Conductive paste, electronic component, and laminated ceramic capacitor
The conductive paste with phenolic compounds aligns the sintering behavior of nickel and ceramic layers, reducing structural defects in multilayer ceramic capacitors by increasing the sintering start temperature, thus enhancing the manufacturing process.
Patent Information
- Application Number
- JP2023058853
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The structural defects such as delamination, cracks, and discontinuities in internal electrode films of multilayer ceramic capacitors are exacerbated by the large difference in shrinkage behavior between the ceramic dielectric layer and nickel internal electrode layer during the firing process, which is not adequately addressed by existing technologies using noble metal-dotted nickel fine particles.
A conductive paste containing conductive powder, organic solvent, binder resin, and an additive phenolic compound, such as 2,6-tert-butyl-p-cresol or 4-tert-butylpyrocatechol, is used to increase the sintering start temperature of the conductive paste, thereby aligning the shrinkage behavior of nickel powder and ceramic green sheet, reducing structural defects.
The use of phenolic compounds in the conductive paste enhances the sintering start temperature, minimizing structural defects like delamination and cracks in the internal electrode films, ensuring smoother sintering and improved conductivity.
Smart Images

Figure 2024146126000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor, and more particularly to a conductive paste, an electronic component, and a multilayer ceramic capacitor used to form internal electrodes of a multilayer ceramic capacitor (MLCC). [Background technology]
[0002] In recent years, with the trend of electronic devices such as mobile phones and digital devices becoming lighter, thinner, shorter, and smaller, various electronic components have been rapidly miniaturized, and multilayer ceramic capacitors, which are chip components, have also been made smaller, with higher capacity and higher performance. Multilayer ceramic capacitors have a structure in which ceramic dielectric layers and internal electrode layers are alternately stacked and sintered to integrate them. Traditionally, precious metals such as palladium have been used as the internal electrode material for multilayer ceramic capacitors, but nickel has now become mainstream to reduce costs. The most effective means of realizing miniaturization, high capacity, and high performance of multilayer ceramic capacitors is to make the nickel internal electrode layers and ceramic dielectric layers thinner and multilayered.
[0003] Generally, a multilayer ceramic capacitor is manufactured, for example, by the following manufacturing process. First, a conductive paste is prepared by dispersing a conductive powder such as nickel powder as an internal electrode material in a vehicle containing an organic resin binder and a solvent. Next, a conductive powder such as barium titanate (BaTiO3) is dispersed in an organic resin binder to form a paste, and the paste is spread into a thin sheet on a plastic carrier film and then dried to prepare a ceramic green sheet. The conductive paste is printed on the green sheet, and then dried to remove the solvent and form a dry film that becomes the internal electrode. The green sheets on which the dry film is formed are stacked in multiple layers and integrated by heat compression to form a dielectric block. The integrated dielectric block is then cut to a predetermined chip size, and the chip is then heat-treated at a temperature of 500°C or less in an oxidizing or inert atmosphere to remove the organic resin binder, thereby performing a debinding process. Next, the chip is heated to about 1300°C in a reducing atmosphere to prevent the internal electrode from being oxidized, and a firing process is performed, and the internal electrode layer and the ceramic dielectric layer are integrally sintered. Next, a conductive paste for the external electrodes is applied to both end surfaces of the sintered chip and baked at about 800°C to form the external electrodes. After that, the surfaces of the external electrodes are plated to obtain a multilayer ceramic capacitor.
[0004] However, in the above-mentioned firing process, the temperature at which the ceramic dielectric layer sinters and begins to shrink is about 1200°C, which is higher than the temperature at which conductive powders such as nickel sinter and begin to shrink. Since the shrinkage behavior of the ceramic dielectric layer and the internal electrode layer differs significantly, structural defects such as delamination and cracks may occur.
