking layer is a layer containing an ultraviolet absorbing agent and / or an ultraviolet reflecting agent, and preferably contains at least one ultraviolet absorbing agent. By containing an ultraviolet absorbing agent in the ultraviolet blocking layer, when a printed matter using the recording paper is used outdoors, the amount of ultraviolet light irradiated to the toner or coating layer can be more effectively reduced, and discoloration and deterioration of the toner can be more effectively prevented. This makes it possible to more sufficiently prevent the reduction in the clarity of the recorded image and the reduction in the adhesion of the image.
[0125] The content of the ultraviolet absorbing agent in the ultraviolet blocking layer is preferably 1 to 50% by mass, more preferably 2 to 40% by mass, and more preferably 5 to 30% by mass, based on the total mass of the ultraviolet blocking layer. When the content of the ultraviolet absorbing agent is within the above range, a clear recorded image tends to be easily obtained due to the effect of suppressing discoloration of the recording paper itself, and the water resistance and solvent resistance of the ultraviolet blocking layer also tends to be easily obtained.
[0126] The ultraviolet blocking layer may be a single layer or may have a multi-layer structure of two or more layers. In addition, the ultraviolet blocking layer is preferably colorless and transparent or white in view of the use of the recording paper.
[0127] Methods for forming the ultraviolet blocking layer include coextrusion with paper and / or synthetic resin film, melt lamination onto paper and / or synthetic resin film, and coating onto paper and / or synthetic resin film.
[0128] Among these, a method of preparing a coating material by mixing a known binder component with an ultraviolet absorbing agent and / or an ultraviolet reflecting agent, and applying the coating material to a paper material or a synthetic resin film to form a coating film is preferred. Specific examples of known binder components include oxidized starch, etherified starch, methoxycellulose, carboxymethylcellulose, hydroxyethylcellulose, casein, gelatin, soy protein, polyvinylhydrin, polyacrylamide, vinyl alcohol, polyacrylic acid, ester urethane resin, ether urethane resin, acrylic urethane resin, terpene resin, petroleum resin, ethylene-vinyl acetate copolymer resin, vinyl chloride resin, vinyl chloride-vinyl acetate copolymer resin, vinylidene chloride resin, vinyl chloride-vinylidene chloride copolymer resin, acrylic acid ester copolymer resin, methacrylic acid ester copolymer resin, butyral resin, silicone resin, polyester resin, nitrocellulose resin, styrene-acrylic copolymer resin, and styrene-butadiene copolymer resin. Among these, polyacrylic acid, ester urethane resin, ether urethane resin, acrylic urethane resin, ethylene-vinyl acetate copolymer resin, acrylic acid ester copolymer resin, methacrylic acid ester copolymer resin, styrene-acrylic copolymer resin, and styrene-butadiene copolymer resin can be mentioned.
[0129] The thickness of the ultraviolet blocking layer is preferably 0.1 μm to 30 μm, more preferably 0.3 μm to 25 μm, and even more preferably 0.5 μm to 20 μm. By having the thickness in the above range, discoloration of the recording paper itself and deterioration of the clarity of the recorded image can be effectively prevented, and since it is easy to produce a recording paper with a uniform thickness, it becomes easier to obtain a uniform recorded image.
[0130] Therefore, the layer structure of the base material layer having an independent ultraviolet blocking layer may include synthetic resin film / ultraviolet blocking layer / adhesive layer / paper material, synthetic resin film / adhesive layer / ultraviolet blocking layer / paper material, synthetic resin film / adhesive layer / ultraviolet blocking layer / adhesive layer / paper material. The layer structure of the base material layer in which the ultraviolet blocking layer is integrated with the adhesive layer may include synthetic resin film / ultraviolet blocking layer (adhesive layer) / paper material.
[0131] (Other base layers) The base layer may be made of an olefin resin film or synthetic paper instead of the above-mentioned paper material or a laminate of paper material and synthetic resin film.
[0132] (Olefin resin film) The olefin resin film preferably contains an olefin resin and inorganic and / or organic fine powder. Here, the olefin resin film more preferably contains 35 to 99 mass% of the olefin resin and 1 to 65 mass% of the inorganic and / or organic fine powder. Still more preferably, the olefin resin film contains 50 to 95 mass% of the olefin resin and 5 to 50 mass% of the inorganic and / or organic fine powder.
[0133] Examples of the olefin-based resin contained in the olefin-based resin film include ethylene-based resins such as high-density polyethylene and medium-density polyethylene, and olefin-based resins such as propylene-based resins, poly(4-methylpent-1-ene), and ethylene-cyclic olefin copolymers. Furthermore, a mixture of two or more of these resins may be used. Among these, it is preferable to use high-density polyethylene and propylene-based resins in terms of cost, water resistance, and chemical resistance.
[0134] Examples of propylene-based resins include polypropylene, which is a propylene homopolymer exhibiting isotactic, syndiotactic and various stereoregularities, and copolymers of propylene as the main component with α-olefins such as ethylene, butene-1, hexene-1, heptene-1, 4-methylpentene-1, etc. The copolymers may be binary, ternary or quaternary, and may be random or block copolymers.
