Ferritic stainless steel plate and producing method thereof

A controlled manufacturing process for ferritic stainless steel achieves high strength and toughness by fine Cr carbide dispersion and grain refinement, addressing the limitations of existing materials in architectural hardware.

JP2024145532APending Publication Date: 2024-10-15NIPPON STEEL STAINLESS STEEL CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023057925
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing ferritic stainless steel materials used in architectural hardware lack sufficient high strength and toughness, and often contain high amounts of expensive elements like Ni and Mo, leading to increased costs.

Method used

A method for producing ferritic stainless steel with controlled hot rolling and heating processes to achieve fine Cr carbide dispersion and grain refinement, ensuring a specific metal structure that maintains toughness while reducing alloy content, by controlling the exit passing speed, end temperature, and heating and holding conditions.

Benefits of technology

The method results in an alloy-saving ferritic stainless steel with high strength and excellent toughness, suitable for architectural hardware, achieving a hardness of 240 HV and impact value of 50 J/cm² at 0°C, while minimizing costly elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145532000003
    Figure 2024145532000003
  • Figure 2024145532000001
    Figure 2024145532000001
  • Figure 2024145532000002
    Figure 2024145532000002
Patent Text Reader

Abstract

To provide a ferritic stainless steel plate excellent in high strength and rigidity and a producing method thereof.SOLUTION: A ferritic stainless steel plate of the present invention has a ferrite host phase of, by mass%, C: 0.16% or more and 0.45% or less, Si: 0.01% or more and 1.00% or less, Mn: 0.01% or more and 1.00% or less, Cr: 11.5% or more and 15.0% or less, Ni: 0% or more and 0.80% or less, N: 0.002% or more and 0.070% or less, P: 0% or more and 0.040% or less, S: 0% or more and 0.0300% or less, the balance being Fe and impurities, an average crystal grain size of 5 μm or less, and a particle size ratio defined by maximum crystal grain size / an average crystal grain size of 4.5 or less, and a residue recovery rate of carbide recovered by an extraction residue method being 2.0 mass% or more, further an average particle diameter of the carbide being 0.20 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel and a method for producing the same. [Background technology]

[0002] Due to changes in the style of civil engineering and architectural structures, there is a demand for further improvements in the properties of metal parts for architectural applications. Materials used in architectural metal parts are required to have the necessary thickness to ensure rigidity, high strength to withstand the weight of the structure, and toughness to withstand the impact of a heavy object being dropped. In addition, to reduce material costs, it is also desired that the content of expensive elements such as Ni and Mo is low (alloy saving).

[0003] Ferritic stainless steel is used as the material for metal parts. Although martensitic stainless steel generally has higher strength than ferritic stainless steel, it may have inferior toughness.

[0004] Patent documents 1 and 2 present ferritic stainless steel, an intermediate material for martensitic stainless steel, and a manufacturing method thereof. Patent documents 1 and 2 are prior art that focus on the material properties after quenching, and the ferritic stainless steel, which is the intermediate material, is thick gauge and has the strength required for metal parts in architectural applications. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-050386 [Patent Document 2] JP 2022-146477 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a ferritic stainless steel having high strength and excellent toughness, and a method for producing the same. More specifically, it aims to provide a thick-gauge steel plate suitable for metal parts in architectural applications, and a method for producing the same. [Means for solving the problem]

[0007] The present inventors have conducted extensive research into ferritic stainless steels and have clarified the characteristics of the metal structure that ensures a desired strength as well as toughness.

[0008] First, we found that strengthening by particle dispersion strengthening of fine Cr carbides, which had not been used in the field of ferritic stainless steels, can be used for certain steel components. We also found that the required strength can be secured by combining grain refinement strengthening and particle dispersion strengthening of fine Cr carbides. On the other hand, we also found that even if a large amount of Cr carbides are dispersed in the ferritic matrix, they do not adversely affect toughness as long as they are fine. In conventional ferritic stainless steels, coarse Cr carbides precipitate at the grain boundaries where they are easily diffused, so they do not contribute to strengthening and often have an adverse effect on toughness.

