Manufacturing method of joint body

The method addresses low thermal conductivity and unreliable bonds in electronic component- substrate joints by using a sintered metal bonding layer with controlled metal paste application patterns, ensuring reliable and crack-free connections.

JP2024145803APending Publication Date: 2024-10-15MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023058315
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for joining electronic components to substrates using solder materials result in low thermal conductivity, crack formation under temperature cycles, and unreliable bonds due to intermetallic compound generation and organic solvent residues, leading to potential short circuits and reduced reliability, especially in high-temperature environments.

Method used

A method involving a sintered metal bonding layer formed by applying a metal paste with controlled application patterns to suppress fillets and voids, utilizing a metal paste application step with defined recessed and protruding areas to promote organic solvent discharge and ensure complete bonding.

Benefits of technology

The method effectively suppresses fillet formation, crack occurrence, and void generation, enhancing bonding reliability and thermal conductivity, suitable for high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145803000002
    Figure 2024145803000002
  • Figure 2024145803000003
    Figure 2024145803000003
  • Figure 2024145803000004
    Figure 2024145803000004
Patent Text Reader

Abstract

To provide a manufacturing method of a joint body that can suppress the formation of fillets and the occurrence of cracks and voids in a joint layer.SOLUTION: A manufacturing method of a joint body includes a metal paste application step of applying a metal paste containing metal powder and a solvent to a portion of the mounting surface of a first member, the joint surface of a second member has a rectangular shape, and the application pattern formed on the mounting surface of the first member in the metal paste application step has a paste-deficient region in which the rectangular side portion of the joint surface of the second member are recessed inward of the joint surface, and the metal paste is not applied, and a paste-protruding region in which the metal paste protrudes outward from a rectangular corner portion of the joint surface of the second member.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a joined body in which a second member is joined to a part of a mounting surface of a first member via a joining layer made of a metal sintered body. [Background technology]

[0002] For example, electronic devices such as LEDs and power modules have a structure in which electronic components such as semiconductor elements are bonded onto a substrate having a circuit layer made of a metal member. Here, when joining electronic components such as semiconductor elements to the mounting surface of a substrate, a method using a solder material is widely used, as shown in Patent Document 1, for example. Furthermore, Patent Document 2 proposes a technique in which a plating film and a Sn-based solder layer are formed, and then alloyed by heat treatment to form an alloy layer, and electronic components are mounted on a substrate.

[0003] Furthermore, Patent Documents 3-6 propose a technique for bonding electronic components such as semiconductor elements to the mounting surface of a substrate using a metal paste containing silver powder and an organic solvent. In this metal paste, a bonding layer made of a conductive sintered body is formed, and the electronic components such as semiconductor elements are bonded to the mounting surface of the substrate via this bonding layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-271782 A [Patent Document 2] Patent No. 6459656 [Patent Document 3] Patent No. 6428339 [Patent Document 4] Patent No. 6712620 [Patent Document 5] Patent No. 6845385 [Patent Document 6] Patent Publication No. 2021-073639 Summary of the Invention [Problem to be solved by the invention]

[0005] However, as described in Patent Documents 1 and 2, when components are joined together using a solder material, an intermetallic compound is generated in the joining layer formed between the components, and there is a risk that the thermal conductivity will be relatively low. Furthermore, when subjected to a temperature cycle, cracks are likely to occur in the joining layer, and there is a risk that the joining reliability will decrease. Furthermore, when an electronic component such as a semiconductor element is joined to a substrate via a solder material, there is a risk that part of the solder will melt when used in a high-temperature environment, resulting in a decrease in the reliability of the joint between the electronic component such as a semiconductor element and the substrate. In particular, in recent years, the heat resistance of semiconductor elements themselves has improved, and semiconductor devices are sometimes used in high-temperature environments such as the engine compartments of automobiles, making it difficult to meet these demands with the conventional structure in which components are joined with solder.

[0006] On the other hand, in the metal pastes described in Patent Documents 3 to 6, the bonding layer is made of a sintered metal body, and therefore has excellent thermal conductivity and bonding reliability. Furthermore, when the bonding layer is formed from a sintered metal, the bonding layer can be formed under relatively low temperature conditions and the melting point of the bonding layer itself is high, so that the bonding strength does not decrease significantly even in a high temperature environment.

