Method for fixing carbon dioxide and method for producing cement admixture
By adding water to hardened cementitious materials at a specific ratio and contacting them with high-temperature carbon dioxide, the method enhances carbon dioxide fixation efficiency and carbonation rates, addressing inefficiencies in existing technologies.
Patent Information
- Application Number
- JP2023058352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing methods for carbon dioxide fixation in cementitious materials are inefficient in terms of carbonation rate and recovery time, and methods involving intermittent drying and moistening are not optimal.
A method involving the addition of water at a solid-liquid ratio of 0.4 to 0.7 to hardened cementitious materials, followed by contact with carbon dioxide gas at a temperature of 70°C or higher, either in a container or a grinding device, to enhance carbon dioxide fixation.
This approach enables efficient immobilization of carbon dioxide in cementitious materials, achieving high carbonation rates and resource utilization through the use of waste materials.
Smart Images

Figure 2024145831000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for sequestration of carbon dioxide and a method for producing a cement mix. [Background technology]
[0002] In order to achieve carbon neutrality in 2050, the reduction of CO2 emitted from factories, including cement factories, is an issue. Therefore, a method for fixing CO2 as CaCO3 in materials containing a lot of calcium, such as cement hardened bodies, has been developed. For example, Patent Document 1 proposes a method of fixing carbon dioxide by contacting a cementitious hardened body with a carbon dioxide-containing gas having a moisture content of 1.5% or more and a temperature of 75 to 175°C. Patent Document 2 proposes a method of fixing CO2 in exhaust gas to solid particles by contacting a gas containing CO2 with an aggregate of solid particles containing CaO and / or Ca(OH)2. Patent Document 3 also proposes a method of obtaining cement paste by grinding waste concrete and separating aggregate and cement paste. Patent Document 4 describes a method of fixing CO2 by collecting materials obtained by crushing waste concrete, supplying water, stirring, and repeating alternating processes of wetting and drying. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-15659 A [Patent Document 2] JP 2000-197810 A [Patent Document 3] Patent Publication No. 2022-126254 [Patent Document 4] JP 2009-90198 A Summary of the Invention [Problem to be solved by the invention]
[0004] Here, Patent Documents 1 and 2 disclose that carbonation is carried out by supplying moisture to a cementitious hardened body, but there is still room for improvement in terms of the degree of carbonation. Patent Document 3 does not describe how to efficiently recover (in a short time and at a high carbonation rate) the cement paste in which CO2 has been fixed. The method of Patent Document 4 is inefficient because the material is repeatedly dried and wetted intermittently.
[0005] The present disclosure has been made in consideration of the above circumstances, and aims to provide a method for efficiently fixing CO2 in a cementitious hardened body, and a method for producing a cement mixture. [Means for solving the problem]
[0006] [1] A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: The method comprises a carbon dioxide fixation step including: adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7; and contacting the cementitious hardened body to which water has been added with a carbon dioxide-containing gas at 70°C or higher. [2] The method according to [1], wherein the gas has a temperature of 100°C or higher. [3] The method according to [1] or [2], wherein the grain size of the cementitious hardened body is 40 mm or less. [4] The method according to any one of [1] to [3], wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing concrete chunks with a pulverizing device in a pulverizing device. [5] A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: The method includes a carbon dioxide fixation step of adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7, and contacting the cementitious hardened body to which water has been added with a carbon dioxide-containing gas at 70°C or higher. [6] The manufacturing method according to [5], wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing concrete chunks with a pulverizing device in a pulverizing device. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a method for efficiently fixing CO2 in a cementitious hardened body and a method for producing a cement mixture. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram of the reaction apparatus used in the examples. [Diagram 2] FIG. 2 is a graph showing the relationship between reaction time and carbonation degree for each of the Reference Examples and Reference Comparative Examples. [Diagram 3] FIG. 3 is a diagram showing the relationship between the reaction time and the degree of carbonation or the solid-liquid ratio for Example 1, Comparative Example 1, and each Reference Example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The method for fixing carbon dioxide in a cementitious hardened body of the present embodiment (hereinafter also referred to as a carbon dioxide fixation method) includes a carbon dioxide fixation step including adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7 (obtaining a mixture containing the cementitious hardened body and water) and contacting the cementitious hardened body (mixture) to which water has been added with a gas containing carbon dioxide and at 70°C or higher. According to such a method, CO2 can be efficiently fixed in the cementitious hardened body. In this specification, the term "solid-liquid ratio" refers to the ratio (mass ratio) of the amount of liquid (water content) to the amount of solids (amount of cementitious hardened body).
[0010] In the carbon dioxide fixation step, the amount of water added may be 0.45 to 0.65, and the amount of water added may be 0.45 to 0.6.
[0011] The cementitious hardened body is a hardened body obtained by hardening a composition containing cement and water. The cementitious hardened body may be any of a hardened body of cement paste, a hardened body of mortar, and a hardened body of concrete. Examples of cement include various cements such as Portland cement, mixed cement, and ecocement. The cementitious hardened body may be waste materials such as waste building materials made of concrete or mortar, waste materials of hardened cement paste, and sludge generated in ready-mixed concrete. The cementitious hardened body may be a pulverized concrete mass. By using such waste materials, it is possible to effectively utilize resources. The shape and size of the cementitious hardened body are not particularly limited.
