Method for predicting fiber content ratio distribution of fiber-reinforced resin molding, fiber content ratio distribution prediction device, fiber content ratio distribution prediction program, and recording medium

By employing a fiber content prediction formula that accounts for fiber orientation and flow influences, the method addresses the accuracy issues in predicting fiber distribution, enhancing the precision of local property variations in fiber-reinforced resin molded products.

JP2024146174AActive Publication Date: 2024-10-15MAZDA MOTOR CORP +1

Patent Information

Application Number
JP2023058917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional methods for predicting fiber content distribution in fiber-reinforced resin molded products lack accuracy, particularly in predicting local variations in physical properties due to uneven fiber distribution, leading to inconsistencies in stiffness and strength.

Method used

A method and device for predicting fiber content distribution using a fiber content prediction formula that accounts for fiber orientation, formulated based on actual phenomena, where fiber content decreases as the orientation approaches a predetermined value, combined with a modified Folgar-Tucker model to consider the influence of both shear and elongation flows.

Benefits of technology

This approach enhances the prediction accuracy of fiber content distribution, allowing for more precise estimation of local variations in physical properties such as rigidity and strength, thereby improving product design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146174000001_ABST
    Figure 2024146174000001_ABST
Patent Text Reader

Abstract

To provide a fiber content ratio distribution prediction method, an apparatus, a program, and a recording medium of fiber reinforced resin molded products that can improve prediction accuracy of a fiber content ratio distribution with a concise model.SOLUTION: A method for predicting a fiber content ratio distribution contained in an injection molded product of a fiber reinforced resin by computer simulation, comprising a fiber content ratio calculation step for calculating the fiber content ratio on the basis of fiber orientation and a fiber content ratio prediction formula, the fiber content ratio prediction formula is a model in which the content ratio decreases as the orientation of the fiber approaches the predetermined orientation.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for predicting the fiber content distribution of a fiber-reinforced resin molded product, a fiber content distribution prediction device, a program for causing a computer to execute the fiber content distribution prediction method, and a computer-readable recording medium having the program recorded thereon. [Background technology]

[0002] Conventionally, in order to facilitate the product design of injection-molded fiber-reinforced resins, the flow and solidification behavior of fiber-reinforced resins in a mold has been analyzed using CAE (Computer-Aided-Engineering).

[0003] In fiber-reinforced resins, if the fiber content distribution is biased, the rigidity, strength, etc. of the molded product may decrease locally in the area where the fiber content is locally low. Therefore, it is important to accurately predict the fiber content distribution in the molded product in order to predict the local variation in physical properties such as rigidity and strength of the injection molded product.

[0004] For example, Patent Document 1 describes an analysis of the volume fraction distribution of the filler when the flow of the fluid stops, using the distribution of the positions, directions, and shapes of the fillers obtained by a filler behavior simulation. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-226871 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the technique of Patent Document 1 does not mention a specific model for analyzing the volume fraction distribution of the filler based on the distribution of the positions, directions, and shapes of the filler.

[0007] In addition, conventional commercial software had low accuracy in predicting the fiber content distribution in molded products, making it difficult to predict local changes in the content distribution and making it impossible to predict local variations in physical properties.

[0008] Therefore, an object of the present disclosure is to provide a fiber content distribution prediction method and fiber content distribution prediction device for a fiber-reinforced resin molded product, which can improve the prediction accuracy of fiber content distribution using a simple model, a program for causing a computer to execute the fiber content distribution prediction method, and a computer-readable recording medium having the program recorded thereon. [Means for solving the problem]

[0009] In order to solve the above problems, one aspect of a method for predicting a fiber content distribution of a fiber-reinforced plastic molded product according to the present disclosure is to A method for predicting the fiber content distribution in a fiber-reinforced resin injection molded product by computer simulation, comprising: A fiber content calculation step of calculating the fiber content based on the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. It is characterized by:

[0010] As a result of intensive research, the inventors of the present application have found that in actual phenomena, the fiber content depends on the fiber orientation, and decreases as the fiber orientation approaches a predetermined orientation. In this configuration, a model formulated based on the above-mentioned actual phenomenon is used as a fiber content prediction formula. This makes it possible to accurately predict the fiber content distribution using a simple model.

[0011] Preferably, the orientation is represented by a fiber orientation tensor in which the flow direction of the molten resin is set to 1 and the direction perpendicular to the flow direction is set to 0.

[0012] In this specification, the fiber orientation tensor is a parameter for treating the degree of fiber orientation as a scalar quantity, and a 3-row, 3-column matrix is ​​calculated from the orientation directions ΔX, ΔY, and ΔZ of each fiber by the tensor product, and the fiber orientation degree in each direction as a composite is indicated by normalizing and averaging (A11 is the X direction (MD), A22 is the Y direction (TD), and A33 is the Z direction (ND). The sum of A11, A22, and A33 is 1.) In addition, in injection molding of fiber-reinforced resin, it is common to use only A11 as an index based on the characteristic that fibers are hardly oriented in the A33:ND direction, and in this specification, the "(fiber) orientation tensor" means the change in the degree of orientation in the tensor of A11. In addition, in this specification, the "(fiber) orientation tensor" may be written as "A11 tensor (MD)". This simplifies the description of fiber orientation, and makes it possible to predict the fiber content distribution with a simpler model.

