Resin film, retardation film, and method of manufacturing resin film

The resin film with controlled anti-blocking agent dispersion achieves both anti-blocking and in-plane birefringence, addressing the challenges of blocking and birefringence reduction, enabling high-quality retardation film production.

JP2024145565AInactive Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023057972
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Resin films struggle to achieve both excellent anti-blocking properties and sufficient in-plane birefringence when stretched, as the addition of anti-blocking agents can reduce birefringence and winding without a release liner leads to blocking and dent formation.

Method used

A resin film comprising a matrix with an anti-blocking agent of specific particle size (0.1 μm to 1.3 μm) and content (350 ppm to 3000 ppm) that maintains low dynamic friction (1.0 or less) and indentation modulus (2.0N to 6.5N), along with a production method involving filtering and extrusion to disperse the agent uniformly.

Benefits of technology

The resin film exhibits excellent anti-blocking properties, preventing dent formation and allowing for sufficient in-plane birefringence development upon stretching, enabling production of high-quality retardation films without a release liner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145565000001_ABST
    Figure 2024145565000001_ABST
Patent Text Reader

Abstract

To provide a resin film which offers a superior anti-blocking property and can exhibit sufficient in-plane birefringence when stretched, and to provide a retardation film and a method of manufacturing the resin film.SOLUTION: A resin film according to an embodiment of the present invention contains a resin material used as a matrix and an anti-blocking agent dispersed in the resin material, where the content of the anti-blocking agent is 350-3000 ppm, and a difference in refractive index between the resin material and the anti-blocking agent is 0.10 or less in absolute terms.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film, a retardation film, and a method for producing a resin film. [Background technology]

[0002] Resin films are widely used in various industrial products. For example, it is known to produce a retardation film by stretching a resin film in a predetermined direction (see, for example, Patent Document 1).

[0003] Such a resin film is generally collected by winding it up into a roll with a release liner attached to its surface. However, when the resin film with the release liner attached is wound up into a roll, the unevenness of the release liner may be transferred to the resin film, forming dents in the resin film.

[0004] For this reason, it has been considered to wind up the resin film without attaching a release liner. However, when the resin film is wound into a roll without a release liner, there is a risk of blocking, in which the resin films stick to each other. In this regard, although it is possible to impart antiblocking properties to the resin film by incorporating an antiblocking agent (hereinafter referred to as an AB agent) into the resin film, it may not be possible to fully express in-plane birefringence when the resin film is stretched. For this reason, it is difficult to achieve both excellent antiblocking properties and the ability to express in-plane birefringence by stretching in a resin film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 7096940 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a resin film, a retardation film, and a method for producing a resin film, which have excellent antiblocking properties and can fully exhibit in-plane birefringence by stretching. [Means for solving the problem]

[0007] [1] A resin film according to one embodiment includes a resin material as a matrix and an antiblocking agent dispersed in the resin material. The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm. The content of the antiblocking agent in the resin film is 350 ppm to 3000 ppm. [2] The resin film according to the above [1] may have an indentation modulus at 25° C. of 2.0 N to 6.5 N. [3] In the resin film according to the above [1] or [2], the dynamic friction coefficient may be 1.0 or less. [4] In the resin film according to any one of [1] to [3] above, the resin material may contain a polycarbonate-based resin. [5] A retardation film according to another aspect of the present invention includes a resin material as a matrix and an antiblocking agent dispersed in the resin material. The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm. The content of the antiblocking agent is 350 ppm to 3000 ppm. In the retardation film, the in-plane birefringence Δn(550) is 0.0045 or more. [6] In yet another aspect of the present invention, a method for producing a resin film includes the steps of: mixing a molten resin material with an antiblocking agent to prepare a resin composition; passing the resin composition through a filter; and extrusion molding the resin composition after passing through the filter. The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm. The content of the antiblocking agent in the resin composition is 350 ppm to 3000 ppm. [7] In the method for producing a resin film according to the above [6], the filter may be a screen mesh, and the opening of the screen mesh may be 0.035 mm to 0.070 mm. [8] The method for producing a resin film according to [6] or [7] above may further include a step of winding up the resin film using a winding member. Effect of the Invention

[0008] According to the embodiment of the present invention, it is possible to realize a resin film having excellent anti-blocking properties and capable of fully exhibiting in-plane birefringence by stretching. Also, it is possible to realize a retardation film having excellent anti-blocking properties and sufficient in-plane birefringence. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a resin film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.