[0135] The inorganic fine powder contained in the olefin resin film may be, for example, calcium carbonate, calcined clay, silica, diatomaceous earth, talc, titanium oxide, barium sulfate, alumina, etc., and may have an average particle size of 0.01 to 15 μm. The organic fine powder contained in the olefin resin film may be preferably one having a melting point or a high glass transition temperature higher than the melting point of the main component resin that is the matrix of the olefin resin film, and incompatible with the olefin resin. Specifically, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, nylon-6, nylon-6,6, homopolymers of cyclic olefins, copolymers of cyclic olefins and ethylene, etc., may be mentioned, which have a melting point of 120°C to 300°C, or a glass transition temperature of 120°C to 280°C.
[0136] The structure of the olefin-based resin film may be any of a single-layer structure, a two-layer structure of a base layer and a surface layer, a three-layer structure in which a surface layer is laminated on both sides of a base layer, and a multilayer structure in which another resin film layer is interposed between the base layer and the surface layer. These multilayer structures can be produced by known methods such as coextrusion, melt lamination, and dry lamination.
[0137] When the olefin resin film has a multi-layer structure having a base layer and a surface layer, the base layer preferably contains 45 to 98% by mass of an olefin resin and 2 to 55% by mass of inorganic and / or organic fine powder. The surface layer preferably contains 25 to 100% by mass of an olefin resin and 75% or less by mass of inorganic and / or organic fine powder or contains no inorganic and / or organic fine powder. More preferably, the base layer contains 50 to 95% by mass of an olefin resin and 5 to 50% by mass of inorganic and / or organic fine powder, and the surface layer contains 30 to 99% by mass of an olefin resin and 1 to 70% by mass of inorganic and / or organic fine powder.
[0138] The olefin resin film may further contain a heat stabilizer, a light stabilizer, a dispersant, a lubricant, etc., as necessary. For example, as the heat stabilizer, a sterically hindered phenol-based, phosphorus-based, amine-based, or other stabilizer may be contained in an amount of 0.001 to 1 mass% based on the total mass of the olefin resin film. As the light stabilizer, a sterically hindered amine, benzotriazole-based, benzophenone-based, or other stabilizer may be contained in an amount of 0.001 to 1 mass% based on the total mass of the olefin resin film. As a dispersant for inorganic fine powder, a silane coupling agent, a higher fatty acid such as oleic acid or stearic acid, a metal soap, etc. may be blended in an amount of 0.01 to 4 mass% based on the total mass of the olefin resin film.
[0139] The olefin-based resin film that can be used for the base layer is preferably a stretched film that is stretched at least in one axial direction during the molding process. Films having fine internal voids due to the stretching can improve the opacity of the recording paper and can also improve the electrostatic capacitance.
[0140] As a method for stretching the resin film, a conventionally known method can be applied, and examples thereof include longitudinal stretching using the difference in peripheral speed between a group of rolls, rolling (longitudinal stretching) using a number of rolls, transverse stretching using a tenter, sequential biaxial stretching combining the longitudinal stretching and the transverse stretching, simultaneous biaxial stretching using a combination of a tenter and a linear motor, simultaneous biaxial stretching by a tubular method, and simultaneous biaxial stretching using a pantograph type stretching machine. The temperature during stretching is appropriately selected according to the type of olefin resin used and the stretching process. Specifically, it is preferable to set the temperature to 110 to 164°C in the case of propylene homopolymer (melting point 155 to 167°C) and 80 to 120°C in the case of high density polyethylene (melting point 121 to 134°C), which is 2 to 60°C lower than the melting point. The stretching speed is preferably 20 to 350 m / min.
[0141] The stretching ratio is not particularly limited and is appropriately selected depending on the purpose and the properties of the olefin resin used. For example, when a propylene homopolymer or a propylene copolymer is used and uniaxial stretching is performed, the stretching ratio is preferably 1.2 to 12 times, more preferably 2 to 10 times, and when biaxial stretching is performed, the area stretching ratio is preferably 1.5 to 60 times, more preferably 10 to 50 times. When another olefin resin is used and uniaxial stretching is performed, the area stretching ratio is preferably 1.2 to 10 times, more preferably 2 to 5 times, and when biaxial stretching is performed, the area stretching ratio is preferably 1.5 to 20 times, more preferably 4 to 12 times. After stretching, a heat treatment (annealing treatment) is performed as necessary.
[0142] By stretching the olefin resin film under the above conditions, fine voids (air holes) are formed inside the film, making it suitable as a paper material for recording paper with an opacity (JIS P-8138) of 85% or more, preferably 90% or more, and a porosity defined by the following formula (1) of 10% to 60%, preferably 15% to 45%.
[0143]
number
[0144] (ρ0 indicates the true density of the resin film, and ρ indicates the density of the resin film) If the porosity of the stretched film is 10% or more, it tends to be easier to adjust the whiteness, opacity, and weight of the recording paper; conversely, if the porosity is 60% or less, it tends to be easier to obtain the strength (tensile strength, bending strength) of the recording paper.