[0013] Preferably, the predetermined orientation is an orientation in which the fiber orientation tensor is greater than or equal to 0.4 and less than or equal to 0.7.

[0014] In experiments conducted by the inventors of the present application, it was found that the fiber content tends to be low in the orientation where the fiber orientation tensor is 0.4 to 0.7 in the real phenomenon. With this configuration, it is possible to predict the fiber content distribution using a fiber content prediction formula that is in line with the real phenomenon, thereby improving the prediction accuracy.

[0015] Preferably, the fiber content prediction formula for the portion other than the skin layer is expressed by the following formula (1).

[0016] Y = aX + b (1) however, a=a 1 <0, b=b 1 (0≦X≦c) a=a 2 >0, b=b 2 (c <X≦1) a 1 =d a1 G 0 +f a1 b 1 =d b1 G0 +f b1 a 2 =d a2 G 0 +f a2 b 2 =d b2 G 0 +f b2 In equation (1), X is the fiber orientation tensor, Y is the fiber content, c is a given value of the fiber orientation tensor, a is the slope, b is the intercept, a 1 is the first slope, b 1 is the first intercept, a 2 is the second slope, b 2 is the second intercept, G 0 is the initial content, and d a1 , f a1 , d b1 , f b1 , d a2 , f a2 , d b2 and f b2 is a constant calculated based on the actual measurement value.

[0017] The above formula (1) is formulated based on the measured values ​​obtained by an actual experiment. According to this configuration, it is possible to predict the fiber content distribution using a fiber content prediction formula that is in line with the actual phenomenon, and the prediction accuracy is improved. In this specification, the skin layer refers to a layer that corresponds to layer 1 including the surface and layer 18 when the plate is divided into 18 layers in the plate thickness direction, and for example, when the plate thickness is 3.5 mm, it refers to a layer from the surface of the molded product to a depth of about 0.15 mm. In this specification, the layer inside the skin layer is called the core layer.

[0018] Preferably, the predetermined orientation is a random orientation.

[0019] The inventors of the present application found that the fiber content decreases as the fiber orientation approaches random orientation. This is thought to mean that when fibers exist in a space of the same volume, many fibers cannot exist unless the fiber orientation is aligned to a certain extent. According to this configuration, it is possible to predict the content distribution based on the actual phenomenon, and the prediction accuracy is improved.

[0020] Preferably, a fiber orientation calculation step is provided before the fiber content calculation step, in which the orientation of the fiber is calculated based on a flow rate of the molten resin and a fiber orientation prediction equation consisting of a modified Folgar-Tucker model, The fiber orientation prediction formula includes a term that takes into account the influence of an elongational flow, which is a flow whose flow speed changes in the flow direction of the molten resin, as a term that takes into account the interference between the fibers.

[0021] The conventional FT model includes only an interference term that takes into account the effect of shear flow as a term that takes into account the interference between fibers, and adopts the idea that the fiber orientation becomes random when fibers interfere with each other, regardless of the type of flow. (Note that in this specification, "randomization" refers to the isotropy (contrasted with anisotropy) of the fiber orientation. In the FT model, δ ij The randomization is expressed by the setting of

[0022] However, the inventors of the present application found through intensive research that the influence of shear flow on the interference between fibers is different from the influence of elongation flow. In this configuration, a modified FT model including an interference term that takes into account the influence of elongation flow is used as the fiber orientation prediction formula. This improves the prediction accuracy of the fiber orientation distribution with a simple model. Thus, the prediction accuracy of the fiber content distribution is also improved.

[0023] Preferably, the fiber orientation prediction equation is expressed by the following equation (2).

[0024]

number

[0025] One aspect of the fiber content distribution prediction device for a fiber reinforced plastic molded product disclosed herein is as follows: An apparatus for predicting the fiber content distribution contained in a fiber-reinforced resin injection molded product by computer simulation, comprising: A fiber content calculation unit is provided that calculates the fiber content based on the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. It is characterized by:

[0026] In addition, one aspect of the fiber content distribution prediction program for a fiber reinforced plastic molded product disclosed herein is, A program for predicting the fiber content distribution in a fiber-reinforced resin injection molded product by computer simulation, The method causes a computer to execute a procedure of calculating the fiber content based on at least the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. It is characterized by:

[0027] The device and program of this configuration use a model formulated based on the actual phenomenon discovered by the inventors that the fiber content depends on the fiber orientation and decreases as the fiber orientation approaches a predetermined orientation as a fiber content prediction equation, which makes it possible to accurately predict the fiber content distribution with a simple model.