[0011] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane birefringence (Δn) "Δn(λ)" is the in-plane birefringence measured with light of wavelength λ nm at 23° C. For example, "Δn(550)" is the in-plane birefringence measured with light of wavelength 550 nm at 23° C. In-plane birefringence (Δn) is calculated from the formula: Δn=nx-ny. (3) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (4) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film).

[0012] A. Overall composition of resin film FIG. 1 is a schematic cross-sectional view of a resin film according to one embodiment of the present invention. The resin film 1 in the illustrated example contains a resin material as a matrix and an antiblocking agent (hereinafter referred to as AB agent) dispersed in the resin material. The average primary particle diameter of the AB agent is 0.1 μm to 1.3 μm. The content ratio (by mass) of the AB agent in the resin film 1 is 350 ppm to 3000 ppm. When the average primary particle size and content of the AB agent are within such ranges, it is possible to impart excellent antiblocking properties to the resin film and to realize a resin film that is capable of fully exhibiting in-plane birefringence by stretching.

[0013] The average primary particle size of the AB agent is preferably 0.1 μm to 1.0 μm, and more preferably 0.5 μm to 1.0 μm. The average primary particle size of the AB agent can be measured by a laser diffraction method. When the average primary particle size of the AB agent is within this range, excellent in-plane birefringence can be stably exhibited when the resin film is stretched.

[0014] The content (by mass) of the AB agent in the resin film 1 is preferably 500 ppm to 3000 ppm, more preferably 500 ppm to 2000 ppm, and further preferably 500 ppm to 1500 ppm. When the content of the AB agent is within this range, sufficient antiblocking properties can be imparted to the resin film, and excellent in-plane birefringence can be more stably exhibited when the resin film is stretched.

[0015] The absolute value of the refractive index difference between the resin material and the AB agent is, for example, 0.10 or less, and preferably 0.08 or less. The lower limit of the absolute value of the refractive index difference between the resin material and the AB agent is typically 0. When the absolute value of the refractive index difference between the resin material and the AB agent is within such a range, the light diffusion caused by the AB agent can be suppressed in the retardation film that can be produced by stretching the resin film. Therefore, the light transmittance can be improved and the haze can be reduced in the retardation film.

[0016] In one embodiment, the refractive index of the AB agent is equal to or lower than the refractive index of the resin material. When the refractive index of the AB agent is equal to or lower than the refractive index of the resin material and the refractive index difference between the resin material and the AB agent is within the above range, the light transmittance can be further improved and the haze can be further reduced in the retardation film.

[0017] The refractive index of the AB agent is, for example, 1.35 or more, preferably 1.40 or more. On the other hand, the refractive index of the AB agent is, for example, 1.65 or less, preferably 1.60 or less, more preferably 1.55 or less, and even more preferably 1.50 or less. The refractive index of the AB agent can be measured at 25°C using light with a wavelength of 590 nm, for example, in accordance with JIS K7142. The refractive index of the resin material is, for example, 1.40 or more, preferably 1.45 or more, more preferably 1.48 or more. On the other hand, the refractive index of the resin material is, for example, 1.70 or less, preferably 1.65 or less, more preferably 1.60 or less. The refractive index of the resin material can be measured at 25° C. using light with a wavelength of 590 nm, for example, in accordance with JIS K7142.

[0018] The dynamic friction coefficient of the resin film 1 is, for example, 1.2 or less, and preferably 1.0 or less. On the other hand, the lower limit of the dynamic friction coefficient of the resin film 1 is typically 0.2. The dynamic friction coefficient of the resin film can be measured according to JIS K7125. If the dynamic friction coefficient of the resin film is within this range, excellent anti-blocking properties can be stably imparted to the resin film.

[0019] As described above, the resin film 1 has excellent anti-blocking properties. Therefore, the resin film 1 can be typically wound into a roll without a release liner. This can prevent dents from being formed on the resin film even when the resin film is wound into a roll.

[0020] The indentation elastic modulus of the resin film 1 at 25° C. is, for example, 2.0 N to 6.5 N, or for example, 2.5 N to 6.0 N. The indentation elastic modulus of the resin film can be measured by a nanoindentation method. Even if the resin film has an indentation modulus in this range, the formation of dents in the resin film can be sufficiently suppressed by winding the resin film without a release liner.

