Method for fixing carbon dioxide and method for producing cement admixture

By controlling water content through pre-calculated evaporation rates to maintain specific solid-liquid ratios, the method addresses inefficiencies in carbon dioxide fixation in cementitious materials, achieving enhanced carbonation efficiency and higher carbonation degrees.

JP2024145581AActive Publication Date: 2024-10-15MITSUBISHI UBE CEMENT CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023057998
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing methods for fixing carbon dioxide in cementitious materials face inefficiencies due to moisture evaporation and inconsistent water content during carbonation processes, leading to low final carbonation degrees and prolonged reaction times.

Method used

A method involving controlled water addition based on pre-calculated evaporation rates to maintain a specific solid-liquid ratio within a predetermined range during the carbon dioxide fixation step, ensuring efficient carbon dioxide immobilization in cementitious hardened bodies.

Benefits of technology

This approach enhances carbon dioxide fixation efficiency by maintaining optimal moisture levels, allowing for high carbonation degrees in a shorter time frame, thereby improving the carbonation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145581000001_ABST
    Figure 2024145581000001_ABST
Patent Text Reader

Abstract

To provide a method for efficiently fixing CO2 in a hardened cementitious body.SOLUTION: A method for fixing carbon dioxide in a hardened cementitious body includes a carbon dioxide fixation process of contacting a mixture containing a hardened cementitious body and water with carbon dioxide-containing gas. The carbon dioxide fixation process is carried out while adding water to the mixture on the basis of, a preliminarily calculated water evaporation rate in the process, and while maintaining a water content in the mixture within a range of 80 to 150 mass% of the water content that is preset in a solid-liquid ratio range of 0.1 to 0.5.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for sequestration of carbon dioxide and a method for producing a cement mix. [Background technology]

[0002] In order to achieve carbon neutrality in 2050, the reduction of CO2 emitted from factories, including cement factories, is an issue. Therefore, a method for fixing CO2 as CaCO3 in materials containing a lot of calcium, such as cement hardened bodies, has been developed. For example, Patent Document 1 proposes a method of fixing carbon dioxide by contacting a cementitious hardened body with a carbon dioxide-containing gas having a moisture content of 1.5% or more and a temperature of 75 to 175°C. Patent Document 2 proposes a method of fixing CO2 in exhaust gas to solid particles by contacting a gas containing CO2 with an aggregate of solid particles containing CaO and / or Ca(OH)2. Patent Document 3 also proposes a method of obtaining cement paste by grinding waste concrete and separating aggregate and cement paste. Patent Document 4 describes a method of fixing CO2 by collecting materials obtained by crushing waste concrete, supplying water, stirring, and repeating alternating processes of wetting and drying. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-15659 A [Patent Document 2] JP 2000-197810 A [Patent Document 3] Patent Publication No. 2022-126254 [Patent Document 4] JP 2009-90198 A Summary of the Invention [Problem to be solved by the invention]

[0004] Here, the methods of Patent Documents 1 and 2 disclose that water is supplied to the cementitious hardened body to perform carbonation, but even if water is supplied, the water evaporates depending on the treatment temperature, resulting in a low final carbonation degree. The method of Patent Document 3 does not describe how to efficiently recover (in a short time and with a high degree of carbonation) the cement paste in which CO2 has been fixed. The method of Patent Document 4 is inefficient because the material is repeatedly dried and wetted intermittently.

[0005] The present disclosure has been made in consideration of the above circumstances, and aims to provide a method for efficiently fixing CO2 in a cementitious hardened body, and a method for producing a cement mixture. [Means for solving the problem]