[0145] The thickness of the olefin resin film is preferably in the range of 20 μm to 300 μm, and more preferably 50 μm to 250 μm. If the film thickness is 20 μm or more, it tends to be easier to produce a stretched film having voids, and if it is 300 μm or less, it tends to be easier to supply the final recording paper to the market in a wound roll form. Note that the olefin resin film has a capacitance of 4 pF / cm 2 ~1000pF / cm 2 It is preferable to use one in which:
[0146] <Optional ingredients> In the present invention, each layer may contain known additives as necessary to the extent that they do not affect the effects of the present invention. Examples of such additives include known additives such as antioxidants, light stabilizers, ultraviolet absorbers, dispersants for inorganic fillers, slip agents such as fatty acid amides, antiblocking agents, dyes, pigments, plasticizers, crystal nucleating agents, release agents, flame retardants, etc. In particular, when durability is required for the recording paper, such as poster paper used outdoors, it is preferable to contain antioxidants, light stabilizers, etc.
[0147] <Method of manufacturing recording paper> The method for producing the recording paper is not particularly limited, but examples include a method in which an antistatic layer is formed on a base layer, and a print-receiving layer is formed on the side of the antistatic layer opposite to the side on which the base layer is present.
[0148] The method for forming the antistatic layer is not particularly limited, but it is preferable to form the antistatic layer by a method including dissolving the above-mentioned components constituting the antistatic layer in a solvent to prepare a coating liquid for forming the antistatic layer, applying the prepared coating liquid for forming the antistatic layer to at least one surface of the substrate layer, and drying (drying and solidifying) the applied coating liquid for forming the antistatic layer.
[0149] The method for forming the print-receiving layer is not particularly limited, but it is preferable to form the print-receiving layer by a method including dissolving each of the above-mentioned components constituting the print-receiving layer in a solvent to prepare a coating liquid for forming the print-receiving layer, applying the prepared coating liquid for forming the print-receiving layer to the side of the antistatic layer opposite to the side on which the substrate layer is present, and drying (drying and solidifying) the applied coating liquid for forming the print-receiving layer.
[0150] Therefore, in another embodiment, the present invention also provides a method for producing a recording paper, which includes the steps of: forming an antistatic layer by applying a coating liquid for forming an antistatic layer containing a cationic polymer, a silane coupling agent, and an antistatic agent on a substrate layer and drying the coating liquid; and forming a print-receiving layer by applying a coating liquid for forming a print-receiving layer containing pigment particles and a binder resin on the surface of the antistatic layer opposite to the surface on which the substrate layer is present and drying the coating liquid. This allows the recording paper to be produced by roll-to-roll production, improving productivity. Furthermore, the thickness of the print-receiving layer can be adjusted relatively easily, so that a recording paper having the desired characteristics can be produced.
[0151] [Antistatic layer coating solution] The coating liquid can be prepared by mixing the above-mentioned components constituting the antistatic layer with a solvent.
[0152] The solvent used in this case may be water, or an organic solvent such as methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, methyl ethyl ketone, ethyl acetate, toluene, or xylene, or may be a mixed solvent of water and an organic solvent. The solvent is preferably water or a solvent containing water as the main component. In this specification, the term "main component" means that 95% by mass or more, preferably 99% by mass or more (upper limit 100% by mass) of the entire solvent used in the coating liquid is water. This makes process management easier and is also preferable from the viewpoint of safety.
[0153] The solid content in the coating liquid for forming the antistatic layer is preferably 0.5% by mass or more, and more preferably 2% by mass or more, based on the total weight of the coating liquid. The solid content in the coating liquid is preferably 40% by mass or less, and more preferably 25% by mass or less.
[0154] In addition, the method of preparing the coating liquid for forming the antistatic layer is not particularly limited, and an example thereof includes a method of adding each component constituting the antistatic layer to a mixing vessel, adding a solvent (preferably water) to obtain a desired solid content concentration, and mixing. The method of adding each component to the mixing vessel may be a lump sum or a sequential addition. In the latter case, the order of addition is not particularly limited. The temperature when mixing each component is not particularly limited, but 10 to 40°C is preferable, and heating may be performed to increase the dissolution rate. In addition, the mixing time is not particularly limited.
[0155] [Coating solution for forming print-receiving layer] The printing-receiving layer-forming coating liquid can be prepared by dissolving the above-mentioned components constituting the printing-receiving layer in a solvent.
[0156] The solvent used in this case is not particularly limited, but since the binder resin contained in the print-receiving layer is preferably water-insoluble, an organic solvent is preferable. Examples of the organic solvent include general organic solvents, and there are no particular limitations. The solubility parameter (hereinafter abbreviated as SP value) is preferably in the range of 6 to 12, more preferably 7 to 11.