[0021] B. Details of the resin film The resin film 1 typically has optical isotropy before stretching. In this specification, "optically isotropic" means that the in-plane retardation Re(550) and the retardation Rth(550) in the thickness direction are in the following ranges. The in-plane retardation Re(550) of the resin film 1 is, for example, 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. On the other hand, the lower limit of the in-plane retardation Re(550) of the resin film 1 is typically 0 nm. The resin film 1 has a thickness direction retardation Rth(550) of, for example, −10 nm to +10 nm, and preferably −5 nm to +5 nm.

[0022] The thickness of the resin film 1 is, for example, 30 μm or more, preferably 40 μm or more. On the other hand, the thickness of the resin film 1 is, for example, 130 μm or less, preferably 120 μm or less. When the thickness of the resin film is in such a range, a retardation film having a desired thickness can be stably produced by stretching the resin film.

[0023] B-1.Resin material The resin film 1 contains a resin material as a main component. Specific examples of the resin material include transparent resins such as cycloolefin (COP) resins such as polynorbornene resins, polyester resins such as polyethylene terephthalate (PET) resins, cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC) resins, (meth)acrylic resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polyolefin resins, and acetate resins. In addition, the resins may include thermosetting resins or ultraviolet curing resins such as (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins. The term "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers may also be used. Polymers described in JP 2001-343529 A (WO01 / 37007) may also be used. As the material of this polymer, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The materials of the resin film can be used alone or in combination.

[0024] In one embodiment, the resin material of the resin film 1 is amorphous. When the resin film is made of an amorphous resin material, excellent transparency can be imparted to a retardation film produced from the resin film.

[0025] Of these resin materials, preferably, PC-based resin and COP-based resin are used, and more preferably, PC-based resin is used.

[0026] In one embodiment, the PC resin contains at least a structural unit derived from a dihydroxy compound having a bond structure represented by the following structural formula (1), and is produced by reacting a dihydroxy compound containing at least a dihydroxy compound having at least one bond structure -CH2-O- in the molecule with a carbonate diester in the presence of a polymerization catalyst. In other words, the PC resin contains a structural unit derived from a dihydroxy compound and a carbonate group derived from a carbonate diester. [ka]

[0027] Here, as the dihydroxy compound having a bond structure represented by structural formula (1), any compound can be used as long as it has two alcoholic hydroxyl groups, contains a structure having a linking group -CH2-O- in the molecule, and can react with a carbonate diester in the presence of a polymerization catalyst to produce a polycarbonate, and multiple types of compounds can be used in combination.

[0028] In addition, a dihydroxy compound not having the bond structure represented by the above structural formula (1) may be used in combination as a dihydroxy compound for use in a PC resin. Hereinafter, a dihydroxy compound having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (A), and a dihydroxy compound not having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (B).

[0029] (Dihydroxy compound (A)) The "linking group -CH2-O-" in the dihydroxy compound (A) means a structure that bonds with atoms other than hydrogen atoms to form a molecule. In this linking group, the atom to which at least an oxygen atom can be bonded or the atom to which a carbon atom and an oxygen atom can be bonded simultaneously is preferably a carbon atom. The number of "linking groups -CH2-O-" in the dihydroxy compound (A) is preferably 1 or more, more preferably 2 to 4.

[0030] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, and 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene. )-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene;Bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2-bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl] 1,1-bis[4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-phenylphenyl]propane, isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane bis(hydroxyalkoxyaryl)alkanes, such as 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; bis(hydroxyalkoxyaryl)cycloalkanes, such as 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxy diaryl ethers, such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxy aryl sulfides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxy aryl sulfoxides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfone and 4,4'-bis[4-(2- bishydroxyalkoxyarylsulfones, such as 1,4-bishydroxyethoxybenzene, bishydroxyalkoxybenzenes, such as 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane, anhydrous sugar alcohols, such as dihydroxy compounds represented by the following formula (2), and compounds having a cyclic ether structure, such as spiro glycols, such as those represented by the following general formula (3). The dihydroxy compounds (A) may be used alone or in combination.

