Epoxy resin powder coating material
The epoxy resin powder coating composition addresses low-temperature curing challenges by using specific epoxy resins and fillers, achieving defect-free coating films on heat-sensitive components.
Patent Information
- Application Number
- JP2023058895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing epoxy resin powder coatings face challenges in curing at low temperatures and short times, leading to defects such as uneven thickness, poor smoothness, and small holes in coating films, especially when applied to heat-sensitive electronic components.
A composition comprising bisphenol A type epoxy resin with specific epoxy equivalents, novolac type epoxy resin, fillers with varying particle sizes, and a hardening agent, allowing for low-temperature curing and improved melt viscosity control to prevent defects.
The composition enables low-temperature curing in a short time, suppressing defects in the coating film, ensuring smooth and uniform application on heat-sensitive components.
Smart Images

Figure 2024146159000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin powder coating, and more particularly to an epoxy resin powder coating that can be applied under low temperature conditions. [Background technology]
[0002] Epoxy resins have excellent mechanical properties, chemical resistance, corrosion resistance, and electrical properties, and are widely used as powder paints. Powder paints using epoxy resins (epoxy resin powder paints) have excellent electrical properties and corrosion resistance, and are used in the field of processed steel materials such as bus bars and steel pipes. They are also used as paints to impart insulation and moisture resistance to the outer surfaces of electronic components such as film capacitors, and as paints to impart insulation to automotive components such as motors.
[0003] In a coating method using epoxy resin powder paint, a preheated object to be coated is immersed in a fluidized bath of epoxy resin powder paint, and the epoxy resin powder paint attached to the surface of the object to be coated is melted. The melted epoxy resin powder paint is then heated in a curing oven or the like to harden it, forming a coating film on the surface of the object to be coated. In such a case, if the object to be coated is an electronic component such as a film capacitor that may fail in a high-temperature environment, it is necessary to preheat and harden the object to be coated at a low temperature as much as possible. Therefore, it is preferable to use an epoxy resin powder paint that hardens even at low temperatures.
[0004] As an epoxy resin powder coating usable under such low-temperature conditions, Patent Document 1 discloses a powder coating composition that is curable at low temperatures, comprising as essential components an epoxy resin (A) having an epoxy equivalent of 500 to 2,500 g / eq and a softening point of 65 to 130°C, a curing agent (B) and a filler (C), in which the epoxy resin (A) is a bisphenol-type epoxy resin and the curing agent (B) is a basic nitrogen-containing heterocyclic compound. It is described that the powder coating composition disclosed in Patent Document 1 cures at 200°C or less, preferably 150°C or less, and in the examples it is described that it cures at 150°C. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-336286 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the substrate is an electronic component such as a film capacitor, which is prone to breakdown due to heat, it is preferable to perform curing at a low temperature (115 to 125°C) for a short time. In addition, when curing at a low temperature, it is difficult to adjust the melt viscosity, and there is a problem that poor coating occurs and defects (uneven film thickness, poor smoothness, small holes, etc.) occur in the coating film.
[0007] The present invention has been made with the above points in mind, and aims to provide an epoxy resin powder coating that can be cured at low temperatures and in a short time, and is capable of forming a coating film in which the occurrence of defects is effectively suppressed. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention is specified as follows (1) to (3). (1) An epoxy resin powder coating for forming a cured product, The following (A), (B), (C), and (D) are included: (A) a bisphenol A type epoxy resin having an epoxy equivalent of 450 to 630 g / eq; (B) Novolac type epoxy resin, (C) a filler having an average particle size D50 of 5 to 12 μm; (D) a hardener, An epoxy resin powder coating material containing 65 to 85 parts by mass of (C) when the total amount of epoxy resins is 100 parts by mass. (2) further comprising (C') a filler having an average particle size D50 of 0.5 to 2 μm, The epoxy resin powder coating according to (1) above, wherein the (C') is contained in an amount of 3 to 20 parts by mass when the total amount of the epoxy resins is taken as 100 parts by mass. (3) The epoxy resin powder coating material according to (1) or (2) above, further comprising (E) a bisphenol A-type novolac-modified epoxy resin. Effect of the Invention
[0009] According to an embodiment of the present invention, an epoxy resin powder coating material can be provided that can be cured at a low temperature in a short time and can form a coating film in which the occurrence of defects is effectively suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes an epoxy resin powder coating according to an embodiment of the present invention, but the present invention should not be construed as being limited thereto, and various changes, modifications, and improvements can be made based on the knowledge of those skilled in the art without departing from the scope of the present invention.
