Polishing pad and method for manufacturing polishing workpiece
The polishing pad with a polyurethane resin and controlled polysiloxane diol and polyethylene glycol content addresses the issue of edge sag by enhancing water repellency and slurry affinity, achieving a high polishing rate and good edge shape.
Patent Information
- Application Number
- JP2023057118
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional polishing pads often prioritize polishing rate over edge shape, leading to excessive polishing at the edges of the object, resulting in edge sag and reduced yield and productivity.
A polishing pad composed of a resin sheet containing a polyurethane resin with specific proportions of polysiloxane diol and polyethylene glycol, which enhances water repellency and affinity with the slurry, preventing edge sag and maintaining a good end shape.
The polishing pad achieves an excellent polishing rate while preventing edge sag, ensuring a flat finish and improved yield by maintaining the edge shape of the polished object.
Smart Images

Figure 2024144933000006 
Figure 2024144933000007 
Figure 2024144933000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad and a method for producing a polished workpiece. [Background technology]
[0002] In general, polishing is performed using a polishing pad on optical materials such as lenses, plane-parallel plates, and reflecting mirrors, semiconductor wafers, semiconductor devices, substrates for hard disks, metals, ceramics, and other materials. Chemical mechanical polishing (CMP) is widely used as a method for such polishing. In general, in CMP, polishing is performed by sliding a polishing pad over the surface of a semiconductor wafer to be polished, while a polishing liquid containing an abrasive component and chemical components such as an oxidizing agent, a chelating agent, and acidic or alkaline components is caused to flow down onto the surface of the polishing pad as necessary.
[0003] As a polishing pad for CMP, various polishing pads have been proposed from the viewpoints of ensuring the polishing rate and flatness, suppressing scratches, etc. For example, Patent Document 1 proposes a polishing molded body that is a polymer of monomers containing a polymer diol, an organic diisocyanate, a first chain extender containing a diol having 4 or less carbon atoms, and a second chain extender containing a diol having 5 or more carbon atoms, and is non-porous. Patent Document 2 proposes a chemical mechanical polishing pad including a polishing layer that is a polyurethane reaction product of a reaction mixture containing a curing agent and a polyisocyanate prepolymer having an unreacted isocyanate (NCO) concentration of 8.3 to 9.8% by weight. Patent Document 3 proposes a polishing pad having a polishing layer made of a polyurethane resin foam, the polyurethane resin foam being a reaction cured product of a polyurethane raw material composition including an isocyanate-terminated prepolymer containing an isocyanate component, a high molecular weight polyol, and a polysiloxane group-containing diol, and a chain extender. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6541683 [Patent Document 2] Patent No. 6981823 [Patent Document 3] Patent No. 5875300 Summary of the Invention [Problem to be solved by the invention]
[0005] According to Patent Document 1, the polishing pad described in the same document is evaluated to have excellent moldability and to exhibit high planarization when used as a polishing layer. According to Patent Document 2, the chemical mechanical polishing pad described in the same document is evaluated to provide an improved defect rate without a decrease in the planarization efficiency of the polishing pad. According to Patent Document 3, the polishing pad described in the same document is evaluated to have high hydrophobicity, improve the slurry dischargeability of the polishing layer, and reduce the water absorption and swelling of the polishing layer, so that the polishing rate can be suppressed from decreasing even when polishing is performed for a long time.
[0006] Thus, although Patent Documents 1 to 3 are considered from the viewpoint of polishing rate and flatness, recently, polishing pads with a higher level of balance between polishing rate and flatness are being aimed for. Here, the inventor has studied that when polishing is performed with a conventional polishing pad that emphasizes polishing rate, the edge of the polished object tends to be polished excessively. In this case, as a result, the edge of the polished object tends to have a shape in which the thickness is rapidly reduced in a narrow range, and such a phenomenon is hereinafter referred to as "edge sagging". In addition, hereinafter, a shape in which edge sagging is prevented is intended to be referred to as "good edge shape". As described above, the techniques described in Patent Documents 1 to 3 still have room for improvement in terms of achieving both an excellent polishing rate and providing a good edge shape to the workpiece.
[0007] The present invention has been made in consideration of the above problems, and has an object to provide a polishing pad etc. which has an excellent polishing rate and gives a good edge shape to an object to be polished. [Means for solving the problem]
[0008] As a result of intensive research by the present inventors to solve the above problems, they discovered that the above problems could be solved by a polishing pad containing specific components, and thus completed the present invention.