[0031] [ka]

[0032] [ka]

[0033] Of these dihydroxy compounds (A), preferred is the dihydroxy compound represented by the above formula (2). Examples of the dihydroxy compound represented by the above formula (2) include isosorbide, isomannide, and isoidite, which are stereoisomeric, and these may be used alone or in combination of two or more. Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as resources, is most preferred in terms of availability, ease of production, optical properties, and moldability.

[0034] The ratio of the structural units derived from the dihydroxy compound (A) to the structural units derived from all dihydroxy compounds contained in the PC resin is, for example, 10 mol% or more, preferably 40 mol% or more, more preferably 60 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (A) is, for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less. When the ratio of the dihydroxy compound (A) is within the above range, the desired refractive index characteristics can be imparted to the retardation film that can be produced from the resin film.

[0035] (Dihydroxy Compound (B)) As a dihydroxy compound that is a structural unit of a PC resin, a dihydroxy compound (B) can be used together with a dihydroxy compound (A). By using the dihydroxy compounds (A) and (B) in combination, a desired refractive index characteristic can be stably imparted to a retardation film that can be produced from a resin film.

[0036] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compounds (B) may be used alone or in combination. Of the dihydroxy compounds (B), preferably, alicyclic dihydroxy compounds are used.

[0037] The alicyclic dihydroxy compound is not particularly limited, but preferably includes a compound having a 5-membered ring structure or a 6-membered ring structure. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. When the alicyclic dihydroxy compound has a 5-membered ring or a 6-membered ring structure, the heat resistance of the resulting PC resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, more preferably 30 or less.

[0038] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II). HOCH2-R 1 -CHOH (I) H.O.R. 2 -OH (II) (In formulas (I) and (II), R 1 and R 2 Each of represents a cycloalkylene group having 4 to 20 carbon atoms.

[0039] Cyclohexanedimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 is represented by the following general formula (Ia) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.

[0040] [ka]

[0041] The alicyclic dihydroxy compound represented by the above general formula (I), tricyclodecane dimethanol or pentacyclopentadecanedimethanol, is represented by the general formula (I), 1 is represented by the following general formula (Ib) (wherein n is 0 or 1):

[0042] [ka]

[0043] Decalin dimethanol or tricyclotetradecane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is a compound represented by the general formula (I) 1 is represented by the following general formula (Ic) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol.

[0044] [ka]

[0045] Norbornane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 The isomers include various isomers represented by the following general formula (Id): Specific examples of such isomers include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.

[0046] [ka]

[0047] Adamantane dimethanol, which is an alicyclic dihydroxy compound represented by general formula (I), is 1The isomers include various isomers represented by the following general formula (Ie): A specific example of such isomers is 1,3-adamantanedimethanol.

[0048] [ka]

[0049] Cyclohexanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.

[0050] [ka]

[0051] The alicyclic dihydroxy compound represented by the above general formula (II), tricyclodecanediol or pentacyclopentadecanediol, is a compound represented by the general formula (II), 2 is represented by the following general formula (IIb) (wherein n is 0 or 1):

[0052] [ka]

[0053] Decalindiol or tricyclotetradecanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is a compound represented by the general formula (II) in which R 2is represented by the following general formula (IIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol.

[0054] [ka]

[0055] Norbornanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IId): Specific examples of such isomers include 2,3-norbornanediol and 2,5-norbornanediol.

[0056] [ka]

[0057] The adamantanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is represented by the following general formula (II): 2 is represented by the following general formula (IIe): A specific example of such an isomer is 1,3-adamantanediol.

[0058] [ka]

[0059] Among the specific examples of the alicyclic dihydroxy compound described above, preferred are cyclohexanedimethanols, tricyclodecane dimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoints of availability and ease of handling, more preferred are 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecane dimethanol, and even more preferred is tricyclodecane dimethanol.

[0060] The ratio of the structural units derived from the dihydroxy compound (B) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (B) is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.

[0061] Details of these PC resins are described, for example, in JP 2012-31370 A (Patent No. 5448264), the disclosure of which is incorporated herein by reference.

[0062] In one embodiment, the PC resin contains a structural unit derived from the dihydroxy compound (A) represented by the above formula (2), a structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group linking them together. When a PC resin containing these structural units is applied to a resin film, excellent in-plane birefringence can be stably exhibited when the resin film is stretched. In such a PC resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2. In such a PC resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.