[0005] However, as a conventional technique for solving this problem, Patent Document 1 discloses a technique for improving the sintering resistance of nickel microparticles by using nickel microparticles having microparticles mainly composed of precious metal elements scattered on the surface of the microparticles mainly composed of nickel element, thereby suppressing shrinkage of the internal electrode layer and discontinuity of the internal electrode film. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-049973 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in recent years, electronic components have become increasingly smaller, and the internal electrode layers and dielectric layers have become thinner. As a result, the problem of structural defects such as delamination, cracks, and discontinuities in the internal electrode film has become more pronounced, and it is difficult to say that the technology disclosed in Patent Document 1 has solved this problem.
[0008] For example, the technology described in Patent Document 1 uses conductive particles in which fine particles mainly made of precious metal elements are scattered on the surface of fine particles mainly made of nickel element. As the nickel powder becomes finer, it is not preferable to uniformly scatter expensive fine particles of precious metals so that the nickel powder does not sinter together, as this increases the cost in terms of both technology and materials.
[0009] The present invention has been made in consideration of the above-mentioned conventional circumstances, and has an object to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that can increase the sintering start temperature of the dried conductive paste in the firing process of the multilayer ceramic capacitor, and bring it closer to the sintering start temperature of the ceramic green sheets. [Means for solving the problem]
[0010] In order to solve the above problems, the conductive paste of the present invention is a conductive paste containing a conductive powder, an organic solvent, a binder resin and an additive, wherein the additive contains a phenol-based compound.
[0011] The phenolic compound may include a tert-butyl group.
[0012] The phenolic compound may be 2,6-tert-butyl-p-cresol or 4-tert-butylpyrocatechol, or a combination thereof.
[0013] The mass ratio of the conductive powder to the phenol-based compound may be 100:0.3-3.
[0014] The binder resin may include ethyl cellulose.
[0015] The conductive paste of the present invention may contain a ceramic powder.
[0016] The conductive powder may have a number average particle size of 30 nm or more and 100 nm or less.
[0017] In order to achieve the above object, the electronic component of the present invention is an electronic component formed by using the conductive paste of the present invention.
[0018] In order to solve the above problems, the multilayer ceramic capacitor of the present invention is a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrode layers are laminated, and the internal electrode layers are formed using the conductive paste of the present invention. Effect of the Invention
[0019] According to the present invention, it is possible to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that can increase the sintering start temperature of the dried conductive paste in the firing process of the multilayer ceramic capacitor, and bring it closer to the sintering start temperature of the ceramic green sheet. [Brief description of the drawings]
[0020] [Figure 1] 1A and 1B are a perspective view and a side cross-sectional view of a multilayer ceramic capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present inventors conducted extensive research into the effects of various additive materials contained in the conductive paste during the sintering process of multilayer ceramic capacitors on the shrinkage behavior due to sintering when forming internal electrode layers, and discovered that adding a phenol-based compound to the conductive paste has the effect of increasing the sintering start temperature of the conductive paste.
[0022] In other words, it is believed that the phenol-based compound improves the heat resistance of the conductive powder during sintering and can maintain a state in which the conductive powder particles are prevented from agglomerating up to higher temperatures, thereby inhibiting the bonding of the conductive powder particles up to higher temperatures during firing and raising the sintering temperature.
[0023] The inventors then discovered that due to the effect of the phenol-based compound in increasing the sintering temperature of the conductive paste, the difference between the sintering start temperature of the conductive powder and the sintering start temperature of the dielectric layer is reduced, and compared to conventional conductive pastes that do not contain phenol-based compounds, the stress generated between the dielectric layer and the internal electrode layer during sintering is reduced, thereby making it possible to suppress the occurrence of delamination and cracks between the dielectric layer and the internal electrode layer during sintering, which led to the development of the present invention.
[0024] Hereinafter, an embodiment of the conductive paste, electronic component, and multilayer ceramic capacitor of the present invention will be described.
[0025] [Conductive paste] The conductive paste of the present invention is suitable as a paste for forming internal electrodes of a multilayer ceramic capacitor, and contains a conductive powder, an organic solvent, a binder resin, and an additive, the additive including a phenol-based compound.
[0026] Furthermore, in the conductive paste of the present invention, in order to bring the shrinkage behavior closer to that of a green sheet, ceramic powder may be contained as the dielectric powder which is a constituent material of the green sheet.