[0007] However, since the above-mentioned metal paste contains an organic component as a solvent, when forming a bonding layer made of a sintered body, the organic component remains at the bonding interface, and there is a risk of cracks or voids occurring in the bonding layer. In particular, when bonding is performed without pressure, the organic component is likely to volatilize rapidly, making it easy for cracks to occur.

[0008] Furthermore, when bonding an electronic component to a substrate, as described in paragraph 0101 of Patent Document 6, a metal paste is usually applied to the mounting surface of the substrate in the same shape and area as the bonding surface of the electronic component, and the electronic component is placed on the applied metal paste and sintered. The bonding surface of the electronic component is usually rectangular. When an electronic component is placed on the applied metal paste, the metal paste may protrude beyond one side of the rectangular joining surface of the electronic component, resulting in the formation of a fillet after sintering. Recently, electronic components have been made thinner, and the formation of the fillet may cause a short circuit, which may hinder the stable manufacture of highly reliable electronic devices.

[0009] This invention has been made in consideration of the above-mentioned circumstances, and aims to provide a method for manufacturing a bonded body that can suppress the formation of fillets and the occurrence of cracks and voids in the bonding layer. [Means for solving the problem]

[0010] In order to solve the above problems, the manufacturing method of a joined body according to aspect 1 of the present invention is a manufacturing method of a joined body in which a second member is joined to a part of a mounting surface of a first member via a joining layer made of a metal sintered body, the joining surface of the second member being rectangular, the manufacturing method of a joined body including a metal paste application process for applying a metal paste containing a metal powder and a solvent to a part of the mounting surface of the first member, a lamination process for laminating the second member on the applied metal paste, and a sintering process for heating the first member and the second member laminated via the metal paste to sinter the metal paste, thereby forming the joining layer made of a sintered body and joining the first member and the second member, the application pattern formed on the mounting surface of the first member in the metal paste application process is characterized in that the rectangular side portions of the joining surface of the second member are recessed inward of the joining surface, and the application pattern includes paste missing regions where the metal paste is not applied, and paste protruding regions where the metal paste protrudes outward from rectangular corner portions of the joining surface of the second member.

[0011] According to the manufacturing method of the bonded body of the first aspect of the present invention, the coating pattern formed on the mounting surface of the first member in the metal paste coating step includes a paste protruding region in which the metal paste protrudes outward from a rectangular corner portion of the bonding surface of the second member, so that when the first member and the second member are laminated with the applied metal paste therebetween, a portion of the applied metal paste is formed that is exposed to the outside. Therefore, when the metal paste is sintered in the sintering step, the discharge of organic components from this exposed portion is promoted, and the occurrence of cracks and voids in the bonding layer can be suppressed. Furthermore, the coating pattern formed on the mounting surface of the first member in the metal paste application process has four sides of the rectangular joint surface of the second member recessed inward, and includes a paste-missing area where the metal paste is not applied. Therefore, when the first member and the second member are stacked together with the applied metal paste between them, the metal paste does not protrude significantly outward from one side of the rectangular joint surface of the second member, thereby suppressing the occurrence of fillets.

[0012] The manufacturing method of a joint body of aspect 2 of the present invention is characterized in that, in the manufacturing method of a joint body of aspect 1 of the present invention, the length of one side of the rectangular shape formed by the joining surface is L, and the area ratio occupied by the paste missing area in the side center area, which is an area that is 1 / 4L length from the center of the one rectangular side formed by the joining surface and 1 / 4L length inward from the one side, is in the range of 10% or more and 70% or less. According to the manufacturing method of the joint body of aspect 2 of the present invention, the length of one side of the rectangular shape formed by the joining surface is defined as L, and the area ratio of the paste missing area in the side center region that is 1 / 4L length from the center of the one side of the rectangular shape formed by the joining surface and 1 / 4L length inward from the one side is within the range of 10% to 70%, so that the metal paste does not protrude significantly outward from one side portion of the second member, and the occurrence of fillets can be reliably suppressed.