[0028] One embodiment of a recording medium disclosed herein is a computer-readable recording medium having recorded thereon the above-mentioned fiber content distribution prediction program for a fiber-reinforced plastic molded product. Effect of the Invention

[0029] As described above, in the present disclosure, a model formulated based on the actual phenomenon discovered by the present inventors that the fiber content depends on the fiber orientation and decreases as the fiber orientation approaches a predetermined orientation is used as a fiber content prediction equation, which makes it possible to accurately predict the fiber content distribution with a simple model. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a diagram showing an example of the configuration of a fiber content distribution prediction device according to the present disclosure. [Diagram 2] 1 is a flowchart for explaining a fiber content distribution prediction method according to the present disclosure. [Diagram 3] 1 is a graph showing actual measured values ​​of fiber content obtained by the experiment of Reference Example 2. [Figure 4] 13 is a graph showing a comparison between the actual measured values ​​of the fiber content obtained by the experiment of Reference Example 2 and the predicted values ​​of the fiber content obtained by the analysis of Analysis Example 1 (conventional example). [Diagram 5] 13 is a graph showing an X-ray CT image at the position indicated by the symbol A6 obtained in the experiment of Reference Example 1 and the fiber content of each layer calculated from the X-ray CT image. [Figure 6] FIG. 2 is a diagram for explaining the concept of the relationship between fiber orientation and fiber content. [Figure 7] Graph showing the relationship between fiber orientation tensor deviation (average thickness) and fiber content (average thickness). [Figure 8] FIG. 13 is a diagram for explaining a method for deriving the relationship between the fiber orientation tensor and the fiber content in each layer in the plate thickness direction. [Figure 9] FIG. 2 is a graph showing the relationship between the fiber orientation tensor and the fiber content in each layer in the plate thickness direction, and shows the influence of the resin MFR and plate thickness. [Figure 10] FIG. 2 is a graph showing the relationship between the fiber orientation tensor and the fiber content in each layer in the plate thickness direction, and shows the effect of the fiber length. [Figure 11] FIG. 1 is a graph showing the relationship between the fiber orientation tensor and the fiber content in each layer in the plate thickness direction, and shows the influence of the initial content. [Figure 12] Graph showing the sensitivity (slope and intercept) of the fiber orientation tensor to fiber content versus initial content. [Figure 13] FIG. 13 is a diagram for explaining a method of deriving a fiber content distribution prediction formula. [Figure 14]1 shows a test piece TP1 used in the experiments of Reference Examples 1 and 2 and a shape model thereof, and a test piece TP2 used in the analyses of Analysis Examples 1 and 2 and an analytical model thereof. FIG. [Figure 15] FIG. 13 is a diagram for explaining a state in which shape data of a test piece is divided in the thickness direction. [Figure 16] 1 is a graph showing a comparison between the actual measured values ​​of the fiber content obtained by the experiment of Reference Example 2 and the predicted values ​​of the fiber content obtained by the analysis of Analysis Example 2 (a verification example of the present prediction method). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present disclosure, its application, or its uses.

[0032] <Fiber content distribution prediction device> 1 shows an example of the configuration of a fiber content distribution prediction device 100 of a fiber reinforced plastic molded product (hereinafter, also referred to as "prediction device 100") according to the present disclosure. The prediction device 100 is a device that predicts the fiber content distribution contained in a fiber reinforced plastic injection molded product by computer simulation, and is a CAE (Computer Aided Engineering) system basically composed of a computer 110.

[0033] The prediction device 100 includes a storage unit 120 and a processor 130. The prediction device 100 also includes a display unit 140 including a display or the like, an input unit 150 including a keyboard or the like, and a reading unit 160 for acquiring information stored in various recording media 170. The storage unit 120 and / or the recording media 170 store information such as programs for arithmetic processing and various analysis data. The processor 130 performs various arithmetic processing based on the information stored in the storage unit 120, information input via the input unit 150, and information acquired from the recording media 170 via the reading unit 160.

[0034] The prediction device 100 creates an analysis model by dividing shape data such as 3D CAD data that defines a cavity of a mold that becomes a flow path of a fiber-reinforced resin into a plurality of minute elements using the analysis model creation unit 131. As the analysis model creation unit 131 that creates the minute elements, for example, a CAE preprocessor such as 3D TIMON (registered trademark)-Pre / Post manufactured by Toray Engineering D Solutions Co., Ltd., FEMAP (registered trademark) manufactured by NST Corporation, Patran (registered trademark) manufactured by MSC Software Co., Ltd., or Hyper mesh (registered trademark) manufactured by Altair can be used.

[0035] The minute elements of the above-mentioned analytical model are not particularly limited, and well-known elements such as solid elements, shell elements, and three-dimensional voxel elements can be used.

[0036] Boundary condition data such as material properties such as resin and fiber type, blend, PVT, viscosity, specific heat, and thermal conductivity, shape properties such as plate thickness and gate position, injection speed, valve opening and closing conditions, and molding conditions such as resin temperature are input, and analysis conditions are set in the analysis condition setting unit 132. Then, in the flow analysis unit 133, a flow analysis is performed to analyze the behavior of the resin when the material is injected into the cavity. By the flow analysis, various data including information on the flow speed of the resin for each minute element can be obtained. In this specification, the term "flow speed" is synonymous with "flow speed" and is used as a concept including both the speed and direction of the flow. As the analysis condition setting unit 132 and the flow analysis unit 133, for example, injection molding CAE software such as Polyflow by Ansys and 3D TIMON (registered trademark) by Toray Engineering D Solutions Co., Ltd. can be used.

[0037] The fiber orientation tensor calculation unit 134 (fiber orientation calculation unit) calculates a fiber orientation tensor indicating the orientation of the fibers based on the flow velocity of the molten resin calculated by the flow analysis unit 133 and a fiber orientation prediction equation. As the fiber orientation tensor calculation unit 134, for example, a fiber orientation analysis solver such as 3D TIMON (registered trademark)-FIBER, 3D TIMON (registered trademark)-DFS, 3D TIMON (registered trademark)-CompositePRESS (registered trademark), or 3D TIMON (registered trademark)-3DCS manufactured by Toray Engineering D Solutions Co., Ltd. can be used.