[0009] In addition to the above, we also discovered that the coarse ferrite grains present in a very small proportion of the ferrite matrix are the cause of the decrease in toughness. We also discovered that the necessary toughness can be secured by keeping the grain size ratio (= maximum grain size / average grain size), defined as the ratio of the average grain size to the maximum grain size in the ferrite matrix, below a certain level. We clarified the characteristics of the steel composition and metal structure that can achieve this effect.

[0010] Furthermore, in order to obtain the above-mentioned beneficial metal structure, a manufacturing method thereof has been clarified. In the ferritic stainless steel of the present invention, it is important to specify the exit side threading speed of the final pass of hot rolling, the end temperature of hot rolling, and further to manage the end temperature of hot rolling in the austenite single phase region. This controls the strain distribution state of the austenite after hot rolling, and obtains a metal structure of unrecrystallized austenite with high strain accumulation. Then, when the metal structure is heated and held in a post-process, not only does a large amount of Cr carbide precipitate finely, but fine ferrite is easily precipitated from within the prior austenite grains, and the precipitation of coarse ferrite from the prior austenite grain boundaries is suppressed. This allows the grain size ratio to be 4.5 or less.

[0011] After the hot rolling, the steel sheet is heated and held continuously. "Continuously" means that the steel sheet is heated and held at a predetermined temperature of 600°C or more and 800°C or less for 30 minutes or more and 360 minutes or less, without lowering the temperature to 600°C or less after the completion of the hot rolling. This allows the transformation from austenite to ferrite and Cr carbide to proceed, and the metal structure of the present invention is obtained.

[0012] Based on the above findings, the present invention discloses the following techniques.

[0013] [1] A ferritic stainless steel sheet comprising, by mass%, C: 0.16% to 0.45%, Si: 0.01% to 1.00%, Mn: 0.01% to 1.00%, Cr: 11.5% to 15.0%, Ni: 0% to 0.80%, N: 0.002% to 0.070%, P: 0% to 0.040%, S: 0% to 0.0300%, with the balance being Fe and impurities, having a ferrite matrix with an average grain size of 5 μm or less and a grain size ratio defined as maximum grain size / average grain size of 4.5 or less, wherein the residue recovery rate of carbides recovered by an extraction residue method is 2.0% by mass or more, the average grain diameter of the carbides is 0.20 μm or less, and the sheet thickness is 4.0 mm to 7.0 mm.

[0014] [2] The ferritic stainless steel plate of [1] above, characterized in that it contains, in place of a portion of the Fe, one or more of the following, by mass%, Al: 0.30% or less, Nb: 0.07% or less, B: 0.0030% or less, Ti: 0.07% or less, Mo: 0.75% or less, V: 0.30% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.0% or less, Co: 0.5% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, and Sb: 0.15% or less.

[0015] [3] Hardness is 240HV or more, and the impact value at 0℃ is 50J / cm 2 The ferritic stainless steel sheet according to [1] or [2] above, characterized in that

[0016] [4] A method for producing a ferritic stainless steel according to any one of [1] to [3] above, comprising: hot rolling a steel having the composition according to [1] or [2] above at an exit threading speed of 200 mpm or more in a final pass and an end temperature of 975°C or less, the end temperature being in the austenite single phase region; and then, following the hot rolling, carrying out a heating hold at a temperature of 600°C or more and 800°C or less for 30 minutes or more and 360 minutes or less.

[0017] [5] A ferritic stainless steel sheet according to any one of [1] to [3] above, used for metal parts for architectural applications. Effect of the Invention

[0018] The present invention can provide an alloy-saving ferritic stainless steel that has high strength and excellent toughness. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a diagram illustrating a test piece used in a Charpy impact test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] 1. Ferritic Stainless Steel The ferritic stainless steel of the present invention will be described below.

[0021] (Chemical Composition) First, the components contained in the ferritic stainless steel of the present invention will be described. Note that the "%" for the content of each element means "% by mass."

