Method for manufacturing sliding member

The directed energy deposition method forms a sliding layer with uniform spherical sulfides in a copper alloy matrix, addressing the issues of sliding properties and wear resistance in sulfide-dispersed copper alloys by enhancing their sliding properties and wear resistance.

JP2024146002AInactive Publication Date: 2024-10-15KAWASAKI JUKOGYO KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058664
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sulfide-dispersed copper alloys exhibit inadequate sliding properties and wear resistance due to dendrite-like or flaky sulfides generated during casting and sintering processes.

Method used

A method involving directed energy deposition to form a sliding layer on a base material using a filler material composed of specific proportions of Sn, S, Fe, and Cu, with rapid cooling to create a uniform dispersion of spherical sulfides, enhancing sliding properties and wear resistance.

Benefits of technology

The method results in a sliding member with improved sliding properties and wear resistance through the uniform dispersion of fine, spherical sulfides in the copper alloy matrix, resulting in a dense structure with high hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146002000001_ABST
    Figure 2024146002000001_ABST
Patent Text Reader

Abstract

To provide a sliding member covered with a sliding layer composed of a sulfide dispersion copper alloy having good slidability and wear resistance.SOLUTION: A method for manufacturing a sliding member includes: laminating a sliding layer composed of a sulfide dispersion copper alloy on a substrate composed of a metal material by a directed energy deposition method by supplying a filler material onto the substrate, and by melting and then cooling a surface layer of the substrate and the filler material. The filler material is composed of 4.0-15.0 mass% of Sn, 0.4-5.0 mass% of S, 1.5 mass% or less of Fe, and the rest consisting of Cu, a deoxygenating agent element and inevitable impurities.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a sliding member coated with a sulfide-dispersed copper alloy. [Background technology]

[0002] As a material for sliding members, sulfide-dispersed copper alloys in which sulfides having solid lubricating properties are dispersed in a copper alloy are known. In the sulfide-dispersed copper alloys, sulfur exists as sulfides combined with copper and iron. The sulfide-dispersed copper alloys are so-called lead-free materials that do not use lead as a main component, which has been used in conventional sliding materials, and yet have high sliding properties. Patent Document 1 discloses this type of sulfide-dispersed copper alloy.

[0003] Patent Document 1 discloses a cast material and a sintered material of a copper alloy for sliding members. The copper alloy for sliding members contains a predetermined amount of tin, iron, and sulfur, with the remainder being copper and impurities, and sulfides, which are compounds of copper, iron, and sulfur, are dispersed in the copper alloy. The cast material is obtained by casting a material of the copper alloy for sliding members. The sintered material is obtained by scattering alloy powder, which is made from the material of the copper alloy for sliding members by an atomizing method, on a steel plate, sintering the alloy powder together with the steel plate, and rolling. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-150649 A Summary of the Invention [Problem to be solved by the invention]

[0005] It is known that the cast material of sulfide-dispersed copper alloy is a matrix in which dendritic sulfides formed during the solidification process of casting are dispersed. It is also known that the sintered material of copper alloy for sliding parts is a matrix in which flake-like sulfides formed during the sintering process are dispersed. These sulfide-dispersed copper alloys have room for improvement in sliding properties (i.e., low friction of the sliding surface) and wear resistance.

[0006] In view of the above, an object of the present disclosure is to provide a method for producing a slide member covered with a slide layer made of a sulfide-dispersed copper alloy having good sliding properties and wear resistance. [Means for solving the problem]