[0157] Specific examples of solvents with an SP value of 6 to 12 include n-hexane (SP value: 7.3), n-butanol (SP value: 11.4), 2-propanol (SP value: 11.5), toluene (SP value: 8.9), xylene (SP value: 8.8), methyl ethyl ketone (SP value: 9.3), acetone (SP value: 10), methyl isobutyl ketone (SP value: 8.4), cyclohexanone (SP value: 9.9), ethyl acetate (SP value: 9.1), isopropyl acetate (SP value: 8.4), butyl acetate (SP value: 8.5), tetrahydrofuran (SP value: 9.5), ethyl cellosolve (SP value: 9.9), and butyl cellosolve (SP value: 8.9). If the SP value is 12 or less, the solubility of the binder resin is improved, and when a crosslinking agent is used, the crosslinking reaction is prevented from starting in the solution, making it easier to increase the stability of the paint. If the SP value is 6 or more, the volatility is not excessively high and it tends to be easy to handle.
[0158] In addition, the method of preparing the coating liquid for forming the print-receiving layer is not particularly limited, and an example thereof is a method of adding each component constituting the print-receiving layer to a mixing vessel, adding a solvent (preferably an organic solvent) to obtain a desired solid content concentration, and mixing. In this case, from the viewpoint of obtaining a recording paper with good ink adhesion, it is preferable to prepare a binder resin solution in which the binder resin is dissolved in a solvent in advance, and mix it with other components.
[0159] The method of adding each component to the mixing vessel may be the same as the coating liquid for forming the antistatic layer, and may be added all at once or successively. In the latter case, the order of addition is not particularly limited. The temperature at which each component is mixed is not particularly limited, but is preferably 10 to 40°C, and may be heated to increase the dissolution rate. The mixing time is also not particularly limited.
[0160] The solid content in the coating liquid for forming the print-receiving layer is preferably 0.5% by mass or more, and more preferably 2% by mass or more, based on the total weight of the coating liquid. The solid content in the coating liquid is preferably 40% by mass or less, and more preferably 25% by mass or less.
[0161] [Coating] The coating liquid for forming the antistatic layer and the coating liquid for forming the print-receiving layer can be applied by a known coating device, specific examples of which include a die coater, a bar coater, a comma coater, a lip coater, a roll coater, a curtain coater, a gravure coater, a spray coater, a blade coater, a reverse coater, and an air knife coater.
[0162] The coating amount of the coating solution for forming the antistatic layer is not particularly limited as long as the antistatic layer has a desired thickness. The coating amount is preferably 0.1 to 20 g / m2 in terms of the solid content after drying. 2 It is preferable that the thickness is 0.5 to 8 g / m 2 It is more preferable that the coating amount is 0.1 g / m 2 If the thickness is more than 20g / m, uniform antistatic performance tends to be obtained. 2 If it is equal to or less than this, the antistatic agent is less likely to have a distribution in the thickness direction depending on the coating conditions and coating environment, and therefore stable antistatic performance and water resistance tend to be easily obtained.
[0163] The amount of the coating liquid for forming the print-receiving layer is not particularly limited as long as the print-receiving layer has a desired thickness. However, the solid content of the print-receiving layer after drying is preferably 0.1 g / m 2 ~5g / m 2 and preferably 0.25 g / m 2 ~3g / m 2 More preferably, it is 0.3 g / m or more. 2 ~1.5g / m 2 By having the coating amount within the above range, it is relatively easy to adjust the coating process, and it is possible to improve the productivity of the printing medium and prevent uneven coating.
[0164] [Drying] After carrying out the coating step as described above, it is preferable to dry the applied coating liquid. In this case, the drying conditions (temperature, time, etc.) are not particularly limited as long as they are conditions that can remove the solvent in the coating liquid. As an example, the drying temperature is preferably 20 to 120°C, and more preferably 35 to 80°C. The drying time is also not particularly limited. In addition, the pressure conditions during drying are not particularly limited, and drying can be carried out under normal pressure (atmospheric pressure), or under increased or reduced pressure.
[0165] The drying means (apparatus) is not particularly limited, and may be, for example, an oven, a reduced pressure dryer, etc. On the other hand, in the case of natural drying, no particular drying means (apparatus) is required.
[0166] <Uses of recording paper> [Recording device] The recording paper according to one embodiment of the present invention is suitable for use in electrophotographic printing, and is capable of good color recording using electrophotographic recording devices such as copiers and laser printers. There are three types of electrophotographic color recording methods: (1) an intermediate transfer method in which one color is transferred to an intermediate transfer body, and then transferred and developed on paper; (2) a tandem method in which two or more photoconductors are used, and one color is transferred to a paper and developed; and (3) a tandem + transfer method in which two or more photoconductors are used, and one color is transferred to an intermediate transfer body, and then transferred and developed on paper. In the present invention, (2) and (3) are collectively referred to as the tandem method. The recording paper according to one embodiment of the present invention can be used in the intermediate transfer method (1), but is preferably used in the tandem methods (2) and (3). In the method (1), in the case of a small electrophotographic copier or the like, the recording paper may be squeezed during transport within the device, making it difficult to use. The tandem methods (2) and (3) are suitable for high speed printing, and because of the structure of the device, the recording paper is less likely to be squeezed during transport, which is preferable.