[0022] (C: 0.16% or more and 0.45% or less) C affects the amount of Cr carbide precipitation and is an element necessary for ensuring the amount of particle dispersion strengthening by Cr carbide. If the C content is less than 0.16%, the amount of carbide precipitation is small, sufficient particle dispersion strengthening cannot be obtained, and strength is insufficient. It is preferably 0.26% or more, more preferably 0.28% or more. On the other hand, if the C content exceeds 0.45%, Cr carbide aggregates and coarsens, sufficient particle dispersion strengthening cannot be obtained, and strength is insufficient. Furthermore, toughness is also insufficient. For this reason, it is set to 0.45% or less. It is preferably 0.40% or less, more preferably 0.35% or less.

[0023] (Si: 0.01% or more and 1.00% or less) Si is an element that improves oxidation resistance. If the Si content is less than 0.01%, sufficient oxidation resistance may not be obtained. Therefore, the Si content is set to 0.01% or more, preferably 0.05% or more, and more preferably 0.15% or more. Moreover, if the Si content is excessively decreased, the manufacturing cost increases. If the Si content exceeds 1.00%, cracking during manufacturing is promoted. Therefore, the Si content is set to 1.00% or less, preferably 0.85% or less, and more preferably 0.60% or less.

[0024] (Mn: 0.01% or more and 1.00% or less) Mn is used as a deoxidizing element. From the viewpoint of stable production, the Mn content is set to 0.01% or more. It is preferably set to 0.10% or more, and more preferably set to 0.20% or more. On the other hand, if the Mn content exceeds 1.00%, compounds such as sulfides may be formed, which may lead to a decrease in corrosion resistance. Therefore, the Mn content is set to 1.00% or less. It is preferably set to 0.85% or less, and more preferably set to 0.70% or less.

[0025] (Cr: 11.5% or more and 15.0% or less) Cr is an element that combines with C to form Cr carbide. It is also an element that improves corrosion resistance. On the other hand, it is also an element that should be regulated in order to make the metal structure mainly composed of austenite at the hot rolling temperature. If the Cr content is less than 11.5%, sufficient corrosion resistance cannot be obtained. Therefore, the Cr content is 11.5% or more, preferably 12.0% or more, and more preferably 12.5% ​​or more. On the other hand, if the Cr content exceeds 15.0%, two phases of austenite and ferrite will be formed in the hot rolling temperature range. Then, the ferrite acts as coarse ferrite in the metal structure after heating and holding, reducing toughness. Therefore, the Cr content is 15.0% or less, preferably 14.5% or less, and more preferably 14.0% or less.

[0026] (Ni: 0% or more and 0.80% or less) Ni is an element that improves toughness and may be added as necessary. It is not essential to add it, and the lower limit of its content is 0. However, since Ni is a rare and expensive element, adding too much of it increases the cost of the alloy and hinders manufacturability. Therefore, the Ni content is set to 0.80% or less. It is preferably 0.60% or less, and more preferably 0.50% or less.

[0027] (N: 0.002% or more and 0.070% or less) N is an element that improves corrosion resistance. From the viewpoint of corrosion resistance, the N content is set to 0.002% or more. It is preferably set to 0.009% or more, and more preferably set to 0.011% or more. On the other hand, if the N content is too high, the hot workability is significantly deteriorated. Therefore, the N content is set to 0.070% or less. It is preferably set to 0.06% or less, and more preferably set to 0.050% or less.

[0028] (P: 0% or more and 0.040% or less) P is an element that reduces formability and corrosion resistance. It is preferable that the content is low. Therefore, the P content is set to 0.040% or less. It is preferably set to 0.030% or less, and more preferably 0.030% or less. The inclusion of P is not essential, and the lower limit is 0. However, if the P content is reduced too much, the manufacturing cost increases. Therefore, the P content may be set to 0.005% or more, or 0.007% or more.

[0029] (S: 0% or more and 0.0300% or less) S is an inevitable impurity element that promotes cracking during manufacturing. Therefore, the S content is set to 0.0300% or less. It is preferably set to 0.0100% or less, and more preferably set to 0.0030% or less. The inclusion of S is not essential, and the lower limit is 0. However, if the S content is excessively reduced, the manufacturing cost increases. From this viewpoint, the S content may be set to 0.0003% or more.