[0007] In order to solve the above problems, a method for producing a slide member according to one embodiment of the present disclosure includes the steps of: The method includes supplying a filler metal onto a substrate made of a metal material, melting a surface layer of the substrate and the filler metal, and then cooling the melted filler metal to form a sliding layer made of a sulfide-dispersed copper alloy on the substrate by a directed energy deposition method; The filler metal is composed of Sn: 4.0 mass% to 15.0 mass%, S: 0.4 mass% to 5.0 mass%, Fe: 1.5 mass% or less, with the balance being Cu, a deoxidizer element, and unavoidable impurities. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a sliding member that is covered with a sliding layer made of a sulfide-dispersed copper alloy having good sliding properties and wear resistance. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a graph showing an example of temperature change of a molten pool during a manufacturing process of a slide member. [Diagram 2] FIG. 2 is a diagram showing the relationship between the absolute maximum length and the diagonal width of sulfides dispersed in the matrix of a sulfide-dispersed copper alloy. [Diagram 3]FIG. 3 is a photograph of the cross-sectional structure of the sulfide-dispersed copper alloy sample according to Example 1. [Figure 4] FIG. 4 is a photograph of the cross-sectional structure of the sulfide-dispersed copper alloy sample according to Comparative Example 1. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, an embodiment of the present disclosure will be described. The sliding member according to the present disclosure has a substrate and a sliding layer covering a part or all of the substrate. That is, a part or all of the sliding member is covered with the sliding layer. The sliding layer is made of a sulfide-dispersed copper alloy in which metal sulfides are dispersed in bronze. The sulfide-dispersed copper alloy contains sulfur S and iron Fe for generating sulfides in addition to copper Cu and tin Sn, which are basic components of bronze. More specifically, the sulfide-dispersed copper alloy is substantially made of 4.0% by mass to 15.0% by mass of Sn, 0.4% by mass to 5.0% by mass of S, 0.01% by mass to 1.5% by mass of Fe, and the balance is Cu, a deoxidizer element, and unavoidable impurities. The sulfide-dispersed copper alloy may contain other elements and impurities that do not adversely affect the dispersion state and particle shape properties of the sulfides in the copper alloy.

[0011] 《Sn》 Sn dissolves in the matrix of the copper alloy to improve the wear resistance of the matrix. If the Sn content of the copper alloy is less than 4.0 mass%, the function of Sn becomes insufficient. From this viewpoint, the Sn content of the copper alloy is 4.0 mass% or more, preferably 7.0 mass% or more. On the other hand, if the Sn content of the copper alloy exceeds 15.0 mass%, the toughness is significantly reduced and cracks are easily caused. From this viewpoint, the Sn content of the copper alloy is 15.0 mass% or less, preferably 13.0 mass% or less.

[0012] "S" In the copper alloy, S exists as a sulfide bonded with Cu or Fe, and contributes to the sliding properties. Since sulfur does not exist alone in the copper alloy but exists in the form of a sulfide, the sulfide content also increases as the sulfur content increases. If the S content of the copper alloy is less than 0.4 mass%, the amount of sulfide produced is small, so the effect of improving the sliding properties is small. From this viewpoint, the S content of the copper alloy is 0.4 mass% or more, preferably 2.0 mass% or more. The higher the S content, the more the sliding properties can be improved, but problems arise in the mechanical strength of the sliding member. From this viewpoint, the S content of the copper alloy is 5.0 mass% or less, preferably 3.0 mass% or less.

[0013] Fe Fe is mixed into the copper alloy raw material in the form of a deoxidizer or other raw material. FFe in the copper alloy exists as a sulfide combined with S. If the content of Fe in the copper alloy is excessive, Fe may precipitate in the copper alloy as a single element, which may lead to a decrease in the sliding properties against iron-based materials. From this viewpoint, the content of Fe in the copper alloy is 0.01% by mass or more and 1.5% by mass or less. However, the lower limit of the content of Fe in the copper alloy may be the detection limit of less than 0.01% by mass, i.e., the minimum amount that can be detected.

[0014] 《Oxygen absorber element》 The sulfide-dispersed copper alloy contains Cu, a deoxidizer element, and unavoidable impurities in addition to Sn, S, and Fe. The deoxidizer element is at least one element selected from manganese Mn, zinc Zn, magnesium Mg, calcium Ca, aluminum Al, and phosphorus P. The deoxidizer element is a residue of a deoxidizer added to the copper alloy raw material during production, and has the effect of deoxidizing the molten metal by dissolving in the copper alloy raw material. The sulfide-dispersed copper alloy may contain multiple elements as deoxidizer elements, and the deoxidizer element is allowed to be contained in a total amount of about several mass % (2 to 3 mass %) or less. However, the sulfide-dispersed copper alloy may not contain a deoxidizer element. In this case, the sulfide-dispersed copper alloy is substantially composed of 4.0 mass% to 15.0 mass% Sn, 0.4 mass% to 5.0 mass% S, 0.01 mass% to 1.5 mass% Fe, 3.0 mass% or less (including 0) of deoxidizer elements, and the balance being Cu and unavoidable impurities. The deoxidizer preferably contains at least Mn. When Mn is added to the copper alloy raw material as a deoxidizer, the content of Mn in the copper alloy is preferably 0.6 mass% or less. Furthermore, when FeSi is added to the copper alloy raw material as a deoxidizer, the content of Si in the copper alloy is preferably 0.5 mass% or less.