[0167] The recording paper according to one embodiment of the present invention may be subjected to normal printing, such as oil-based offset printing, UV offset printing, gravure printing, flexographic printing, etc., before recording using the recording device. If necessary, a barcode for management may be printed by these printing methods, a thermal transfer method, or an electrophotographic method. In addition, the recording paper according to one embodiment of the present invention may be subjected to full printing or partial printing on the side opposite the print-receiving layer of the recording paper in order to promote sales and improve visibility. Similarly, the surface of the paper material on which the synthetic resin film is to be laminated may be subjected to full printing or partial printing before the synthetic resin film is laminated. It is preferable that these printings are applied so that the information appears as regular information when viewed through the synthetic resin film.
[0168] [Recordings] Examples of recorded items using the recording paper according to one embodiment of the present invention include POP cards (posters, stickers, displays, etc.), store guides (pamphlets, company guides, product lists, menus, etc.), writing pads (lunch mats, table mats, stationery, etc.), manuals (manuals on duties, tasks, operations, etc., schedules, timetables, etc.), charts (nautical charts, weather charts, diagrams, ruled lines, etc.), catalogs, cards (price cards, point cards, membership cards, various membership cards, student ID cards, driver's licenses, employee ID cards, entry and exit permits, association ID cards, identification cards, student attendance cards, library cards, patient registration cards, management cards, parking permits, ski passes, CDs, MD title cards, CDs, MD index cards, photo cards, etc.), panels, plates (substitutes for metal plates), bromides, preserved documents (word processing documents, various rosters, appraisals, certificates, important documents, awards, etc.), illustrated books, drawings (architectural drawings, civil engineering site drawings, Examples of usable materials include: maps (nautical charts, route maps, outdoor maps, etc.), commuter passes, in-store price lists, mountain climbing guides, business cards, lost child tags, recipes, signboards (sales floor guides, direction / destination guides, snacks / food, etc.), gardening POP (hanging labels, insert labels, etc.), schedules, road signs (funerals, home exhibition areas, etc.), circulars, room nameplates, school record lists, signboards (no entry, forest road work, etc.), boundary posts, nameplates, calendars (with images), simple whiteboards, postcards, greeting cards, flyers, picture books / paper theaters, portable timetables, photo album picture diaries, paper crafts, photocopied manuscripts, fans, megaphones, mouse pads, bookmarks, pet toilets, packaging materials (wrapping paper, boxes, bags, etc.), coasters, flower pots, printed materials that do not require lamination, printed materials as an alternative to label writers, adhesive labels, tags (aviation tags, IC tags, triage tags), etc., all of which can be used. It can be particularly suitably used for paper for printed matter intended for outdoor use.
[0169] Although the embodiments of the present invention have been described in detail, it is clear that the same are illustrative and exemplary, not restrictive, and the scope of the present invention should be interpreted by the appended claims. EXAMPLES
[0170] The effects of the present invention will be explained using the following examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following manufacturing examples and examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the technical scope of the present invention is not limited only to the following examples. The ratios of the raw materials used as the solution or dispersion (units: "parts by mass", "% by mass") are all values calculated as solid content. Unless otherwise specified, each operation was performed at room temperature (25°C).
[0171] [Preparation of base layer] A 25 μm-thick polyethylene terephthalate film (manufactured by Toray Industries, Inc., product name: Lumirror, melting point: 260°C) was used as a synthetic resin film, and an adhesive coating consisting of 60 parts by mass of a polyether urethane adhesive (manufactured by Toyo-Morton Co., Ltd., product name: TM-317), 40 parts by mass of a polyisocyanate curing agent (manufactured by Toyo-Morton Co., Ltd., product name: CAT-11B), and 5 parts by mass of a benzotriazole ultraviolet absorber (manufactured by BASF Japan Ltd., product name: Tinuvin-384-2) was applied to the synthetic resin film at a dry solid content of 4 g / m. 2 The adhesive layer was applied to a 170 μm-thick OTP base paper for photographic paper (manufactured by Oji Paper Co., Ltd., Cobb method water absorption: 24.8 g / m 2 ,Basic weight: 175g / m 2 ) and pressed to obtain a substrate layer having a thickness of 220 μm and a five-layer structure (PET film / adhesive layer / OTP base paper for photographic paper / adhesive layer / PET film).
[0172] [Production of coating solution for forming antistatic layer] The components of the coating solution for forming the antistatic layer will be described below.
[0173] <Aqueous solution of cationic polymer (A)> A commercially available polyethyleneimine resin (manufactured by Mitsubishi Chemical Corporation, product name: Saftomer AC-72), which is a polymer containing primary to tertiary amino groups, was used as the cationic polymer aqueous solution (A).
[0174] <Silane coupling agent (B)> A commercially available silane coupling agent, 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403), was used as the silane coupling agent (B).
[0175] <Antistatic agent (C-1)> A commercially available antistatic agent, diallyldimethylammonium chloride (product name: DADMAC (manufactured by Osaka Soda Co., Ltd.), solid content concentration: 65.8%), was used as the antistatic agent (C-1).