[0027] The conductive powder, the ceramic powder, the organic solvent, the binder resin and the additives will be described in detail below.
[0028] (conductive powder) The conductive powder is not particularly limited, and a metal powder can be used, for example, one or more metal powders selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. Among these, Ni or Ni alloy powder is preferred from the viewpoints of conductivity, corrosion resistance, and cost. As the Ni alloy, for example, an alloy of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd (Ni alloy) can be used. The Ni content in the Ni alloy is, for example, 50 mass% or more, preferably 80 mass% or more.
[0029] In addition, Ni powder may contain several hundred ppm of sulfur during the manufacturing process of the Ni powder, as a result of a sulfur coating process that treats the surface of the Ni powder in order to suppress the sudden generation of gas due to partial thermal decomposition of the binder resin during the debinding process.
[0030] The number average particle size of the conductive powder is preferably 30 nm or more and 100 nm or less, more preferably 40 nm or more and 90 nm or less. When the average particle size of the conductive powder is in the above range, it can be suitably used as a conductive paste for an internal electrode of a thin-film multilayer ceramic capacitor, and the smoothness of the dried film is improved. Here, the number average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 10,000 times.
[0031] The content of the conductive powder in the total amount of the conductive paste is preferably 40% by mass to 65% by mass, and more preferably 45% by mass to 60% by mass. When the content of the conductive powder is in the above range, the conductive paste has excellent conductivity and dispersibility.
[0032] (ceramic powder) The ceramic powder is not particularly limited, and for example, in the case of a conductive paste for an internal electrode of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected depending on the type of multilayer ceramic capacitor to be applied. Examples of the ceramic powder include perovskite oxides containing Ba and Ti, and preferably barium titanate (BaTiO3).
[0033] The ceramic powder may be a ceramic powder containing barium titanate as a main component and oxides as subcomponents. Examples of oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. The ceramic powder may be a perovskite-type oxide ferroelectric ceramic powder in which the Ba and Ti atoms of barium titanate (BaTiO3) are replaced with other atoms, such as Sn, Pb, and Zr.
[0034] In the conductive paste for the internal electrodes, a powder having the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor may be used as the ceramic powder. This suppresses the occurrence of cracks due to a mismatch in shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the above, examples of such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element)2O3, and TiO2. Note that one type of ceramic powder may be used, or two or more types may be used.
[0035] The number average particle diameter of the ceramic powder is, for example, 10 nm to 100 nm, and preferably in the range of 10 nm to 70 nm. When the number average particle diameter of the ceramic powder is in the above range, when the ceramic powder is used as a conductive paste for an internal electrode, a sufficiently fine, thin, and uniform internal electrode can be formed. The number average particle diameter is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle diameter of each of a plurality of particles from an image observed with an SEM at a magnification of 50,000 times.
[0036] When the conductive paste contains ceramic powder, the content of the ceramic powder is preferably 1 to 30 parts by mass, and more preferably 3 to 30 parts by mass, relative to 100 parts by mass of the conductive powder. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0037] When the conductive paste contains ceramic powder, the content of the ceramic powder is preferably 1 mass % to 20 mass %, more preferably 3 mass % to 20 mass %, based on the entire conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0038] (Organic solvent) The conductive paste may further contain an organic solvent for viscosity adjustment. As the organic solvent, a general organic solvent used in the conductive paste may be used, but it is preferable to use an organic solvent used in the organic vehicle. As the organic solvent, for example, dihydroterpineol may be included. By using dihydroterpineol, the viscosity of the conductive paste can be made suitable for use in screen printing.
[0039] The total content of the organic solvents is preferably 40 parts by mass to 120 parts by mass, more preferably 70 parts by mass to 110 parts by mass, relative to 100 parts by mass of the conductive powder. When the content of the organic solvents is within the above range, the conductivity and dispersibility are excellent.