[0030] (balance: Fe and impurities) The balance of the ferritic stainless steel of the present invention is Fe and impurities, where the term "impurities" refers to substances that are mixed in from raw materials such as ores and scraps or from the manufacturing environment during industrial production of steel and that are acceptable within a range that does not impair the desired properties of the ferritic stainless steel of the present invention.

[0031] In addition to the above basic composition, the ferritic stainless steel of the present invention may contain, in place of a portion of Fe, one or more of the following, by mass%, Al: 0.30% or less, Nb: 0.07% or less, B: 0.0030% or less, Ti: 0.07% or less, Mo: 0.75% or less, V: 0.30% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.0% or less, Co: 0.5% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, and Sb: 0% or more and 0.15% or less.

[0032] (Al: 0.30% or less, Nb: 0.07% or less, B: 0.0030% or less, Ti: 0.07% or less) The elements Al, Nb, B, and Ti do not have to be added. If these elements are added, they have the effect of improving the formability of ferritic stainless steel and suppressing defects during hot working. When added, the Al content is 0.30% or less, the Nb content is 0.07% or less, the B content is 0.030% or less, and the Ti content is 0.07% or less. In order to reliably obtain the above effects, it is preferable that the Al, Nb, and Ti contents are 0.01% or more, and the B content is 0.001% or more.

[0033] (Mo: 0.75% or less, V: 0.30% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.0% or less, Co: 0.5% or less) The elements Mo, V, Sn, Cu, W and Co do not have to be added. These elements have the effect of improving corrosion resistance. When added, the Mo content is 0.75% or less, the V content is 0.30% or less, the Sn content is 0.12% or less, the Cu content is 0.40% or less, the W content is 1.0% or less, and the Co content is 0.50% or less. In order to reliably obtain the above effects, it is preferable that the Mo, V, Sn, Cu and Co contents are 0.01% or more, and the W content is 0.1% or more.

[0034] (Ca: 0.0050% or less, Mg: 0.0050% or less, Sb: 0.15% or less) The elements Ca, Mg, and Sb do not have to be added. These elements have the effect of changing inclusions such as oxides and sulfides to suppress hot working defects. When added, the Ca content is 0.0050% or less, the Mg content is 0.0050% or less, and the Sb content is 0.15% or less. In order to reliably obtain the above effects, it is preferable that the Ca and Mg contents are 0.0001% or more.

[0035] In addition to the above elements, the ferritic stainless steel of the present invention may further contain elements other than the above elements in place of a part of Fe, within a range in which the above-mentioned problems can be solved. For example, Zr, Y, Hf, and REM. Zr: 0.10% or less, Y: 0.10% or less, Hf: 0.20% or less, and REM: 0.10% or less may be used. Bi, Pb, Se, H, Ta, etc. may also be contained, but it is preferable to reduce the contents of these elements as much as possible. The content ratios of these elements are controlled to the extent that the above-mentioned problems can be solved, and one or more of Bi≦100 ppm, Pb≦100 ppm, Se≦100 ppm, H≦100 ppm, and Ta≦500 ppm may be contained.

[0036] In this specification, "REM" refers to elements having atomic numbers of 57 to 71 (lanthanoids), such as Ce, Pr, and Nd, but does not include Y.

[0037] (Metal structure) Next, the metal structure of the ferritic stainless steel of the present invention will be described.

[0038] The metal structure of the ferritic stainless steel of the present invention is composed of a ferrite phase and numerous fine carbides, which account for only a small proportion at room temperature. However, the presence of phases other than the ferrite phase and carbides can be tolerated to a certain extent. For example, the ferritic stainless steel of the present invention can be made to contain a total of 5% or less of phases other than the main phase ferrite, such as austenite and martensite, in terms of area ratio at room temperature. The area ratio of austenite (γ) (unit: [%]) is calculated by the following formula using the number of plots F and B (unit: [pieces]) of the FCC structure and the BCC structure, respectively, obtained by EBSD measurement.