[0176] <Antistatic agent (C-2)> A commercially available polymer-type antistatic agent (product name: Saftomer ST-3200 (manufactured by Mitsubishi Chemical Corporation), solid content concentration: 25% by mass, quaternary ammonium salt) was used as the antistatic agent (C-2).
[0177] <Inorganic filler> Calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd., product name: Softon 1800, average particle size 1.2 μm (measurement method: air permeability method)) was used as the inorganic filler.
[0178] (Preparation Example of Coating Fluid for Forming Antistatic Layer) <Preparation Example 1> An aqueous solution containing 40 parts by mass (solid content equivalent) of the above cationic polymer (A), 30 parts by mass of a silane coupling agent (B), and 30 parts by mass of an antistatic agent (C-1) (solid content equivalent) was prepared as a coating liquid (a) for forming an antistatic layer.
[0179] <Preparation Example 2> An aqueous solution containing 33 parts by mass (solid content equivalent) of the cationic polymer (A), 25 parts by mass of the silane coupling agent (B), 40 parts by mass (solid content equivalent) of the antistatic agent (C-1), and 2 parts by mass of the inorganic filler (D) was prepared as coating liquid (b) for forming an antistatic layer. The ratio of the inorganic filler (D) to the cationic polymer (A) (solid content equivalent) contained in coating liquid (b) for forming an antistatic layer was 6% by mass.
[0180] <Preparation Example 3> An aqueous solution containing 42 parts by mass (solid content equivalent) of the cationic polymer (A), 40 parts by mass of the silane coupling agent (B), 15 parts by mass (solid content equivalent) of the antistatic agent (C-1), and 3 parts by mass of the inorganic filler (D) was prepared as the coating liquid (c) for forming the antistatic layer. The ratio of the inorganic filler (D) to the cationic polymer (A) (solid content equivalent) contained in the coating liquid (c) for forming the antistatic layer was 7% by mass.
[0181] <Preparation Example 4> An aqueous solution containing 35 parts by mass (solid content equivalent) of the above cationic polymer (A), 35 parts by mass of a silane coupling agent (B), and 30 parts by mass (solid content equivalent) of an antistatic agent (C-2) was prepared as a coating liquid (d) for forming an antistatic layer.
[0182] <Preparation Example 5> An aqueous solution containing 34 parts by mass (solid content equivalent) of the cationic polymer (A), 25 parts by mass of the silane coupling agent (B), 40 parts by mass (solid content equivalent) of the antistatic agent (C-2), and 1 part by mass of the inorganic filler (D) was prepared as the coating liquid (e) for forming the antistatic layer. The ratio of the inorganic filler (D) to the cationic polymer (A) (solid content equivalent) contained in the coating liquid (e) for forming the antistatic layer was 3% by mass.
[0183] <Preparation Example 6> An aqueous solution containing 42 parts by mass (solid content equivalent) of the cationic polymer (A), 40 parts by mass of the silane coupling agent (B), 15 parts by mass (solid content equivalent) of the antistatic agent (C-2), and 3 parts by mass of the inorganic filler (D) was prepared as the coating liquid (f) for forming the antistatic layer. The ratio of the inorganic filler (D) to the cationic polymer (A) (solid content equivalent) contained in the coating liquid (f) for forming the antistatic layer was 7% by mass.
[0184] Preparation examples 1 to 6 of the coating solutions (a) to (f) for forming the antistatic layer are shown in Table 2 below.
[0185] [Table 1]
[0186] [Production of coating solution for forming print-receiving layer] Each of the components of Preparation Example A of the coating liquid for forming the print-receiving layer will be described below.
[0187] <Preparation Example A of Coating Solution for Forming Print Receptive Layer> (Preparation example of mixed solution of binder resin and hardener) 15 parts by mass of 2-hydroxyethyl methacrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., reagent), 50 parts by mass of methyl methacrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., reagent), 35 parts by mass of ethyl acrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., reagent), and 100 parts by mass of toluene were charged into a three-necked flask equipped with a stirrer, a reflux condenser, and a thermometer, and after nitrogen replacement, 0.6 parts by mass of 2,2'-azobisisobutyronitrile (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., reagent) was added as an initiator and polymerized at 80°C for 4 hours. The resulting solution was a 50% by mass toluene solution of a hydroxyl group-containing (meth)acrylic acid ester copolymer resin with a hydroxyl value of 65. Next, 40 parts by mass of a 20% by mass solution of vinyl chloride-vinyl acetate copolymer (manufactured by Shin-Daiichi Vinyl Co., Ltd., product name: ZEST C150ML) in methyl ethyl ketone and 5.8 parts by mass of a 75% by mass solution of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name: Coronate HL) in ethyl acetate as a curing agent were added to 100 parts by mass of this solution, and a solvent made by mixing toluene and methyl ethyl ketone in a 1:1 ratio was further added to this mixture to adjust the solids content to 20% by mass, thereby obtaining a mixed solution of binder resin and curing agent.