[0015] The content of elements contained as inevitable impurities is preferably as small as possible. Examples of inevitable impurities include Mo. The sulfide-dispersed copper alloy according to the present disclosure has a composition equivalent to the bronze material of the CAC400 series specified in JIS H 5120 "Copper and copper alloy castings".

[0016] <<Method for manufacturing slide member>> The sliding member is manufactured by laminating a sliding layer made of a sulfide-dispersed copper alloy on the surface of a substrate. The substrate is made of a metal material. Examples of the metal material include iron-based materials such as cast iron, stainless steel, and carbon steel, and non-ferrous materials such as nickel-based alloys, aluminum-based materials, magnesium-based materials, titanium-based materials, and copper-based materials.

[0017] The method of laminating and forming a sliding layer on a substrate includes a step of melting a raw material of a sulfide-dispersed copper alloy together with the substrate, and a step of rapidly cooling and solidifying the molten raw material. The method of forming the sliding layer is not particularly limited, but an example is a directed energy deposition method. The directed energy deposition method is also called "DED (Directed Energy Deposition)" or "deposition method", and is capable of precisely forming a sliding layer in a portion of a sliding member where sliding properties are required. A known directed energy deposition method forming device can be used to form the sliding layer.

[0018] In the method for forming a sliding layer by the directed energy deposition method, a molten pool is formed on the surface of the substrate by irradiating the substrate with focused thermal energy, and a filler metal made of a raw material of a sulfide-dispersed copper alloy is supplied to the molten pool. After the surface of the substrate and the filler metal are completely melted, the molten pool is rapidly cooled and solidified to form an overlay made of a sulfide-dispersed copper alloy on the surface of the substrate. Here, a shielding gas made of an inert gas is supplied to the molten pool and its surroundings to prevent oxidation of the overlay. By repeating the formation of the overlay, a sliding layer made of a sulfide-dispersed copper alloy is formed on the surface of the substrate. A laser beam or an arc discharge is used as a means for supplying thermal energy. As the laser, a semiconductor laser, a carbon dioxide gas laser, a YAG laser, etc. can be used.

[0019] A cored wire is used as the filler material. The cored wire is a U-shaped thin steel plate filled with particles of the raw material of the sulfide-dispersed copper alloy, coated, and formed into a long wire shape. Alternatively, a mixed powder of the raw material of the sulfide-dispersed copper alloy may be used as the filler material. As the mixed powder, a mixture of powders of the raw materials of the sulfide-dispersed copper alloy, or a raw material of the sulfide-dispersed copper alloy that is melted and formed into a powder shape is used. The sulfide-dispersed copper alloy formed into a powder shape may be an atomized powder.

[0020] The molten pool, consisting of the molten filler metal and base material, is rapidly cooled by natural cooling or forced cooling, solidifying and becoming a build-up. Examples of forced cooling methods for the molten pool include water cooling, oil cooling, and air cooling. As shown in Figure 1, the temperature of the molten pool drops rapidly after reaching a maximum temperature above the melting temperature of the sulfide-dispersed copper alloy. In the quenching process, when the molten pool temperature is in the temperature range below the liquidus temperature, the maximum cooling rate is 2000°C / sec to 5000°C / sec. The liquidus temperature varies depending on the composition and pressure of the molten pool, and can be set based on the solid-liquid equilibrium diagram of the molten pool.

[0021] In the sliding layer of the sliding member obtained by the above-mentioned manufacturing method, sulfides functioning as a solid lubricant are dispersed in a copper alloy matrix. The sulfides are substantially spherical and are dispersed almost uniformly in the copper alloy matrix.

[0022] Average circular equivalent diameter of sulfides The average circle equivalent diameter of the sulfides dispersed in the matrix of the sulfide-dispersed copper alloy (i.e., the sliding layer) is 0.5 μm or more and 3.0 μm or less. The circle equivalent diameter (ECD) is the diameter of a circle having an area equal to the area of ​​the sulfide. The area of ​​the sulfide may be the projected area of ​​the sulfide. The average circle equivalent diameter is the average value of the circle equivalent diameters of the sulfides included in the observation range. The fact that the sulfides have the above average circle equivalent diameter means that the sulfides are fine and the structure of the sulfide-dispersed copper alloy is dense, compared with the case where the sulfides are dendritic like cast materials. The fine sulfides are widely dispersed in the matrix of the copper alloy without being unevenly distributed. As a result, a sliding layer in which fine solid lubricants are uniformly dispersed is obtained, and the sliding properties of the sliding layer (i.e., less friction of the sliding surface) are improved. In addition, the dense structure of the sulfide-dispersed copper alloy improves the hardness of the sulfide-dispersed copper alloy. As a result, the wear resistance of the sliding layer is improved.