[0039] γ = F / (F + B) × 100 … (1)

[0040] On the other hand, the presence or absence of martensite can be determined by Vickers hardness. If 5% or more martensite is present, the hardness will exceed 300HV. If a Vickers hardness tester is used to measure 10 times with a load of 500g and the average value is 300HV or less, it can be determined that martensite is not present.

[0041] (Average grain size of ferrite: 5μm or less, grain size ratio: 4.5 or less) In order to ensure strength, it is necessary that the average crystal grain size of ferrite is 5 μm or less. The average crystal grain size is preferably 4 μm or less, more preferably 2.5 μm or less. The lower limit of the average crystal grain size is not particularly limited, but it is 1 μm or more based on past experience. On the other hand, if the average crystal grain size exceeds 5 μm, the possibility of not being able to ensure strength increases. Furthermore, if there are crystal grains in the ferrite whose grain size ratio exceeds 4.5 with respect to the average value, these coarse ferrite crystal grains become the starting point and cause a decrease in toughness. For this reason, it is necessary that the grain size ratio defined as the maximum grain size / average grain size is 4.5 or less. The grain size ratio is preferably 4.0 or less, more preferably 3.5 or less.

[0042] Average grain size of ferrite (D ave.The L-section of a steel plate sample prepared by electrolytic polishing is measured using EBSD. The measurement area is 300 μm x 300 μm at the 1 / 4t position of the plate thickness, with a measurement step size of 0.1 μm. The measurement data is then analyzed using the analysis software "OIM." If the crystal orientation difference between adjacent plot data is less than 15°, they are considered to be the same crystal grain, and if there is an orientation difference of 15° or more, they are considered to be different crystal grains. If the measurement area contains phases other than ferrite, only ferrite is extracted and calculations are performed. Meanwhile, the grain size ratio (R) is defined as the value shown in formula (2). The maximum grain size (D max [μm]) is the maximum value of the above measurement data.

[0043] R=D max / D ave. …(2)

[0044] (Average particle diameter of Cr carbide: 0.20 μm or less, residue recovery rate: 2.0 mass% or more)

[0045] In order to ensure strength, it is necessary that Cr carbides are precipitated in a certain amount or less and of a certain size, and the C added to the ferritic stainless steel of the present invention is almost entirely present as Cr carbides. On the other hand, if either the size or the amount of precipitation of the Cr carbides does not satisfy the specified range, strength cannot be ensured. 23 Any composition is acceptable, including C6.

[0046] The average particle diameter of the Cr carbide is 0.20 μm or less. The average particle diameter is preferably 0.15 μm or less, and more preferably 0.10 μm or less. On the other hand, the lower limit of the average particle diameter is not particularly limited, but is 0.01 μm or more based on past experience. On the other hand, if the average particle diameter exceeds 0.20 μm, strength cannot be ensured. In ferritic stainless steel, coarse Cr carbides often precipitate at the grain boundaries where diffusion is easy, in which case they do not contribute to strengthening and have a negative effect on toughness.

[0047] The average particle diameter of Cr carbide is determined by the following method. First, the L-section of the steel plate is mirror-polished, and then the grain boundaries and Cr carbides are revealed by electrolytic polishing to prepare the sample, and the size and number density of the Cr carbides are measured by SEM observation. The measurement area is 200 μm × 200 μm in total area at the 1 / 4t position of the plate thickness, and SEM observation is performed at a magnification of 5000 times. The size of the Cr carbide is calculated by converting the observed Cr carbide into a circle equivalent diameter, and this value is taken as the average particle diameter. The Cr carbide confirmed in the ferritic stainless steel of the present invention is (Cr,Fe) 23 Most of it is C6, but it may contain some (Cr,Fe)7C3. Cr carbides can be confirmed by EDX.

[0048] The amount of precipitated Cr carbide must be 2.0 mass% or more in terms of residue recovery rate when recovered by the extraction residue method. The residue recovery rate of Cr carbide is preferably 6.0 mass% or more, and more preferably 10.0 mass% or more. On the other hand, if the residue recovery rate is less than 2.0 mass%, the strength cannot be ensured.