[0188] (pigment particles) As the pigment particles, inorganic pigment particles, precipitated silica (average particle size 1.6 μm, oil absorption 180 ml / 100 g, manufactured by Mizusawa Chemical Industry Co., Ltd., trade name: Mizukasil P-527) and barium sulfate (average particle size 0.3 μm, manufactured by Sakai Chemical Industry Co., Ltd., trade name: BARIACE B-32) were used.
[0189] (Example of preparation of coating liquid) While gently stirring the methyl ethyl ketone with a Cowles mixer, 30 parts by mass of precipitated silica and 15 parts by mass of barium sulfate were added little by little to prepare a solid content concentration of 20% by mass, and then the rotation speed of the Cowles mixer was increased and stirred for 30 minutes to prepare a particle dispersion. Next, the rotation speed of the Cowles mixer was reduced, and the above-mentioned mixed solution of binder resin and hardener was added to this dispersion, and the mixture was stirred for 20 minutes as it was, and then the mixture was passed through a 100 mesh filter to remove coarse particles, thereby preparing a coating liquid (A) for forming a print-receiving layer. The coating liquid (A) for forming a print-receiving layer was prepared so that the blending ratio (parts by mass (solids)) of the binder resin, pigment particles, and hardener in the print-receiving layer formed using the coating liquid (A) was the value shown in Preparation Example A in Table 2.
[0190] <Preparation Example B of Coating Solution for Forming Print Receptive Layer> In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen gas inlet tube, 40 parts by mass of dimethylaminoethyl methacrylate, 20 parts by mass of ethyl methacrylate, 20 parts by mass of cyclohexyl methacrylate, 150 parts by mass of ethyl alcohol, and 1 part by mass of 2,2'-azobisisobutyronitrile were added. After replacing the inside of the system with nitrogen, a polymerization reaction was carried out for 6 hours at a temperature of 80°C under a nitrogen gas flow. The obtained copolymer was neutralized with glacial acetic acid (manufactured by Wako Pure Chemical Industries, Ltd.). Ethyl alcohol was distilled off while dropping water to obtain an aqueous solution with a concentration of 30% by mass of acrylic resin, which was used as a binder resin solution. A commercially available epichlorohydrin adduct of polyamine polyamide (manufactured by Japan PMC Co., Ltd., product name: WS-570 (solid content 12.5% by weight)) was added as a curing agent to this binder resin solution to obtain a mixed solution of binder resin and curing agent.
[0191] Except for using the mixed solution of the binder resin and the curing agent, the printing-receiving layer forming coating liquid (B) was prepared in the same manner as in Preparation Example A of the printing-receiving layer forming coating liquid. The printing-receiving layer forming coating liquid (B) was prepared so that the blending ratio (parts by mass) of the binder resin, pigment particles, and curing agent in the printing-receiving layer formed using the coating liquid (B) was the value shown in Preparation Example B in Table 2.
[0192] <Preparation Example C of Coating Solution for Forming Print Receptive Layer> 100 parts by weight of polyethylene glycol monomethacrylate (manufactured by Nippon Oil & Fats Co., Ltd., product name: Blemmer PE-350), 20 parts by weight of lithium perchlorate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), 1 part by weight of hydroquinone (manufactured by Wako Pure Chemical Industries, Ltd., reagent), and 400 parts by weight of methyl ethyl ketone were introduced into a four-neck flask equipped with a stirrer, a condenser, a nitrogen inlet tube, and a thermometer, the atmosphere in the system was replaced with nitrogen, and the reaction was carried out at 60°C for 40 hours. To this were added 20 parts by weight of stearyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), 20 parts by weight of n-butyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd., reagent), and 1 part by weight of azobisisobutyronitrile (manufactured by Wako Pure Chemical Industries, Ltd., reagent), and a polymerization reaction was carried out at 80°C for 3 hours, after which methyl ethyl ketone was added to adjust the solid content to 20% by weight, thereby obtaining a polymer antistatic agent solution having a weight-average molecular weight of approximately 300,000 and a lithium concentration in the solid content of 0.8% by weight, which was used as an antistatic agent.
[0193] A coating liquid (C) for forming a print-receiving layer was prepared in the same manner as in Preparation Example A of the coating liquid for forming a print-receiving layer, except that the above-mentioned antistatic agent was added to the dispersion in addition to the mixed solution of the binder resin and the curing agent. The coating liquid (C) for forming a print-receiving layer was prepared so that the blending ratio (parts by mass) of the binder resin, pigment particles, antistatic agent, and curing agent in the print-receiving layer formed using the coating liquid (C) was the value shown in Preparation Example C in Table 2.
[0194] [Table 2]
[0195] [Creating a recording sheet] Example 1 The coating liquid for forming the antistatic layer obtained in Preparation Example 1 was applied to one side of the substrate layer using a bar coater so that the thickness after drying would be 2 μm, and the coating liquid was dried in a dryer at 60° C. to form an antistatic layer. Next, the coating liquid for forming the print-receiving layer obtained in Preparation Example A was applied to the surface of the dried antistatic layer (the side opposite to the side on which the substrate layer is present) using a bar coater so that the thickness after drying would be 2 μm, and the coating liquid was dried in a dryer at 70° C. to obtain the recording paper of Example 1.