[0040] The total content of the organic solvents is preferably 20% by mass to 60% by mass, and more preferably 35% by mass to 55% by mass, based on the entire conductive paste. When the content of the organic solvents is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0041] (binder resin) The binder resin is not particularly limited, but may contain, for example, ethyl cellulose having a mass average molecular weight of 30,000 to 150,000 and an ethoxy group content of 45 to 50 mass%. By containing such ethyl cellulose, a conductive paste having high smoothness as a conductive film after drying can be obtained. In addition, there is a firing step in the process of processing the conductive paste into an internal electrode, and the residual carbon content after this firing does not increase excessively, so that printability can be sufficiently ensured.
[0042] If the mass average molecular weight of the ethyl cellulose is less than 30,000, it may be difficult to obtain sufficient viscosity for printing, and if the molecular weight is more than 150,000, the resulting conductive paste may become too viscous, resulting in poor printability.
[0043] Furthermore, if the ethoxy group content of ethyl cellulose is 45 to 50 mass %, the compatibility with organic solvents is excellent and the solubility is good, so that a conductive paste having a high smoothness as a conductive film after drying can be obtained. The ethoxy group content of ethyl cellulose is more preferably 47 to 50 mass %.
[0044] The binder resin may be the above-mentioned ethyl cellulose alone or may further contain a resin other than ethyl cellulose. For example, the binder resin may further contain, in addition to ethyl cellulose, at least one resin selected from methyl cellulose, ethyl hydroxyethyl cellulose, nitrocellulose, and polyvinyl butyral.
[0045] For example, when used as a conductive paste for internal electrodes, polyvinyl butyral may be used from the viewpoint of improving the adhesive strength with the green sheet.
[0046] In the binder resin selected from methyl cellulose, ethyl hydroxyethyl cellulose, nitrocellulose, and polyvinyl butyral, the mass average molecular weight is preferably, for example, about 20,000 to 300,000. If the mass average molecular weight is less than 20,000, it is difficult to obtain sufficient viscosity for printing. A more preferable lower limit of the mass average molecular weight is 30,000. If the lower limit is 30,000 or more, the printability can be sufficiently ensured without increasing the residual carbon content. On the other hand, if the mass average molecular weight exceeds 300,000, the obtained conductive paste may become viscous and the printability may deteriorate. If the mass average molecular weight is 300,000 or less, a conductive paste with excellent printability can be obtained while ensuring compatibility with ethyl cellulose. The preferable upper limit of the mass average molecular weight depends on the compounding ratio with ethyl cellulose, etc., but by setting it to 300,000 or less, it is possible to reduce the residual carbon after baking the coating film obtained by drying the conductive paste.
[0047] When a resin other than ethyl cellulose is contained as the binder resin, the mass ratio of ethyl cellulose:resin other than ethyl cellulose=30-70:70-30 is preferably set.
[0048] The content of the binder resin is preferably 1 to 10 parts by mass, more preferably 1 to 8 parts by mass, relative to 100 parts by mass of the conductive powder. When the content of the binder resin is within the above range, the conductivity and dispersibility are excellent.
[0049] The content of the binder resin is preferably 0.5% by mass to 10% by mass, and more preferably 1% by mass to 6% by mass, based on the entire conductive paste. When the content of the binder resin is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0050] (Additives) The additive used in the conductive paste of the present invention contains a phenolic compound. As described above, the phenolic compound has heat resistance and inhibits the bonding between conductive powders at temperatures higher than normal sintering temperatures, which is thought to increase the sintering temperature of the conductive powder. Such a phenolic compound contains a tert-butyl group. Examples of phenolic compounds containing a tert-butyl group include 2,6-tert-butyl-p-cresol and 4-tert-butylpyrocatechol, and these may be used in combination.
[0051] In addition, the additives used in the nickel paste for multilayer ceramic capacitors of the present invention may contain additives other than phenolic compounds in addition to the phenolic compounds. Examples of additives other than phenolic compounds that can be contained in addition to the phenolic compounds include additives that are generally used in conductive pastes, such as acid dispersants such as higher fatty acids and polymer surfactants, and base dispersants such as amine base dispersants.
[0052] The content of the phenol-based compound in the conductive paste of the present invention is preferably 0.3 parts by mass or more and 3 parts by mass or less with respect to 100 parts by mass of the conductive powder.