[0006] [1] A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas containing carbon dioxide, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a range of 80 to 150 mass% of a preset water content in a solid-liquid ratio range of 0.1 to 0.5. [2] The carbon dioxide fixation step is carried out in a container while monitoring the water evaporation rate, The container has an inlet for introducing the gas and an outlet for discharging the gas from within the container, The method of claim 1, wherein the water evaporation rate is calculated from the difference between the amount of water vapor contained in the gas discharged at the outlet and the amount of water vapor contained in the gas flowing in at the inlet. [3] A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas containing carbon dioxide, The carbon dioxide fixation step is carried out while water is added to the mixture based on a water evaporation rate in the step that is calculated in advance, and while the water content in the mixture is maintained within a range of 0.08 to 0.75 in terms of solid-liquid ratio. [4] The method according to any one of [1] to [3], wherein in the carbon dioxide fixation step, the mixture is contacted with the gas at 20 to 120°C. [5] The method according to any one of [1] to [4], wherein the grain size of the cementitious hardened material is 40 mm or less. [6] The method according to any one of [1] to [5], wherein the carbon dioxide fixation step is carried out while pulverizing the cementitious hardened body in a grinding device. [7] A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: A carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a preset range of 80 to 150 mass% of the water content in the mixture with a solid-liquid ratio of 0.1 to 0.5. [8] A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: A carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a solid-liquid ratio range of 0.08 to 0.75. [9] The manufacturing method according to [7] or [8], wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing concrete chunks with a pulverizing device in a pulverizing device. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a method for efficiently fixing CO2 in a cementitious hardened body and a method for producing a cement mixture. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram of the reaction apparatus used in the examples. [Diagram 2] FIG. 2 is a graph showing the relationship between reaction time and carbonation degree for each of the Reference Examples and Reference Comparative Examples. [Diagram 3] FIG. 3 is a graph showing the relationship between the reaction time and the degree of carbonation or the solid-liquid ratio for Reference Example 3 and Reference Example 3B. [Figure 4] FIG. 4 is a graph showing the relationship between the reaction time and the degree of carbonation or the solid-liquid ratio for Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for fixing carbon dioxide in a cementitious hardened body (method for fixing carbon dioxide) of the present embodiment includes a carbon dioxide fixation step of contacting a mixture containing a cementitious hardened body and water with a gas containing carbon dioxide, and satisfies the following condition (1) or (2). (1) The carbon dioxide fixation process is carried out by adding water to the mixture based on a previously calculated water evaporation rate in the process, while maintaining the water content in the mixture within a preset range of 80 to 150 mass% (hereinafter also referred to as the fluctuation range) of the water content in the mixture with a solid-liquid ratio in the range of 0.1 to 0.5. (2) The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and the water content in the mixture is maintained within a range of 0.08 to 0.75 in terms of solid-liquid ratio. In this specification, the term "solid-liquid ratio" refers to the ratio (mass ratio) of the amount of liquid (water content) to the amount of solids (amount of cementitious hardened body).

[0010] In conventional methods, the moisture content in the sample (a mixture containing cementitious hardened body and water) is not maintained during the carbon dioxide fixation reaction, and as the reaction proceeds, the moisture content decreases, resulting in a decrease in reaction efficiency. However, according to the carbon dioxide fixation method of the present embodiment, the moisture content is maintained within a constant range during the carbon dioxide fixation reaction, making it possible to increase the reaction efficiency.

[0011] In condition (1), first, the amount of moisture contained in the material in the carbon dioxide fixation step is preset. The amount of moisture is determined by a value within the range of 0.1 to 0.5 in terms of solid-liquid ratio. Then, during the carbon dioxide fixation step, water is supplied to the mixture so that the moisture contained in the mixture is within the range of fluctuation. For example, if the preset amount of moisture is 0.25 in terms of solid-liquid ratio, the carbon dioxide fixation step is performed while maintaining the moisture content in the mixture within the range of 80 to 150 mass % of 0.25 (i.e., within the range of 0.2 to 0.375 in terms of solid-liquid ratio).

[0012] The preset water content may be a solid-liquid ratio of 0.15 to 0.40, or 0.15 to 0.35. The fluctuation range may be 90 to 130 mass %, or 95 to 120 mass %.

[0013] In condition (1), when the carbon dioxide fixation step is carried out in a vessel (such as a reactor), the vessel may have an inlet for introducing gas and an outlet for discharging the gas in the vessel, and the amount of water evaporation over time may be measured from the difference between the amount of water vapor contained in the gas discharged at the outlet and the amount of water vapor contained in the gas flowing in at the inlet, and the water evaporation rate may be calculated from the result. This allows the carbon dioxide fixation step to be carried out while monitoring the water evaporation rate, and the amount of water added may be readjusted based on the monitoring results.