[0013] The manufacturing method of a joined body of aspect 3 of the present invention is characterized in that, in the manufacturing method of a joined body of aspect 1 or aspect 2 of the present invention, the ratio S1 / S0 of the area S1 of the paste protruding region to the area S0 of the joining surface of the second member is 8% or more. According to the manufacturing method of the bonded body of aspect 3 of the present invention, the ratio S1 / S0 of the area S1 of the paste protruding region to the area S0 of the bonding surface of the second member is set to 8% or more, thereby ensuring the area of ​​the paste protruding region and promoting the discharge of organic components, thereby further suppressing the occurrence of cracks and voids in the bonding layer.

[0014] The method for producing a bonded body of aspect 4 of the present invention is preferably the method for producing a bonded body of any one of aspects 1 to 3 of the present invention, wherein the first member is a substrate, the second member is an electronic component, and the bonded body is an electronic device. According to the method for manufacturing a bonded body of aspect 4 of the present invention, the first member is a substrate, the second member is an electronic component, and the bonded body is an electronic device. Therefore, it is possible to manufacture a highly reliable electronic device in which the occurrence of cracks and voids in the bonding layer is suppressed and the occurrence of fillets is suppressed. Effect of the Invention

[0015] According to the present invention, it is possible to provide a method for manufacturing a bonded body that can suppress the formation of fillets and the occurrence of cracks and voids in the bonding layer. [Brief description of the drawings]

[0016] [Figure 1] 1 is an explanatory diagram of a bonded body manufactured by a method for manufacturing a bonded body according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a flow diagram showing a method for producing a bonded body according to an embodiment of the present invention. [Diagram 3] 10 is an explanatory diagram showing a metal paste application pattern in a metal paste application process. FIG. [Figure 4] FIG. 13 is an explanatory diagram of the area ratio of the paste missing area in the side center area. [Diagram 5] 13A to 13C are explanatory views showing application patterns of metal paste in a manufacturing method of a bonded body according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A method for producing a bonded body according to an embodiment of the present invention will be described below. The method for producing a bonded body according to the present embodiment produces a bonded body 10 in which a first member 11 and a second member 12 are bonded together via a bonding layer 13.

[0018] 1, the joined body 10 in this embodiment is formed by joining a second member 12 to a part of a mounting surface of a first member 11 via a joining layer 13 made of a metal sintered body. In this embodiment, the joined body 10 is a semiconductor device (electronic device) in which a semiconductor element (second member 12) is joined via the joining layer 13 to a part of a mounting surface of a circuit layer (first member 11) of an insulating circuit board.

[0019] Here, a method for producing the bonded body 10 according to this embodiment will be described with reference to FIGS. The method for manufacturing the bonded body 10 according to the present embodiment includes a metal paste application step S01, a lamination step S02, and a sintering step S03.

[0020] (Metal paste application process S01) First, metal paste 23 containing metal powder and a solvent is applied to a part of the mounting surface of first member 11. In this embodiment, an Ag paste containing silver powder is used as the metal paste 23. There is no particular limitation on the metal paste 23, and for example, a Cu paste containing copper powder may be used.

[0021] In this embodiment, as shown in FIG. 3, the application pattern 25 of the metal paste 23 formed on the mounting surface of the first member 11 includes paste missing regions 25a where the four sides of the rectangular joining surface of the second member 12 are recessed inward and where the metal paste 23 is not applied, and paste protruding regions 25b where the metal paste 23 protrudes outward from the corners of the rectangular joining surface of the second member 12. In this embodiment, as shown in FIG. 3, when viewed from the direction facing the mounting surface, the coating pattern 25 has a rough cross-like shape of a shuriken, with the center portions of the four sides of the rectangle formed by the joining surface of the second member 12 curved inward and concave, and the four corner portions extending diagonally protruding outward.

[0022] In this embodiment, as shown in FIG. 4, the length of one side of the rectangular joining surface of the second member 12 is L, and in a side center region A which is a region that is 1 / 4L long from the center of one side of the rectangular joining surface and 1 / 4L long from the one side to the inside of the joining surface, it is preferable that the area ratio of the paste missing region 25a (occupancy rate of the paste missing region 25a) is within the range of 10% or more and 70% or less. Moreover, it is preferable that the ratio S1 / S0 (area ratio of paste overhanging region 25b) of the area S1 of paste overhanging region 25b to the area S0 of the joining surface of second member 12 is 8% or more.