[0063] B-2. Anti-blocking agents The resin film 1 contains an AB agent in addition to a resin material. The AB agent typically has a particulate form, and is dispersed in the resin material as aggregates in which a plurality of particles of the AB agent are aggregated together.

[0064] The AB agent is preferably transparent. Examples of materials constituting the AB agent include metal oxides, resins, and glass. Examples of metal oxides include silica, alumina, titania, zirconia, and calcium oxide. Examples of resins include polymethyl methacrylate, polystyrene, polyurethane, (meth)acrylic resins, (meth)acrylic-styrene copolymers, benzoguanamine, melamine, polycarbonate, and silicone. Examples of glass include magnesium fluoride. The surface of the AB agent may be subjected to any suitable surface modification, for example, chemical modification, preferably alkyl group modification. The AB agents may be used alone or in combination of two or more. Of these AB agents, metal oxides are preferred, silica is more preferred, alkyl group-modified silica is further preferred, and methyl-modified silica is particularly preferred.

[0065] The resin film 1 may contain any suitable additive in addition to the above-mentioned resin material and AB agent. Examples of the additive include antioxidants, UV absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents. Any suitable surface treatment layer may be provided on the surface of the resin film 1 (the surface opposite to the pressure-sensitive adhesive layer 2). Examples of the surface treatment layer include an easy-adhesion layer, an easy-slip layer, an antistatic layer, an antireflection layer, and an oligomer prevention layer.

[0066] C. Manufacturing method of resin film The above-mentioned resin film 1 can be produced by any appropriate method. In one embodiment, the method for producing the resin film includes a step of preparing a resin composition (preparation step), a step of passing the resin composition through a filter (filter passing step), and a step of extruding the resin composition after passing through the filter (extrusion molding step).

[0067] In the preparation step, typically, the above-mentioned resin material is melted, and then the molten resin material is mixed with the above-mentioned AB agent to prepare a resin composition.

[0068] The resin material before melting may have any suitable shape. In one embodiment, the resin material is pelletized in advance. The method of pelletizing the resin material is not particularly limited, and may be a strand cut method or a hot cut method. Details of the pellet preparation process are described in, for example, JP 2013-181105 A. The description of this patent document is incorporated herein by reference.

[0069] Next, the resin material (typically pellets) is heated to melt. The heating temperature may be any appropriate value depending on the resin material. The molten resin material is mixed with the AB agent. This prepares a molten resin composition. The range of the content ratio of the AB agent in the resin composition is, for example, the same as the range of the content ratio of the AB agent in the resin film 1 described above.

[0070] In the filter passing step, the molten resin composition is passed through a filter, whereby foreign matter and / or aggregates of the AB agent contained in the resin composition can be removed from the resin composition.

[0071] The filter may have any suitable configuration, and examples of the filter include a screen mesh and a disk filter, and preferably a screen mesh. The opening of the screen mesh is, for example, 0.080 mm or less, preferably 0.070 mm or less, and more preferably 0.055 mm or less. When the screen mesh has such openings, it is possible to prevent excessively large foreign matter and / or aggregates of the AB agent from being mixed into the formed resin film. On the other hand, the mesh size of the screen mesh is, for example, 0.025 mm or more, preferably 0.035 mm or more. When the screen mesh has such mesh size, the resin composition can smoothly pass through the screen mesh. Therefore, the resin composition can be prevented from being retained and from being excessively heated. This can prevent the generation of gel-like matter due to thermal crosslinking of the resin material.

[0072] In the extrusion molding step, the molten resin after passing through the filter is typically extruded into a film shape using a die, thereby preparing the resin film 1. The above-mentioned preparation step, filter passing step, and extrusion molding step can be performed by any appropriate film forming device.

[0073] The method for producing the resin film 1 may include, in addition to the above-mentioned preparation step and the above-mentioned film-forming step, a step (winding step) in which a winding member winds up the resin film. In the winding step, the winding member winds up the resin film 1 into a roll. The winding member typically has a cylindrical shape and is rotatable about its axis. Since the resin film 1 has excellent anti-blocking properties, even when the resin film 1 is wound into a roll, the resin films 1 can be sufficiently prevented from sticking to each other. In this manner, the resin film 1 is manufactured.