[0014] In (2), the water content in the mixture during the carbon dioxide fixation step may be 0.12 to 0.60, or 0.12 to 0.525, in terms of solid-liquid ratio. In (2), the water content in the mixture during the carbon dioxide fixation step may be 0.09 to 0.65, or 0.135 to 0.52, or 0.135 to 0.455, in terms of solid-liquid ratio. In (2), the water content in the mixture during the carbon dioxide fixation step may be 0.095 to 0.60, or 0.1425 to 0.48, or 0.1425 to 0.42, in terms of solid-liquid ratio. In (2), the water content in the mixture during the carbon dioxide fixation step may be 0.22 to 0.30, or 0.24 to 0.30, in terms of solid-liquid ratio.

[0015] The cementitious hardened body is a hardened body obtained by hardening a composition containing cement and water. The cementitious hardened body may be any of a hardened body of cement paste, a hardened body of mortar, and a hardened body of concrete. Examples of cement include various cements such as Portland cement, mixed cement, and ecocement. The cementitious hardened body may be waste materials such as waste building materials made of concrete or mortar, waste materials of hardened cement paste, and sludge generated in ready-mixed concrete. The cementitious hardened body may be a pulverized concrete mass. By using such waste materials, it is possible to effectively utilize resources. The shape and size of the cementitious hardened body are not particularly limited.

[0016] The age of the cementitious hardened body is not particularly limited, and may be, for example, 1 day or more, 7 days or more, 14 days or more, or 1 year or more.

[0017] The cementitious hardened body may contain water. The water content in the cementitious hardened body may be, for example, 15% by mass or more, or 20% by mass or more. The water content W in the cementitious hardened body may be, for example, 70% by mass or less, or 60% by mass or less.

[0018] The gas containing carbon dioxide is not particularly limited, and may be exhaust gas, exhaust gas from a factory, or exhaust gas discharged from equipment such as an incinerator or an electric dust collector. The inflow rate of the gas may be, for example, 0.5 to 5 L / min, or 1 to 3 L / min. The temperature of the gas may be 20 to 120° C. When the reaction is carried out in a vessel, the temperature of the gas may be the temperature at the inlet of the vessel.

[0019] The carbon dioxide content in the gas may be 1% by volume or more, 5 to 50% by volume, or 10 to 30% by volume relative to the total volume of the gas. The gas may contain nitrogen, oxygen, volatile organic compounds, water (water vapor), etc. in addition to carbon dioxide.

[0020] The method for adding water to the mixture is not particularly limited, and may be, for example, by supplying water (liquid water) to the mixture with a pump.

[0021] The carbon dioxide fixation step may be carried out in a container containing the mixture. The container may be one into which gas can be easily introduced and which can heat the mixture in the container (filled type heating device). For example, such a device may be a reactor equipped with a heater or having a function as a heater. The heater is not particularly limited, and may be an external heating device such as a rubber heater, or an internal heating device such as an infrared ray irradiation device. In the carbon dioxide fixation step, the carbonation reaction may be carried out at a temperature (treatment temperature) of the mixture within a range of 20°C to the boiling point of water (100°C at normal pressure). The temperature of the mixture can be measured by a temperature measuring means such as a thermocouple arranged in the reactor.

[0022] The carbon dioxide fixation step may be carried out in a grinding device. In the grinding device, the carbon dioxide fixation step may be carried out while grinding the cementitious hardened body (such as a concrete block). In addition, after the carbon dioxide fixation step is carried out in a heating device such as a filling type heating device, the cementitious hardened body in which the carbon dioxide has been fixed may be further ground by a grinding device. The grinding may be carried out by a plurality of grinding devices.

[0023] The grinding apparatus may be provided with a water supplying means for supplying water so that the water content of the mixture containing the cementitious hardened body and water in the grinding apparatus is within a certain range.

[0024] The cementitious hardened body may be a pulverized product. The cementitious hardened body may be classified using a test sieve as specified in JIS Z8801-1:2019, or the average particle size (d50 on a volume basis or a number basis, etc.) may be measured using a laser particle size distribution measuring device. The particle size may be 40 mm or less, 10 mm or less, or 1 mm or less.