[0038] The fiber content calculation unit 135 calculates the fiber content based on the fiber orientation tensor calculated by the fiber orientation tensor calculation unit 134 and a fiber content prediction equation described later. The fiber content calculation unit 135 can be based on the above-mentioned fiber orientation analysis solver or the like.

[0039] <Injection molded products> The injection molded product to be analyzed is not particularly limited, but examples thereof include automobile parts, rockets, aircraft parts, sporting goods, etc. Preferably, the injection molded product is a plate-shaped injection molded product such as an interior or exterior member of a vehicle.

[0040] The resin is not particularly limited and may be any known resin, specific examples of which include polypropylene resin, polycarbonate resin, polyester resin, polyamide (PA) resin, etc. These resins may be used alone or in a mixture of two or more. The fibers are not particularly limited and may be any known fiber, specific examples of which include glass fiber, carbon fiber, cellulose nanofiber, etc. These fibers may be used alone or in a mixture of two or more. The fiber diameter, fiber length, etc. are not particularly limited and may be generally used conditions. The fiber content in the entire molded product, i.e., the initial content G in the molding material, 0Although not intended to be limited, it can be, for example, 1% by mass or more and 50% by mass or less, and from the viewpoint of improving the prediction accuracy of the fiber content distribution described later, it can be preferably 2% by mass or more and 45% by mass or less, more preferably 5% by mass or more and 40% by mass or less. In addition, although not intended to be limited, this prediction method can be suitably applied to a high concentration suspension defined by C>D / L when, for example, C is the fiber volume concentration, L is the fiber length, D is the fiber diameter, and the fiber length distribution is uniform. For example, under the condition of a fiber length of 0.5 mm and a fiber diameter of 18 μm in the analysis described later, it can be applied under the condition that the fiber content is 7.1% by mass or more in terms of mass content. In addition, the molded product may contain additives such as fillers, pigments, dyes, impact modifiers, UV absorbers, etc., of about 5% by mass, from the viewpoint of improving moldability, strength, design, functionality, etc. These additives can be added alone or in combination.

[0041] <Method for predicting fiber content distribution> 2 is a flowchart showing the steps of implementing the method for predicting fiber content distribution in a fiber-reinforced plastic molded product (hereinafter also referred to as the "prediction method") according to the present disclosure. The prediction method is a method for predicting fiber content distribution by computer simulation, and includes an analysis model creation step S1, an analysis condition setting step S2, a flow analysis step S3, a fiber orientation tensor calculation step S4 (fiber orientation calculation step), a fiber content calculation step S5, and a repeat step S6.

[0042] First, in the analysis model creation step S1, as described above, the analysis model creation unit 131 divides the shape data of the cavity of the mold created using 3D CAD or the like into infinitesimal elements for numerical analysis to create an analysis model.

[0043] Next, in the analysis condition setting process S2, boundary condition data such as material properties, shape properties, molding conditions, etc. are input to set the analysis conditions. Then, in the flow analysis process S3, a flow analysis is performed to calculate the resin flow velocity for each minute element and each minute time step.

[0044] Next, in the fiber orientation tensor calculation process S4, the fiber orientation tensor is calculated for each infinitesimal element and each infinitesimal time step based on the resin flow velocity data obtained from the flow analysis and the fiber orientation prediction equation.

[0045] The fiber orientation prediction formula is not particularly limited, and a generally known model can be used. Specifically, for example, the fiber orientation prediction formula predicts the fiber orientation state using the Folgar-Tucker model (hereinafter also referred to as the "FT model") shown in the following formula (3).

[0046]

number

[0047] Also, for example, an improved model of the FT model, represented by the above formula (2), may be adopted as the fiber orientation prediction formula. The improved model of formula (2) includes a second interference term that considers the influence of elongational flow in addition to a first interference term that considers the influence of shear flow on the interference between fibers. This allows the influence of shear flow and the influence of elongational flow on the interference between fibers to be considered independently. Also, the interference term of the FT model is set based on the assumption that the stronger the interference between fibers, the closer the fiber orientation is to a random orientation, whereas in the improved model of formula (2), the first interference term is set based on the shear flow orientation A where the fibers show the first orientation due to the influence of the shear flow. 11 The second interaction term of the improved model is expressed so as to converge to the convergence value C1. In addition, the second interaction term of the improved model is the orientation A of the elongational flow (expansion flow) in which the fiber orientation shows the second orientation due to the expansion flow, which is a flow in which the flow velocity decreases as the flow of the molten resin progresses. 11 The convergence value C2 is expressed as convergence, and the orientation of the fiber shows the third orientation due to the contraction flow in which the flow velocity increases. 11 It is expressed so as to converge to the convergence value C3. This enables prediction of fiber orientation based on the actual phenomenon, and further improves the prediction accuracy of fiber orientation distribution.

[0048] Next, in the fiber content calculation process S5, the fiber content is calculated for each micro element and each micro time step based on the fiber orientation tensor calculated in the fiber orientation tensor calculation process S4 and the fiber content prediction equation described below.