[0023] In this metal paste application step S01, the method of applying the metal paste 23 is not particularly limited, but for example, a metal mask method, a screen printing method, a dispensing method, etc. can be applied. In this embodiment, the metal paste 23 is printed on the mounting surface of the first member 11 by screen printing. Moreover, the coating thickness of the metal paste 23 is preferably within a range of 20 μm to 500 μm.

[0024] The metal paste 23 to be applied contains silver powder and a solvent. In addition to the silver powder and the solvent, the metal paste 23 may contain a resin, a dispersant, a plasticizer, etc., as necessary. The silver powder used preferably has a purity of 99 mass% or more and an average particle size of 10 nm to 10 μm. It may also be a mixture of multiple silver particle groups having a specific particle size distribution.

[0025] Examples of the solvent include alcohol-based solvents, glycol-based solvents, acetate-based solvents, hydrocarbon-based solvents, and mixtures thereof. Examples of alcohol-based solvents include α-terpineol, isopropyl alcohol, ethyl hexanediol, and mixtures thereof. Examples of glycol-based solvents include ethylene glycol, diethylene glycol, polyethylene glycol, and mixtures thereof. Examples of acetate-based solvents include butyl carbitol acetate. Examples of hydrocarbon-based solvents include decane, dodecane, tetradecane, and mixtures thereof.

[0026] Alternatively, the Ag paste described in Japanese Patent No. 6930578 may be used as the metal paste 23 .

[0027] (Lamination process S02) Next, the second member 12 is laminated on the metal paste 23 applied to the mounting surface of the first member 11. Note that the second member 12 may be laminated after the metal paste 23 applied to the mounting surface of the first member 11 is dried, or the second member 12 may be laminated without drying. Here, since the application pattern 25 of the metal paste 23 is defined as described above, a part of the applied metal paste 23 protrudes and is exposed from the corner portions of the laminated second members 12 .

[0028] (Sintering process S03) Next, the first member 11 and the second member 12 stacked with the metal paste 23 interposed therebetween are heat-treated to sinter the metal paste 23, thereby forming a bonding layer 13 made of a sintered metal body, and bonding the first member 11 and the second member 12 together. In the sintering step S03, the holding temperature is preferably within a range of 200° C. or more and 300° C. or less, and the holding time is preferably within a range of 0 minute or more and 120 minutes or less. Furthermore, the temperature increase rate in the sintering step S03 is desirably within the range of 10° C. / min to 50° C. / min.

[0029] The bonded body 10 of this embodiment is manufactured by the above-mentioned steps.

[0030] According to the manufacturing method of the bonded body of the present embodiment configured as described above, in the metal paste application step S01, the application pattern 25 of the metal paste 23 formed on the mounting surface of the first member 11 includes a paste protruding region 25b in which the metal paste 23 protrudes outward from a rectangular corner portion of the bonding surface of the second member 12, so that when the first member 11 and the second member 12 are laminated via the applied metal paste 23, a part of the applied metal paste 23 is formed in which the part is exposed from the bonding interface to the outside. Therefore, when the metal paste 23 is sintered in the sintering step S03, the discharge of organic components from this exposed part is promoted, and the occurrence of cracks and voids in the bonding layer 13 can be suppressed.

[0031] In the metal paste application process S01, the application pattern 25 of the metal paste 23 formed on the mounting surface of the first member 11 has four sides of the rectangular shape formed by the joining surface of the second member 12 recessed inward, and has a paste-missing area 25a where the metal paste 23 is not applied. Therefore, when the first member 11 and the second member 12 are stacked together with the applied metal paste 23 between them, the metal paste 23 does not protrude significantly outward from one side portion of the second member 12, thereby suppressing the occurrence of fillets.