[0011] In this specification, the term "to" indicating a range of values indicates a range including the values given as the upper and lower limits. When a unit is given only for the upper limit of a range of values, it means that the lower limit is expressed in the same unit as the upper limit. In the present specification, in which numerical ranges are described stepwise, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described stepwise. In addition, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0012] (Epoxy resin powder coating) The epoxy resin powder coating according to an embodiment of the present invention is an epoxy resin powder coating for forming a cured product, and contains the following (A), (B), (C), and (D). (A) a bisphenol A type epoxy resin having an epoxy equivalent of 450 to 630 g / eq; (B) Novolac type epoxy resin, (C) a filler having an average particle size D50 of 5 to 12 μm; (D) Hardener.
[0013] Hereinafter, each component contained in the epoxy resin powder coating material according to the embodiment of the present invention will be described.
[0014] <(A) Bisphenol A type epoxy resin> The powder coating containing the bisphenol A type epoxy resin has good mechanical properties, chemical resistance, electrical properties, and corrosion resistance of the coating film, which is a cured product formed after coating. The bisphenol A type epoxy resin (A) has an epoxy equivalent of 450 to 630 g / eq. By making the epoxy equivalent of the bisphenol A type epoxy resin 450 g / eq or more, it is possible to prevent the melt viscosity of the powder coating from being too low, and to prevent problems such as dripping of the molten powder coating when coating the powder coating. In addition, by making it 630 g / eq or less, the melt flowability is good when coating the powder coating in a low temperature (115 to 125°C) environment, and problems such as small holes occurring in the coating film can be prevented. The softening point of the bisphenol A type epoxy resin (A) is preferably 65 to 95°C from the viewpoint of curability. The bisphenol A type epoxy resin may be used in combination of two or more types having different epoxy equivalents so that the epoxy equivalent falls within the range of 450 to 630 g / eq. Commercially available bisphenol A epoxy resins (A) include YD-011, YD-012, YD-014 (all manufactured by KUKDO Chemical Corporation), JER-1001, JER-1002, JER-1004, JER-1007 (all manufactured by Mitsubishi Chemical Corporation), GESR-901, GESR-902, GESR-904, GESR-907 (all manufactured by Epoxy Base Electronic Material Corporation Limited), and the like.
[0015] <(B) Novolac type epoxy resin> Examples of the novolac type epoxy resin of (B) include phenol novolac type epoxy resin, cresol novolac type epoxy resin, etc. Among these, cresol novolac type epoxy resin is preferred from the viewpoint of heat resistance. Commercially available cresol novolac epoxy resins include YDCN-500-10P (manufactured by KUKDO Chemical Co., Ltd.), Epicron N-660, Epicron N-665, Epicron N-670, Epicron N-673, Epicron N-695 (all manufactured by DIC Corporation), EOCN-1020, EOCN-102S, EOCN-104S (all manufactured by Nippon Kayaku Co., Ltd.), and the like.
[0016] Furthermore, the epoxy resin powder coating according to the embodiment of the present invention contains these two types of epoxy resins (A) and (B), and thus can be cured at a low temperature.
[0017] From the viewpoint of low temperature curing, the compounding ratio (B) / (A) of the bisphenol A epoxy resin (A) to the novolac epoxy resin (B) is preferably 0.14 to 0.65, and more preferably 0.23 to 0.54. In this specification, unless otherwise specified, the "mixing ratio" refers to the mass ratio.
[0018] <(C) Filler> Examples of the filler (C) include oxides such as silica, alumina, zirconium dioxide, magnesium oxide, zinc oxide, iron oxide, barium titanate, and silica-alumina composite oxide; nitrides such as silicon nitride, titanium nitride, boron nitride, and aluminum nitride; sparingly soluble ion crystals such as calcium fluoride, barium fluoride, calcium sulfate, and barium sulfate; covalent crystals such as graphite, silicon, and silicon dioxide; calcium carbonate, aluminum sulfate, aluminum hydroxide, magnesium hydroxide, potassium titanate, calcium silicate, magnesium silicate, talc, kaolinite, montmorillonite, sericite, mica, bentonite, zeolite, boehmite, and mullite, as well as compounds containing these. Among these, aluminum hydroxide and magnesium hydroxide are particularly preferred because they can improve the flame retardancy of the epoxy resin powder coating by generating water when heated.