[0009] That is, the present invention is as follows. [1] A polishing pad comprising a resin sheet having a polishing surface, the resin sheet contains a polyurethane resin, The polyurethane resin is A unit (a) derived from a polysiloxane diol (A) represented by the following formula (I), A unit (b) derived from polyethylene glycol (B); having The content of the unit (a) is 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin; The content of the unit (b) is 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin. [ka] (In formula (I), each R independently represents an organic group having 1 to 10 carbon atoms or a hydrogen atom, and n represents an integer of 5 to 25.) [2] The polishing pad according to [1], wherein the polysiloxane diol (A) comprises a polysiloxane diol (A1) in which all of the R in the formula (I) are methyl groups. [3] The polishing pad according to [1] or [2], wherein the resin sheet has an A hardness of 50 degrees or more and a DO hardness of 90 degrees or less. [4] The density of the resin sheet is 0.3 to 0.6 g / cm 3 The polishing pad according to any one of [1] to [3], [5] A method for producing a polished product, comprising a polishing step of polishing a workpiece with the polishing pad according to any one of [1] to [4] in the presence of a polishing slurry. [6] The method for producing a polished product according to [5], wherein the polished product is a silicon wafer. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polishing pad and the like which has an excellent polishing rate and gives a good edge shape to an object to be polished. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the measurement results of the flatness of a silicon wafer polished using the polishing pad of Example 1. [Diagram 2] FIG. 2 is a graph showing the measurement results of the flatness of a silicon wafer polished using the polishing pad of Comparative Example 1. [Diagram 3] FIG. 3 is a graph showing the measurement results of the flatness of a silicon wafer polished using the polishing pad of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0013] [Polishing pad] The polishing pad of this embodiment is a polishing pad comprising a resin sheet having a polishing surface, the resin sheet containing a polyurethane resin, the polyurethane resin having units (a) derived from polysiloxane diol (A) represented by the above formula (I) and units (b) derived from polyethylene glycol (B), the content of the units (a) being 0.3 to 10.0 mass% relative to 100 mass% of the polyurethane resin, and the content of the units (b) being 0.3 to 10.0 mass% relative to 100 mass% of the polyurethane resin. The polishing pad of this embodiment has the above-mentioned configuration, and therefore has an excellent polishing rate and can give a good edge shape to the polished object. The polishing pad of this embodiment can particularly prevent the edge sagging of the polished object. If the edge sagging occurs and the edge shape is damaged, for example, in the polishing process of a semiconductor wafer, it becomes difficult to obtain a product from the edge vicinity, resulting in a problem of reduced yield and productivity. However, by using the polishing pad of this embodiment, the edge shape can be improved by finishing it flat to the outer edge vicinity.
[0014] The polishing pad of this embodiment is provided with at least a predetermined resin sheet having a polishing surface. That is, the polishing pad of this embodiment may be made of only the resin sheet of this embodiment, or may have a configuration other than the resin sheet. In this embodiment, the configuration other than the resin sheet may include various known polishing layers, cushion layers, adhesive layers, etc.
[0015] In this embodiment, "resin sheet having an abrasive surface" means that at least one surface of the abrasive pad of this embodiment corresponds to the surface of the resin sheet of this embodiment, and that the surface of the resin sheet becomes the abrasive surface that is pressed against the workpiece during polishing in this embodiment.
[0016] The polishing pad of this embodiment may have a groove, embossed, and / or hole (punched) on the polishing surface as required, and may have a light transmitting portion. The shape of the groove and embossed is not particularly limited, and examples thereof include a lattice type, a concentric circle type, and a radial type.
[0017] (Resin sheet) (Polyurethane resin) The resin sheet in this embodiment contains a polyurethane resin. That is, the resin sheet in this embodiment can be obtained by forming the polyurethane resin into a sheet shape, or the like. In general, the polyurethane resin can be specified as a reaction product of at least a polyisocyanate and a polyol, and can also be specified as a reaction product of a urethane prepolymer having at least an isocyanate terminal and a polyamine. In other words, the polyurethane resin generally has a urethane bond in its molecule, and may further have a urea bond.
[0018] The polyurethane resin in this embodiment has units (a) derived from the polysiloxane diol (A) represented by the above formula (I) and units (b) derived from the polyethylene glycol (B).
[0019] (Unit (a)) The unit (a) in this embodiment is derived from the polysiloxane diol (A). The polysiloxane diol (A) is represented by the following formula (I), and by containing a silane-based repeating unit, it is possible to give the polishing pad appropriate water repellency and to suppress the softening of the polishing layer due to the slurry being immersed in the polishing pad. As a result, it is possible to prevent the end sagging. In addition, since the polysiloxane diol (A) has hydroxyl groups at both ends of the molecular chain, the strength of the polishing pad is improved compared to polysiloxane diol having a hydroxyl group at one end. As a result, it is possible to suppress the performance of the polishing pad from changing over time during polishing, and the flatness of the polished object can be further improved. Furthermore, since the side chain R is an organic group having 1 to 10 carbon atoms or a hydrogen atom, it is possible to achieve both an excellent polishing rate and a good end shape for the polished object without affecting the physical properties and reactivity of the polishing pad, and it is also easy to control the physical properties and reactivity of the polishing pad. [ka] (In formula (I), each R independently represents an organic group having 1 to 10 carbon atoms or a hydrogen atom, and n represents an integer of 5 to 25.)
[0020] The unit (a) in this embodiment can also be specified as a chemical structure in which a hydrogen atom has been removed from the terminal OH group of the above formula (I).
[0021] In the above formula (I), each R may be the same group or different groups.
[0022] The organic group having 1 to 10 carbon atoms in the above formula (I) is not particularly limited, but examples thereof include alkyl groups having 1 to 10 carbon atoms. The alkyl group having 1 to 10 carbon atoms is not particularly limited, but examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, 1,2-dimethylpropyl, n-hexyl, n-heptyl, isoheptyl, n-octyl, isooctyl, n-nonyl, n-decyl, and the like.
[0023] In this embodiment, from the viewpoint of imparting appropriate water repellency to the polishing pad, R is preferably an alkyl group having 1 to 5 carbon atoms, more preferably a methyl group. In addition, in this embodiment, from the viewpoint of suppressing the influence on the physical properties and reactivity of the polishing pad and making it easier to control the physical properties and reactivity, it is particularly preferable that the polysiloxane diol (A) contains a polysiloxane diol (A1) in which all of the R in formula (I) are methyl groups.
[0024] In the above formula (I), n is an integer of 5 or more from the viewpoint of imparting appropriate water repellency to the polishing pad, and from the viewpoint of making it easier to adjust the physical properties of the polishing pad, n is an integer of 25 or less. From the same viewpoint as above, n is preferably an integer of 10 to 20.
[0025] The polysiloxane diol (A) can be synthesized based on various known methods, and can also be obtained as a commercially available product.