[0049] The residue recovery rate is determined by the following method. For a steel plate with a thickness (t [mm]), a portion from both surfaces of the steel plate to 1 / 4t of the plate thickness is cut to prepare a sample of 30 mmL x 20 mmW x 1 / 2t. The extracted residue is then collected by constant current electrolysis using a non-solvent electrolyte (10% acetylacetone-1% tetramethylammonium chloride-methanol). The size of the residue filter used is 0.2 μm. Here, the residue recovery rate (W [mass%]) of Cr carbide is defined as the value calculated by formula (2). Here, g [g] and G [g] respectively represent the weight of the residue collected in the residue filter and the weight change of the sample before and after the extraction residue.

[0050] W = g / G × 100 … (3)

[0051] The residue obtained in the ferritic stainless steel of the present invention is (Cr,Fe) 23 The majority of the residue is C6, but it may contain some (Cr,Fe)7C3. The substances that make up the residue can be confirmed by XRD.

[0052] (Hardness) The hardness of the ferritic stainless steel of the present invention is preferably 240HV or more, taking into consideration the strength required for architectural hardware parts, which are the main application of the material of the present invention. The hardness is determined by measuring the cross-sectional hardness at the 1 / 4t position of the plate thickness using a Vickers hardness tester. In the present invention, 10 measurements are performed with a test load of 500g, and the average value is taken as the hardness.

[0053] (Toughness) The ferritic stainless steel of the present invention has an impact strength of 50 J / cm at 0°C, taking into consideration the toughness required for architectural hardware components, which are the main application of the material of the present invention. 2 It is preferable that it is equal to or higher. The impact value at 0℃ is determined by carrying out a Charpy impact test conforming to JIS Z2242 at 0℃. The test piece is a 2mm V-notch test piece (Fig. 1) measuring 55mm x 10mm x plate thickness. The sample is taken so that the L direction of the sample coincides with the longitudinal direction of the test piece (55mm), and the test is carried out at N5. The toughness is evaluated as the N5 average of the impact value, which is calculated by dividing the absorbed energy by the cross-sectional area.

[0054] (Thickness) The plate thickness of the ferritic stainless steel of the present invention is 4.0 mm or more from the viewpoint of rigidity required for architectural hardware parts, which are the main applications of the material of the present invention. It is preferably 4.5 mm or more, and more preferably 5.0 mm or more. Also, from the viewpoint of toughness, it is 7.0 mm or less. It is preferably 6.5 mm or less, and more preferably 6.0 mm or less.

[0055] 2. Manufacturing method of ferritic stainless steel A method for producing the ferritic stainless steel of the present invention will now be described.

[0056] First, steel having the above composition is melted and cast to produce an ingot. The ingot is then heated. The heating temperature may be any temperature generally used in stainless steel manufacturing. The heating temperature is 1150°C or higher, preferably 1180°C or higher, and more preferably 1200°C or higher. There is no upper limit. However, if the heating temperature is excessively high, there is a concern that uneven patterns may occur on the surface of the steel sheet after pickling. From this viewpoint, the heating temperature is preferably 1350°C or lower.

[0057] (Hot Rolling) Next, the heated ingot is subjected to hot rolling. In the ferritic stainless steel of the present invention, it is important that the exit threading speed of the final pass of hot rolling is controlled to 200 mpm or more. The exit threading speed of the final pass is preferably 250 mpm or less, more preferably 350 mpm or more. The upper limit is not particularly limited, but is 500 mpm or less based on past experience. Furthermore, it is important that the end temperature of hot rolling is controlled to 975°C or less. The end temperature is preferably 950°C or less, more preferably 925°C or less. It is also important that the end temperature during hot rolling is controlled to be in the austenite single phase region. The austenite single phase means that the austenite phase is 95% or more, more preferably 97% or more. The remainder is a compound such as ferrite or Cr carbide.