[0019] The filler (C) has an average particle diameter D50 of 5 to 12 μm, and is contained in an amount of 65 to 85 parts by mass when the total amount of the epoxy resin is taken as 100 parts by mass. By containing 65 to 85 parts by mass of a filler having a relatively large particle diameter of 5 to 12 μm, the epoxy resin powder coating material can obtain a suitable flowability when melted, and the melt viscosity can be easily adjusted, and dripping from the surface of the coated object can be effectively suppressed, and further, the occurrence of defects in the coating film (uneven film thickness, etc.) due to poor coating can be effectively suppressed. It is more preferable that the filler (C) has an average particle diameter D50 of 5 to 12 μm, and is contained in an amount of 70 to 80 parts by mass when the total amount of the epoxy resin is taken as 100 parts by mass.
[0020] The average particle size D50 is the 50% cumulative volume particle size (also called the median size) measured by the laser diffraction / scattering method (JIS Z8825:2022). The average particle size D50 can be measured using a laser diffraction particle size distribution analyzer (SYMPATEC, HELOS and RODOS analysis software:WINDOX5) or the like.
[0021] <(C') Filler> The epoxy resin powder coating according to the embodiment of the present invention preferably further contains a filler having an average particle size D50 of 0.5 to 2 μm. The material of the filler (C') can be the same as the above-mentioned filler (C), and aluminum hydroxide and magnesium hydroxide are particularly preferred from the viewpoint of improving flame retardancy.
[0022] The filler (C') having a relatively small particle size, ie, average particle size D50 of 0.5 to 2 μm, has a larger total contact area with the resin than the filler (C) having a relatively large particle size, ie, average particle size D50 of 5 to 12 μm, and therefore has a larger frictional resistance. Therefore, by using the filler (C') having a relatively small particle size in combination with the filler (C) having a relatively large particle size, the epoxy resin powder coating material can obtain a more appropriate flowability when melted, and the melt viscosity can be adjusted more easily. As a result, dripping from the surface of the coated object can be more effectively suppressed, and furthermore, the occurrence of defects in the coating film (uneven film thickness, etc.) due to poor coating can be more effectively suppressed. From the viewpoint of imparting an appropriate flowability to the epoxy resin powder coating material when melted, the filler (C') is preferably contained in an amount of 3 to 20 parts by mass, more preferably 5 to 15 parts by mass, when the total amount of the epoxy resin is taken as 100 parts by mass.
[0023] The compounding ratio (C') / (C) of the filler (C') to the filler (C) is preferably 0.01 to 0.35, more preferably 0.05 to 0.25. By making the compounding ratio (C') / (C) within the range of 0.01 to 0.35, it is possible to better control the appropriate flowability of the epoxy resin powder coating material when melted, and thereby to better suppress the occurrence of coating film defects (uneven film thickness, etc.) due to poor coating.
[0024] <(D) Hardener> The curing agent (D) is not particularly limited as long as it is capable of curing the epoxy resin powder coating material according to the embodiment of the present invention at low temperatures, and imidazole derivatives, amine compounds, or addition reaction products of amine compounds and epoxy resins can be used alone or in combination.
[0025] The imidazole derivative is a compound in which a substituent or the like is introduced into imidazole, and includes, for example, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and triazine compounds having an imidazole ring. Examples of triazine compounds having an imidazole ring include 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. Two or more imidazole derivatives may be used in combination. Among them, from the viewpoint of fast curing, it is preferable to use 2-methylimidazole and triazine compounds having an imidazole ring. Commercially available imidazole derivatives include Curesol (registered trademark) 2MZ-H and Curesol (registered trademark) 2MZ-A (both manufactured by Shikoku Chemical Industries, Ltd.).
[0026] Examples of the amine compound include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, modified polyamidoamines, etc. Among these, it is preferable to use modified polyamidoamines from the viewpoint of low temperature curing properties.
[0027] The addition reaction product of an imidazole compound and an epoxy resin has a structure in which the imidazole compound is ring-opened and added to both terminal epoxy groups of an epoxy resin. The imidazole compound includes imidazole and imidazole derivatives. The epoxy resin includes bisphenol-type epoxy resins and the like. The addition reaction product of an imidazole compound and an epoxy resin includes, for example, an addition reaction product of 2-methylimidazole and a bisphenol A-type epoxy resin, and an addition reaction product of 2-ethyl-4-methylimidazole and a bisphenol A-type epoxy resin. The addition reaction product of an imidazole compound and an epoxy resin may be used in combination of two or more kinds. Among them, it is preferable to use an addition reaction product of 2-methylimidazole and a bisphenol A-type epoxy resin from the viewpoint of low-temperature curing. The curing agent (D) is contained in an amount of preferably 1.0 to 4.0 parts by mass, and more preferably 1.5 to 3.0 parts by mass, based on 100 parts by mass of the total amount of the epoxy resin.