[0026] The content of the unit (a) is 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin. The content is 0.3% by mass or more from the viewpoint of providing the polishing pad with appropriate water repellency, and 10.0% by mass or less from the viewpoint of having an excellent polishing rate. If the content is less than 0.3% by mass, the slurry may penetrate into the polishing pad, softening the polishing layer and deteriorating the flatness of the polished object, and if it exceeds 10.0% by mass, the polishing pad may become highly water repellent and the polishing rate may decrease. Thus, by having the content of the unit (a) of 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin, it is possible to achieve both an excellent polishing rate and a good edge shape for the polished object without affecting the physical properties and reactivity of the polishing pad, and it is easy to control the physical properties and reactivity of the polishing pad. In addition, the frictional resistance between the polishing layer and the polished object can be reduced, and thermal deterioration such as softening of the polishing layer due to frictional heat can be suppressed. As a result, the workpiece rotates smoothly during polishing, which tends to improve the flatness of the workpiece. From the above viewpoints, the content is preferably 0.3 to 5.0 mass%, more preferably 0.3 to 3.0 mass%. Furthermore, from the same viewpoints as above, the content of the unit derived from the polysiloxane diol (A1) is preferably 0.3 to 10.0 mass%, more preferably 0.3 to 5.0 mass%, and even more preferably 0.3 to 3.0 mass%, based on 100 mass% of the polyurethane resin.
[0027] The content of the unit (a) can be determined from the charge ratio when preparing the polyurethane resin (when preparing the composition described below), or can be determined by analysis using known elemental analysis or structural analysis means.
[0028] (Unit (b)) In this embodiment, the unit (b) is derived from polyethylene glycol (B). That is, the unit (b) is -(CH2-CH2-O) m - (where m represents the number of repeating units and is an arbitrary integer). The range of m is not particularly limited, but may be, for example, 4 to 455.
[0029] The polyethylene glycol (B) is a polymer of ethylene oxide, and although there are no particular limitations, it is preferable that the number average molecular weight is 200 to 20,000 from the viewpoint of ease of handling.
[0030] The polyethylene glycol (B) can be synthesized based on various known methods, or can be obtained as a commercially available product.
[0031] The content of the unit (b) is 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin. The content is 0.3% by mass or more from the viewpoint of increasing the affinity between the polishing pad and the slurry, and 10.0% by mass or less from the viewpoint of suppressing the softening of the polishing layer due to the slurry soaking into the inside of the polishing pad. If the content is less than 0.3% by mass, the affinity between the polishing pad and the slurry may decrease, and the polishing rate may decrease, and if it exceeds 10.0% by mass, the slurry may soak into the inside of the polishing pad, softening the polishing layer, and the polished object may sink into the polishing pad and excessively polish the edge. Thus, by having the content of the unit (b) of 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin, it is possible to achieve both an excellent polishing rate and a good edge shape for the polished object without affecting the physical properties and reactivity of the polishing pad, and it is also easy to control the physical properties and reactivity of the polishing pad. From the above viewpoints, the content is preferably 0.3 to 5.0 mass %, and more preferably 0.3 to 3.0 mass %.
[0032] The content of the unit (b) can be determined from the charge ratio when preparing the polyurethane resin (when preparing the composition described below), or can be determined by analysis using known elemental analysis or structural analysis means.
[0033] (Unit (c)) The polyurethane resin in this embodiment may contain other units (c) that do not fall under the units (a) and (b). The units (c) are not particularly limited, and may be, for example, various units derived from the raw materials of the polyurethane resin in this embodiment. That is, the units (c) may be units derived from various polyurethane resin raw materials described in the [Method of manufacturing a polishing pad] described later. The content of unit (c) is not particularly limited, but can be 80.0 to 99.4 mass%, 90.0 to 99.4 mass%, or 94.0 to 99.4 mass%, taking the polyurethane resin as 100 mass%.
[0034] (Other Ingredients) The resin sheet in this embodiment may contain components derived from additives other than polyurethane resin. Such additives are not particularly limited, but may include, for example, defoamers, catalysts, foaming agents, foam stabilizers, abrasive grains, dyes, pigments, solid fine particles, flame retardants, hydrophilic agents, hydrophobic agents, light resistance agents, antioxidants, and antistatic agents, which will be described later in the method for producing a polishing pad in this embodiment. These may be derived from unreacted raw materials, etc., among the materials used in the production of polyurethane. The additives may be used alone or in combination of two or more.
[0035] (Thickness of resin sheet) The thickness of the resin sheet is not particularly limited, but is preferably 0.5 mm to 10.0 mm, more preferably 0.6 mm to 8.0 mm, and even more preferably 0.7 mm to 5.0 mm. The thickness of the resin sheet is measured in accordance with the measurement method described in JIS K 6505. That is, the thickness of the resin sheet is measured at an initial load of 1 cm in the thickness direction of the resin sheet. 2 This is the thickness when a load of 100g is applied (stressed).
[0036] (Physical properties of resin sheet) (hardness) In this embodiment, from the viewpoint of further improving the flatness of the polished product, the resin sheet preferably has a hardness A of 50 degrees or more. In addition, from the viewpoint of further suppressing scratches on the polished workpiece, it is preferable that the D hardness of the resin sheet in this embodiment is 60 degrees or less, and from the viewpoint of achieving both an excellent polishing rate and imparting a good end shape to the polished workpiece, it is more preferable that the resin sheet in this embodiment has an A hardness of 50 degrees or more and a D hardness of 60 degrees or less. Furthermore, from the viewpoint of further suppressing scratches on the polished workpiece, it is preferable that the DO hardness of the resin sheet in this embodiment is 90 degrees or less, and from the viewpoint of achieving both an excellent polishing rate and imparting a good end shape to the polished workpiece, it is more preferable that the resin sheet in this embodiment has an A hardness of 50 degrees or more and a DO hardness of 90 degrees or less. In particular, when the polished object is a silicon wafer, the resin sheet in this embodiment has both an excellent polishing rate and a good edge shape for the polished object, so that the D hardness is preferably 30 degrees or more and 60 degrees or less. From the same viewpoint as above, the resin sheet in this embodiment more preferably has a DO hardness of 60 degrees or more and 90 degrees or less. The A hardness and DO hardness can be measured based on the method described in the Examples below. The D hardness can be measured using a D-type hardness tester (JIS K 7311). The A hardness, DO hardness and D hardness can be adjusted to fall within the above-mentioned ranges, for example, by adjusting the amounts of the constituent components of the polyurethane resin and the foaming agent added.