[0053] If the content of the phenol-based compound is less than 0.3 parts by mass, the compound may not be sufficiently distributed in the conductive powder, and the effect of increasing the sintering start temperature during firing may not be exhibited.
[0054] On the other hand, if the content of the phenol-based compound exceeds 3 parts by mass, the effect of increasing the sintering start temperature becomes saturated, and after the conductive paste is applied to a green sheet and dried, the additive may bleed out onto the surface of the dried film.
[0055] In addition, in the conductive paste of the present invention, the total content of additives including additives other than the phenol-based compound is preferably 0.09 mass % or more and 5 mass % or less with respect to 100 mass % of the conductive paste.
[0056] If the total content of additives, including additives other than the phenol-based compound, is less than 0.09 mass %, it is undesirable because the paste constituent materials, including the conductive powder, may not be dispersed sufficiently uniformly.
[0057] On the other hand, if the total content of additives, including additives other than the phenol-based compound, exceeds 5 mass %, this is not preferable because the additives may bleed out onto the surface layer of the dried film after the conductive paste is applied to the green sheet and dried.
[0058] (Evaluation of sintering behavior of laminates using nickel paste) When a laminate using nickel paste using nickel as the conductive powder is fired, sintering begins at a temperature of about 730°C to 1000°C, and by further increasing the temperature to about 1300°C, the nickel and ceramic green sheets progress in sintering and shrink. This shrinkage due to sintering occurs due to a combination of the sintering behavior of the nickel powder, which starts sintering at a relatively low temperature of about 730°C to 1000°C and progresses rapidly after sintering begins, and the sintering behavior of the ceramic green sheets, which starts sintering at a relatively high temperature of about 1200°C and progresses slowly after sintering begins.
[0059] Here, since the sintering start temperature of the ceramic green sheet is not affected by the nickel paste forming the conductor and is considered to change very little, if the sintering start temperature of the nickel powder is low and sintering is started at a lower temperature, the difference with the sintering start temperature of the ceramic green sheet will become larger. On the other hand, the higher the sintering start temperature of the nickel powder, the closer the shrinkage behavior of the ceramic green sheet and the nickel powder become, and it can be said that structural defects are less likely to occur.
[0060] Therefore, in the examples described below, the sintering start temperature of each evaluation sample of a nickel paste for a multilayer ceramic capacitor having the configuration of the present invention and a conventional nickel paste for a multilayer ceramic capacitor not having the configuration of the present invention is evaluated to evaluate the degree of similarity between the shrinkage behavior of the nickel powder and the shrinkage behavior of the ceramic green sheet.
[0061] (Method of manufacturing conductive paste) The method for producing the conductive paste of the present invention is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced, for example, by preparing the above-mentioned components and stirring and kneading them with a three-roll mill, a ball mill, a mixer, or the like. In this case, if a dispersant is applied to the surface of the conductive powder in advance, the conductive powder is sufficiently loosened without agglomeration, and the dispersant is distributed over the surface, making it easy to obtain a uniform conductive paste. Alternatively, the binder resin may be dissolved in an organic solvent for a vehicle to produce an organic vehicle, and the conductive powder, ceramic powder, organic vehicle, and dispersant may be added to the organic solvent for the paste, and the mixture may be stirred and kneaded with a mixer to produce the conductive paste.
[0062] The conductive paste can be suitably used in electronic components such as multilayer ceramic capacitors, varistors, etc. A multilayer ceramic capacitor has dielectric layers formed using dielectric green sheets and internal electrode layers formed using the conductive paste.
[0063] In the multilayer ceramic capacitor, the dielectric ceramic powder contained in the dielectric green sheet and the ceramic powder contained in the conductive paste are preferably powders of the same composition. In the multilayer ceramic capacitor manufactured using the conductive paste of this embodiment, even if the thickness of the dielectric green sheet is, for example, 2 μm or less, sheet attack and peeling failure of the green sheet are suppressed.