[0049] The flow analysis step S3, the fiber orientation tensor calculation step S4, and the fiber content calculation step S5 are repeated until the filling of the material into the cavity is completed (repetition step S6). Then, the fiber content distribution of the molded product is obtained from the finally obtained fiber content.

[0050] [Fiber content calculation process] The prediction method according to this embodiment is characterized in that the fiber orientation prediction equation for calculating the fiber content in the fiber content calculation step S5 is a model in which the fiber content decreases as the fiber orientation tensor approaches a predetermined value (predetermined orientation) at least in the portion other than the skin layer, i.e., the core layer.

[0051] An example of such a model is given by the following formula (1).

[0052] Y = aX + b (1) however, a=a 1 <0, b=b 1 (0≦X≦c) a=a 2 >0, b=b 2 (c <X≦1) a 1 =d a1 G 0 +f a1 b 1 =d b1 G 0 +f b1 a 2 =d a2 G 0 +f a2 b 2 =d b2 G 0 +f b2 In equation (1), X is the fiber orientation tensor, Y is the fiber content, c is a given value of the fiber orientation tensor, a is the slope, b is the intercept, a 1 is the first slope, b 1 is the first intercept, a 2 is the second slope, b 2 is the second intercept, G 0 is the initial content, and d a1 , f a1 , d b1 , f b1 , d a2 , f a2 , d b2 and f b2 is a constant calculated based on the actual measured value.

[0053] Details will be described below with reference to Figures 3 to 16. Note that, in the following description, a case where a plate-shaped molded product is used as the injection molded product will be described as an example, but the prediction method according to the present disclosure can also be applied to molded products other than plate-shaped products.

[0054] In this specification, the direction of flow of the molten resin is called the MD direction, the thickness direction is called the ND direction, and the direction perpendicular to the flow direction and thickness direction is called the TD direction. In the analysis, the MD direction, TD direction, and ND direction are the x-axis, y-axis, and z-axis, respectively (see Figure 14).

[0055] -Actual measured fiber content- Here, when the measured values ​​of the fiber content are examined, the following is found.

[0056] Fig. 3 shows the average fiber content (mass%) in the plate thickness at the positions indicated by the symbols B1 to B8 (see Fig. 14) obtained in an experiment of Reference Example 2 described later. The initial content was set to 40 mass%, and three test pieces TP1 were prepared for each plate thickness and each resin, and the experiment was performed.

[0057] As shown in FIG. 3, in both the center region (reference symbols B1-B4) and the side region (reference symbols B5-B8), the fiber content tended to increase at the end portion (reference symbols B4, B8) of the test piece TP1, regardless of the plate thickness of the test piece TP1 and the MFR (viscosity) of the resin. The range represented by the difference between the maximum and minimum values ​​of the fiber content in the same test piece was 4.1-10.6 mass%. The range indicates that the larger the value, the higher the non-uniformity in the fiber content distribution in the same test piece. The range of 10.6 mass% corresponds to a difference of 45% and 14.6% in the bending stiffness and bending strength of the molded product, respectively. That is, from the test results in FIG. 3, it can be seen that the fibers are distributed non-uniformly to some extent in the molded product, and that predicting the fiber content distribution is important in predicting stiffness and strength.

[0058] The upper part of Fig. 4 is a graph of the results of Fig. 3, for resin A-2 and plate thickness 3.5 mm. The range was 5.99 mass%. In contrast, in the analysis of Analysis Example 1 (conventional example) described later, when the fiber content (average plate thickness) at the positions of symbols A2, A4, A5, and A8 to A12 corresponding to symbols B1 to B4 in Reference Example 2 was calculated using commercially available software, the range was 0.15 mass%. Thus, in the actual phenomenon, a certain degree of non-uniformity was confirmed in the fiber content distribution within the same test piece, whereas in the conventional technology, the predicted result was that the fibers were distributed almost uniformly within the molded product, and it was found that there was a large difference between the predicted and actual values.

[0059] Figure 5 shows an X-ray CT image of the position indicated by the symbol A6 in the test piece TP1 of resin A-1 and plate thickness 3.5 mm obtained in the experiment of Reference Example 1, and the fiber content of each layer. As shown in Figure 5, it was found that there is a tendency for fibers to be present in greater amounts in the core layer than in the skin layer, and that this tendency becomes stronger as the fiber length becomes longer. In addition, experiments by the inventors of the present application have revealed that the fibers contained in the core layer are mainly TD-oriented.

[0060] From the results of Figures 3 to 5, the following hypothesis can be made: That is, as shown in Figure 6, it can be considered that the content increases when the fibers are oriented in a certain specific orientation, such as TD orientation or MD orientation, while the content decreases in a random orientation where the fibers are not oriented in a specific direction.

[0061] FIG. 7 is a graph showing the relationship between the fiber content (mass ratio, average thickness) at the positions indicated by symbols B1 to B8 in Reference Example 2 and the deviation from 0.5 (absolute value of difference when 0.5 is subtracted from the value of the fiber orientation tensor) of the average thickness (average value of the fiber orientation tensor of 18 layers) of the fiber orientation tensor at the positions indicated by symbols A2, A4, A5, A8 to A12 obtained in the experiment of Reference Example 1. The initial content is 40 mass%. As shown in FIG. 7, the larger the deviation of the fiber orientation tensor, that is, the stronger the tendency to align to a specific orientation, the higher the fiber content, and the smaller the deviation, that is, the stronger the tendency to random orientation, the lower the fiber content. The result in FIG. 7 means that the hypothesis in FIG. 6 is correct.