[0025] When the carbon dioxide fixation step is carried out in a grinding machine, the cementitious hardened body in which carbon dioxide has been fixed may be collected by a dust collector as fine powder contained in the gas from the grinding machine.

[0026] The method for producing a cement mixture according to the present embodiment is for obtaining a cement mixture by fixing carbon dioxide in a cementitious hardened body. Specifically, for example, the method for producing a cement mixture of the present embodiment includes a carbon dioxide fixation step of contacting a mixture containing a cementitious hardened body and water with a gas, and satisfies the following condition (1) or (2). (1) The carbon dioxide fixation process is carried out while adding water to the mixture based on a previously calculated water evaporation rate in the process, and while the water content in the mixture is maintained within a preset range of 80 to 150 mass% of the water content in the mixture with a solid-liquid ratio in the range of 0.1 to 0.5. (2) The carbon dioxide fixation step is performed while adding water to the mixture based on a water evaporation rate in the step calculated in advance, and while the water content in the mixture is kept within a range of 0.08 to 0.75 in terms of solid-liquid ratio. That is, the cement mixture of the present embodiment may be one produced by the carbon dioxide fixation method of the present embodiment.

[0027] There are no particular limitations on the use of the cement admixture as long as it is used by mixing with cement, but it can also be used as a solidification material such as a soil improvement material. EXAMPLES

[0028] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0029] <Preparation of hardened cementitious material> Ordinary Portland cement was mixed with water to achieve a water-cement ratio (W / C) of 0.4, and then cured for 28 days. After curing, the cementitious hardened body was pulverized in a ball mill until the particle size was 0.3 mm or less, obtaining a cement paste powder. The particle size (average particle diameter) of the cementitious hardened body was measured using a laser particle size distribution analyzer. Table 1 shows the chemical composition of the cement paste powder.

[0030] [Table 1]

[0031] <Reaction Apparatus> Carbon dioxide was fixed in a reactor. A schematic diagram of the reactor is shown in Figure 1. The reactor has the following components: First, the reaction device 10 has a reactor 1 for performing a CO2 fixation reaction on a sample (a mixture of cement paste powder and water). A Hobart mixer 2 is attached to the reactor 1, and it is possible to stir the sample in the reactor. A CO2 cylinder 3 and an N2 cylinder 4 are connected to the inlet of the reactor 1, and it is possible to flow gas into the reactor 1. The reaction device 10 has a pump 5. The pump 5 is connected to the reactor 1 and a tank 6 containing water, and it is possible to share water with the reactor 1. A rubber heater 7 is attached to the reactor 1, and it is possible to heat the reactor 1. A temperature controller 8 is further connected to the rubber heater, and a thermocouple 9 attached inside the reactor is connected to the temperature controller 8. This makes it possible to manage the temperature of the sample in the reactor by controlling the temperature of the rubber heater with the temperature controller 8 while measuring the temperature inside the reactor 1 with the thermocouple 9.

[0032] <Carbon dioxide fixation (carbonation) reaction> The prepared cement paste powder (200g) was put into the reactor of the above-mentioned reactor and stirred with a Hobart mixer. The temperature inside the reactor was adjusted to 20°C with a rubber heater installed at the bottom of the reactor. Gas with a CO2 concentration adjusted to 20% by volume using N2 and CO2 cylinders was passed into the reactor at a flow rate of 2.0L / min, and water was added to obtain the W / P value in Table 2, and the CO2 fixation reaction was carried out on the mixture obtained. During the fixation reaction, samples were collected at regular intervals and the carbonation degree was measured using the following formula (1) with a thermogravimetric differential thermal analyzer (TG-DTA). W / P is the mass ratio of water (W) to cement paste powder (P).