[0032] Here, in this embodiment, when the length of one side of the rectangular joint surface of the second member 12 is L, and the area ratio of the paste missing area 25a in the side center region A that is 1 / 4L length from the center of one side of the rectangular joint surface of the second member 12 and 1 / 4L length inward from the one side is set to 10% or more, the metal paste 23 will not protrude significantly outward from one side portion of the rectangular joint surface of the second member 12, and the occurrence of fillets can be reliably suppressed. On the other hand, when the proportion of paste missing area 25a in the side center region A is 70% or less, the metal paste 23 can be sufficiently filled at the bonding interface, and the generation of voids in the bonding layer 13 can be reliably suppressed. It is more preferable that the lower limit of the area ratio occupied by paste-missing region 25a in side center region A is 20% or more. It is more preferable that the upper limit of the area ratio occupied by paste-missing region 25a in side center region A is 50% or less.

[0033] Furthermore, in this embodiment, when the ratio S1 / S0 of the area S1 of the paste protruding region 25b to the area S0 of the bonding surface of the second member 12 is 8% or more, the area of ​​the paste protruding region 25b is secured, and the discharge of organic components from the portion of the metal paste 23 that protrudes from the bonding interface is promoted, thereby further suppressing the occurrence of cracks and voids in the bonding layer 13. It is more preferable that the ratio S1 / S0 of the area S1 of the paste overhanging region 25b to the area S0 of the bonding surface of the second member 12 is 15% or more. There is no particular upper limit to the ratio S1 / S0 of the area S1 of the paste overhanging region 25b to the area S0 of the bonding surface of the second member 12, but it is preferable that the ratio be 30% or less.

[0034] In this embodiment, when the first member 11 is a circuit layer (substrate) of an insulating circuit board, the second member 12 is a semiconductor element (electronic component), and the bonded body 10 is a semiconductor device (electronic device), it is possible to manufacture a highly reliable electronic device in which the occurrence of cracks and voids in the bonding layer 13 is suppressed and the occurrence of fillets is suppressed.

[0035] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in the present embodiment, a semiconductor element (second member) is bonded as an electronic component to a circuit layer (first member) of an insulating circuit board, but this is not limited thereto, and it is sufficient that the bonded body is one in which a first member and a second member are bonded via a bonding layer.

[0036] In addition, in this embodiment, the application pattern of the metal paste 23 has been described as the shape shown in Figure 3, but is not limited to this, and for example, as shown in Figures 5(a) to (c), it is sufficient if the application pattern includes paste missing regions 25a in which the four sides of the rectangular shape formed by the joining surface of the second member 12 are recessed inward, and paste protruding regions 25b in which the metal paste 23 protrudes outward from the corners of the rectangular shape formed by the joining surface of the second member 12. EXAMPLES

[0037] The results of an evaluation test performed to evaluate the effects of the method for producing a bonded body according to the present invention will be described below.

[0038] As a first member, a copper substrate (made of oxygen-free copper) measuring 35 mm×35 mm×2 mmt was prepared. A 10 mm x 10 mm x 0.4 mm thick silicon element was prepared as the second member. The bonding surface of the silicon element was coated with a Ti / Ni / Au multilayer plating. Here, in Inventive Examples 1 to 6 and Comparative Examples 1 and 2, the Ag paste of Inventive Example 7 of Japanese Patent No. 6930578 was prepared as the metal paste. In addition, in Example 7 of the present invention and Comparative Examples 3 and 4, a Cu paste (Example 1 of JP 2022-128185 A) was prepared as the metal paste.

[0039] Next, a metal paste was applied to the mounting surface of the copper substrate by screen printing using a metal mask and a metal squeegee, with the thickness of the applied metal paste being 150 μm. At this time, the application pattern of the metal paste was set so that the occupancy rate of the paste missing area and the area ratio of the paste overhanging area described in the above embodiment were as shown in Table 1.

[0040] Then, without drying the applied metal paste, a Si element was laminated on it.

[0041] The copper substrate and the Si element laminated with the metal paste were placed in a heat treatment furnace and heat-treated to sinter the metal paste, bonding the copper substrate and the Si element together through a bonding layer made of a sintered metal. At this time, the holding temperature was 250° C., the holding time was 10 minutes, and the heating rate from room temperature (25° C.) to the holding temperature was 10° C. / min. In the present invention examples 1 to 6 and the comparative examples 1 and 2, since Ag paste is used as the metal paste, the heat treatment atmosphere is an inert gas (N 2 The atmosphere was oxygen (oxygen concentration: 1% by volume or less). In Example 7 of the present invention and Comparative Examples 3 and 4, a Cu paste was used as the metal paste, and the heat treatment atmosphere was an active gas (approximately 3% by volume of formic acid / remainder N 2 ) atmosphere.