[0062] For further verification, the relationship between fiber orientation and content was examined using the method shown in Fig. 8. Specifically, the measured values ​​of the fiber orientation tensor of each layer of Reference Example 1 and the measured values ​​of the fiber content (mass ratio) of each layer of Reference Example 1 were combined to graph the relationship between the measured values ​​of the fiber orientation tensor of each layer and the measured values ​​of the fiber content.

[0063] FIG. 9 shows the relationship between the measured fiber orientation tensor and the measured fiber content of each layer at the positions of reference symbols A1 to A3 and A5 to A8 in Reference Example 1, which is graphed by the method shown in FIG. 8. As shown in FIG. 9, the fiber content increases as the fibers are aligned in a specific direction, that is, as the fiber orientation tensor approaches 0 or 1, and the fiber content decreases as the fiber orientation tensor approaches the vicinity of random orientation (for example, the fiber orientation tensor is 0.4 to 0.7), which is a so-called V-shaped tendency. FIG. 9 shows the results of changing the plate thickness and the type of resin, but all of them show almost the same V-shaped tendency, and it is considered that the influence of the plate thickness and the MFR of the resin on the V-shaped tendency is small. Note that the skin layer (especially the 1st layer L1 and the 18th layer L18, see FIG. 15) does not follow the V-shaped tendency and tends to have a low fiber content.

[0064] Figure 10 is a graph similar to Figure 9, showing the results when the fiber length was changed for resin A-1 and plate thickness of 3.5 mm. As shown in Figure 10, the change in fiber length is not thought to have a significant effect on the V-shaped tendency described above.

[0065] Figure 11 is a graph similar to Figures 9 and 10, showing the results when the initial content was changed for resin A-1, plate thickness 3.5 mm, and fiber length 10 mm. As can be seen from Figure 11, as the initial content increases, the V-shaped tendency, that is, the tendency for the fiber content to decrease as the fiber orientation approaches the random orientation vicinity, becomes more pronounced.

[0066] In each graph of Fig. 11, upon further examination, it was found that in the experiment of Reference Example 1, the fiber orientation tensor with the most significant decrease in fiber content was approximately 0.65. Also, when fitting the measured values in the range where the fiber orientation tensor is between 0 and 0.65, it becomes like the dashed line. By calculating the slope and intercept of the straight line represented by the dashed line, the results shown in Fig. 12(a) were obtained. When plotting the calculated values of the slope and intercept against the initial content, the graphs in Figs. 12(b) and (c) are obtained respectively. By performing fitting, approximate equations of y = -0.005x + 0.0169 and y = 0.011x + 0.0121 are obtained respectively. Thus, it is considered that the above slope and intercept, that is, the sensitivity of fiber orientation to fiber content, are in a proportional relationship with the initial content.

[0067] -Fiber Content Prediction Equation in this Prediction Method- Based on the results of Figs. 11 and 12, the fiber content prediction equation was formulated as the above-mentioned equation (1).

[0068] Specifically, Fig. 13 is a graph schematically showing the fiber content prediction equation of equation (1). As shown in Fig. 11, it is considered that there is a value of a predetermined fiber orientation tensor where the fiber content decreases most significantly in the V-shaped trend. Let the predetermined fiber orientation tensor where the fiber content decreases most significantly be c. Then, in the range of 0 ≤ X ≤ c, the prediction equation is a straight line with a negative first slope a 1 and a first intercept b 1 ; in the range of c < X ≤ 1, it can be modeled as a straight line with a positive second slope a 2 and a second intercept b 2 .

[0069] And these first slope a 1 , first intercept b 1 , second slope a 2 and second intercept b 2 can be calculated as values in a proportional relationship with the initial content G 0 as shown in Fig. 12.

[0070] Based on the measured values ​​of Reference Example 1, particularly the results calculated in the same manner as in FIGS. 11 and 12, the following specific examples of formula (1) are given: c=0.65, d a1 =-0.005206, f a1 =0.018922, d b1 =0.0117661, f b1 =0.004254, d a2 =0.0125, f a2 =0, d b2 =0.00036, f b2 = 0, the following formula is obtained. In this case, the unit of fiber content Y is mass ratio, and the initial content G 0 The unit is mass%.

[0071] Y = aX + b (1') however, a=a 1 <0, b=b 1 (0≦X≦0.65) a=a 2 >0, b=b 2 (0.65 <X≦1) a 1 =-0.005206G 0 +0.018922 b 1 =0.0117661G 0 +0.004254 a 2 =0.0125G 0 b 2 =0.00036G 0 In this way, by using a fiber content prediction formula formulated based on actual phenomena, it is possible to accurately predict the fiber content distribution with a simple model. In particular, formula (1) is 0 Since the fiber content can be predicted based on the information on the fiber orientation tensor and the fiber orientation tensor, it is possible to improve the prediction accuracy while suppressing an increase in the calculation load using a simple model.

[0072] In addition, the predetermined value c in the fiber orientation tensor is preferably 0.4 to 0.7, more preferably 0.5 to 0.65. When the predetermined value c is 0.5 to 0.65, it can be considered that the orientation is roughly random.