[0196] (Examples 2 to 7, Comparative Examples 1 to 5) Examples 2 to 7 and Comparative Examples 1 to 5 were prepared in the same manner as Example 1, except that the coating liquid for forming the print-receiving layer, the coating liquid for forming the antistatic layer, and the thicknesses of each after drying were set to the values shown in Table 3. In addition, "-" in the table means that the corresponding layer is not provided. In other words, Comparative Examples 1 and 3 are examples of recording paper not provided with an antistatic layer, and Comparative Example 4 is an example of recording paper not provided with a print-receiving layer.
[0197] [evaluation] The recording papers prepared above in Examples 1 to 7 and Comparative Examples 1 to 5 were evaluated for antistatic properties and water resistance according to the following methods. The results are shown in Table 3.
[0198] <Antistatic properties> The surface resistivity of the print-receiving layer side surface of each recording paper was measured under the conditions of a temperature of 23°C and a relative humidity of 50% and a temperature of 10°C and a relative humidity of 30%. 7 For resistances of Ω or more, measurements were performed using a double ring electrode in accordance with JIS K6911: 2006. The results are shown in Table 3 using common logarithms.
[0199] "water resistance" A color laser printer (manufactured by Casio Corporation, product name: N4-612II) was used to record a test image on the print receiving layer of each recording paper using four color toners: yellow, cyan, magenta, and black. The recording paper on which the test image was recorded was then immersed for 24 hours in water (ion-exchanged water) adjusted to 40°C that had been filled in a vat, so that the paper would not float. The immersed recording paper was attached to a Gakushin-type dyeing abrasion fastness tester (manufactured by Suga Test Instruments Co., Ltd., device name: abrasion tester type II) and subjected to a friction test in which the paper was rubbed 100 times with a white cotton cloth moistened with water at a load of 500 g. The recorded image was rubbed hard with a coin and visually evaluated according to the following evaluation criteria.
[0200] -Evaluation criteria- ○: No change in the recorded image.
[0201] Δ: Peeling occurs in part of the rubbed portion of the recorded image.
[0202] ×: Peeling occurs over the entire surface of the rubbed portion of the recorded image.
[0203] In addition to the above evaluation, the recording sheets of Examples 1 to 7 and Comparative Examples 1 to 5 were also evaluated for toner transferability in accordance with the following method.
[0204] <Toner transferability> Using a color laser printer (manufactured by Casio Corporation, product name: N4-612II), test images were recorded on the print-receiving layer of each recording paper using four color toners: yellow, cyan, magenta, and black. The recording quality, such as density, color tone, and gradation, was visually evaluated according to the following evaluation criteria.
[0205] -Evaluation criteria- ◯: Density, color tone, and gradation are all good.
[0206] △: The recording density is slightly low.
[0207] x: Any one of density, color tone, and gradation is poor and unsuitable for use.
[0208] [Table 3]
[0209] As shown in Table 3, the recording papers of Examples 1 to 7 all had excellent water resistance while maintaining excellent antistatic properties, whereas Comparative Examples 1 to 5 were inferior in either antistatic properties or water resistance.
[0210] The recording papers of Examples 1 to 7 also showed good results in terms of toner transferability. [Explanation of symbols]
[0211] 1 Recording paper, 2 base material layer, 21 Paper materials, 22 adhesive layer, 23 Synthetic resin film, 3 Antistatic layer, 4 Print receptive layer.
Claims
1. A recording paper having a base layer, an antistatic layer, and a print-receiving layer laminated in this order, the antistatic layer comprises a reaction product of a cationic polymer and a silane coupling agent, and an antistatic agent; the print-receiving layer comprises pigment particles and a binder resin; The recording paper, wherein the print-receiving layer has a thickness of 0.1 μm or more and less than 3 μm.
2. 2. The recording paper according to claim 1, wherein the cationic polymer has a primary or secondary amino group, or a primary or secondary ammonium salt structure.
3. 3. The recording paper according to claim 1, wherein the binder resin is water-insoluble.
4. 3. The recording paper according to claim 1, wherein the content of the antistatic agent in the antistatic layer is 10 to 50% by mass with respect to the total mass of the antistatic layer.
5. 3. The recording paper according to claim 1, wherein the antistatic agent comprises a diallyldimethylammonium salt.
6. 3. The recording paper according to claim 1, wherein the antistatic layer contains inorganic particles, and the content of the inorganic particles in the antistatic layer is 9 parts by mass or less per 100 parts by mass of the cationic polymer.
7. 3. The recording paper according to claim 1, wherein the antistatic layer does not contain thermoplastic resin particles.
8. 3. The recording paper according to claim 1, which is used for electrophotographic printing.
Citation Information
Patent Citations
Electrophotographic recording paper and recorded matter
JP2008299017A