[0012] The age of the cementitious hardened body is not particularly limited, and may be, for example, 1 day or more, 7 days or more, 14 days or more, or 1 year or more.
[0013] The cementitious hardened body may contain water. The water content in the cementitious hardened body may be, for example, 15% by mass or more, or 20% by mass or more. The water content W in the cementitious hardened body may be, for example, 70% by mass or less, or 60% by mass or less.
[0014] The gas containing carbon dioxide is not particularly limited, and may be exhaust gas, exhaust gas from a factory, or exhaust gas discharged from equipment such as an incinerator or an electric dust collector. The inflow rate of the gas may be, for example, 0.5 to 5 L / min, or 1 to 3 L / min. The temperature of the gas may be 100° C. or higher, but may be 70 to 150° C., or 100 to 120° C. When the reaction is carried out in a vessel, the temperature of the gas may be the temperature at the inlet of the vessel.
[0015] The carbon dioxide content in the gas may be 1% by volume or more, 5 to 50% by volume, or 10 to 30% by volume relative to the total volume of the gas. The gas may contain nitrogen, oxygen, volatile organic compounds, water (water vapor), etc. in addition to carbon dioxide.
[0016] The method for adding water to the cementitious hardened body is not particularly limited, and for example, water (liquid water) may be supplied by a pump.
[0017] The carbon dioxide fixation step may be carried out in a container containing the mixture. The container may be one in which gas can be easily introduced and the mixture in the container can be heated (filled type heating device). For example, such a device may be a reactor equipped with a heater or having a function as a heater. The heater is not particularly limited, and may be an external heating device such as a rubber heater, or an internal heating device such as an infrared ray irradiation device. Water may be contained in the cementitious hardened body before being introduced into the container, or may be added to the cementitious hardened body in the container after being introduced into the container and before introducing the gas. In the carbon dioxide fixation step, the carbonation reaction may be carried out at a temperature (treatment temperature) of the mixture within a range of 70°C to the boiling point of water (100°C at normal pressure). The temperature of the mixture can be measured by a temperature measuring means such as a thermocouple arranged in the reactor.
[0018] The carbon dioxide fixation step may be carried out in a grinding device. In the grinding device, the carbon dioxide fixation step may be carried out while grinding the cementitious hardened body (such as a concrete block). In addition, after the carbon dioxide fixation step is carried out in a heating device such as a filling type heating device, the cementitious hardened body in which the carbon dioxide has been fixed may be further ground by a grinding device. The grinding may be carried out by a plurality of grinding devices.
[0019] When the carbon dioxide fixation step is carried out in a grinding machine, the cementitious hardened body in which carbon dioxide has been fixed may be collected by a dust collector as fine powder contained in the gas from the grinding machine.
[0020] The cementitious hardened body may be a pulverized product. The cementitious hardened body may be classified using a test sieve as specified in JIS Z8801-1:2019, or the average particle size (d50 on a volume basis or a number basis, etc.) may be measured using a laser particle size distribution measuring device. The particle size may be 40 mm or less, 10 mm or less, or 1 mm or less.
[0021] The method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body of the present embodiment includes a carbon dioxide fixation step including adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7, and contacting the cementitious hardened body to which the water has been added with a carbon dioxide-containing gas at 70°C or higher. That is, the cement mixture of the present embodiment may be one produced by the carbon dioxide fixation method of the present embodiment.
[0022] There are no particular limitations on the use of the cement admixture as long as it is used by mixing with cement, but it can also be used as a solidification material such as a soil improvement material. EXAMPLES
[0023] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0024] <Preparation of hardened cementitious material> Ordinary Portland cement was mixed with water to achieve a water-cement ratio (W / C) of 0.4, and then cured for 28 days. After curing, the cementitious hardened body was pulverized in a ball mill until the particle size was 0.3 mm or less, obtaining a cement paste powder. The particle size (average particle diameter) of the cementitious hardened body was measured using a laser particle size distribution analyzer. Table 1 shows the chemical composition of the cement paste powder.
[0025] [Table 1]
[0026] <Reaction Apparatus> Carbon dioxide was fixed in a reactor. A schematic diagram of the reactor is shown in Figure 1. The reactor has the following components: First, the reaction device 10 has a reactor 1 for performing a CO2 fixation reaction on a sample (a mixture of cement paste powder and water). A Hobart mixer 2 is attached to the reactor 1, and it is possible to stir the sample in the reactor. A CO2 cylinder 3 and an N2 cylinder 4 are connected to the inlet of the reactor 1, and it is possible to flow gas into the reactor 1. The reaction device 10 has a pump 5. The pump 5 is connected to the reactor 1 and a tank 6 containing water, and it is possible to share water with the reactor 1. A rubber heater 7 is attached to the reactor 1, and it is possible to heat the reactor 1. A temperature controller 8 is further connected to the rubber heater, and a thermocouple 9 attached inside the reactor is connected to the temperature controller 8. This makes it possible to manage the temperature of the sample in the reactor by controlling the temperature of the rubber heater with the temperature controller 8 while measuring the temperature inside the reactor 1 with the thermocouple 9.