[0074] D. Retardation film The above-mentioned resin film 1 can be applied to any suitable application. The resin film 1 is excellent in the expression of in-plane birefringence by stretching, and therefore can be suitably used for the manufacture of a retardation film. Specifically, by stretching the resin film, the in-plane birefringence can be sufficiently expressed, and a retardation film can be manufactured. The stretching conditions (e.g., stretching temperature, stretching ratio, stretching direction) and stretching method (e.g., longitudinal uniaxial stretching) can be arbitrarily and appropriately adjusted depending on the type of polymer and the desired optical properties (e.g., refractive index properties, in-plane retardation, retardation in the thickness direction).

[0075] Such a retardation film contains the above-mentioned resin material and the above-mentioned AB agent. The range of the content ratio of the AB agent in the retardation film is, for example, the same as the range of the content ratio of the AB agent in the resin film 1 described above. Therefore, the retardation film has excellent anti-blocking properties, and therefore can be typically wound into a roll without a release liner.

[0076] In addition, the retardation film exhibits sufficient in-plane birefringence. In other words, the refractive index of the retardation film satisfies the relationship nx>ny. The in-plane birefringence Δn(550) of the retardation film is, for example, 0.0042 or more, preferably 0.0045 or more, and more preferably 0.0048 or more. On the other hand, the upper limit of Δn(550) of the retardation film is typically 0.0050.

[0077] The retardation film may exhibit a reverse dispersion wavelength characteristic in which the in-plane birefringence increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the in-plane birefringence decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the in-plane birefringence hardly changes according to the wavelength of the measurement light. In one embodiment, the retardation film exhibits a flat wavelength dispersion characteristic.

[0078] The thickness of the retardation film can be arbitrarily and appropriately adjusted so as to obtain an in-plane retardation according to the application. The thickness of the retardation film is, for example, 1 μm or more, preferably 4 μm or more, more preferably 10 μm or more. On the other hand, the thickness of the retardation film is, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less.

[0079] The total light transmittance of the retardation film is, for example, 80% or more, more preferably 85% or more, and even more preferably 90% or more. The upper limit of the total light transmittance of the retardation film is typically 100%. The total light transmittance of the retardation film can be measured in accordance with JIS R3106-2019. The haze value of the retardation film is, for example, 2.0% or less, preferably 1.5% or less, more preferably 1.0% or less, and further preferably 0.8% or less. The lower limit of the haze value of the retardation film is typically 0%. The haze value of the resin film can be measured in accordance with JIS K7136.

[0080] The absolute value of the photoelastic coefficient of the retardation film is, for example, 20×10 -12 (m 2 / N) or less, preferably 1.0 × 10 -12 (m 2 / N)~15×10 -12 (m 2 / N), more preferably 2.0×10 -12 (m 2 / N)~12×10 -12 (m 2 When the absolute value of the photoelastic coefficient is within such a range, display unevenness can be suppressed when the retardation film is applied to an image display device. EXAMPLES

[0081] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.

[0082] (1) Slipperiness (anti-blocking properties) The resin films obtained in the Examples and Comparative Examples were rubbed against each other to evaluate the slipperiness (anti-blocking property) according to the following criteria. The results are shown in Table 1. If the slipperiness is sufficient, blocking between the resin films can be sufficiently suppressed even when the resin film alone is wound into a roll. ◎: The base films slide easily and do not stick to each other. ◯: The base films do not stick to each other, but they are slightly slippery compared to ◎ ×: The base films stick together and do not slide.

[0083] (2) In-plane birefringence Δn The resin films obtained in the examples and comparative examples were stretched laterally by 1.6 times at a stretching temperature of 135° C. and a stretching speed of 1% / sec, thereby preparing retardation films having a thickness of 25 μm. Next, the in-plane birefringence of the retardation film was automatically measured using Axoscan (manufactured by Axometrics). The measurement wavelength was 550 nm, and the measurement temperature was 23° C. The results are shown in Table 1.

[0084] <<Preparation Example 1: PC Resin Film>> 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecane dimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, the temperature of the heating vessel was heated to 150°C as the first step of the reaction, and the raw materials were dissolved (about 15 minutes) while stirring as necessary. Next, the pressure was changed from normal pressure to 13.3 kPa, and the temperature of the heating vessel was raised to 190°C in one hour, while the generated phenol was extracted outside the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, the pressure in the reaction vessel was changed to 6.67 kPa, the temperature of the heating vessel was raised to 230°C in 15 minutes, and the generated phenol was extracted outside the reaction vessel as the second step. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure inside the reaction vessel was lowered to 0.200 kPa or less in order to remove the phenol that was generated. After the predetermined stirring torque was reached, the reaction was terminated and the reaction product was extruded into water to obtain pellets of PC resin.