[0073] In the measured values ​​of Reference Example 1, the fiber orientation tensor tended to have a low content, especially in the orientation in the above-mentioned numerical range. As described above, it is considered to mean that when fibers are present in a space of the same volume, many fibers cannot exist unless the orientation of the fibers is aligned to a certain degree. By setting the predetermined value c in the above numerical range, it becomes possible to predict the content distribution using a fiber content prediction formula that is in line with the actual phenomenon, and the prediction accuracy is effectively improved.

[0074] <Program and its recording medium> Each step of the fiber content distribution prediction method described above is programmed. That is, the program according to this embodiment is a program for causing a computer to execute at least the procedure of the fiber content calculation step S5 described above, and is characterized in that the above-mentioned formula (1) is used as the fiber content prediction formula. This program can be executed by the processor 130 in a state stored in the storage unit 120. Moreover, the program is not limited to being stored in the storage unit 120, and can be recorded in various well-known computer-readable recording media 170, such as optical disk media and magnetic tape media. Then, the program can be executed by loading such a recording medium into the reading unit 160 and reading out the program.

[0075] <Other embodiments> In the above embodiment, the fiber orientation tensor substituted into the fiber content prediction equation is a predicted value calculated based on the flow velocity obtained as a result of flow analysis and the fiber orientation prediction equation, but this is not limited to the above configuration.

[0076] The fiber orientation tensor substituted into the fiber content prediction equation may be an experimental value experimentally obtained in advance, for example, by the experiment of the reference example described later.

[0077] <Experimental Example> Next, specific examples will be described.

[0078] [Reference example] FIG. 14(a) shows a test piece TP1 used in the experiment of the reference example and its shape model.

[0079] The test piece TP1 is a plate with a width of 100 mm and a length of 190 mm, and is L-shaped with a right angle (R15 mm) bent at approximately 80 mm in length (the bent part is indicated by dotted hatching in the shape model at the bottom of Figure 14(a)). There were three types of plate thickness: 1.5 mm, 2.5 mm, and 3.5 mm. The test piece TP1 was actually manufactured by injection molding under the following other conditions. (A) Resin: Polypropylene resin (A-1) Novatec (registered trademark) PP, SA08A (MFR: 75g / 10min) manufactured by Japan Polypropylene Corporation (A-2) Prime Polymer polypropylene resin J107G (MFR: 30g / 10min) (A-3) Maleic acid modified polypropylene (used as the base resin for glass fiber-containing pellets, with a content of 4% by mass in the material (total of resin and fiber) (B) Fiber: Pellets containing glass fibers E-glass (average fiber diameter 18μm) manufactured by Nitto Boseki Co., Ltd. Fiber length: 0.5mm, 10mm Fiber content in the material (total of resin and fiber): 1.5 mass%, 10 mass%, 20 mass%, 30 mass%, 40 mass% (C) Molding conditions Resin temperature 200℃ Mold temperature: 40℃ Injection time 0.2 seconds (average flow velocity 900mm / s) -Reference example 1- As shown in the shape model of the lower test piece TP1 in Fig. 14(a), a sample of about 3.5 mm square was cut out at the positions indicated by symbols A1 to A12. For this sample, an X-ray CT device (3D CT X-ray microscope manufactured by Rigaku Corporation) was used to take X-ray CT images of each layer L1 to L18 (see Fig. 15) divided into 18 layers in the plate thickness direction, similar to the analysis model of the analysis example described later. From the obtained X-ray CT images, the fiber orientation tensor and fiber content of each layer L1 to L18 were calculated using image analysis software (Avizo manufactured by ThermoFisher SCIENTIFIC Co., Ltd.) and used as the measured value data of Reference Example 1.

[0080] -Reference example 2- Samples of about 20 mm square were cut out from the positions indicated by symbols B1 to B8 of the test piece TP1. The resin of the samples was incinerated in an electric furnace to obtain glass fibers, and the number of fibers was counted to determine the fiber content throughout the plate thickness relative to the mass of the sample. The measured data of Reference Example 2 was obtained.

[0081] [Analysis example] FIG. 14(b) shows the test piece TP2 used in the CAE analysis of the analysis example and its analytical model.

[0082] The test piece TP2 is a straight-shaped version of the test piece TP1 in order to simplify the calculation process. The plate thickness was 3.5 mm. The shape data of the test piece TP2 was divided into 18 layers in the thickness direction as shown in Fig. 15, and each layer was divided into three-dimensional voxel elements of a cube (length 1 mm × width 1 mm × thickness 0.194 mm) to create an analysis model. Note that each element shown in Fig. 14 and Fig. 15 is shown diagrammatically and does not accurately reflect the actual element size.

[0083] Among the conditions shown in the above reference example, A-1 was used as the resin, the plate thickness was 3.5 mm, and the initial resin content in the material was 40 mass%. Flow analysis was performed when the material was injected into the cavity. The flow analysis was performed using 3D TIMON (registered trademark, manufactured by Toray Engineering D Solutions Co., Ltd.).

[0084] -Analysis example 1 (conventional example)- Using the information obtained from the flow analysis, the fiber content and the average sheet thickness of each layer L1 to L18 at the positions indicated by symbols A2, A4, A5, A8 to A12 of the analysis model were calculated. The fiber content was calculated using 3D TIMON (registered trademark, manufactured by Toray Engineering D Solutions Co., Ltd.)-DFS. The results are shown in FIG. 4.