[0058] When the exit threading speed and the end temperature of the final pass of hot rolling satisfy the above conditions, the strain distribution state of the austenite after hot rolling is controlled, and a metal structure of unrecrystallized austenite with high strain accumulation is obtained. When this metal structure is heated and held in a post-process, fine and large amounts of Cr carbides are precipitated, and fine ferrite is easily precipitated from the prior austenite grains, and the precipitation of coarse ferrite from the prior austenite grain boundaries is suppressed. This makes it possible to make the grain size ratio 4.5 or less. On the other hand, when any one of the requirements of the exit threading speed, the end temperature, and the metal structure of the final pass of hot rolling is not satisfied, the strain accumulation of the austenite after hot rolling is insufficient, and coarse ferrite precipitates from the prior austenite grain boundaries during the heating and holding, resulting in a grain size ratio exceeding 4.5.

[0059] (heat retention) After the hot rolling is completed, the material is subsequently heated and held. Here, "subsequently heated and held" means that the material obtained after hot rolling is inserted into a heating furnace without being intentionally cooled between the steps of hot rolling and holding, and without being cooled to less than 600°C. Even if the exit speed of the sheet at the final pass and the end temperature of hot rolling are controlled to be equal to or higher than a predetermined value, in the case of a typical manufacturing process in the conventional manufacturing method of ferritic stainless steel, that is, a thermal history in which the material is once cooled to room temperature after hot rolling, reheated, and held at a temperature, a long time is required for reheating, and therefore the ferrite grains and Cr carbides become coarse.

[0060] If the temperature of the heating and holding is less than 600°C, the transformation from austenite to ferrite and Cr carbide is insufficient, and when the plate is cooled to room temperature after the heating and holding, the amount of Cr carbide precipitated is insufficient. In addition, the metal structure contains a lot of hard martensite, and there is a concern that the plate may break during the subsequent process of passing the plate. On the other hand, if the temperature exceeds 800°C, the transformation from austenite to ferrite and Cr carbide is insufficient, and when the plate is cooled to room temperature after the heating and holding, the amount of Cr carbide precipitated is insufficient. In addition, if the heating and holding time is less than 30 minutes, the transformation from austenite to ferrite and Cr carbide is insufficient, and when the plate is cooled to room temperature after the heating and holding, the amount of Cr carbide precipitated is insufficient. In addition, the metal structure contains a lot of hard martensite, and there is a concern that the plate may break during the subsequent process of passing the plate. On the other hand, if the heating and holding time exceeds 360 minutes, the average particle size of the Cr carbide becomes coarse. Therefore, the heating and holding is performed at a temperature of 600°C to 800°C for 30 minutes to 360 minutes. Preferably, the heating and holding is performed at a temperature of 650°C to 770°C for 60 minutes to 300 minutes. More preferably, the heating and holding is performed at a temperature of 700°C to 760°C for 120 minutes to 240 minutes. The cooling rate after the heating and holding is not particularly limited. For example, the cooling rate may be 0.05°C / s or more, or air cooling may be performed.

[0061] After the heating and holding is completed, the steel sheet is obtained by pickling. Pickling is a process for removing oxide scale from the surface, and a method commonly used in the production of stainless steels can be used without any problem. EXAMPLES

[0062] The effects of the ferritic stainless steel sheet of the present invention will be described with reference to examples.

[0063] Steel having the composition shown in Table 1 was melted to obtain an ingot having a thickness of 100 mm. This ingot was heated at 1230°C for 100 minutes, and then hot-rolled under the conditions shown in Table 2 to obtain hot-rolled sheets of various thicknesses. The hot-rolled sheets were then heated and held under the conditions shown in Table 2, and then air-cooled. Furthermore, pickling with sulfuric acid was carried out to obtain steel sheets. For comparison, a thermal history process was also carried out for No. 26, in which the sheets were cooled to room temperature after hot rolling, heated again, and held at that temperature.

[0064] The average crystal grain size of the ferrite matrix, grain size ratio, average particle diameter of Cr carbide recovered by the extraction residue method, residue recovery rate, hardness, and impact value at 0°C were measured for the obtained steel sheets according to the above-mentioned methods. As a result, it was determined that if the hardness was 240HV or more, the required strength was satisfied. In addition, if the impact value (N5 average) at 0°C was 50J / cm 2 If it was equal to or greater than this, it was determined that it had the necessary toughness.