[0028] <(E) Bisphenol A type novolac modified epoxy resin> The epoxy resin powder coating according to the embodiment of the present invention preferably further contains a bisphenol A type novolac modified epoxy resin. By adding the bisphenol A type novolac modified epoxy resin, the flowability of the epoxy resin powder coating when melted is further improved. Examples of the bisphenol A type novolac modified epoxy resin include bisphenol A-epichlorohydrin-phenol-formaldehyde polycondensates. From the viewpoint of improving low-temperature curing property and flowability, the compounding ratio (E) / (A) of the bisphenol A type epoxy resin (E) to the bisphenol A type epoxy resin (A) is preferably 0.1 to 0.45, more preferably 0.15 to 0.35. When the epoxy resin powder coating according to the embodiment of the present invention does not contain the bisphenol A type novolac modified epoxy resin (E), it is preferable that the bisphenol A type epoxy resin (A) is contained in an amount of 60 parts by mass or more, more preferably 70 parts by mass or more, when the total amount of the epoxy resin is taken as 100 parts by mass. Commercially available bisphenol A type novolac modified epoxy resins include Epiclon 5500, Epiclon 5800 (both manufactured by DIC Corporation), NPES-660U (manufactured by NANYA Corporation), and the like.
[0029] In the epoxy resin powder coating according to the embodiment of the present invention, the total epoxy equivalent of all epoxy resins is preferably 300 to 500 g / eq. When the total epoxy equivalent of all epoxy resins is 300 g / eq or more, the melt viscosity of the powder coating is prevented from decreasing too much, and when the powder coating is applied, problems such as dripping of the molten powder coating can be prevented. In addition, when the total epoxy equivalent of all epoxy resins is 500 g / eq or less, when the powder coating is applied in a low temperature (115 to 125 ° C) environment, the melt flowability is good, and problems such as small holes occurring in the coating film can be prevented. In the epoxy resin powder coating according to the embodiment of the present invention, the total epoxy equivalent of all epoxy resins is more preferably 350 to 450 g / eq.
[0030] <Other ingredients> The epoxy resin powder coating material according to the embodiment of the present invention may contain, as appropriate, conventional auxiliary components such as epoxy resins, curing accelerators, flame retardants, colorants, surface modifiers, thixotropic agents, anti-settling agents, coupling agents, defoamers, release agents, and flowability adjusters other than the above-mentioned components, provided that the effects of the present invention are not impaired. Examples of the flame retardant include phosphorus compounds, halogen compounds, antimony compounds such as antimony trioxide, and metal hydroxides. Examples of the surface modifier include (meth)acrylic acid alkyl ester polymers. Colorants include titanium dioxide, ferric oxide, carbon black, phthalocyanine blue, copper, and the like. The flowability adjusting agent may include amorphous silica.
[0031] <Gelation time> The epoxy resin powder coating material according to the embodiment of the present invention has a curing property in which the time required for gelation at 120°C according to JIS C 2104 is 260 to 340 seconds, preferably 280 to 320 seconds. If the gelation time is 260 seconds or more, not only can a cured product sufficient to exhibit the desired properties be obtained, but it can also be said to have excellent melting properties when heated. If the gelation time at 120°C is too long, the horizontal flow rate of the coating material becomes too large, and the viscosity becomes low when melted, making the coating material easy to flow, which may result in coating defects such as small holes and a phenomenon called sagging. If the gelation time is 340 seconds or less, the horizontal flow rate of the coating material at 120°C can be maintained at, for example, 30% or less. Also, if the gelation time is 340 seconds or less, in the present invention, short-term curing is possible.
[0032] <Horizontal flow rate> The epoxy resin powder coating material according to the embodiment of the present invention has a horizontal flow rate at 120°C of 20 to 30%, preferably 22 to 28%. If the horizontal flow rate of the coating material is too small, the coating material will not flow when melted, which makes it easy for coating defects such as small holes to occur and makes it difficult to obtain a smooth coating film. If the horizontal flow rate of the coating material is too large, sagging will occur during the process from melting to curing when obtaining a cured coating film, making it difficult to form a desired film thickness. The horizontal flow rate indicates the melting property of the powder paint when heated, and a large value indicates that the paint has a low viscosity when melted and flows easily, while a small value indicates that the paint has a high viscosity when melted and flows less easily. The method for measuring the horizontal flow rate will be described later.