[0027] <Carbon dioxide fixation (carbonation) reaction> The prepared cement paste powder (200g) was put into the reactor of the above-mentioned reactor and stirred with a Hobart mixer. The temperature inside the reactor was adjusted to 20°C with a rubber heater installed at the bottom of the reactor. Gas with a CO2 concentration adjusted to 20% by volume using N2 and CO2 cylinders was passed into the reactor at a flow rate of 2.0L / min, and water was added to achieve the W / P value in Table 2, and a CO2 fixation reaction was performed. No water was added during the reaction. During the fixation reaction, samples were collected at regular intervals and the carbonation degree was measured using the following formula (1) with a thermogravimetric differential thermal analyzer (TG-DTA). W / P is the mass ratio of water (W) to cement paste powder (P).
[0028] (How to calculate carbonation degree) The carbonation degree was calculated using the following formula (1).
number
[0029] (Reference Examples 1 to 5, Reference Comparative Examples 1 and 2) Table 2 shows the W / P, treatment temperature, and carbonation degree 4 hours after the start of the reaction for each Example and Comparative Example. Figure 2 also shows the relationship between time and carbonation degree for each Example and Comparative Example in Table 2. As shown in Figure 2, it was confirmed that when the W / P was 0.1 to 0.5, treatment with a high carbonation degree was possible in a short time. On the other hand, it was found that when the solid-liquid ratio was increased, initial carbonation was slow.
[0030] [Table 2]
[0031] (Example 1 and Comparative Example 1) A carbon dioxide fixation reaction was carried out in the same manner as in Reference Example 1, except that the conditions were as shown in Table 3. The results are shown in Table 3. FIG. 3 shows the relationship between time and degree of carbonation for the Examples and Reference Examples in Table 3. As shown in FIG. 3, it was confirmed that treatment with a high degree of carbonation could be achieved in a short time when W / P was 0.1 to 0.5. On the other hand, it was found that initial carbonation was slow when the solid-liquid ratio was increased.
[0032] [Table 3]
[0033] Referring to Figure 3, when carbonation was performed under conditions of a solid-liquid ratio of 0.5 and a treatment temperature of 20°C, the carbonation progress rate was slower and the degree of carbonation at 240 minutes was also lower than when the solid-liquid ratio was 0.2 to 0.3. On the other hand, when carbonation was performed under conditions of a treatment temperature of 100°C and a solid-liquid ratio of 0.5, the initial carbonation acceleration was slower than when the solid-liquid ratio was 0.2 to 0.3, but the final carbonation degree was high at 76%. It was confirmed that when water was added so that the solid-liquid ratio was 0.4 to 0.7 and carbonation was performed at a high temperature of 70°C or higher, CO2 could be fixed at a high carbonation rate. [Explanation of symbols]
[0034] 10...Reactor, 1...Reactor, 2...Hobart mixer, 3...CO2 cylinder, 4...N2 cylinder, 5...Pump, 6...Tank, 7...Rubber heater, 8...Temperature controller, 9...Thermocouple.
Claims
1. A method for fixing carbon dioxide in a hardened cementitious material, comprising the steps of: The method includes a carbon dioxide fixation step including: adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7; and contacting the cementitious hardened body to which water has been added with a carbon dioxide-containing gas at 70°C or higher.
2. The method of claim 1 , wherein the temperature of the gas is 100° C. or greater.
3. The method according to claim 1 or 2, wherein the particle size of the cementitious hardened body is 40 mm or less.
4. 3. The method according to claim 1 or 2, wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing concrete chunks with the pulverizing device in a pulverizing device.
5. A method for producing a cement mixture obtained by fixing carbon dioxide in a cementitious hardened body, comprising the steps of: The method includes a carbon dioxide fixation step including: adding water to the cementitious hardened body in a solid-liquid ratio of 0.4 to 0.7; and contacting the cementitious hardened body to which water has been added with a carbon dioxide-containing gas at 70°C or higher.
6. 6. The method according to claim 5, wherein the carbon dioxide fixation step is carried out by contacting the gas with a cementitious hardened body obtained by pulverizing the concrete blocks with a pulverizing device in a pulverizing device.
Citation Information
Patent Citations
Method for lessening carbon dioxide gas emission
JP2000197810A
Method of manufacturing carbonated solidified substance
JP2006188368A
Immobilization method of carbon dioxide
JP2020131076A
Producing method of cement mixture, mixed cement and carbon dioxide adsorbent
JP2021138574A
Method for recovering cement paste from waste concrete
JP2022126254A
Cited By
Methods for absorbing carbon dioxide, and methods for manufacturing carbon dioxide-fixed cementites.
JP2026161635A