[0085] As described above, in the conventional example, the range was 0.15 mass %, and the result was that the non-uniformity of the fiber content distribution in the molded product could not be adequately predicted.

[0086] -Analysis example 2 (Verification example of this prediction method)- Among the measured values ​​of the fiber orientation tensor of Reference Example 1, the measured values ​​at the positions indicated by symbols A2, A4, A5, A8 to A12 of the analysis model were input as X in the above formula (1') to obtain predicted values. A graph plotting the predicted values ​​and the measured values ​​of the fiber orientation tensor of Reference Example 2 is shown in FIG.

[0087] As shown in Figure 16, the above formula (1'), which was formulated based on actual measurements, largely reproduces the tendency for the content to increase toward the ends of the test piece. In addition, the range also shows closer values ​​than analysis example 1, and it is believed to be able to predict to some extent the actual phenomenon in which fibers are distributed unevenly depending on the part of the molded product. This suggests that the use of formula (1') can improve the accuracy of predicting fiber content distribution. [Industrial Applicability]

[0088] The present disclosure is extremely useful because it can provide a fiber content distribution prediction method and fiber content distribution prediction device for fiber-reinforced plastic molded products that can improve the prediction accuracy of fiber content distribution using a simple model, a program for causing a computer to execute the fiber content distribution prediction method, and a computer-readable recording medium having the program recorded thereon. [Explanation of symbols]

[0089] 100 Fiber content distribution prediction device 134 Fiber orientation tensor calculation part (Fiber orientation calculation part) 135 Fiber content calculation section S4 Fiber orientation tensor calculation process (fiber orientation calculation process) S5 Fiber content calculation process

Claims

1. A method for predicting the fiber content distribution in a fiber-reinforced resin injection molded product by computer simulation, comprising: A fiber content calculation step of calculating the fiber content based on the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

2. In claim 1, The orientation is expressed by a fiber orientation tensor in which the flow direction of the molten resin is 1 and the direction perpendicular to the flow direction is 0. A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

3. In claim 2, The predetermined orientation is an orientation in which the fiber orientation tensor is 0.4 or more and 0.7 or less. A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

4. In claim 2 or 3, The fiber content prediction formula for the portion other than the skin layer is represented by the following formula (1): A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product. Y=aX+b...(1) however, a=a 1 <0, b=b 1 (0≦X≦c) a=a 2 >0, b=b 2 (c<X≦1) a 1 = d a1 G 0 +f a1 b 1 = d b1 G 0 +f b1 a 2 = d a2 G 0 +f a2 b 2 = d b2 G 0 +f b2 In formula (1), X is the fiber orientation tensor, Y is the fiber content, c is a predetermined value of the fiber orientation tensor, a is the slope, b is the intercept, a 1 is the first slope, b 1 is the first intercept, a 2 is the second slope, b 2 is the second intercept, G 0 is the initial content, and d a1 , f a1 , d b1 , f b1 , d a2 , f a2 , d b2 and f b2 is a constant calculated based on the actual measurement value.

5. In claim 1 or 2, The predetermined orientation is a random orientation. A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

6. In claim 1 or 2, A fiber orientation calculation step of calculating the orientation of the fibers based on a flow rate of the molten resin and a fiber orientation prediction formula consisting of a modified Folgar-Tucker model, prior to the fiber content calculation step; The fiber orientation prediction formula includes a term that takes into account the influence of an elongation flow, which is a flow whose flow speed changes in the flow direction of the molten resin, as a term that takes into account the interference between the fibers. A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

7. In claim 6, The fiber orientation prediction formula is represented by the following formula (2): A method for predicting the fiber content distribution of a fiber-reinforced plastic molded product. [0010]

8. An apparatus for predicting the fiber content distribution contained in a fiber-reinforced resin injection molded product by computer simulation, comprising: A fiber content calculation unit is provided that calculates the fiber content based on the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. A fiber content distribution prediction device for a fiber reinforced plastic molded product.

9. A program for predicting the fiber content distribution in a fiber-reinforced resin injection molded product by computer simulation, The method causes a computer to execute a procedure of calculating the fiber content based on at least the fiber orientation and a fiber content prediction formula, The fiber content prediction formula is a model in which the content decreases as the orientation of the fibers approaches a predetermined orientation. A program for predicting the fiber content distribution of a fiber-reinforced plastic molded product.

10. A computer-readable recording medium having recorded thereon the program for predicting the fiber content distribution of a fiber-reinforced resin molded product according to claim 9.

Citation Information

Patent Citations

  • Manufacture of fiber reinforced resin gear by injection molding

    JP1989011810A

  • Structural analysis method, structural analysis apparatus, structural analysis program, physical property calculation method for structural analysis, physical property calculation apparatus for structural analysis, and physical property calculation program for structural analysis

    JP2010069654A

  • A method and apparatus for describing the statistical orientation distribution of particles in the simulation of a mold filling process.

    JP2010531752A

  • Method for simulating behavior of filler, and method for analyzing physical property of composite material

    JP2014226871A

  • Method, device, program, and recording medium for predicting fiber orientation condition of fiber reinforced resin molded article

    JP2022118541A

Cited By

  • Forming method of composite material special-shaped yacht cab

    CN120985955A