[0037] (density) In this embodiment, the density of the resin sheet is not particularly limited, but is, for example, 0.3 to 0.8 g / cm 3 and preferably 0.3 to 0.6 g / cm 3 That is, from the viewpoint of reducing the frictional resistance between the polishing pad and the workpiece to be polished and imparting a better edge shape to the workpiece, the density of the resin sheet is 0.3 g / cm 3 From the viewpoint of further suppressing scratches on the polished product, the density of the resin sheet is preferably 0.6 g / cm or more. 3 It is preferable that: The density can be measured based on the method described in the Examples below. The density can be adjusted to the above range, for example, by adopting the manufacturing method of the polishing pad of the present embodiment described later, etc. For example, in the manufacturing process of the resin sheet of the present embodiment, when the amount of the foaming agent is reduced, the density of the resin sheet tends to be high.
[0038] (Compressibility and Compressive Elasticity) (Compression ratio) The compression ratio of the resin sheet is not particularly limited, but is preferably 0.1 to 10.0%, and more preferably 0.5 to 5.0%. When the compression ratio is within the above range, the polishing pad tends to be able to adequately wipe off and remove the polishing debris present on the workpiece during polishing. Therefore, there is a tendency to be able to suppress microdefects caused by aggregates of polishing debris, etc. The compression ratio can be controlled, for example, by adjusting the size, number, shape, etc. of the bubbles in the resin sheet. The compression ratio is measured according to the following method.
[0039] (Compressive elastic modulus) The compressive elastic modulus of the resin sheet is not particularly limited, but is preferably 65-98%, more preferably 70-95%. By having the compressive elastic modulus within the above range, it tends to be possible to further reduce microdefects in the polished object. The compressive elastic modulus can be controlled, for example, by adjusting the type and composition of the resin used in the resin sheet. The compressive elastic modulus is measured according to the following method.
[0040] (Method of measuring compressibility and compressive elasticity) The compressibility and compressive modulus of the resin sheet are determined using a Shopper-type thickness gauge (pressure surface: circular with a diameter of 1 cm) in accordance with JIS L 1021. Specifically, at room temperature, an initial load is applied for 30 seconds from an unloaded state, and a thickness t0 is measured. Then, a final load is applied from the thickness t0 state, and the sheet is left for 1 minute, after which a thickness t1 is measured. Furthermore, all loads are removed from the thickness t1 state, the sheet is left for 1 minute, and the initial load is again applied for 30 seconds, after which a thickness t0' is measured. From these values, the compressibility and compressive modulus are calculated using the following formula: Compression ratio (%) = (t0-t1) / t0 x 100 Compressive elastic modulus (%) = (t0'-t1) / (t0-t1) x 100 In this case, the initial load is 100g / cm 2 , final load is 1120g / cm 2 Let us assume that.
[0041] [Polishing pad manufacturing method] The method for producing the polishing pad of this embodiment is not particularly limited as long as it is a method that can obtain a polishing pad having the above-mentioned configuration, but for example, the polishing pad can be produced by the following method. That is, the method for producing the polishing pad of this embodiment includes a step of subjecting a composition containing a polyurethane resin raw material to a curing reaction to obtain a resin sheet containing a polyurethane resin. Examples of polyurethane resin raw materials include polyols, polyisocyanates, urethane prepolymers, and polyamines. Examples of the curing reaction include (i) reacting at least a polyol with a polyisocyanate, (ii) reacting at least a urethane prepolymer with a polyamine, and (iii) reacting at least a urethane prepolymer with a polyamine and a polyol. In this embodiment, the units (a) and (b) may each be independently derived from any of polyol, polyisocyanate, and urethane prepolymer, but it is preferable that both the units (a) and (b) are derived from polyol. That is, the curing reaction in this embodiment is the above (iii) reaction of at least urethane prepolymer, polyamine, and polyol, and the polyol preferably contains polysiloxane diol (A) and polyethylene glycol (B). The reason is presumed to be as follows, although it is not intended to be limited to the following. That is, when the urethane prepolymer contains units (a) and / or units (b) derived from polysiloxane diol (A) and / or polyethylene glycol (B), respectively, the viscosity of the composition tends to increase due to the prepolymer, and as a result, uniform stirring cannot be performed in the preparation process of the polyurethane resin, which may cause unevenness in the composition of the obtained resin sheet. On the other hand, when the prepolymer does not contain units (a) and / or units (b) derived from polysiloxane diol (A) and / or polyethylene glycol (B), respectively, an increase in viscosity tends to be prevented, and uniform stirring becomes possible, so that the composition of the obtained resin sheet also tends to be uniform, and a polishing pad having an excellent polishing rate and imparting a good edge shape to the workpiece is obtained.
[0042] A preferred method for producing the polishing pad of this embodiment (hereinafter also referred to as "production method (α)") includes a composition containing polysiloxane diol (A), polyethylene glycol (B), urethane prepolymer (C1), and polyamine (C2), where the urethane prepolymer (C1) is a reaction product of at least a polyisocyanate compound (PI) and a polyol compound (PO), the reaction product having an isocyanate group at the end, and the polyol compound (PO) is different from the polysiloxane diol (A) and the polyethylene glycol (B). The method preferably includes a step of subjecting the composition (hereinafter also referred to as "composition (α)") to a curing reaction to obtain a resin sheet containing a polyurethane resin (hereinafter also referred to as "polyurethane resin (α)"). Here, the polysiloxane diol (A), polyethylene glycol (B), and polyamine (C2) in the composition (α) can function as a curing agent for the urethane prepolymer (C1).