[0033] <How to calculate carbonation> The carbonation degree was calculated using the following formula (1).

number

[0034] (Reference Examples 1 to 5, Reference Comparative Examples 1 and 2) Table 2 shows the W / P and carbonation degree 4 hours after the start of the reaction for each of the reference and reference comparative examples. Figure 2 also shows the relationship between time and carbonation degree for each of the reference and reference comparative examples. As shown in Figure 2, it was confirmed that when the W / P was 0.1 to 0.5, treatment with a high carbonation degree could be achieved in a short time. On the other hand, it was found that when the solid-liquid ratio was increased, the initial carbonation was slow.

[0035] [Table 2]

[0036] (Reference example 3B) The heater temperature was set to 20°C or 100°C, and carbon dioxide was fixed in the mixture with a solid-liquid ratio of 0.25 in the same manner as in Reference Example 1, and the carbonation degree was measured. The results are shown in Figure 3. In Figure 3, the plots of white squares and black triangles show the treatment at 100°C, the solid line shows the carbonation degree, and the dashed line shows the solid-liquid ratio. In Figure 3, the plots of white circles and black circles show the treatment at 20°C, the solid line shows the carbonation degree, and the dashed line shows the solid-liquid ratio. From Figure 3, it can be seen that when treatment was performed at 100°C, the initial carbonation rate was the same as when treatment was performed at 20°C, but the final carbonation degree was lower.

[0037] (Examples 1 and 2) The water evaporation rate at treatment temperatures of 20°C and 100°C was calculated from the slope of the graph of time versus solid-liquid ratio in Figure 3. Using the calculated water evaporation rate, water was added so that the solid-liquid ratio remained within a certain range of 0.25, while carbonation was carried out in the same manner as above. Table 3 shows the W / P and treatment temperature, and the fixation of carbon dioxide and measurement of the degree of carbonation were carried out in the same manner as in Reference Example 1, except for the addition of water, W / P and treatment temperature. The results are shown in Table 3 and Figure 4. It was confirmed that when water was added so that the solid-liquid ratio was within a certain range, treatment could be performed with a high degree of carbonation in a short time regardless of the treatment temperature.

[0038] [Table 3] [Explanation of symbols]

[0039] 10...Reactor, 1...Reactor, 2...Hobart mixer, 3...CO2 cylinder, 4...N2 cylinder, 5...Pump, 6...Tank, 7...Rubber heater, 8...Temperature controller, 9...Thermocouple.

Claims

1. A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas containing carbon dioxide, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a range of 80 to 150 mass% of a preset water content in a solid-liquid ratio range of 0.1 to 0.

5.

2. The carbon dioxide fixation step is carried out in a container while monitoring the water evaporation rate, The container has an inlet for introducing the gas and an outlet for discharging the gas from within the container, The method according to claim 1 , wherein the water evaporation rate is calculated from a difference between an amount of water vapor contained in the gas discharged at the outlet and an amount of water vapor contained in the gas flowing in at the inlet.

3. A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: a carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas containing carbon dioxide, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a solid-liquid ratio range of 0.08 to 0.

75.

4. The method according to claim 1 or 3, wherein in the carbon dioxide fixation step, the mixture is contacted with the gas at 20 to 120° C.

5. The method according to claim 1 or 3, wherein the particle size of the cementitious hardened body is 40 mm or less.

6. The method according to claim 1 or 3, wherein the carbon dioxide fixation step is carried out while pulverizing the cementitious hardened body in a grinding device.

7. A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: A carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a range of 80 to 150 mass% of a preset water content in a solid-liquid ratio range of 0.1 to 0.

5.

8. A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: A carbon dioxide fixation step of contacting a mixture containing the cementitious hardened body and water with a gas, The carbon dioxide fixation step is carried out while water is added to the mixture based on a previously calculated water evaporation rate in the step, and while the water content in the mixture is maintained within a range of 0.08 to 0.75 in terms of solid-liquid ratio.

9. 9. The method according to claim 7 or 8, wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing the concrete chunks with a pulverizing device in a pulverizing device.

Citation Information

Patent Citations

  • Carbon dioxide consuming material and method for producing carbon dioxide consuming material from waste construction material

    JP1993212278A

  • Apparatus for treating concrete sludge

    JP2009136770A

  • Method for using cement-containing waste material

    JP2014117636A

  • Method for producing cement powder composition

    JP2020152631A