[0064] [Electronic components] Hereinafter, embodiments of electronic components and the like that can be manufactured using the conductive paste of the present invention will be described with reference to the drawings. In the drawings, the components may be shown in schematic form or at a different scale as appropriate. The positions and directions of components will be described with reference to the XYZ orthogonal coordinate system shown in FIG. 1 as appropriate. In this XYZ orthogonal coordinate system, the X and Y directions are horizontal directions, and the Z direction is vertical (up-down direction).
[0065] 1A and 1B are a perspective view and a side cross-sectional view showing a multilayer ceramic capacitor 1, which is an example of an electronic component according to an embodiment. The multilayer ceramic capacitor 1 includes a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately laminated, and an external electrode 20.
[0066] A method for manufacturing the multilayer ceramic capacitor 1 using the conductive paste will be described below. First, the conductive paste is printed on a dielectric layer made of a ceramic green sheet, and dried to form a dry film. A plurality of dielectric layers having this dry film on the upper surface are laminated by pressure bonding to obtain a laminate, and the laminate is then fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately laminated. Then, a pair of external electrodes 20 is formed on both ends of the ceramic laminate 10 to manufacture the multilayer ceramic capacitor 1. A more detailed description will be given below.
[0067] First, a ceramic green sheet, which is an unfired ceramic sheet, is prepared. For example, the ceramic green sheet is prepared by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a raw powder of a specific ceramic such as barium titanate, applying the dielectric layer paste to a support film such as a PET film in a sheet form, and drying to remove the solvent. The thickness of the dielectric layer made of the ceramic green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less from the viewpoint of the demand for miniaturization of the multilayer ceramic capacitor.
[0068] Next, the above-mentioned conductive paste is printed (applied) on one side of the ceramic green sheet by a known method such as screen printing, and then dried to form a dry film, to prepare a plurality of sheets. Note that, from the viewpoint of the requirement for thinning of the internal electrode layer 11, it is preferable that the thickness of the printed conductive paste (dried film) is 1 μm or less after drying.
[0069] Next, the ceramic green sheet is peeled off from the support film, and the dielectric layer made of the ceramic green sheet and the dry film formed on one side thereof are alternately laminated, and then a laminate is obtained by a heat and pressure treatment. Note that a configuration in which protective ceramic green sheets not coated with the conductive paste are further arranged on both sides of the laminate may be adopted.
[0070] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal treatment and fired under a reducing atmosphere to produce the ceramic laminate 10. The binder removal treatment is preferably performed in air or N2 gas. The temperature during the binder removal treatment is, for example, 200°C or higher and 400°C or lower. The temperature is preferably held for 0.5 hours or higher and 24 hours or lower during the binder removal treatment. The firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layers, and the temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature is held for, for example, 0.5 hours or higher and 8 hours or lower.
[0071] By firing the green chip, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. The organic vehicle in the dried film is also removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrodes, forming a multilayer ceramic sintered body in which the dielectric layers 12 and the internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layers to increase reliability and suppressing reoxidation of the internal electrodes, the multilayer ceramic sintered body after firing may be subjected to an annealing treatment.
[0072] A pair of external electrodes 20 is then provided on the produced fired laminated ceramic body to manufacture the laminated ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. The external electrode 20 is preferably made of, for example, copper, nickel, or an alloy thereof. The electronic component is not limited to a laminated ceramic capacitor, and may be an electronic component other than a laminated ceramic capacitor, such as a varistor. EXAMPLES
[0073] Examples of the present invention will be described in detail below, but the present invention is not limited in any way by the results of each evaluation sample in the examples.
[0074] <Example 1> (Preparation of nickel paste) The raw materials prepared in a ratio of 100 parts by mass of nickel powder (number average particle diameter 60 nm), 109 parts by mass of an organic vehicle obtained by dissolving 6 parts by mass of ethyl cellulose in 103 parts by mass of dihydroterpineol, 0.3 parts by mass of 2,6-tert-butyl-p-cresol as an additive, and 8 parts by mass of barium titanate (number average particle diameter 10 nm) as ceramic particles were simultaneously kneaded using a three-roll mill to produce the nickel paste of Example 1.