[0043] (composition) The content of the polysiloxane diol (A) in the composition (α) is preferably 0.3 to 10.0 mass% with respect to the composition (α) being 100 mass% from the viewpoint of adjusting the content of the unit (a) in the polyurethane resin (α) to 0.3 to 10.0 mass% with respect to the polyurethane resin (α) being 100 mass%. From the viewpoint of adjusting the content of the unit (a) in the polyurethane resin (α) to a more preferable range, the content of the polysiloxane diol (A) in the composition (α) is more preferably 0.3 to 5.0 mass%, and even more preferably 0.3 to 3.0 mass%. Furthermore, from the same viewpoint as above, the content of the polysiloxane diol (A1) in the composition (α) is preferably 0.3 to 10.0 mass%, more preferably 0.3 to 5.0 mass%, and even more preferably 0.3 to 3.0 mass%, with respect to the composition (α) being 100 mass%. The content of polyethylene glycol (B) in composition (α) is preferably 0.3 to 10.0 mass% with respect to 100 mass% of composition (α) from the viewpoint of adjusting the content of unit (b) in polyurethane resin (α) to 0.3 to 10.0 mass% with respect to 100 mass% of polyurethane resin (α). From the viewpoint of adjusting the content of unit (b) in polyurethane resin (α) to a more preferable range, the content of polyethylene glycol (B) in composition (α) is more preferably 0.3 to 5.0 mass%, and further preferably 0.3 to 3.0 mass%.
[0044] The polyisocyanate compound (PI) is not particularly limited as long as it is a compound having two or more isocyanate groups in the molecule. For example, diphenylmethane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), naphthalene-1,4-diisocyanate, diphenylmethane-4,4'-diisocyanate, 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, xylylene diisocyanate, 1,1'-dimethyl- ... Examples of the diisocyanate include 1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, trimethylene diisocyanate, hexamethylene diisocyanate (HDI), isophorone diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate. Among these, diisocyanate compounds are preferred, and 2,4-TDI, 2,6-TDI, and MDI are more preferred. As the polyisocyanate compound (PI), one type may be used alone, or two or more types may be used in combination.
[0045] The polyol compound (PO) is not particularly limited as long as it is a compound having two or more alcoholic hydroxyl groups (OH) in the molecule and is different from the polysiloxane diol (A) and the polyethylene glycol (B). Specific examples of such compounds include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 3-methyl-1,2-butanediol, 1,2-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, and 3-methyl-4,3-pentanediol. , 3-methyl-4,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol, 2,5-hexanediol, 1,4-cyclohexanedimethanol, diol compounds such as neopentyl glycol, triol compounds such as glycerin, trimethylolpropane, trimethylolethane, trimethylolmethane, etc.; polyether polyol compounds such as polypropylene glycol (PPG) and poly(oxytetramethylene) glycol (PTMG); polyester polyol compounds such as the reaction product of ethylene glycol and adipic acid, the reaction product of butylene glycol and adipic acid, etc.; polycarbonate polyol compounds, polycaprolactone polyol compounds, etc. Also, trifunctional propylene glycol to which ethylene oxide has been added can be used. As the polyol compound (PO), one type may be used alone, or two or more types may be used in combination.
[0046] The polyamine (C2) means a compound having two or more amino groups in the molecule, and for example, a diamine compound can be used. The diamine compound is not particularly limited, but examples thereof include alkylene diamines such as ethylene diamine, propylene diamine, and hexamethylene diamine; diamines having an aliphatic ring such as isophorone diamine and dicyclohexylmethane-4,4'-diamine; diamines having an aromatic ring such as 3,3'-dichloro-4,4'-diaminodiphenylmethane (also known as methylene bis-o-chloroaniline) (hereinafter also referred to as MOCA); diamines having a hydroxyl group such as 2-hydroxyethyl ethylene diamine, 2-hydroxyethyl propylene diamine, di-2-hydroxyethyl ethylene diamine, di-2-hydroxyethyl propylene diamine, 2-hydroxypropyl ethylene diamine, and di-2-hydroxypropyl ethylene diamine. Among these, diamines having an aromatic ring are preferred, and MOCA is more preferred. As the polyamine compound, one type may be used alone, or two or more types may be used in combination.
[0047] The polyurethane resin (α) molecule contains both urethane bonds and urea bonds. That is, in the polyurethane resin (α) molecule, the unit (c1) derived from the urethane prepolymer (C1) contains a urethane bond, and the unit (c2) derived from the polyamine (C2) contains a urea bond. For example, when the polyamine (C2) is MOCA, the unit (c2) can be specified as a chemical structure represented by -NHC(=O)NH-CH(Cl)-CH-CH(Cl)-NHC(=O)NH-.
[0048] In preparing the composition, for example, the polyurethane resin raw materials, polysiloxane diol (A), polyethylene glycol (B), urethane prepolymer (C1) and polyamine (C2), which have been heated to 30°C to 90°C, are charged into a temperature-adjustable jacketed mixer and stirred at 30°C to 130°C. At this time, at least one of the polyurethane resin raw materials may be placed in a tank with a jacket equipped with a stirrer and aged, if necessary. The polyurethane resin raw materials may be stirred and / or aged together. The stirring time may be appropriately adjusted depending on the number of teeth, rotation speed, clearance, etc. of the mixer, and is, for example, 0.1 seconds to 60 seconds.