[0042] The bonded bodies produced as described above were evaluated for fillet height, and voids and cracks in the bonded layer as follows.

[0043] (Fillet height) The height of the fillet that protruded from the Si element was measured using a measuring microscope (Nikon Solutions MM-800 / LUFA), and the maximum height is shown in Table 1. The height of the fillet is the position of the farthest point from the copper substrate surface in the vertical direction.

[0044] (Voids and cracks) Using an ultrasonic flaw detector (FSP8V manufactured by Hitachi Power Solutions), the entire bonding layer was observed from the direction opposite to the mounting surface of the copper substrate. If the diameter of a circle with the same area as the unbonded area shown in white, i.e., the equivalent circle diameter, was 1 mm or more, it was judged to be a void. Also, if the white or black line was 1 mm or more, it was judged to be a crack. In Table 1, the samples in which voids or cracks were observed are indicated with "x", and the samples in which voids or cracks were not observed are indicated with "o".

[0045] [Table 1]

[0046] In Comparative Examples 1 and 3, the occupancy rate of the paste-deficient area in the side central region A was 0%, meaning that substantially no paste-deficient area was formed, and the fillet height was high at 230 μm. In Comparative Examples 2 and 4, the area ratio of the paste overhanging region was 0%, meaning that substantially no paste overhanging region was formed, and the evaluation of voids and cracks in the bonding layer was "x".

[0047] In contrast, in Examples 1-7 of the present invention, the metal paste application pattern included paste-deficient areas where no metal paste was applied and paste-protruding areas where the metal paste protruded outward, the fillet height was kept to 150 μm or less, and no cracks or voids were observed in the bonding layer.

[0048] From the above, it was confirmed that the present invention can provide a manufacturing method for a bonded body that can suppress the formation of fillets and the occurrence of cracks and voids in the bonding layer. [Explanation of symbols]

[0049] 10 zygote 11 First member 12 Second member 13 Bonding layer 23 Metal Paste 25 Coating Pattern 25a Paste missing area 25b Paste overhang area

Claims

1. A method for manufacturing a joined body in which a second member is joined to a part of a mounting surface of a first member via a joining layer made of a metal sintered body, comprising: The joining surface of the second member is rectangular, a metal paste applying step of applying a metal paste containing a metal powder and a solvent to a part of the mounting surface of the first member; a laminating step of laminating the second member on the applied metal paste; and a sintering step of heat-treating the first member and the second member laminated with the metal paste therebetween to sinter the metal paste and form the bonding layer made of a sintered body to bond the first member and the second member, A method for manufacturing a joint body, characterized in that the application pattern formed on the mounting surface of the first member in the metal paste application process includes paste-deficient areas where the rectangular side portions of the joining surface of the second member are recessed inward of the joining surface, and where the metal paste is not applied, and paste-protruding areas where the metal paste protrudes outward from the rectangular corner portions of the joining surface of the second member.

2. 2. The method for manufacturing a joint body according to claim 1, characterized in that, when the length of one side of the rectangular shape formed by the joining surface is L, the area ratio occupied by the paste missing area in a side center area which is a region that is 1 / 4L length from the center of the one side of the rectangular shape formed by the joining surface and 1 / 4L length inward from the one side is in the range of 10% or more and 70% or less.

3. 3. The method for manufacturing a joint body according to claim 1, wherein a ratio S1 / S0 of an area S1 of the paste protruding region to an area S0 of the joint surface of the second member is 8% or more.

4. 3. The method for producing a bonded body according to claim 1, wherein the first member is a substrate, the second member is an electronic component, and the bonded body is an electronic device.

Citation Information

Patent Citations

  • Power semiconductor device and method of manufacturing power semiconductor device

    JP2015188026A

  • Electronic device and method for manufacturing electronic device

    WO2021149637A1

  • Aluminum casting alloy for intake manifold

    JP1989028339A

  • Optical head for magneto-optical recording carrier

    JP1989059656A

  • Metal paste for soldering and soldering method

    JP2000271782A