[0033] <Application> The epoxy resin powder coating according to the embodiment of the present invention can be used, like general epoxy resin powder coatings, as a coating that imparts corrosion resistance, insulation, moisture resistance, etc. to the surfaces of processed steel materials such as bus bars and steel pipes, electronic components, etc. In addition, since it can be cured in a short time even at low temperatures (115 to 125°C), it can be used as a coating for the outer surfaces of heat-sensitive electronic components such as film capacitors, and as a coating that imparts insulation properties to the surfaces of in-vehicle components such as motors.
[0034] The method of coating with the epoxy resin powder coating material according to the embodiment of the present invention is not particularly limited, and any known coating method can be used. Specifically, electrostatic coating, triboelectric coating, non-charged coating, fluidized bed coating, etc. can be mentioned. From the viewpoint that the epoxy resin powder coating according to the embodiment of the present invention can be cured at a low temperature in a short time, it is particularly preferable to use a coating method by fluidized bed immersion. A specific example of fluidized bed immersion is a method in which a preheated coating object is immersed in a fluidized bed of coating material to melt the epoxy resin powder coating adhering to the surface of the coating object. The molten epoxy resin powder coating is then cured by heating in a curing oven or the like to form a coating film on the surface of the coating object.
[0035] (Manufacturing method of epoxy resin powder coating) The epoxy resin powder coating according to the embodiment of the present invention can be produced, for example, by the following method. First, the above-mentioned (A) bisphenol A type epoxy resin, (B) novolac type epoxy resin, (C) filler, and (D) curing agent are mixed, and if necessary, a (C') filler, (E) bisphenol A type novolac modified epoxy resin, epoxy resins other than the above-mentioned components, curing accelerators, flame retardants, colorants, surface modifiers, thixotropic agents, anti-settling agents, coupling agents, defoamers, mold release agents, flow control agents, and other commonly used auxiliary components are added to prepare a composition. When the total amount of the epoxy resins in this composition is 100 parts by mass, the filler (C) is contained in an amount of 65 to 85 parts by mass. Next, the composition is melt-kneaded. The melt-kneading is preferably completed in a short time using an extruder or the like. Thereafter, the obtained mixture is cooled and solidified, and the solidified mixture (melted and kneaded product) is pulverized to obtain the epoxy resin powder coating material according to the embodiment of the present invention. EXAMPLES
[0036] The following examples of the present invention are provided for a better understanding of the present invention and its advantages, and are not intended to limit the invention.
[0037] 1. Preparation of Epoxy Resin Powder Coating <Examples 1 to 5 and Comparative Examples 1 to 5> A composition was prepared by mixing all the materials for each experimental example in the compounding ratio (mass ratio) shown in Table 1. The raw materials of each component shown in Table 1 are shown below. The average particle size D50 of the fillers (C) and (C') was measured using a laser diffraction particle size distribution measuring device (SYMPATEC, HELOS and RODOS analysis software: WINDOX5).
[0038] (A) Bisphenol A epoxy resin (a1) Bisphenol A type epoxy resin with an epoxy equivalent of 470 g / eq (a2) Bisphenol A type epoxy resin with an epoxy equivalent of 635 g / eq. (a3) Bisphenol A type epoxy resin with an epoxy equivalent of 910 g / eq (B) Novolac type epoxy resin (b1) Orthocresol novolac epoxy resin (epoxy equivalent: 210 g / eq) (C) Filler (c1) Aluminum hydroxide (average particle size D50 8μm) (C') Filler (c'1) Aluminum hydroxide (average particle size D50 1μm) (D) Hardener (d1) 2,4-Diamino-6-[2′-methylimidazolyl-(1′)]-ethyl-s-triazine (E) Bisphenol A type novolac modified epoxy resin (e1) Bisphenol A-epichlorohydrin-phenol-formaldehyde polycondensate (epoxy equivalent 480g / eq)
[0039] Next, each composition was melt-kneaded using an extruder. Thereafter, the resulting mixture was cooled and solidified, and the solidified mixture (melted and kneaded product) was pulverized to obtain a sample of an epoxy resin powder coating material.
[0040] 2. Evaluation The epoxy resin powder coating samples obtained in each experimental example were evaluated for curability, coatability, and cured product properties by the methods described below.