[0049] The active hydrogen equivalents (e.g., OH equivalent and NH2 equivalent) of the polyols such as the polysiloxane diol (A) and the polyethylene glycol (B), and the polyamine (C2) are not particularly limited, and may be, for example, each independently 50 or more and 5,000 or less, 100 or more and 4,000 or less, or 130 or more and 3,000 or less. The OH equivalent weight of the polysiloxane diol (A) and the polyethylene glycol (B) may each independently be 100 or more and 5,000 or less, 200 or more and 4,000 or less, or 200 or more and 3,000 or less. The NH2 equivalent of the polyamine (C2) may be 50 or more and 2000 or less, 75 or more and 1000 or less, or 100 or more and 300 or less.
[0050] The NCO equivalent of a urethane prepolymer such as the urethane prepolymer (C1) is preferably from 150 to 700, more preferably from 200 to 600, and even more preferably from 200 to 500. The "NCO equivalent" is a numerical value indicating the molecular weight of the urethane prepolymer (C1) per NCO group, which is calculated by "(parts by mass of polyisocyanate compound+parts by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound×parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound)-(number of functional groups per molecule of polyol compound×parts by mass of polyol compound / molecular weight of polyol compound)]".
[0051] The amount of the urethane prepolymer (C1) used is not particularly limited, and is preferably from 30 to 90 parts by mass, more preferably from 40 to 80 parts by mass, based on the total amount of the composition.
[0052] The composition in this embodiment may contain components other than the polysiloxane diol (A), the polyethylene glycol (B), the urethane prepolymer (C1) and the polyamine (C2) as additives having various functions.Specific examples thereof include, but are not limited to, a solvent (diluent) such as polypropylene glycol; an antifoaming agent such as a silicone-based antifoaming agent; a catalyst; a foaming agent such as water or hollow fine particles; a foam stabilizer such as a silicone-based foam stabilizer; and a filler (abrasive grain) such as cerium oxide; a dye; a pigment; a solid fine particle; a flame retardant; a hydrophilizing agent; a hydrophobizing agent; a light resistance agent; an antioxidant; an antistatic agent, etc.
[0053] (Preparation of resin sheet) In this embodiment, the composition obtained as described above is subjected to a curing reaction to obtain a resin sheet containing a polyurethane resin. Specifically, for example, the composition in this embodiment is poured into a mold preheated to 30°C to 150°C, and heated at about 30°C to 150°C for about 10 minutes to 5 hours. In an example of subjecting the composition (α) to a curing reaction by such an operation, the polysiloxane diol (A), the polyethylene glycol (B), the urethane prepolymer (C1) and the polyamine (C2) react to obtain a polyurethane resin (α). Here, the composition may be further heated in an oven at about 50°C to 180°C for about 10 minutes to 10 hours to perform secondary curing. The reaction temperature when curing the composition as described above can be appropriately adjusted depending on the type and compounding ratio of the polyurethane resin raw material used, and by adjusting the reaction temperature, the reaction rate of the curing reaction can be controlled, and various physical properties of the resulting polishing pad can be controlled.
[0054] The resin sheet obtained as described above can be cut into resin sheets of an appropriate thickness for use, and the resin sheet obtained may be aged at 30° C. to 150° C. for about 1 hour to 24 hours.
[0055] The resin sheet obtained as described above can then be used as the polishing pad of this embodiment by attaching a fixing means to a polishing device, such as a double-sided tape, to one side of the sheet, cutting the sheet into a predetermined shape, preferably a disk shape, and using the sheet as the polishing pad of this embodiment. The fixing means to the polishing device is not particularly limited, and can be arbitrarily selected from conventionally known double-sided tapes, adhesive tapes, adhesives, pressure sensitive adhesives, hook-and-loop fasteners, and the like.
[0056] In addition, the polishing pad of this embodiment may be a single-layer structure consisting of only a resin sheet, or may be a multi-layer structure in which another layer (cushion layer or substrate layer) is attached to one side of a resin sheet. In the case of a multi-layer structure, a double-sided tape or adhesive may be used to bond and fix multiple layers together while applying pressure as necessary. The double-sided tape and adhesive used are not particularly limited, and can be arbitrarily selected from conventionally known double-sided tapes and adhesives.
[0057] Furthermore, the polishing pad of this embodiment may have a groove, embossed, and / or hole (punched) formed on the surface as required. The shape of the groove and embossed is not particularly limited, and examples thereof include a lattice type, a concentric circle type, and a radial type.
[0058] The polishing pad may be dressed (grinded) on the front and / or back surface of the resin sheet. The dressing method is not particularly limited, and may be a known method such as grinding with a diamond dresser.
[0059] (Method of manufacturing polished products) The method for producing the polished product of this embodiment includes a polishing step of polishing a polished object using the polishing pad of this embodiment in the presence of a polishing slurry to obtain the polished product. The polishing step may be a primary polishing (rough polishing), a finish polishing, or a combination of both polishing steps.
[0060] In the manufacturing method of the polished product of this embodiment, the polishing slurry is supplied, and the holding platen and the polishing platen are rotated relative to each other while the polishing object is pressed against the polishing pad by the holding platen, so that the processed surface of the polishing object is polished by the polishing pad by chemical mechanical polishing. The holding platen and the polishing platen may rotate in the same direction at different rotation speeds, or in different directions. Also, the polishing object may be polished while moving (rotating) inside the frame during the polishing process.
[0061] The polishing slurry may contain water, an oxidizing agent such as hydrogen peroxide, chemical components such as acid components and alkaline components, additives, and abrasive grains (polishing particles; e.g., SiC, SiO2, Al2O3, and CeO2), depending on the object to be polished and the polishing conditions.