[0065] The results are shown in Table 2. It can be seen that No. 1 to No. 16, in which the average crystal grain size, grain size ratio, average particle diameter of Cr carbide, and residue recovery rate are within the specified range, have the necessary strength and toughness. In contrast to the above, No. 21, in which the hot rolling delivery speed was less than the specified, had a grain size ratio greater than the specified and insufficient toughness. No. 22, in which the hot rolling end temperature was greater than the specified, had a grain size ratio greater than the specified and insufficient toughness. No. 23, in which the added C and Cr were insufficient, had a Cr carbide residue recovery rate less than the specified and insufficient strength. In addition, since the two phases of austenite and ferrite were formed at the hot rolling end temperature, the grain size ratio was greater than the specified and the toughness was also insufficient. No. 24, in which the added C was excessive, had Cr carbide aggregated and coarsened, and the strength was insufficient. In addition, the toughness was also insufficient. No. 25, in which the plate thickness exceeded the specified thickness, had the metal structure of the present invention, but the toughness was insufficient. In the case of No. 26, which had a thermal history of being cooled to room temperature after the completion of hot rolling and then heated again and held at that temperature, both the average grain size of ferrite and the average grain diameter of Cr carbide were larger than the specified values, and the strength and toughness were insufficient.

[0066] [Table 1]

[0067] [Table 2] [Industrial Applicability]

[0068] The alloy-saving ferritic stainless steel of the present invention has both high strength and high toughness, and can contribute to further improving the load-bearing capacity and impact resistance of metal parts for architectural applications, for example.

Claims

1. In mass percent, C: 0.16% or more and 0.45% or less, Si: 0.01% or more and 1.00% or less, Mn: 0.01% or more and 1.00% or less, Cr: 11.5% or more and 15.0% or less, Ni: 0% or more and 0.80% or less, N: 0.002% or more and 0.070% or less, P: 0% or more and 0.040% or less, S: 0% or more and 0.0300% or less with the balance being Fe and impurities; The ferrite matrix has an average crystal grain size of 5 μm or less and a grain size ratio defined as maximum crystal grain size / average crystal grain size of 4.5 or less, The residue recovery rate of the carbonized material recovered by the extraction residue method is 2.0 mass% or more, and the average particle diameter of the carbonized material is 0.20 μm or less; The plate thickness is 4.0 mm or more and 7.0 mm or less.

1. A ferritic stainless steel sheet comprising:

2. Instead of a part of the Fe, In mass percent, Al: 0.30% or less, Nb: 0.07% or less, B: 0.0030% or less, Ti: 0.07% or less, Mo: 0.75% or less, V: 0.30% or less, Sn: 0.12% or less, Cu: 0.40% or less, W: 1.0% or less, Co: 0.5% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Sb: 0.15% or less The ferritic stainless steel sheet according to claim 1, further comprising one or more of the following:

3. Hardness is 240HV or more, and the impact value at 0°C is 50J / cm 2 3. The ferritic stainless steel sheet according to claim 1, wherein the ferritic stainless steel sheet is made of a ferritic material.

4. A method for producing the ferritic stainless steel according to claim 1 or 2, comprising the steps of: A steel having the composition according to claim 1 or 2 is subjected to hot rolling in which the final pass has an outlet threading speed of 200 mpm or more and an end temperature of 975°C or less, the end temperature being in the austenite single phase region, Following the hot rolling, the steel sheet is heated and held at a temperature of 600° C. to 800° C. for 30 minutes to 360 minutes. A method for producing ferritic stainless steel comprising the steps of:

5. The ferritic stainless steel sheet according to claim 1 or 2, which is used for metal parts for architectural purposes.

Citation Information

Patent Citations

  • Ferritic stainless steel and method for producing ferritic stainless steel

    JP2021050386A

  • Ferritic stainless steel, ferritic stainless steel sheet, and manufacturing method thereof