[0085] [Example 1 and Comparative Example 1] The PC resin pellets obtained in Preparation Example 1 were vacuum dried at 100°C for 12 hours. Thereafter, the PC resin pellets and an AB agent (fine particles of methyl-modified silica, average primary particle size: 0.5 μm, refractive index: 1.43, manufactured by Nippon Shokubai Co., Ltd., product name: Sea Hoster KE) were supplied to a film forming device. The ratio of the AB agent to the total amount of the pellets and the AB agent, and the average primary particle size of the AB agent are shown in Table 1. The film-forming equipment was equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250°C), a screen mesh with an opening of 0.045 mm, a T-die (width 1700 mm, set temperature: 250°C), a casting roll (set temperature: 60°C), and a winding member. More specifically, the pellets and the AB agent were supplied to a single-screw extruder and heated. As a result, the pellets were melted, and the molten PC resin and the AB agent were kneaded to prepare a resin composition. Thereafter, the resin composition was extruded from the single-screw extruder and passed through a screen mesh and a T-die in this order. As a result, a PC resin film having a thickness of 40 μm was produced. After passing through a cast roll, the PC resin film was taken up by a take-up member. In this manner, a PC resin film (resin film) was obtained.

[0086] [Example 2] A PC resin film (resin film) was obtained in the same manner as in Example 1, except that the AB agent (polymer particles, average primary particle size: 0.5 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) was changed to an AB agent (average primary particle size: 1.0 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) and the addition ratio of the AB agent to the total amount of pellets and AB agent was changed to 500 ppm.

[0087] [Comparative Example 2] A PC resin film (resin film) was obtained in the same manner as in Example 1, except that the AB agent was not used.

[0088] [Table 1]

[0089] [evaluation] As is clear from Table 1, when the average primary particle diameter of the AB agent in a resin film is 0.1 μm to 1.3 μm and the content of the AB agent is 350 ppm to 3000 ppm, the resin film can be imparted with excellent antiblocking properties, and sufficient in-plane birefringence can be exhibited by stretching the resin film. [Industrial Applicability]

[0090] The resin film of the present invention can be applied to various industrial products, and can be particularly suitably used in the production of retardation films. [Explanation of symbols]

[0091] 1 Resin film

Claims

1. A resin material as a matrix; an antiblocking agent dispersed in the resin material; The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm; A resin film, wherein the content of the antiblocking agent is 350 ppm to 3000 ppm.

2. The resin film according to claim 1, having an indentation modulus of elasticity at 25°C of 2.0 N to 6.5 N.

3. The resin film according to claim 1 , which has a dynamic friction coefficient of 1.0 or less.

4. The resin film according to claim 1 , wherein the resin material includes a polycarbonate-based resin.

5. A resin material as a matrix; an antiblocking agent dispersed in the resin material; The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm; The content of the antiblocking agent is 350 ppm to 3000 ppm, A retardation film having an in-plane birefringence Δn(550) of 0.0045 or more.

6. A step of mixing a molten resin material and an antiblocking agent to prepare a resin composition; Passing the resin composition through a filter; and extrusion molding the resin composition after passing through the filter. The average primary particle size of the antiblocking agent is 0.1 μm to 1.3 μm; The content of the antiblocking agent in the resin composition is 350 ppm to 3000 ppm.

7. The filter is a screen mesh, The method for producing a resin film according to claim 6, wherein the opening of the screen mesh is 0.035 mm to 0.070 mm.

8. The method for producing a resin film according to claim 6 or 7, further comprising a step of winding up the resin film with a winding member.

Citation Information

Patent Citations

  • Manufacture of member for liquid crystal display

    JP1997325329A

  • Optical film, backlight system, and liquid crystal display device

    JP2006163169A

  • Polycarbonate-based resin film, material for optical recording medium given by using the same, and material for liquid crystal display

    JP2006182879A

  • Filter and method for manufacturing resin composition using the same

    JP2010221432A

  • Method of manufacturing retardation film

    JP2011017761A