[0062] The object to be polished is not particularly limited, but examples thereof include optical materials such as lenses, parallel plane plates, and reflective mirrors, semiconductor wafers, semiconductor devices, substrates for hard disks, metals, and ceramics. From the viewpoint of the rotation performance of the object to be polished (low frictional resistance with the polishing pad) and the requirement for precision in the physical properties of the polishing pad, a semiconductor wafer is preferable, and a silicon wafer is more preferable, in which case the effects of this embodiment will be more easily manifested. EXAMPLES
[0063] The present embodiment will be described in more detail below using examples and comparative examples, but the present embodiment is not limited to the following examples.
[0064] [Example 1] First, 1.2 parts by mass of polysiloxane diol (in the above formula (I) all of R are methyl groups, n = 13.65; active hydrogen equivalent 588), 1.2 parts by mass of polyethylene glycol (difunctional, active hydrogen equivalent 294), 0.1 parts by mass of water as a foaming agent, 0.1 parts by mass of a catalyst (manufactured by Tosoh Corporation, product name "TOYOCAT ET"), and 0.2 parts by mass of a silicone-based foam stabilizer (manufactured by Dow Corning Toray Silicones Co., Ltd., product name "SH-193") were mixed and degassed under reduced pressure to obtain a first mixed solution. Next, 78.8 parts by mass of an isocyanate-terminated urethane prepolymer (hereinafter also referred to as "prepolymer") having an NCO equivalent of 400 and containing units derived from 2,4-tolylene diisocyanate (TDI; main component) and a polyol compound (PTMG; weight average molecular weight 650) was degassed under reduced pressure and then added to the first mixed liquid to obtain a second mixed liquid. Furthermore, 18.4 parts by mass of 3,3′-dichloro-4,4′-diaminodiphenylmethane (MOCA) was degassed under reduced pressure and then added to the second mixed liquid, thereby obtaining a composition according to Example 1. Based on the charging ratio when the composition was prepared, the content of polysiloxane diol (A) in the composition was specified to be 1.2 mass% based on 100 mass% of the composition, and the content of polyethylene glycol (B) in the composition was specified to be 1.2 mass% based on 100 mass% of the composition.
[0065] The composition according to Example 1 was poured into a mold (square shape of 850 mm x 850 mm) heated to 80°C, and primarily cured at 80°C for 40 minutes to obtain a first resin foam. The resin foam was removed from the mold and secondary cured in an oven at 130°C for 8 hours to obtain a second resin foam. The second resin foam was sliced in the thickness direction to a thickness of 1.3 mm to obtain a resin sheet according to Example 1. The obtained resin sheet was used as the polishing pad according to Example 1 and was evaluated as described below. Based on the charging ratio during composition preparation, in the polyurethane resin constituting the resin sheet, the content of unit (a) was specified to be 1.2 mass%, with the polyurethane resin being 100 mass%, and the content of unit (b) was specified to be 1.2 mass%, with the polyurethane resin being 100 mass%.
[0066] [Comparative Example 1] In Example 1, the amount of prepolymer used was changed to 78.7 parts by mass, the amount of MOCA used to 18.8 parts by mass, the amount of polysiloxane diol used to 0.0 part by mass (not used), the amount of polyethylene glycol used to 0.7 parts by mass, the amount of foaming agent used to 0.1 parts by mass, and the amount of silicone-based foam stabilizer used to 0.2 parts by mass, and 1.4 parts by mass of polypropylene glycol (active hydrogen equivalent 1009) as a dispersant was added to the first mixed liquid. Except for this, a composition related to Comparative Example 1 was obtained in the same manner as in Example 1. Based on the charging ratio during the preparation of the composition, the content of polyethylene glycol (B) in the composition was determined to be 0.7% by mass, with the composition being 100% by mass.
[0067] The composition according to Comparative Example 1 was processed in the same manner as in Example 1 to obtain a resin sheet according to Comparative Example 1. The obtained resin sheet was used as a polishing pad according to Comparative Example 1 and was subjected to the evaluation described below. Based on the charging ratio during the preparation of the composition, the content of the unit (b) in the polyurethane resin constituting the resin sheet was specified to be 0.7% by mass, with the polyurethane resin being 100% by mass.
[0068] [Comparative Example 2] A composition according to Comparative Example 2 was obtained in the same manner as in Example 1, except that in Example 1, the amount of prepolymer used was changed to 78.2 parts by mass, the amount of MOCA used to 19.2 parts by mass, the amount of polysiloxane diol used to 0.8 parts by mass, the amount of polyethylene glycol used to 0.0 parts by mass (not used), and the amount of silicone-based foam stabilizer used to 0.4 parts by mass, and 1.2 parts by mass of polypropylene glycol (active hydrogen equivalent 1009) as a dispersant was added to the first mixed liquid. Based on the charging ratio during the preparation of the composition, the content of polysiloxane diol (A) in the composition was determined to be 0.8% by mass, with the composition being 100% by mass.
[0069] The composition according to Comparative Example 2 was processed in the same manner as in Example 1 to obtain a resin sheet according to Comparative Example 2. The obtained resin sheet was used as a polishing pad according to Comparative Example 2 and was subjected to the evaluation described below. Based on the charging ratio during the preparation of the composition, the content of the unit (a) in the polyurethane resin constituting the resin sheet was specified to be 0.8% by mass, with the polyurethane resin being 100% by mass.
[0070] Thickness The thickness of the resin sheet in Example 1 and Comparative Examples 1 and 2 (hereinafter also referred to as "each example") was measured in accordance with the measurement method described in JIS K 6505. That is, the resin sheet was subjected to an initial load of 1 cm in the thickness direction. 2 The thickness was measured when a load of 100 g was applied (stressed).