[0023] Average aspect ratio of sulfides The average aspect ratio (here, average acicular ratio) of the sulfides dispersed in the matrix of the sulfide-dispersed copper alloy (i.e., the sliding layer) is 1.0 or more and 1.7 or less. The aspect ratio is the ratio of the major axis diameter to the minor axis diameter of the sulfide. The average aspect ratio is the average value of the aspect ratios of the sulfides included in the observation range. The fact that the sulfide has the above aspect ratio means that the sulfide is isotropic and approximately spherical. The sulfide-dispersed copper alloy in which the approximately spherical sulfides are dispersed in the matrix has good cutting workability because the cutting chips are finely divided, and has excellent workability.

[0024] <Determination coefficient of absolute maximum length and diagonal width of sulfides> The coefficient of determination between the absolute maximum length and diagonal width of sulfides dispersed in the matrix of the sulfide-dispersed copper alloy (i.e., the sliding layer) is 0.85 or more. The absolute maximum length of a sulfide is the long axis diameter of the sulfide. The diagonal width is the distance between two lines parallel to the long axis of the sulfide when the sulfide is sandwiched between them. As shown in Figure 2, a scatter plot is created in which the relationship between the absolute maximum length and diagonal width of the sulfide is plotted on a graph with the absolute maximum length on the first axis and the diagonal width on the second axis. A regression line is drawn on this scatter plot based on the least squares method, and the coefficient of determination (R 2 ) is calculated. The coefficient of determination is the square of the correlation coefficient, and the closer the coefficient of determination is to 1, the closer the points are to the regression line. Compared to copper alloys in which roughly spherical sulfides are dispersed in the matrix, sulfide-dispersed copper alloys have a coefficient of determination for the absolute maximum length and diagonal width of sulfides that is closer to 1, the aspect ratio of the sulfides is uniform, and there is little variation in the shape of the sulfides.

[0025] [Example] Samples of the above sliding members of Examples 1 and 2 and Comparative Example 1 were prepared, the structure of each sample was observed, and the sliding performance of each sample was evaluated.

[0026] Sample Preparation (1) Example 1 A plate of 80 mm long x 40 mm wide x 20 mm thick made of carbon steel equivalent to JIS S55C was prepared as the substrate. A cored wire made of the copper alloy raw material shown in Table 1 was prepared as the filler material. The filler material was used to form a build-up layer on the substrate using the directed energy deposition method. The filler material was supplied onto the substrate, and the surface of the substrate and the filler material were melted by the thermal energy of a laser beam to form a molten pool, which was then naturally cooled by exposure to air. The maximum temperature of the molten pool measured by a thermocouple was approximately 1700°C, and the temperature of the molten pool rose to the maximum temperature and then dropped rapidly. The maximum cooling rate in the temperature range below the liquidus temperature during quenching was 5000°C / sec. (2) Comparative Example 1 The copper alloy raw materials shown in Table 1 were molded by casting to produce test pieces with a diameter of 4.9 mm and a thickness of 2 mm. In the casting process, the sulfide-dispersed copper alloy raw materials were melted, the molten metal was poured into a mold, and then the alloy was allowed to cool naturally in the air. The maximum cooling rate in the temperature range below the liquidus temperature during cooling was 1°C / sec.

[0027] [Table 1]

[0028] Observation and Testing (1) Tissue Observation The cross section of each sulfide-dispersed copper alloy sample was polished and observed under an electron microscope (Schottky scanning electron microscope SU5000 manufactured by Hitachi High-Tech Corporation). The metal structures obtained by the observation are shown in Fig. 3 and Fig. 4. Fig. 3 shows the cross-sectional structure of the sulfide-dispersed copper alloy sample according to Example 1, and Fig. 4 shows the cross-sectional structure of the sulfide-dispersed copper alloy sample according to Comparative Example 1.