[0041] <2-1: Curing property (gelation time)> The curability of the epoxy resin powder coating was evaluated by measuring the gel time. Approximately 0.05g of the epoxy resin powder coating obtained in each experiment was placed in the circular recess of a hot plate maintained at 120℃, and stirred with a stirring rod, and the time until the coating no longer formed strings, i.e., the time until gelation (seconds), was measured. Measurements were performed in accordance with JIS C 2104. The evaluation results are shown in Table 1.
[0042] <2-2: Paintability (horizontal flow rate)> The coatability of the epoxy resin powder coating was evaluated by measuring the horizontal flow rate. About 1.0 g of the epoxy resin powder coating material obtained in each experimental example was placed in a tablet forming die with an inner diameter of 16 mmφ, and pressed at a load of 70 to 80 MPa for 60 seconds to form a tablet, after which it was dried for 15 minutes in a desiccator with a reduced pressure of 1333 Pa or less, and the diameter (a) of the tablet was measured with a vernier caliper. Next, the obtained tablet was placed on a slide glass, heated at 120°C for 10 minutes in a hot air dryer, removed, and similarly measured for the diameter (b) of the tablet. Then, the increase in diameter (ba) due to heating was divided by the diameter (a) before heating, and this was multiplied by 100 to calculate the horizontal flow rate for each powder coating material obtained in each experimental example. The evaluation results are shown in Table 1.
[0043] <2-3: Properties of the cured product (appearance of the coating film)> The appearance of the coating was evaluated as a property of the cured product of the epoxy resin powder coating. A test piece of bonded steel (subject to be coated: length x width x thickness = 90 mm x 75 mm x 1 mm) preheated to 150°C was immersed in a fluidized bath of the epoxy resin powder paint obtained in each experimental example, and allowed to adhere to the surface of the subject to be coated. Next, the epoxy resin powder paint melted on the surface of the subject to be cured by heating in a curing oven or the like, forming a coating film. Next, the appearance of the coating film was observed with the human eye. The evaluation criteria were as follows. The evaluation results are shown in Table 1. Very good: smooth. Good: Some unevenness but usable. Defective: Unusable due to unevenness on the entire surface.
[0044] [Table 1]
[0045] 3. Discussion As shown in Table 1, the epoxy resin powder coatings according to Examples 1 to 5, which contain the above-mentioned (A), (B), (C), and (D) as components and contain 65 to 85 parts by mass of (C) when the total amount of epoxy resin is 100 parts by mass, showed good results in terms of curability, coatability, and cured product properties. That is, in Examples 1 to 5, curing at low temperatures and in a short time was possible, and a coating film in which the occurrence of defects was well suppressed could be formed. In particular, in Examples 2 and 3, which used fillers (C) and (C') with different particle sizes, the molten horizontal flow rate was smaller than in Example 1, which used only the large particle size (C) as the filler, and problems such as dripping of the molten powder paint when applying the powder paint could be suppressed. In Comparative Example 1, not only was the epoxy equivalent of the bisphenol A epoxy resin (A) greater than 630 g / eq, but the content of (C) was less than 65 parts by mass, so the horizontal flow rate and the appearance of the coating film were poor. In all of Comparative Examples 2 to 5, the content of (C) was less than 65 parts by mass when the total amount of the epoxy resin was taken as 100 parts by mass, and therefore the horizontal flow rate and the coating film appearance were poor.
Claims
1. An epoxy resin powder coating for forming a cured product, comprising: The present invention includes the following (A), (B), (C), and (D): (A) a bisphenol A type epoxy resin having an epoxy equivalent of 450 to 630 g / eq; (B) a novolac type epoxy resin, (C) a filler having an average particle size D50 of 5 to 12 μm; (D) a curing agent, The epoxy resin powder coating contains 65 to 85 parts by mass of (C) when the total amount of the epoxy resins is 100 parts by mass.
2. Further, (C') a filler having an average particle size D50 of 0.5 to 2 μm is contained, 2. The epoxy resin powder coating according to claim 1, wherein the (C') is contained in an amount of 3 to 20 parts by mass when the total amount of the epoxy resins is 100 parts by mass.
3. 3. The epoxy resin powder coating according to claim 1 or 2, further comprising (E) a bisphenol A type novolak modified epoxy resin.
Citation Information
Patent Citations
Low temperature curing type powder coating composition and method for fornming coating film on inner surface of metallic pipe using the same powder coating
JP2000336286A
Cited By
Powder coating composition
JP7829973B1