[0071] [Compressibility and compressive elasticity] The compressibility and compressive modulus of the resin sheet in each example were determined using a Shopper-type thickness gauge (pressure surface: circular with a diameter of 1 cm) in accordance with JIS L 1021. That is, at room temperature, the thickness t0 was measured after applying an initial load for 30 seconds from an unloaded state, and then the final load was applied from the thickness t0 state and left as is for 1 minute, after which the thickness t1 was measured. Furthermore, all loads were removed from the thickness t1 state, and after leaving it for 1 minute, the initial load was again applied for 30 seconds, and the thickness t0' was measured. From these, the compressibility and compressive modulus were calculated using the following formula: Compression ratio (%) = (t0-t1) / t0 x 100 Compressive elastic modulus (%) = (t0'-t1) / (t0-t1) x 100 Here, the initial load was 100g / cm 2 , final load is 1120g / cm 2 It was decided.
[0072] [density] The density was calculated from the volume and weight of a sample cut out from the resin sheet in each example.
[0073] [hardness] A sample of 10 cm x 10 cm was cut from the resin sheet in each example, and multiple sheets were stacked to a thickness of 4.5 mm or more, and measured using a DO type hardness tester in accordance with ASTM D2240. The A hardness was measured using an A type hardness tester (Japanese Industrial Standards, JIS K 7311).
[0074] [Flatness measurement] Both sides of a silicon wafer were polished using the polishing pad of each example. Specifically, the surface shape of the silicon wafer was monitored while polishing, and polishing was stopped when the average thickness of the silicon wafer was approximately the same as the thickness of the carrier (the material to hold the polished object) and the surface shape was at its best. The polishing conditions were as follows. (polishing conditions) Polished object: Silicon wafer (diameter 300 mmφ, thickness 779 μm, 5 pieces each) Polishing machine: Speedfam Co., Ltd. "DSM20B-5P-5D" Polishing solution: Fujimi Incorporated alkaline solution (containing colloidal silica, pH 10.5) Lower surface plate rotation speed: 35.0rpm Upper platen rotation speed: -13.4 rpm Internal rotation speed: 7.0 rpm Sun gear rotation speed: 25.0 rpm Grinding load: 5287N
[0075] The surface shape (thickness) of the silicon wafer polished as described above was measured using a flatness measuring device (KOBELCO's "LSW3020FE") to obtain a graph. The edge shape (edge sagging) and polishing rate were evaluated from the obtained graph.
[0076] [Evaluation Results] The evaluation results for the polishing pads of each example are shown in Table 1 below.
[0077] [Table 1]
[0078] FIG. 1 shows the results of measuring the flatness of a silicon wafer polished using the polishing pad of Example 1. In the graph of FIG. 1, the horizontal axis represents the distance (mm) from the center of the polished surface of the silicon wafer, and the vertical axis represents the thickness (μm) of the silicon wafer at the corresponding position (the same applies to FIGS. 2 and 3 described below). In FIG. 1, there is no sudden drop at both ends of the graph (no end sagging occurs), and the difference between the maximum and minimum thickness values is small, so the silicon wafer was evaluated to have a good end shape. The sudden drop at both ends of the graph indicates that the thickness of the end of the silicon wafer is extremely reduced (end sagging occurs) compared to the thickness of other parts. The results of measuring the flatness of a silicon wafer polished using the polishing pad of Comparative Example 1 are shown in Figure 2. In Figure 2, while the difference between the maximum and minimum thickness values was equivalent to that of the Example, the thickness suddenly dropped in a narrow range of about 20 mm at both ends (edge sagging occurred), and the flatness of the silicon wafer was evaluated as poor. The results of measuring the flatness of a silicon wafer polished using the polishing pad of Comparative Example 2 are shown in Figure 3. In Figure 3, both ends of the graph do not drop sharply (no edge sagging occurs), and the difference between the maximum and minimum thickness values is the same as in the Example, so the silicon wafer was evaluated to have a good edge shape. However, the polishing rate was evaluated to be low. [Industrial Applicability]
[0079] The polishing pad of the present invention has industrial applicability as a polishing pad used for polishing (particularly chemical mechanical polishing (CMP)) materials such as optical materials such as lenses, parallel plane plates, and reflecting mirrors, semiconductor wafers, semiconductor devices, substrates for hard disks, metals, and ceramics.
Claims
1. A polishing pad comprising a resin sheet having a polishing surface, the resin sheet contains a polyurethane resin, The polyurethane resin is A unit (a) derived from a polysiloxane diol (A) represented by the following formula (I), Units (b) derived from polyethylene glycol (B); having The content of the unit (a) is 0.3 to 10.0% by mass, based on 100% by mass of the polyurethane resin; The content of the unit (b) is 0.3 to 10.0 mass % relative to 100 mass % of the polyurethane resin. 【Chemistry 1】 (In formula (I), each R independently represents an organic group having 1 to 10 carbon atoms or a hydrogen atom, and n represents an integer of 5 to 25.)
2. 2. The polishing pad according to claim 1, wherein the polysiloxane diol (A) comprises a polysiloxane diol (A1) in which all of the R in the formula (I) are methyl groups.
3. 2. The polishing pad according to claim 1, wherein the resin sheet has an A hardness of 50 degrees or more and a DO hardness of 90 degrees or less.
4. The density of the resin sheet is 0.3 to 0.6 g / cm 3 2. The polishing pad of claim 1 ,
5. 5. A method for producing a polished product, comprising a polishing step of polishing a workpiece with the polishing pad according to claim 1 in the presence of a polishing slurry.
6. The method for producing a polished workpiece according to claim 5, wherein the polished workpiece is a silicon wafer.
Citation Information
Patent Citations
Measuring system
JP1983075300A
Molded body for polishing layer and polishing pad
JP6541683B2
High planarization efficiency chemical mechanical polishing pad and manufacturing method
JP6981823B2