[0029] The average equivalent circular diameter of each sample was measured. In detail, image data from 20 fields of view was binarized using image analysis and measurement software (WinROOF manufactured by Mitani Shoji Co., Ltd.), and the equivalent circular diameter was measured in measurement mode. The average of the measured equivalent circular diameters was regarded as the average equivalent circular diameter of the sample.

[0030] The average aspect ratio of each sample was measured. In detail, image data from 20 fields of view was binarized using image analysis and measurement software (WinROOF manufactured by Mitani Shoji Co., Ltd.), the acicular ratio was measured in measurement mode, and the average of the measured acicular ratios was taken as the average aspect ratio of the sample.

[0031] The absolute maximum length and diagonal width of the sulfides of each sample were measured, and the coefficient of determination was calculated. In detail, image data from 20 fields of view were binarized using image analysis and measurement software (WinROOF manufactured by Mitani Shoji Co., Ltd.), and the absolute maximum length and diagonal width were measured in measurement mode. The coefficient of determination was calculated when the measured absolute maximum length was y and the diagonal width was x.

[0032] Table 2 shows the measured average equivalent circular diameter, average aspect ratio, and coefficient of determination for the examples and comparative examples.

[0033] [Table 2]

[0034] "evaluation" (1) Metal structure In the sulfide-dispersed copper alloy (i.e., the sliding layer) of the sample according to the embodiment, the matrix had a structure in which approximately spherical and fine sulfides were dispersed almost uniformly. In the embodiment, such a structure is considered to have been formed by melting the copper alloy material and then rapidly solidifying it. In the comparative example 1, the matrix had unevenly distributed coarse dendrite-like sulfides.

[0035] (2) Sliding properties In the sulfide-dispersed copper alloy (i.e., sliding layer) of the sample according to the embodiment, sulfide as a solid lubricant is dispersed, and therefore the sulfide-dispersed copper alloy has uniform and good sliding properties over the entire surface, compared to Comparative Example 1. Furthermore, the sulfide-dispersed copper alloy of the sample according to the embodiment has a denser structure, higher hardness, and better wear resistance, compared to Comparative Example 1.

[0036] [Summary] As described above, the method for producing a slide member according to the first aspect of the present disclosure includes the steps of: The method includes supplying a filler metal onto a substrate made of a metal material, melting a surface layer of the substrate and the filler metal, and then cooling the melted filler metal to form a sliding layer made of a sulfide-dispersed copper alloy on the substrate by a directed energy deposition method; The filler metal is composed of Sn: 4.0 mass% to 15.0 mass%, S: 0.4 mass% to 5.0 mass%, Fe: 1.5 mass% or less, with the balance being Cu, a deoxidizer element, and unavoidable impurities.

[0037] A manufacturing method for a slide member according to a second aspect of the present disclosure is the manufacturing method for a slide member according to the first aspect, wherein a maximum cooling rate of a molten pool consisting of a surface layer portion of the base material and a filler metal in a temperature range not exceeding a liquidus temperature of the molten pool is 2000° C. / sec or more and 5000° C. / sec or less during cooling.

[0038] In the sulfide-dispersed copper alloy forming the sliding layer of the sliding member produced by the above-mentioned production method, sulfides as solid lubricants are dispersed, and the sulfide-dispersed copper alloy has uniform and good sliding properties over the entire surface. In addition, the sulfide-dispersed copper alloy forming the sliding layer of the sliding member has a dense structure, high hardness, and excellent wear resistance. Therefore, according to the present disclosure, a production method for a sliding member coated with a sliding layer made of a sulfide-dispersed copper alloy having good sliding properties and wear resistance can be provided.

Claims

1. The method includes supplying a filler metal onto a substrate made of a metal material, melting a surface layer of the substrate and the filler metal, and then cooling the melted filler metal to form a sliding layer made of a sulfide-dispersed copper alloy on the substrate by a directed energy deposition method; The filler metal is composed of Sn: 4.0 mass% or more and 15.0 mass% or less, S: 0.4 mass% or more and 5.0 mass% or less, Fe: 1.5 mass% or less, and the balance is Cu, a deoxidizer element, and inevitable impurities. A method for manufacturing a sliding member.

2. In the cooling, the maximum cooling rate of the molten pool consisting of the surface layer portion of the base material and the filler metal in a temperature range below the liquidus temperature of the molten pool is 2000° C. / sec or more and 5000° C. / sec or less. The method for producing a sliding member according to claim 1 .

Citation Information

Patent Citations

  • Copper alloy for sliding member

    JP2010150649A