[0075] (Evaluation of sintering behavior) The conductive paste obtained was dried at 120°C for 40 minutes to volatilize the organic solvent, and the dried product obtained was pulverized to obtain a dry powder sample. 0.15g of the dry powder sample prepared was placed in a cylindrical mold (bottom diameter 5mm) and a load of 98mN was applied to prepare a pellet for sintering behavior evaluation. The pellet for sintering behavior evaluation prepared was placed in a thermomechanical analyzer (hereinafter, TMA, Rigaku: EVO2G TMA 8311B) and first subjected to a binder removal treatment. In the binder removal treatment, the pellet for sintering behavior evaluation was heated at 310°C for 3 hours while applying a load of 98mN to it and introducing nitrogen gas at a flow rate of 200mL / min. After the binder removal treatment, a firing treatment was performed. In the firing process, a load of 98 mN was applied to the pellets for evaluating the sintering behavior after the binder removal process, while nitrogen containing 0.15% by volume of hydrogen was introduced at a flow rate of 200 mL / min. Furthermore, water vapor was introduced so that the relative humidity at 40°C was 90%, and the pellets were heated from 25°C to 1300°C at a heating rate of 5°C / min. In the firing process, the temperature at which the height of the pellets contracted by 8% or more was defined as the sintering start temperature. The sintering behavior was determined to be the best (○) when the sintering start temperature was 730°C or higher, good (△) when it was between 700°C and less than 730°C, and poor (×) when it was less than 700°C. The evaluation results of the sintering behavior are shown in Table 1.
[0076] <Example 2> A nickel paste was prepared in the same manner as in Example 1, except that 0.3 parts by mass of 4-tert-butylpyrocatechol was used instead of 2,6-tert-butyl-p-cresol as an additive, and the sintering behavior was evaluated. The evaluation results of the sintering behavior are shown in Table 1.
[0077] <Comparative Example 1> A nickel paste was prepared in the same manner as in Example 1, except that no additive was used, and the sintering behavior was evaluated. The evaluation results of the sintering behavior are shown in Table 1.
[0078] [Table 1]
[0079] It can be inferred that the sintering behavior of the nickel powder and the ceramic green sheet is closer to each other because the sintering start temperature is higher in Examples 1 and 2 compared to Comparative Example 1. From this, it can be inferred that by setting the content of the phenolic compound within the preferred range of the present invention, it becomes difficult for delamination to occur between the conductive layer made of nickel powder and the dielectric layer made of ceramic green sheet, cracks to occur in the conductive layer due to stress difference, and discontinuities to occur in the internal electrode film.
[0080] The results of this evaluation indicate that by approximating the sintering behavior of nickel powder and ceramic green sheets, it is possible to reduce the occurrence of defective multilayer ceramic capacitors, which have thinner internal electrode layers and dielectric layers. [Explanation of symbols]
[0081] 1. Multilayer ceramic capacitor 10...Ceramic laminate 11...Internal electrode layer 12...Dielectric layer 20…External electrode 21...External electrode layer 22…Plating layer
Claims
1. A conductive paste comprising a conductive powder, an organic solvent, a binder resin and an additive, The conductive paste, wherein the additive comprises a phenolic compound.
2. The conductive paste of claim 1 , wherein the phenolic compound includes a tert-butyl group.
3. The conductive paste of claim 1 , wherein the phenolic compound is 2,6-tert-butyl-p-cresol or 4-tert-butylpyrocatechol, or a combination thereof.
4. 2. The conductive paste according to claim 1, wherein a mass ratio of the conductive powder to the phenol-based compound is 100:0.3-3.
5. The conductive paste of claim 1 , wherein the binder resin comprises ethyl cellulose.
6. The conductive paste of claim 1 comprising a ceramic powder.
7. The conductive paste according to claim 1 , wherein the number average particle size of the conductive powder is 30 nm or more and 100 nm or less.
8. An electronic component formed by using the conductive paste according to claim 1.
9. The laminate has at least a dielectric layer and an internal electrode layer stacked thereon, A multilayer ceramic capacitor, wherein the internal electrode layers are formed using the conductive paste according to claim 1 .
Citation Information
Patent Citations
Conductive paste and method for manufacturing composite nickel fine particle used therefor